A welding process for multiple cables in parallel

The welding process of multiple cables side by side solves the problem of cable friction damage when the tank chain is fixed, achieves independent movement and long life of the cables, improves production efficiency and safety, and simplifies the troubleshooting and cleaning process.

CN114388198BActive Publication Date: 2024-10-11SHENZHEN HAIHONGXIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210130522.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-11
Publication Date
2024-10-11
Estimated Expiration
2042-02-11

AI Technical Summary

Technical Problem

In the prior art, multiple cables are easily damaged due to friction when being fixed by tank chains during use, affecting safety and production efficiency.

Method used

Multiple cables are used side by side and the welding process is used, including cable grinding, arrangement, glue injection, preliminary compaction, vulcanization heating, cooling, seam filling and flat glue air drying, etc. The cables are welded together through welding glue to form Independent moving tank chain structure to avoid friction damage.

Benefits of technology

It effectively increases the service life of cables and equipment safety, saves production time for sorting cables, improves production efficiency, simplifies terminal problem troubleshooting, prevents dust residue, and improves performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a welding process for using a plurality of cables in parallel, and the process comprises the following steps: S1, cable polishing, deburring and polishing the outer walls of a plurality of cables to make the outer walls of the cables smooth and neat, S2, cable arrangement, arranging the plurality of polished cables obtained in step S1 and arranging them into a whole row structure, S3, cable glue injection, injecting welding glue into the joints between the neatly arranged cables in step S2, and through this welding process, a single or a plurality of disordered cables can be welded together through glue and welding process for side-by-side use, so that the plurality of cables can get rid of the restraint of the tank chain when in use, and avoid friction generated during the movement of the tank chain, resulting in the generation of foreign matter, affecting the product yield, and the abrasion of the wires and cables during the movement, resulting in poor equipment shutdown and affecting production, thereby improving the use effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a welding process for using a plurality of cables in parallel, belonging to the technical field of using a plurality of cables. Background Art

[0002] Cable is a general term for items such as optical cables and electrical cables. Cables have many uses, mainly used for controlling installation, connecting equipment, transmitting electricity and other multiple functions. They are common and indispensable in daily life. Since cables are charged, installation requires special caution. Cables are mainly made of PVC plastic particles, sheath insulation and various specifications of copper wires twisted into cables. Existing cables will use multiple cables at the same time when in use. When multiple cables are in use, they need to be fixed uniformly. The existing technology is to fix multiple cables by using tank chains so that the movement of the cables follows the tank chains. However, when this method is actually used, the inner wall of the tank chain will rub against the internal cables during movement. After long-term use, foreign matter is easy to be generated inside it. At the same time, the cables are easy to be damaged after long-term friction, affecting the safety of use. Summary of the invention

[0003] The purpose of the present invention is to solve the above-mentioned shortcomings and provide a welding process for using multiple cables side by side.

[0004] A welding process is used to weld multiple cables side by side, the process comprising the following steps:

[0005] S1, cable polishing, deburring and polishing the outer walls of several cables to make the outer walls of the cables smooth and neat;

[0006] S2, cable arrangement, arranging the plurality of polished cables obtained in step S1 and arranging them into a row structure;

[0007] S3, cable glue injection, injecting welding glue into the joints between the neatly arranged structural cables obtained in step S2;

[0008] S4, preliminary compaction, using an external pressurizing tool or manually compacting the glue at the joints between two adjacent cables after the cables are injected with glue in step S3;

[0009] S5, vulcanization preheating, turn on the hot vulcanization welding machine, and preheat the hot vulcanization welding machine;

[0010] S6, cable placement, placing the cable arrangement structure obtained in step S4 and subjected to preliminary compaction in hot vulcanization welding;

[0011] S7, vulcanization heating, the hot vulcanization welding machine vulcanizes and heats the placed cable arrangement structure, so that the injection joints are vulcanized and bonded with rubber;

[0012] S8, cable cooling, cooling the vulcanized and bonded arranged cables obtained in step S7 to achieve a molding effect at room temperature;

[0013] S9, filling the seams, injecting glue into the seams of the arranged cables after cooling in step S8 to fill the gaps, so that the seams are flush with the height of the cables;

[0014] S10, air-drying the flat glue, placing the cable injected with the flat glue obtained in step S9 under room temperature for air-drying and forming, so as to form a tank chain cable structure.

[0015] Preferably, in step S1, the cable is polished using a deburring device, the motor speed of the deburring device is not less than 3500 r / min, and the polishing time of each cable is not less than 3 min.

[0016] Preferably, when the cable is injected with glue in step S3, the viscosity of the welding glue is not less than 60000C.PS, the solid content is not more than 34%, the temperature range after curing is between -50°C and +260°C, the complete curing time is not more than 24H at room temperature, and the bonding gap is not more than 0.05mm.

[0017] Preferably, in step S4, when the welding glue is being compacted and fitted, glue may be squeezed out and the squeezed welding glue needs to be cleaned.

[0018] Preferably, in step S7, the heating temperature of the hot vulcanization welding machine is not less than 150° C., and the heating time is not less than 10 minutes.

[0019] Preferably, in step S8, the cable cooling time is not less than 8 minutes.

[0020] Preferably, in S9, the height of the filling glue is flush with the height of the entire row of cables, the total height difference is no more than 1 mm, and the height difference between two adjacent cable gaps is no more than 0.5 mm.

[0021] Preferably, in step S10, the normal temperature environment is in the range of 15-28° C., and the normal temperature environment is a windless environment.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present process is a welding process for using multiple cables side by side. Through this welding process, a single or multiple disordered cables can be welded together through glue and welding process for side-by-side use, so that multiple cables can get rid of the constraints of the tank chain when in use, avoid friction during the movement of the tank chain, which leads to the generation of foreign matter, affecting the product yield, and the wear of the wires and cables during the movement, causing equipment to shut down and affect production, thereby improving the use effect. The cables welded by this process can move independently after being welded side by side. No foreign matter is generated during the movement, and they are not damaged by friction. The service life of the cables and the safety of the equipment are effectively increased. A lot of production time for arranging the cables in the tank chain is saved during production and use, and production efficiency is improved. It is simple and convenient for the end user to troubleshoot problems, and by filling the joints between the cables, dust residue can be effectively prevented, which is convenient for cleaning and has good performance. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] A welding process is used to weld multiple cables side by side, the process comprising the following steps:

[0026] S1, cable polishing, deburring and polishing the outer walls of several cables to make the outer walls of the cables smooth and neat;

[0027] S2, cable arrangement, arranging the plurality of polished cables obtained in step S1 and arranging them into a row structure;

[0028] S3, cable glue injection, injecting welding glue into the joints between the neatly arranged structural cables obtained in step S2;

[0029] S4, preliminary compaction, using an external pressurizing tool or manually compacting the glue at the joints between two adjacent cables after the cables are injected with glue in step S3;

[0030] S5, vulcanization preheating, turn on the hot vulcanization welding machine, and preheat the hot vulcanization welding machine;

[0031] S6, cable placement, placing the cable arrangement structure obtained in step S4 and subjected to preliminary compaction in hot vulcanization welding;

[0032] S7, vulcanization heating, the hot vulcanization welding machine vulcanizes and heats the placed cable arrangement structure, so that the injection joints are vulcanized and bonded with rubber;

[0033] S8, cable cooling, cooling the vulcanized and bonded arranged cables obtained in step S7 to achieve a molding effect at room temperature;

[0034] S9, filling the seams, injecting glue into the seams of the arranged cables after cooling in step S8 to fill the gaps, so that the seams are flush with the height of the cables;

[0035] S10, air-drying the flat glue, placing the cable injected with the flat glue obtained in step S9 under room temperature for air-drying and forming, so as to form a tank chain cable structure.

[0036] As an optimization technical solution of the present invention, in step S1, the cable is polished using a deburring device, the motor speed of the deburring device is not less than 3500r / min, and the polishing time of each cable is not less than 3min.

[0037] As an optimized technical solution of the present invention, when the cable is injected with glue in step S3, the viscosity of the welding glue is not less than 60000C.PS, the solid content is not more than 34%, the temperature range after curing is between -50°C and +260°C, the complete curing time is not more than 24H at room temperature, and the bonding gap is not more than 0.05mm.

[0038] As an optimization technical solution of the present invention, in the step S4, when the welding glue is being compacted and fitted tightly, glue is squeezed out and the squeezed welding glue needs to be cleaned.

[0039] As an optimization technical solution of the present invention, in step S7, the heating temperature of the hot vulcanization welding machine is not less than 150° C., and the heating time is not less than 10 minutes.

[0040] As an optimization technical solution of the present invention, in step S8, the cable cooling time is not less than 8 minutes.

[0041] As an optimization technical solution of the present invention, in S9, the height of the filling glue is flush with the height of the entire row of cables, the total height difference is no more than 1 mm, and the height difference between two adjacent cable gaps is no more than 0.5 mm.

[0042] As an optimization technical solution of the present invention, in step S10, the normal temperature environment temperature range is between 15-28° C., and the normal temperature environment is a windless environment.

[0043] Embodiment 1:

[0044] A welding process is used to weld multiple cables side by side, the process comprising the following steps:

[0045] S1, cable polishing, deburring and polishing the outer walls of several cables to make the outer walls of the cables smooth and neat;

[0046] S2, cable arrangement, arranging the plurality of polished cables obtained in step S1 and arranging them into a row structure;

[0047] S3, cable glue injection, injecting welding glue into the joints between the neatly arranged structural cables obtained in step S2;

[0048] S4, preliminary compaction, using an external pressurizing tool or manually compacting the glue at the joints between two adjacent cables after the cables are injected with glue in step S3;

[0049] S5, vulcanization preheating, turn on the hot vulcanization welding machine, and preheat the hot vulcanization welding machine;

[0050] S6, cable placement, placing the cable arrangement structure obtained in step S4 and subjected to preliminary compaction in hot vulcanization welding;

[0051] S7, vulcanization heating, the hot vulcanization welding machine vulcanizes and heats the placed cable arrangement structure, so that the injection joints are vulcanized and bonded with rubber;

[0052] S8, cable cooling, cooling the vulcanized and bonded arranged cables obtained in step S7 to achieve a molding effect at room temperature;

[0053] S9, filling the seams, injecting glue into the seams of the arranged cables after cooling in step S8 to fill the gaps, so that the seams are flush with the height of the cables;

[0054] S10, air-drying the flat glue, placing the cable injected with the flat glue obtained in step S9 under normal temperature for air-drying and forming, so as to form a tank chain cable structure.

[0055] In this embodiment, the cable is polished using a deburring device in step S1, the motor speed of the deburring device is not less than 3500 r / min, and the polishing time of each cable is not less than 3 minutes.

[0056] In this embodiment, when the cable is injected with glue in step S3, the viscosity of the welding glue is not less than 60000C.PS, the solid content is not more than 34%, the temperature range after curing is between -50°C and +260°C, the complete curing time is not more than 24H at room temperature, and the bonding gap is not more than 0.05mm.

[0057] In this embodiment, in step S4, when the welding glue is being compacted and adhered, glue is squeezed out and the squeezed welding glue needs to be cleaned.

[0058] In this embodiment, in step S7, the heating temperature of the hot vulcanization welding machine is not less than 150° C., and the heating time is not less than 10 minutes.

[0059] In this embodiment, in step S8, the cable cooling time is not less than 8 minutes.

[0060] In this embodiment, in S9, the height of the filling glue is flush with the height of the entire row of cables, the total height difference is no more than 1 mm, and the height difference between two adjacent cable gaps is no more than 0.5 mm.

[0061] In this embodiment, in step S10, the normal temperature environment is in the range of 15-28° C., and the normal temperature environment is a windless environment.

[0062] Embodiment 2:

[0063] A welding process is used to weld multiple cables side by side, the process comprising the following steps:

[0064] S1, cable polishing, deburring and polishing the outer walls of several cables to make the outer walls of the cables smooth and neat;

[0065] S2, cable arrangement, arranging the plurality of polished cables obtained in step S1 and arranging them into a row structure;

[0066] S3, cable glue injection, injecting welding glue into the joints between the neatly arranged structural cables obtained in step S2;

[0067] S4, preliminary compaction, using an external pressurizing tool or manually compacting the glue at the joints between two adjacent cables after the cables are injected with glue in step S3;

[0068] S5, vulcanization preheating, turn on the hot vulcanization welding machine, and preheat the hot vulcanization welding machine;

[0069] S6, cable placement, placing the cable arrangement structure obtained in step S4 and subjected to preliminary compaction in hot vulcanization welding;

[0070] S7, vulcanization heating, the hot vulcanization welding machine vulcanizes and heats the placed cable arrangement structure, so that the injection joints are vulcanized and bonded with rubber;

[0071] S8, cable cooling, cooling the vulcanized and bonded arranged cables obtained in step S7 to achieve a molding effect at room temperature;

[0072] S9, filling the seams, injecting glue into the seams of the arranged cables after cooling in step S8 to fill the gaps, so that the seams are flush with the height of the cables;

[0073] S10, air-drying the flat glue, placing the cable injected with the flat glue obtained in step S9 under normal temperature for air-drying and forming, so as to form a tank chain cable structure.

[0074] In this embodiment, the cable is polished using a deburring device in step S1, the motor speed of the deburring device is not less than 3500 r / min, and the polishing time of each cable is not less than 3 minutes.

[0075] In this embodiment, when the cable is injected with glue in step S3, the viscosity of the welding glue is not less than 60000C.PS, the solid content is not more than 34%, the temperature range after curing is between -50°C and +260°C, the complete curing time is not more than 24H at room temperature, and the bonding gap is not more than 0.05mm.

[0076] In this embodiment, in step S4, when the welding glue is being compacted and adhered, glue is squeezed out and the squeezed welding glue needs to be cleaned.

[0077] In this embodiment, in step S7, the heating temperature of the hot vulcanization welding machine is not less than 150° C., and the heating time is not less than 10 minutes.

[0078] In this embodiment, in step S8, the cable cooling time is not less than 8 minutes.

[0079] In this embodiment, in S9, the height of the filling glue is flush with the height of the entire row of cables, the total height difference is no more than 1 mm, and the height difference between two adjacent cable gaps is no more than 0.5 mm.

[0080] In this embodiment, in step S10, the normal temperature environment is in the range of 15-28° C., and the normal temperature environment is a windless environment.

[0081] The present process is a welding process for using multiple cables side by side. Through this welding process, a single or multiple disordered cables can be welded together through glue and welding process for side-by-side use, so that multiple cables can get rid of the constraints of the tank chain when in use, avoid friction during the movement of the tank chain, which leads to the generation of foreign matter, affecting the product yield, and the wear of the wires and cables during the movement, causing equipment to shut down and affect production, thereby improving the use effect. The cables welded by this process can move independently after being welded side by side. No foreign matter is generated during the movement, and they are not damaged by friction. The service life of the cables and the safety of the equipment are effectively increased. A lot of production time for arranging the cables in the tank chain is saved during production and use, and production efficiency is improved. It is simple and convenient for the end user to troubleshoot problems, and by filling the joints between the cables, dust residue can be effectively prevented, which is convenient for cleaning and has good performance.

[0082] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A welding process for connecting multiple cables in parallel, characterized in that: The process includes the following steps: S1, cable polishing, deburring and polishing the outer walls of several cables to make the outer walls of the cables smooth and neat; S2, cable arrangement, arranging the plurality of polished cables obtained in step S1 and arranging them into a row structure; S3, cable glue injection, injecting welding glue into the joints between the neatly arranged structural cables obtained in step S2; S4, preliminary compaction, using an external pressurizing tool or manually compacting the glue at the joints between two adjacent cables after the cables are injected with glue in step S3; S5, vulcanization preheating, turn on the hot vulcanization welding machine, and preheat the hot vulcanization welding machine; S6, cable placement, placing the cable arrangement structure obtained in step S4 after preliminary compaction in hot vulcanization welding; S7, vulcanization heating, the hot vulcanization welding machine vulcanizes and heats the placed cable arrangement structure, so that the injection joints are vulcanized and bonded with rubber; S8, cooling the cables, cooling the arranged cables after vulcanization and bonding obtained in step S7, so that they can achieve a molding effect at room temperature; S9, filling the seams, injecting glue into the seams of the arranged cables after cooling in step S8 to fill the gaps, so that the seams are flush with the height of the cables; S10, air-drying the flat glue, placing the cable injected with the flat glue obtained in step S9 under room temperature for air-drying and forming to form a tank chain cable structure.

2. A welding process for connecting multiple cables in parallel according to claim 1, characterized in that: In the step S1, the cable is polished using a deburring device, the motor speed of the deburring device is not less than 3500 r / min, and the polishing time of each cable is not less than 3 minutes.

3. A welding process for connecting multiple cables in parallel according to claim 1, characterized in that: When the cable is injected with glue in step S3, the viscosity of the welding glue is not less than 6000 0C.PS, the solid content is not more than 34%, the temperature range after curing is between -50°C and +2 60°C, the complete curing time is not more than 24 hours at room temperature, and the bonding gap is not more than 0.05mm.

4. A welding process for connecting multiple cables in parallel according to claim 3, characterized in that: In the step S4, when the welding glue is being compacted and adhered, glue is squeezed out and the squeezed welding glue needs to be cleaned.

5. The welding process for connecting multiple cables in parallel according to claim 1, characterized in that: In step S7, the heating temperature of the hot vulcanizing welding machine is not less than 150° C., and the heating time is not less than 10 minutes.

6. A welding process for connecting multiple cables in parallel according to claim 1, characterized in that: In step S8, the cable cooling time is not less than 8 minutes.

7. A welding process for connecting multiple cables in parallel according to claim 1, characterized in that: In the above S9, the height of the filling glue is flush with the height of the entire row of cables, the total height difference is no more than 1 mm, and the height difference between two adjacent cable gaps is no more than 0.5 mm.

8. The welding process for connecting multiple cables in parallel according to claim 1, characterized in that: In step S10, the normal temperature environment has a temperature range of 15-28° C., and the normal temperature environment is a windless environment.