Solar cell manufacturing method and solar cell
By depositing and etching a borosilicate glass layer on the front side of a silicon substrate and then performing boron doping, the damage to the silicon substrate caused by the laser SE process is solved, simplifying the process flow, reducing costs, and improving the performance of solar cells.
Patent Information
- Application Number
- CN202111680754.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-12-30
AI Technical Summary
Existing laser SE processes damage the silicon substrate during the fabrication of selective emitter structures for solar cells, affecting minority carrier lifetime. Furthermore, these processes are complex, costly, and challenging.
The method involves depositing a borosilicate glass layer on the front side of a silicon substrate, then coating an etching paste within a pre-defined patterned area to etch away the borosilicate glass layer. Boron doping is then performed at a diffusion temperature to form a selective emitter structure, thus avoiding damage from high-temperature exposure and laser etching.
It improves minority carrier lifetime, reduces process complexity and cost, and enhances battery open-circuit voltage and conversion efficiency.
Smart Images

Figure CN114388658B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solar photovoltaic technology, and in particular to a solar cell preparation method and a solar cell. Background Art
[0002] TOPCon (Tunnel Oxide Passivated Contact) battery is a high-efficiency battery based on the principle of selective carriers. An ultra-thin silicon oxide layer is first prepared on the back, and then a silicon-doped layer is deposited to form a passivated contact structure on the back, which effectively reduces surface recombination and metal contact recombination and improves battery efficiency.
[0003] TOPCon cells can improve efficiency by stacking a boron SE (Selective Emitter) structure on the front. Under the boron SE structure on the front, the area where the front fine grid lines contact has low square resistance, high doping concentration, and low contact resistance, which can further improve the fill factor; other areas have high square resistance and low doping concentration, which can reduce surface recombination and improve optical response, thereby increasing open circuit voltage and short circuit to improve cell efficiency. Currently, laser SE process is commonly used to prepare SE structure.
[0004] However, the laser SE process causes damage to the silicon substrate, affecting the minority carrier lifetime, and the process is complex, costly, and difficult. Moreover, the laser SE process requires two boron diffusions, each at a high temperature of around 1000°C, affecting the life of the silicon substrate and thus the efficiency of the battery. Summary of the invention
[0005] The present invention provides a method for preparing a solar cell and a solar cell, aiming to reduce damage to a silicon substrate in the preparation process of a selective emitter structure, increase the minority carrier lifetime, simplify the process flow, thereby reducing costs, and increase the body life of the silicon substrate, thereby improving the efficiency of the cell.
[0006] In a first aspect of the implementation of the present invention, an embodiment of the present invention provides a method for preparing a solar cell, which may include:
[0007] providing a silicon substrate;
[0008] Depositing a borosilicate glass layer on the front side of the silicon substrate;
[0009] Coating an etching slurry in a preset graphic area on the front side of the silicon substrate to etch away the borosilicate glass layer in the graphic area;
[0010] The front side of the etched silicon substrate is subjected to boron doping at a diffusion temperature for a first process time to form a first boron doping concentration in the graphic region and a second boron doping concentration outside the graphic region on the silicon substrate.
[0011] Optionally, depositing a borosilicate glass layer on the front side of the silicon substrate comprises:
[0012] A borosilicate glass layer is deposited on the front side of the silicon substrate using a normal pressure chemical vapor deposition device based on a deposition source.
[0013] Optionally, the atmospheric pressure chemical vapor deposition equipment includes a preheating chamber, a reaction chamber, and a cooling chamber, and the use of the atmospheric pressure chemical vapor deposition equipment to deposit a borosilicate glass layer on the front side of the silicon substrate based on a deposition source includes:
[0014] The silicon substrate is transferred to the preheating chamber, and the silicon substrate is preheated at a temperature of 390° C. to 410° C.;
[0015] The silicon substrate is transferred into the reaction chamber, and a second process time is deposited on the front side of the silicon substrate based on the deposition source at a temperature of 590° C. to 610° C. to prepare a borosilicate glass layer;
[0016] The silicon substrate is transferred to the cooling chamber to cool the silicon substrate.
[0017] Optionally, the deposition source includes diborane, silane, oxygen, and nitrogen.
[0018] Optionally, the volume ratio of diborane:silane:oxygen:nitrogen in the deposition source is 8:12:12:15.
[0019] Optionally, the thickness of the borosilicate glass layer is 90nm-100nm.
[0020] Optionally, the sheet resistance of the borosilicate glass layer ranges from 800Ω / □ to 1200Ω / □.
[0021] Optionally, the diffusion temperature is 950°C-1050°C.
[0022] Optionally, the first process time is 170 min-190 min.
[0023] Optionally, the second process time is 7 min-9 min.
[0024] Optionally, the step of performing boron doping on the front surface of the etched silicon substrate at a diffusion temperature for a first process time, and forming a first boron doping concentration in the graphic region and a second boron doping concentration outside the graphic region on the silicon substrate, further comprises:
[0025] Sequentially preparing a tunneling oxide layer and a phosphorus-doped polysilicon layer on the back side of the silicon substrate to form a passivation contact structure;
[0026] Preparing an aluminum oxide layer on the front side of the silicon substrate;
[0027] Preparing a silicon nitride layer on the front side of the silicon substrate and on the back side of the silicon substrate;
[0028] Electrodes are prepared on the front side of the silicon substrate and on the back side of the silicon substrate.
[0029] In a second aspect of the present invention, a solar cell is provided. The solar cell is prepared by the solar cell preparation method as described in the first aspect.
[0030] In the implementation of the present invention, after providing a silicon substrate, a borosilicate glass layer is deposited on the front of the silicon substrate, and an etching slurry is coated in a preset graphic area on the front of the silicon substrate to etch away the borosilicate glass layer in the graphic area, and then the front of the etched silicon substrate is subjected to boron doping for a first process time at a diffusion temperature to form a first boron doping concentration in the graphic area and a second boron doping concentration outside the graphic area on the silicon substrate. In the implementation of the present invention, a borosilicate glass layer is prepared by deposition on the front of the silicon substrate, and only one step of boron diffusion is required after etching to prepare a selective emitter structure with a first boron doping concentration in the graphic area and a second boron doping concentration outside the graphic area, which reduces the time that the silicon substrate is exposed to high temperature in the process flow, improves the minority carrier lifetime, reduces the probability of bending deformation of the silicon substrate due to high temperature stress changes, and reduces the impact on the life of the silicon wafer. At the same time, instead of using a laser SE process, slurry etching is used, which also avoids damage to the silicon substrate during the laser removal of the borosilicate glass layer, improves the open circuit voltage of the battery, and reduces the process complexity and process cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0032] Figure 1 A flowchart of a method for preparing a solar cell provided by an embodiment of the present invention is shown;
[0033] Figure 2 A flowchart showing another method for preparing a solar cell provided by an embodiment of the present invention is shown;
[0034] Figure 3A schematic structural diagram of a solar cell provided by an embodiment of the present invention is shown.
[0035] Description of reference numerals:
[0036] 30-solar cell; 301-N-type silicon substrate; 302-passivation contact structure; 303-silicon nitride layer; 304-back electrode; 305-selective emitter structure; 306-aluminum oxide / silicon nitride layer; 307-front electrode; 3051-first boron doping concentration region; 3052-second boron doping concentration region. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Reference Figure 1 , Figure 1 A flowchart of a method for preparing a solar cell provided by an embodiment of the present invention is shown. The method may include:
[0039] Step 101: Provide a silicon substrate.
[0040] In the embodiment of the present invention, the N-type silicon wafer can be processed according to the process requirements to provide a silicon substrate. Optionally, the N-type silicon wafer can be cleaned, textured, etc., wherein the cleaning can remove organic impurities or inorganic impurities in the form of atoms, ions, particles, thin films, etc. on the surface of the N-type silicon wafer. Chemical cleaning such as acid cleaning, solvent extraction cleaning, plasma cleaning, etc. can be selected, and physical cleaning can be high-pressure cleaning, ultrasonic cleaning, etc.; textured can be acid textured, alkaline textured, electrochemical textured, laser textured, etc. The embodiment of the present invention does not specifically limit the method of providing a silicon substrate.
[0041] Step 102: depositing a borosilicate glass layer on the front surface of the silicon substrate
[0042] In an embodiment of the present invention, a borosilicate glass layer can be deposited on the front side of a silicon substrate by a deposition method, that is, a chemical reaction is carried out on the front side of the silicon substrate based on a gas boron source to generate a borosilicate glass layer. Optionally, a chemical vapor deposition method can be used to deposit the borosilicate glass layer, such as preparing the borosilicate glass layer by normal pressure chemical vapor deposition, plasma enhanced chemical vapor deposition, etc. There is no need to perform a boron diffusion light doping process under high temperature conditions of about 1000°C to form a borosilicate glass layer on the front side of the silicon substrate, thereby avoiding damage to the silicon substrate due to high temperature conditions. In the embodiment of the present invention, there is no specific limitation on the method for depositing the borosilicate glass layer and the gas boron source.
[0043] Step 103: coating an etching slurry in a preset graphic area on the front side of the silicon substrate, and etching away the borosilicate glass layer in the graphic area.
[0044] In the embodiment of the present invention, the borosilicate glass layer can be etched by etching slurry, and the slurry can be applied in the preset graphic area on the front of the silicon substrate to remove the borosilicate glass layer in the preset graphic area on the front of the silicon substrate, so that the silicon substrate in the graphic area is exposed, so that different doping concentrations are formed in the graphic area and outside the graphic area of the silicon substrate in the subsequent boron diffusion process to realize the selective emitter structure. Optionally, the etching slurry can be applied in the preset graphic area on the front of the silicon substrate by screen printing. The graphic area can be set according to the front sub-grid pattern of the solar cell, so as to realize high-concentration doping in the contact area between the metal grid line and the front of the silicon substrate, so that the square resistance is low, the contact resistance is small, and the filling factor is improved; low-concentration doping is realized in the area outside the contact area between the metal grid line and the front of the silicon substrate, so as to improve the open circuit voltage, short-circuit current, etc., and effectively improve the conversion efficiency of the solar cell. In the process of slurry etching, the damage to the silicon substrate caused by the laser burning to remove part of the borosilicate glass layer in the laser SE process is also avoided.
[0045] Step 104 , performing boron doping on the front surface of the etched silicon substrate at a diffusion temperature for a first process time, so as to form a first boron doping concentration in the graphic region and a second boron doping concentration outside the graphic region on the silicon substrate.
[0046] In an embodiment of the present invention, after etching away the borosilicate glass layer in a preset graphic area on the front side of the silicon substrate, the silicon substrate can be doped with boron at a diffusion temperature. Optionally, the diffusion temperature and the first process time can be specifically set according to the doping concentration and doping depth required for boron doping. Since the borosilicate glass layer in the graphic area is etched away in step 103, a first boron doping concentration is formed in the graphic area and a second boron doping concentration is formed outside the graphic area under the local blocking effect of the borosilicate glass layer, thereby realizing a selective emitter structure, wherein the area outside the graphic area is other areas on the front side of the silicon substrate except the graphic area.
[0047] In the embodiment of the present invention, a passivation contact structure or other functional layers such as a passivation layer, an anti-reflection layer, and a metal electrode may be further prepared on the back side of the silicon substrate to prepare a solar cell. In the embodiment of the present invention, there is no specific limitation on the process for further preparing the solar cell.
[0048] In the implementation of the present invention, after providing a silicon substrate, a borosilicate glass layer is deposited on the front of the silicon substrate, and an etching slurry is coated in a preset graphic area on the front of the silicon substrate to etch away the borosilicate glass layer in the graphic area, and then the front of the etched silicon substrate is subjected to boron doping for a first process time at a diffusion temperature to form a first boron doping concentration in the graphic area and a second boron doping concentration outside the graphic area on the silicon substrate. In the implementation of the present invention, a borosilicate glass layer is prepared by deposition on the front of the silicon substrate, and only one step of boron diffusion is required after etching to prepare a selective emitter structure with a first boron doping concentration in the graphic area and a second boron doping concentration outside the graphic area, which reduces the time that the silicon substrate is exposed to high temperature in the process flow, improves the minority carrier lifetime, reduces the probability of bending deformation of the silicon substrate due to high temperature stress changes, and reduces the impact on the life of the silicon wafer. At the same time, instead of using a laser SE process, slurry etching is used, which also avoids damage to the silicon substrate during the laser removal of the borosilicate glass layer, improves the open circuit voltage of the battery, and reduces the process complexity and process cost.
[0049] Reference Figure 2 , Figure 2 A flowchart of another method for preparing a solar cell provided by an embodiment of the present invention is shown. The method may include:
[0050] Step 201: Provide a silicon substrate.
[0051] In the embodiment of the present invention, step 201 may correspond to the relevant description of the aforementioned step 101, and will not be described again here to avoid repetition.
[0052] In an embodiment of the present invention, an alkali texturing process can be used to texturize an N-type silicon wafer to provide a silicon substrate. Optionally, a mixed solution of potassium hydroxide and a texturing additive can be used, wherein the volume fraction of potassium hydroxide is approximately 1%. The N-type silicon wafer is corroded for 495 seconds to 505 seconds at a temperature of 77°C to 83°C to form the texturing. The volume ratio of the mixed solution can be water: potassium hydroxide: texturing additive 354:5.5:2. Under this ratio, the volume fraction of potassium hydroxide is 1.5%. The etching amount of the N-type silicon wafer by the alkali texturing process can be 0.55 grams to 0.65 grams. The reflectivity of the N-type silicon wafer after texturing can be 8.7% to 9.3%. The texturing additive can include surfactants, nucleating agents, dispersants, catalysts, defoaming agents, etc.
[0053] Step 202: deposit a borosilicate glass layer on the front side of the silicon substrate using a normal pressure chemical vapor deposition device based on a deposition source.
[0054] In the embodiment of the present invention, the atmospheric pressure chemical vapor deposition equipment is a device that realizes the atmospheric pressure chemical vapor deposition process. Deposition can be performed under conditions where the reaction environment pressure is close to the atmospheric pressure. The atmospheric pressure chemical vapor deposition equipment uses a deposition source to deposit a borosilicate glass layer on the front side of a silicon substrate under atmospheric pressure conditions. The deposition process parameters are controllable, the deposition uniformity is high, and the prepared film layer has high quality.
[0055] Optionally, the deposition source includes diborane, silane, oxygen, and nitrogen.
[0056] In an embodiment of the present invention, the deposition source may include gases such as diborane, silane, oxygen, and nitrogen. Different gases are introduced into a normal-pressure chemical vapor deposition device as needed to mix and react on the front side of the silicon substrate to generate a borosilicate glass layer. Those skilled in the art may select other gases as deposition sources according to process conditions, application requirements, etc., and the embodiment of the present invention does not impose specific restrictions on this.
[0057] Optionally, the volume ratio of diborane:silane:oxygen:nitrogen in the deposition source is 8:12:12:15.
[0058] In an embodiment of the present invention, the volume ratio of diborane, silane, oxygen and nitrogen in the deposition source can be 8:12:12:15. On this basis, 8 equivalents of diborane, 12 equivalents of silane, 12 equivalents of oxygen and 15 equivalents of nitrogen can be introduced into the reaction chamber as deposition sources to prepare a borosilicate glass layer on the front side of the silicon substrate.
[0059] Optionally, the atmospheric pressure chemical vapor deposition equipment includes a preheating chamber, a reaction chamber, and a cooling chamber.
[0060] In an embodiment of the present invention, the atmospheric pressure chemical vapor deposition equipment may include a preheating chamber, a reaction chamber, and a cooling chamber. The silicon substrate to be processed can be transmitted between different chambers through a conveyor belt to realize preheating, deposition, cooling and other processes on the silicon substrate, thereby depositing a borosilicate glass layer.
[0061] Optionally, the step 202 includes:
[0062] Step S11, transferring the silicon substrate to the preheating chamber, and preheating the silicon substrate at a temperature of 390° C.-410° C.
[0063] In an embodiment of the present invention, the silicon substrate can be first transferred to a preheating chamber, and the preheating chamber can preheat the silicon substrate at a temperature of 390°C-410°C. Optionally, the temperature of the preheating chamber can be any temperature within the range of 390°C-410°C, such as 390°C, 391°C, 392°C, 393°C, 394°C, 395°C, 400°C, 405°C, 410°C, etc.
[0064] Step S12, transferring the silicon substrate to the reaction chamber, and depositing a second process time on the front side of the silicon substrate at a temperature of 590°C-610°C based on the deposition source to prepare a borosilicate glass layer, wherein the deposition source includes diborane, silane, oxygen, and nitrogen.
[0065] In an embodiment of the present invention, after preheating the silicon substrate, the silicon substrate can be transferred to a reaction chamber, where a deposition source can react on the front side of the silicon substrate to generate a deposited film layer based on the deposition source. wherein, at a temperature of 590°C-610°C, diborane, silane, oxygen, nitrogen and other deposition sources can be used to react on the front side of the silicon substrate for a second process time to prepare a borosilicate glass layer. For example, the reaction chamber can be at any temperature within the range of 590°C-610°C, such as 590°C, 591°C, 592°C, 593°C, 594°C, 595°C, 600°C, 605°C, 610°C, etc.
[0066] In the embodiment of the present invention, diborane, silane, oxygen and nitrogen are used as deposition sources to deposit a borosilicate glass layer on the front surface of a silicon substrate. Reaction equations (1) and (2) are as follows:
[0067] SiH4+O2→SiO2+2H2··························(1)
[0068] 2B2H6+3O2→2B2O3+6H2························(2)
[0069] Wherein, silane and diborane react with oxygen respectively to form a borosilicate glass layer on the front side of the silicon substrate.
[0070] Optionally, the thickness of the borosilicate glass layer is 90nm-100nm.
[0071] In an embodiment of the present invention, the thickness of the borosilicate glass layer can be any thickness between 90nm and 100nm, such as 90nm, 91nm, 92nm, 93nm, 94nm, 95nm, 96nm, 97nm, 98nm, 99nm, 100nm, etc.
[0072] Optionally, the sheet resistance of the borosilicate glass layer ranges from 800Ω / □ to 1200Ω / □.
[0073] In an embodiment of the present invention, the square resistance range of the borosilicate glass layer can be any square resistance between 800Ω / □ and 1200Ω / □, such as 800Ω / □, 810Ω / □, 820Ω / □, 830Ω / □, 840Ω / □, 850Ω / □, 900Ω / □, 950Ω / □, 1000Ω / □, 1050Ω / □, 1100Ω / □, 1150Ω / □, 1200Ω / □, etc.
[0074] Optionally, the second process time is 7 min-9 min.
[0075] In an embodiment of the present invention, the second process time may be any time between 7 min and 9 min, such as 7.1 min, 7.2 min, 7.3 min, 7.4 min, 7.5 min, 8 min, 8.5 min, 9 min, etc.
[0076] Step S13: transferring the silicon substrate to the cooling chamber to cool the silicon substrate.
[0077] In an embodiment of the present invention, after a borosilicate glass layer is deposited on the front side of a silicon substrate in a reaction chamber, the silicon substrate can be transferred to a cooling chamber to be cooled. The silicon substrate can be cooled to room temperature and then taken out from a normal pressure chemical vapor deposition device to obtain a silicon substrate with a borosilicate glass layer prepared on the front side.
[0078] Step 203: coating an etching slurry in a preset graphic area on the front side of the silicon substrate, and etching away the borosilicate glass layer in the graphic area.
[0079] In the embodiment of the present invention, an etching slurry is coated in a preset image area on the borosilicate glass layer on the front side of the silicon substrate, wherein the pattern area may be the area of the front sub-gate pattern on the front side of the silicon substrate, so as to etch and remove the borosilicate glass layer in the pattern area on the silicon substrate, and based on the blocking effect of the remaining borosilicate glass layer, a first boron doping concentration in the pattern area and a second boron doping concentration outside the pattern area are formed on the front side of the silicon substrate in a subsequent boron diffusion process, and optionally, the etching slurry may include fluoride, such as hydrofluoric acid, ammonium fluoride, etc. The etching slurry may be coated in the preset pattern area by screen printing, and after screen printing, it may be left to stand for 15-25 minutes to allow the etching slurry to fully react with the borosilicate glass layer, fully remove the borosilicate glass layer in the pattern area, and expose the silicon substrate in the pattern area.
[0080] Step 204 , performing boron doping on the front surface of the etched silicon substrate at a diffusion temperature for a first process time, so as to form a first boron doping concentration in the pattern region and a second boron doping concentration outside the pattern region on the silicon substrate.
[0081] In the embodiment of the present invention, step 204 may correspond to the relevant description of the aforementioned step 104, and will not be described again here to avoid repetition.
[0082] Optionally, the diffusion temperature is 950°C-1050°C.
[0083] In the embodiment of the present invention, the diffusion temperature may be any temperature in the range of 950°C-1050°C, such as 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C, 1050°C, etc.
[0084] Optionally, the first process time is 170 min-190 min.
[0085] In an embodiment of the present invention, the first process time may be any time within the range of 170 min-190 min, such as 170 min, 171 min, 172 min, 173 min, 174 min, 175 min, 180 min, 185 min, 190 min, etc.
[0086] Step 205 : sequentially prepare a tunneling oxide layer and a phosphorus-doped polysilicon layer on the back side of the silicon substrate to form a passivation contact structure.
[0087] In an embodiment of the present invention, a silicon oxide layer can be prepared on the back side of a silicon wafer as a tunneling oxide layer. The silicon oxide layer can reduce the interface state density through chemical passivation, so that the majority carriers are transported through tunneling to achieve a tunneling effect. Minority carriers are difficult to tunnel through the silicon oxide layer due to potential barriers, field effects, etc., which can reduce the probability of electron-hole recombination and the selective contact of majority carriers, thereby effectively improving battery efficiency. Optionally, the silicon oxide layer can be grown by wet chemical growth or thermal growth.
[0088] In the embodiment of the present invention, a phosphorus-doped polysilicon layer can be further prepared on the tunnel oxide layer. Optionally, LPCVD (Low Pressure Chemical Vapor Deposition) can be used to first deposit a polysilicon layer, and then phosphorus diffusion or ion implantation can be performed on the polysilicon layer to form a phosphorus-doped polysilicon layer. PECVD (Plasma Enhanced Chemical Vapor Deposition) can also be used to deposit a phosphorus-doped amorphous silicon or microcrystalline silicon layer, and then annealed to obtain a phosphorus-doped polysilicon layer, thereby forming a passivation contact structure with the back of the silicon substrate of the tunnel oxide layer. Among them, the polysilicon layer coated on the front side of the silicon substrate can be removed to avoid affecting subsequent processes, battery efficiency, etc.
[0089] Step 206: Prepare an aluminum oxide layer on the front side of the silicon substrate.
[0090] In the embodiment of the present invention, the aluminum oxide layer has a good field effect passivation effect, passivates the surface of the boron-doped layer, reduces carrier recombination, and increases the minority carrier lifetime, thereby improving the photoelectric conversion efficiency of the battery. Optionally, an aluminum oxide layer can be prepared on the surface of the boron-doped layer, wherein the aluminum oxide layer can be prepared by plasma enhanced chemical vapor deposition, atomic layer deposition and other methods.
[0091] Step 207: Prepare a silicon nitride layer on the front side of the silicon substrate and on the back side of the silicon substrate.
[0092] In the embodiment of the present invention, a silicon nitride layer can also be prepared on the aluminum oxide layer and the phosphorus-doped polysilicon layer, that is, on the front and back sides of the silicon substrate. The silicon nitride layer has good hydrogen passivation and anti-reflection effects and can achieve good body passivation. Optionally, a stacked silicon nitride layer can be prepared on the aluminum oxide layer to achieve front passivation and anti-reflection effects of the battery, and a silicon nitride layer with a low refractive index can be prepared on the phosphorus-doped polysilicon layer to reduce light loss and improve light utilization. Those skilled in the art can prepare the silicon nitride layer according to process conditions and application requirements, and the embodiment of the present invention does not impose specific restrictions on this.
[0093] Step 208: Prepare electrodes on the front side of the silicon substrate and on the back side of the silicon substrate.
[0094] In the embodiment of the present invention, after preparing each film layer, electrodes can be prepared on the front and back sides of the silicon substrate to obtain a solar cell. Optionally, the electrodes can be prepared by screen printing metal slurry and sintering, or by photolithography and electroplating, or by vacuum evaporation. Optionally, the electrodes can be silver electrodes, copper electrodes, aluminum electrodes, etc., and the embodiment of the present invention does not impose specific restrictions on this.
[0095] In the implementation of the present invention, after providing a silicon substrate, a borosilicate glass layer is deposited on the front of the silicon substrate, and an etching slurry is coated in a preset graphic area on the front of the silicon substrate to etch away the borosilicate glass layer in the graphic area, and then the front of the etched silicon substrate is subjected to boron doping for a first process time at a diffusion temperature to form a first boron doping concentration in the graphic area and a second boron doping concentration outside the graphic area on the silicon substrate. In the implementation of the present invention, a borosilicate glass layer is prepared by deposition on the front of the silicon substrate, and only one step of boron diffusion is required after etching to prepare a selective emitter structure with a first boron doping concentration in the graphic area and a second boron doping concentration outside the graphic area, which reduces the time that the silicon substrate is exposed to high temperature in the process flow, improves the minority carrier lifetime, reduces the probability of bending deformation of the silicon substrate due to high temperature stress changes, and reduces the impact on the life of the silicon wafer. At the same time, instead of using a laser SE process, slurry etching is used, which also avoids damage to the silicon substrate during the laser removal of the borosilicate glass layer, improves the open circuit voltage of the battery, and reduces the process complexity and process cost.
[0096] Figure 3 FIG. 4 shows a schematic diagram of the structure of a solar cell 30 provided in an embodiment of the present invention. Figure 3 As shown, the solar cell 30 includes an N-type silicon substrate 301, and a passivation contact structure 302, a silicon nitride layer 303, and a back electrode 304 on the back of the N-type silicon substrate 301. The solar cell 30 also includes a selective emitter structure 305, an aluminum oxide / silicon nitride layer 306, and a front electrode 307 on the front of the N-type silicon substrate 301, wherein the graphic area where the selective emitter structure 305 contacts the metal grid line is a first boron doping concentration area 3051, and the other graphic areas are outside the second boron doping concentration area 3052, and the first boron doping concentration is greater than the second boron doping concentration. In the implementation of the present invention, a structure such as Figure 3 The sample battery and the comparative battery shown in the figure, wherein the sample battery adopts Figure 1 , Figure 2 The solar cell is prepared by any of the above-mentioned methods, and the comparison cell is prepared by conventional process, as shown below:
[0097] Preparation of sample cells
[0098] Step S21, performing an alkali texturing process on an N-type silicon wafer by a tank-type texturing cleaning machine to obtain a silicon substrate, wherein a mixed solution of potassium hydroxide and a texturing additive is used as an alkali solution, and the volume ratio of the alkali solution can be water: potassium hydroxide: texturing additive is 354:5.5:2, wherein the texturing additive includes a surfactant, a nucleating agent, a dispersant, a catalyst, a defoaming agent, etc.; the process temperature of the texturing process can be 77°C-83°C, and the process time can be 495 seconds-505 seconds; the etching amount of the N-type silicon wafer by the texturing process is 0.55 grams-0.65 grams, and the reflectivity is 8.7%-9.3%;
[0099] Step S22, transferring the silicon substrate to a preheating chamber of a normal pressure chemical vapor deposition device through a conveyor belt, and preheating the silicon substrate at a temperature of 390°C-410°C; then transferring the silicon substrate to a reaction chamber through a conveyor belt, and depositing a borosilicate glass layer on the front side of the silicon substrate in the reaction chamber by reacting diborane, silane, oxygen, and nitrogen, wherein the process temperature for depositing the borosilicate glass layer is 590°C-610°C, the process time is 7min-9min, and the thickness of the deposited borosilicate glass layer is 100±10nm; then transferring the silicon substrate to a cooling chamber for cooling, and taking out a wafer after the silicon substrate is cooled to room temperature, and testing the borosilicate glass layer, and the square resistance range is 800-1200Ω / □;
[0100] Step S23, in a screen printer, coating the front side of the silicon substrate with etching slurry according to the front side grid pattern of the solar cell, standing for 15-25 minutes after screen printing, and then washing and drying in a tank cleaning machine for subsequent process treatment, wherein the etching slurry mainly includes fluoride;
[0101] Step S24, placing the dried silicon substrate in a boron diffusion furnace and performing a heavy doping process at a process temperature of 950° C.-1050° C. for a process time of 170 min-190 min, so that the front side resistance of the silicon substrate is 55Ω / □-65Ω / □;
[0102] Step S25, performing alkaline polishing on the back side of the silicon substrate in a tank cleaning machine, wherein the alkaline solution is a mixed solution of potassium hydroxide and a polishing additive, wherein the volume concentration of potassium hydroxide is 3.5%-4.5%, and the volume ratio of water: potassium hydroxide: polishing additive in the solution is 340:16:4; wherein the polishing additive may include a surfactant, sodium citrate, sodium benzoate, etc., the process temperature in the alkaline polishing is 53°C-57°C, and the process time is 215 seconds-225 seconds; the etching amount of the silicon substrate after the alkaline polishing is 0.18 g-0.22 g, and the back reflectivity of the silicon substrate is 41%-43%;
[0103] Step S26, using LPCVD to deposit a tunneling oxide layer (SiO2) and a polysilicon (Poly) layer on the back side of the silicon substrate, wherein the thickness of the tunneling oxide layer is 1.2nm-1.8nm, and the thickness of the polysilicon layer is 100nm-140nm;
[0104] Step S27, using a phosphorus diffusion furnace to implant phosphorus into the polysilicon layer to form a passivation contact structure;
[0105] Step S28, removing the polysilicon layer plated on the front side of the silicon substrate in a tank cleaning machine, using a mixed solution of potassium hydroxide and a polishing additive, wherein the volume concentration of potassium hydroxide is 3.5%-4.5%, the process temperature is 63° C.-69° C., and the process time is 190 seconds-210 seconds;
[0106] Step S29, preparing an AlOx+SiNx (aluminum oxide+silicon nitride) passivation layer on the front side of the silicon substrate and a SiNx passivation layer on the back side;
[0107] Step S210, screen printing and sintering are performed on the front and back sides of the silicon substrate to prepare electrodes, and sample batteries are obtained by testing and sorting.
[0108] Preparation of comparative batteries
[0109] Step S31, performing an alkali texturing process on an N-type silicon wafer by a tank-type texturing cleaning machine to obtain a silicon substrate, wherein a mixed solution of potassium hydroxide and a texturing additive is used as an alkali solution, and the volume ratio of the alkali solution can be water: potassium hydroxide: texturing additive is 354:5.5:2, wherein the texturing additive includes a surfactant, a nucleating agent, a dispersant, a catalyst, a defoaming agent, etc.; the process temperature of the texturing process can be 77°C-83°C, and the process time can be 495 seconds-505 seconds; the etching amount of the N-type silicon wafer by the texturing process is 0.55 grams-0.65 grams, and the reflectivity is 8.7%-9.3%;
[0110] Step S32, placing the textured silicon substrate into a boron diffusion furnace for a light doping process, so that the front side resistance of the silicon substrate is 190Ω / □-210Ω / □, wherein the process temperature of the light doping process is 950℃-1050℃, and the process time is 140min-160min;
[0111] Step S33, in the laser, according to the front side grid pattern of the solar cell, a portion of the borosilicate glass layer is laser burned off on the front side of the silicon substrate, and then the laser damage is removed by alkali washing in a tank cleaning machine for subsequent process processing;
[0112] Step S34, placing the alkali-washed silicon substrate in a boron diffusion furnace and performing a heavy doping process at a process temperature of 950° C.-1050° C. for a process time of 170 min-190 min, so that the front side resistance of the silicon substrate is 55Ω / □-65Ω / □;
[0113] Step S35, performing alkaline polishing on the back side of the silicon substrate in a tank cleaning machine, wherein the alkaline solution is a mixed solution of potassium hydroxide and a polishing additive, wherein the volume concentration of potassium hydroxide is 3.5%-4.5%, and the volume ratio of water: potassium hydroxide: polishing additive in the solution is 340:16:4; wherein the polishing additive may include a surfactant, sodium citrate, sodium benzoate, etc., the process temperature in the alkaline polishing is 53°C-57°C, and the process time is 215 seconds-225 seconds; the etching amount of the silicon substrate after the alkaline polishing is 0.18 g-0.22 g, and the back reflectivity of the silicon substrate is 41%-43%;
[0114] Step S36, using LPCVD to deposit a tunneling oxide layer (SiO2) and a polysilicon (Poly) layer on the back side of the silicon substrate, wherein the thickness of the tunneling oxide layer is 1.2nm-1.8nm, and the thickness of the polysilicon layer is 100nm-140nm;
[0115] Step S37, using a phosphorus diffusion furnace to implant phosphorus on the polysilicon layer to form a passivation contact structure;
[0116] Step S38, removing the polysilicon layer plated on the front side of the silicon substrate in a tank cleaning machine, using a mixed solution of potassium hydroxide and a polishing additive, wherein the volume concentration of potassium hydroxide is 3.5%-4.5%, the process temperature is 63° C.-69° C., and the process time is 190 seconds-210 seconds;
[0117] Step S39, preparing an AlOx+SiNx (aluminum oxide+silicon nitride) passivation layer on the front side of the silicon substrate and a SiNx passivation layer on the back side;
[0118] Step S310: Screen printing and sintering are performed on the front and back sides of the silicon substrate to prepare electrodes, and then testing and sorting are performed to obtain a comparison battery.
[0119] In the implementation of the present invention, performance tests were also conducted on the sample cells and the comparison cells, including the open circuit voltage (Voc), fill factor (FF), short circuit current (Isc), conversion efficiency (Eta) and the like of the solar cells. The test results are shown in Table 1 below:
[0120] Table 1
[0121]
[0122] In the implementation of the present invention, according to the test results described in Table 1, the open circuit voltage of the sample battery is increased by 5mV, the short circuit current is increased by 20mA, the fill factor is increased by 0.4%abs, and the conversion efficiency is increased by 0.3%abs in general. It can be seen from the data that the sample battery prepared by the implementation of the present invention is improved in open circuit voltage, short circuit current, fill factor and conversion efficiency compared with the control battery of the conventional process. It can be seen that in the implementation of the present invention, by adopting atmospheric pressure chemical vapor deposition equipment to deposit the borosilicate glass layer, the damage to the silicon substrate caused by high temperature conditions in the boron diffusion and light doping process in the conventional process is avoided, including bending deformation due to high temperature stress, and the influence of high temperature conditions on the life of the silicon substrate; further, the borosilicate glass layer is etched by screen printing, which also avoids damage to the silicon substrate by laser etching, thereby improving the conversion efficiency of the battery, and effectively prepares the selective emitter structure in the subsequent boron diffusion step, wherein the front fine gate line and the front contact area of the silicon substrate have low square resistance, high boron doping concentration, and small contact resistance, which can further improve the filling factor, and other areas have high square resistance, low boron doping concentration, low surface recombination, and effectively improve the optical response, which can improve the open circuit voltage, short circuit current and other performance parameters of the solar cell.
[0123] It should be noted that, for the method embodiments, for the sake of simplicity of description, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the embodiments of the present application are not limited by the described order of actions, because according to the embodiments of the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of the present application.
[0124] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0125] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention, or the part that contributes to the prior art, can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, a magnetic disk, or an optical disk), and includes a number of instructions for enabling a terminal (which can be a mobile phone, a computer, a server, an air conditioner, or a network device, etc.) to execute the methods described in each embodiment of the present invention.
[0126] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A method for preparing a solar cell, characterized in that: The method comprises: providing a silicon substrate; A borosilicate glass layer is deposited on the front side of the silicon substrate using a normal pressure chemical vapor deposition device based on a deposition source; the deposition source includes diborane, silane, oxygen, and nitrogen; Coating an etching slurry in a preset graphic area on the front side of the silicon substrate to etch away the borosilicate glass layer in the graphic area; Performing boron doping on the front side of the etched silicon substrate at a diffusion temperature for a first process time to form a first boron doping concentration in the pattern area and a second boron doping concentration outside the pattern area on the silicon substrate; The diffusion temperature is 950° C.-1050° C.; the first process time is 170 min-190 min.
2. The method according to claim 1, characterized in that: The atmospheric pressure chemical vapor deposition equipment comprises a preheating chamber, a reaction chamber, and a cooling chamber. The atmospheric pressure chemical vapor deposition equipment is used to deposit a borosilicate glass layer on the front side of the silicon substrate based on a deposition source, comprising: The silicon substrate is transferred to the preheating chamber, and the silicon substrate is preheated at a temperature of 390° C. to 410° C.; The silicon substrate is transferred into the reaction chamber, and a second process time is deposited on the front side of the silicon substrate based on the deposition source at a temperature of 590° C. to 610° C. to prepare a borosilicate glass layer; The silicon substrate is transferred to the cooling chamber to cool the silicon substrate.
3. The method according to claim 1, characterized in that The volume ratio of diborane:silane:oxygen:nitrogen in the deposition source is 8:12:12:
15.
4. The method according to claim 2, characterized in that The second process time is 7 min-9 min.
5. The method according to claim 1, characterized in that The thickness of the borosilicate glass layer is 90nm-100nm; or, The sheet resistance of the borosilicate glass layer ranges from 800Ω / □ to 1200Ω / □.
6. The method according to claim 1, characterized in that After performing boron doping on the front side of the etched silicon substrate at a diffusion temperature for a first process time, and forming a first boron doping concentration in the pattern area and a second boron doping concentration outside the pattern area on the silicon substrate, the method further comprises: Sequentially preparing a tunneling oxide layer and a phosphorus-doped polysilicon layer on the back side of the silicon substrate to form a passivation contact structure; Preparing an aluminum oxide layer on the front side of the silicon substrate; Preparing a silicon nitride layer on the front side of the silicon substrate and on the back side of the silicon substrate; Electrodes are prepared on the front side of the silicon substrate and on the back side of the silicon substrate.