Polarizing plate with adhesive layer and image display device
By using a polarizing plate with an adhesive layer in combination of a polarizing film with an absolute value of less than 0.03 in the display device, the problem of light leakage of the polarizing plate after narrowing or omitting the frame is solved, and better results are achieved display effect.
Patent Information
- Application Number
- CN202080065065.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-20
- Filing Date
- 2020-09-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-09-14
AI Technical Summary
After narrowing or omitting the frame in the display device, light leakage occurs easily at the end of the polarizing plate, affecting the display effect.
The polarizing plate with an adhesive layer composed of a polarizing film, a first cured product layer, a first resin film and an adhesive layer is used to ensure that the absolute value of the refractive index difference between the first cured product layer and the first resin film is at 0.03 or less, and the first cured product layer and the second cured product layer are formed using an active energy ray curing adhesive composition, and the first resin film and the second resin film are formed with a thermoplastic resin to optimize the thickness of the adhesive layer and Refractive index to suppress light leakage at the end of the polarizing plate.
The light leakage of the polarizing plate in the middle end of the display device with narrowed bezels or omitted bezels is effectively suppressed, ensuring an improvement in the display effect.
Smart Images

Figure CN114402238B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polarizing plate with an adhesive layer and an image display device including the polarizing plate. Background Art
[0002] The polarizing plate has a structure in which a protective film is laminated on at least one surface of a polarizing film via an adhesive layer. The polarizing plate is usually installed in a display device via an adhesive layer (for example, Patent Document 1). In order to suppress impact from the outside, a metal frame called a frame is usually provided in such a display device to protect the periphery of the display device.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-42383 Summary of the invention
[0006] Problems to be solved by the invention
[0007] In recent years, there has been a trend toward further slimming and larger screens for display devices. In line with this trend, the following scheme has been proposed, namely, by narrowing the width of the frame, lowering the height of the frame, or omitting the frame, the display screen can be enlarged even for a display device of the same size. However, it has been found that if a polarizing plate is installed in a display device with a narrowed frame width, lowered frame height, or omitted frame, the end of the polarizing plate installed in the display device will be exposed, and when the power of the display device is turned on, light from the backlight and the organic light-emitting element will leak from the end of the polarizing plate.
[0008] Means for solving problems
[0009] The present invention includes the following inventions.
[0010] [1] A polarizing plate with an adhesive layer, comprising, in this order, a polarizing film, a first cured layer, a first resin film, and an adhesive layer.
[0011] The polarizing film is in direct contact with the first cured material layer.
[0012] The first cured product layer is in direct contact with the first resin film,
[0013] The first resin film is in direct contact with the adhesive layer,
[0014] The absolute value of the difference between the average refractive index of the first cured product layer and the average refractive index of the first resin film is 0.03 or less.
[0015] [2] The polarizing plate according to [1], wherein the first cured product layer is a cured product of an active energy ray-curable composition.
[0016] [3] The polarizing plate according to [1] or [2], wherein the refractive index of the first cured layer is 1.55 or less.
[0017] [4] The polarizing plate according to any one of [1] to [3], wherein the first resin film includes a film formed of a thermoplastic resin.
[0018] [5] The polarizing plate according to any one of [1] to [4], wherein the first resin film has a thickness of 6 μm or more.
[0019] [6] The polarizing plate according to any one of [1] to [5], further comprising a second resin film on a surface of the polarizing film opposite to the first cured layer via a second cured layer.
[0020] [7] An image display device comprising an image display panel and the polarizing plate with a pressure-sensitive adhesive layer according to any one of [1] to [6] disposed on a viewing side of the image display panel.
[0021] Effects of the Invention
[0022] The polarizing plate of the present invention can suppress light leakage from the edge of the polarizing plate even when incorporated in a display device with a narrow frame width, a display device with a reduced frame height, or a display device with no frame. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A cross-sectional view showing a structure of one embodiment of the polarizing plate of the present invention is shown.
[0024] Figure 2 A cross-sectional view showing a structure of one embodiment of the image display device of the present invention.
[0025] Figure 3 A cross-sectional view showing a method for checking light leakage in an image display device according to the present invention. DETAILED DESCRIPTION
[0026] Hereinafter, embodiments of the present invention will be described in detail. It should be noted that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made within the scope that does not impair the gist of the present invention.
[0027] based on Figure 1 The structure of one embodiment of the polarizing plate of the present invention will be described. The polarizing plate 10 of the present invention has a first cured material layer 2 and a first resin film 3 laminated in this order on one surface of a polarizing film 1. In addition, the polarizing plate of the present invention may also be as follows: Figure 2As shown, the polarizing film 1 has a structure in which the second resin film 5 is provided on the surface opposite to the first cured material layer 2 via the second cured material layer 4. Alternatively, the display device 30 may be formed by laminating the panel 7 via the adhesive layer 6.
[0028] Hereinafter, each constituent component of the polarizing plate of the present invention will be described in detail.
[0029] [Polarizing plate with adhesive layer]
[0030] The polarizing plate with an adhesive layer of the present invention comprises, in order, a polarizing film 1, a first cured material layer 2, a first resin film 3, and an adhesive 6. In the polarizing plate with an adhesive layer of the present invention, the absolute value of the difference between the average refractive index of the first cured material layer 2 and the average refractive index of the first resin film 3 is 0.03 or less. In addition, the polarizing film 1 is in direct contact with the first cured material layer 2, the first cured material layer 2 is in direct contact with the first resin film 3, and the first resin film 3 is in direct contact with the adhesive layer 6.
[0031] It should be noted that the average refractive index in the present invention refers to the average refractive index at a wavelength of 589 nm.
[0032] In the polarizing plate with an adhesive layer of the present invention, the absolute value of the difference between the average refractive index n2 of the first cured layer 2 and the average refractive index of the first resin film 3 is 0.03 or less, preferably 0.025 or less, more preferably 0.02 or less, and further preferably 0.01 or less. By making the difference between the average refractive index of the first cured layer 2 and the refractive index of the first resin film 3 satisfy this range, when the polarizing plate is applied to a display device, light leakage from the end of the polarizing plate can be effectively suppressed.
[0033] based on Figure 3 For explanation, the light leakage from the end of the polarizing plate of the present invention refers to that when the display device 30 is powered on and the display device is observed from an angle of θ (°) tilted in the cross-sectional direction relative to the front of the display device, light from the display device leaks from the cross-section of the polarizing plate, and the cross-sectional light of the polarizing plate can be observed. The larger θ is (for example, 15° to 90°), the more strongly the light leakage tends to be observed. When θ is greater than 40° (especially greater than 80°), light leakage is significantly observed. According to the polarizing plate with an adhesive layer of the present invention, when the display device is observed from an angle of θ of 30° to 90° (especially 40° to 90°, especially 80° to 90°), the light leakage of the polarizing plate can also be suppressed.
[0034] <First cured material layer>
[0035] The first cured product layer 2 is not particularly limited as long as the average refractive index difference with the first resin film is within a specified range, and is usually a layer formed by a resin composition, which is a cured product layer of a resin composition. Specifically, as the first cured product layer 2, a layer (adhesive layer) formed by an adhesive composition, a layer formed by a water-based adhesive composition, a layer formed by an active energy ray-curable adhesive composition, etc. can be cited. Among them, from the aspect of being able to easily adjust the average refractive index, it is preferably a layer formed by an active energy ray-curable adhesive composition (a cured product layer of an active energy ray-curable adhesive composition).
[0036] An active energy ray-curable adhesive composition is a composition that cures after being irradiated with active energy rays. For example, there can be mentioned a cationically polymerizable active energy ray-curable adhesive composition containing a cationically polymerizable compound and a cation polymerization initiator (hereinafter sometimes referred to as a photocationically polymerizable adhesive composition), a radically polymerizable active energy ray-curable adhesive composition containing a radically polymerizable compound and a radical polymerization initiator (hereinafter sometimes referred to as a photoradical polymerizable adhesive composition), an active energy ray-curable adhesive composition containing both a cationically polymerizable compound and a radically polymerizable compound and containing a cationic polymerization initiator and a radical polymerization initiator, and an electron beam-curable adhesive composition that is cured by irradiating an active energy ray-curable adhesive that does not contain an initiator with an electron beam, etc.
[0037] The cationically polymerizable compound refers to a compound or oligomer that undergoes a cationic polymerization reaction and cures by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, or by heating, and specifically includes epoxy compounds, oxetane compounds, and vinyl compounds. The active energy ray-curable adhesive composition may contain two or more cationically polymerizable compounds.
[0038] The epoxy compound is a compound having one or more (preferably two or more) epoxy groups in the molecule. Examples of the epoxy compound include alicyclic epoxy compounds, aromatic epoxy compounds, and aliphatic epoxy compounds.
[0039] The alicyclic epoxy compound is a compound having one or more epoxy groups bonded to an alicyclic ring in the molecule, and examples thereof include 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, 3,4-epoxy-6-methylcyclohexanecarboxylate, ethylenebis(3,4-epoxycyclohexanecarboxylate), bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexanemethyl)adipate, diethylene glycol, Bis(3,4-epoxycyclohexyl methyl ether), ethylene glycol bis(3,4-epoxycyclohexyl methyl ether), 2,3,14,15-diepoxy-7,11,18,21-tetraoxatrispiro[5.2.2.5.2.2]eicosane, 3-(3,4-epoxycyclohexyl)-8,9-epoxy-1,5-dioxaspiro[5.5]undecane, 4-vinylcyclohexene dioxide, limonene dioxide, bis(2,3-epoxycyclopentyl) ether, dicyclopentadiene dioxide.
[0040] Aromatic epoxy compounds are compounds having an aromatic ring and an epoxy group in the molecule, and examples thereof include bisphenol-type epoxy compounds or oligomers thereof such as the diglycidyl ether of bisphenol A, the diglycidyl ether of bisphenol F, and the diglycidyl ether of bisphenol S; novolac-type epoxy resins such as phenol novolac epoxy resin, cresol novolac epoxy resin, and hydroxybenzaldehyde phenol novolac epoxy resin; polyfunctional epoxy compounds such as the glycidyl ether of 2,2',4,4'-tetrahydroxydiphenylmethane and the glycidyl ether of 2,2',4,4'-tetrahydroxybenzophenone; and polyfunctional epoxy resins such as epoxidized polyvinylphenol.
[0041] Aliphatic epoxy compounds are compounds having at least one oxirane ring (three-membered cyclic ether) bonded to an aliphatic carbon atom in the molecule. Examples include monofunctional epoxy compounds such as butyl glycidyl ether and 2-ethylhexyl glycidyl ether; bifunctional epoxy compounds such as 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and neopentyl glycol diglycidyl ether; trifunctional or higher epoxy compounds such as trimethylolpropane triglycidyl ether and pentaerythritol tetraglycidyl ether; and epoxy compounds having one epoxy group directly bonded to an alicyclic ring and an oxirane ring bonded to an aliphatic carbon atom, such as 4-vinylcyclohexene dioxide and limonene dioxide.
[0042] Oxetane compounds are compounds containing one or more oxetane rings (oxetane groups) in the molecule. Specifically, for example, 3-ethyl-3-hydroxymethyloxetane (also known as oxetane alcohol), 2-ethylhexyloxetane, 1,4-bis ({(3-ethyloxetane-3-yl)methoxy}methyl)benzene (also known as xylene dioxetane), 3-ethyl-3 ({(3-ethyloxetane-3-yl)methoxy}methyl)oxetane, 3-ethyl-3-(phenoxymethyl)oxetane, 3-(cyclohexyloxy)methyl-3-ethyloxetane. Oxetane compounds can be used as the main component of a cationic polymerizable compound, or can be used in combination with an epoxy compound.
[0043] Examples of vinyl compounds include aliphatic or alicyclic vinyl ether compounds. Examples include vinyl ethers of alkyl or alkenyl alcohols having 5 to 20 carbon atoms, such as n-pentyl vinyl ether, isopentyl vinyl ether, n-hexyl vinyl ether, n-octyl vinyl ether, 2-ethylhexyl vinyl ether, n-dodecyl vinyl ether, stearyl vinyl ether, and oleyl vinyl ether; vinyl ethers containing hydroxyl groups, such as 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, and 4-hydroxybutyl vinyl ether; vinyl ethers of monoalcohols having an aliphatic ring or an aromatic ring, such as cyclohexyl vinyl ether, 2-methylcyclohexyl vinyl ether, cyclohexyl methyl vinyl ether, and benzyl vinyl ether; glycerol monovinyl ether, 1,4-butanediol monovinyl ether, 1,4-butanediol divinyl ether, Mono- to polyvinyl ethers of polyhydric alcohols such as 1,6-hexanediol divinyl ether, neopentyl glycol divinyl ether, pentaerythritol divinyl ether, pentaerythritol tetravinyl ether, trimethylolpropane divinyl ether, trimethylolpropane trivinyl ether, 1,4-dihydroxycyclohexane monovinyl ether, 1,4-dihydroxycyclohexane divinyl ether, 1,4-dihydroxymethylcyclohexane monovinyl ether, and 1,4-dihydroxymethylcyclohexane divinyl ether; polyalkylene glycol mono- to divinyl ethers such as diethylene glycol divinyl ether, triethylene glycol divinyl ether, and diethylene glycol monobutyl monovinyl ether; other vinyl ethers such as glycidyl vinyl ether and ethylene glycol vinyl ether methacrylate.
[0044] The cationic polymerization initiator is preferably a photocationic polymerization initiator. The photocationic polymerization initiator is a substance that generates cationic species or Lewis acid due to irradiation with active energy rays and initiates the polymerization reaction of a cationic curable compound. Since the photocationic polymerization initiator exerts a catalytic effect through light, even if it is mixed into a photocationic polymerizable compound, the storage stability and operability are excellent. As the photocationic polymerization initiator, for example, onium salts such as aromatic iodonium salts and aromatic sulfonium salts, aromatic diazonium salts, iron-arene complexes, etc. can be cited. The active energy ray-curable adhesive composition can use two or more cationic polymerization initiators. The content of the cationic polymerization initiator is generally 0.5 to 10 parts by mass relative to 100 parts by mass of the cationic polymerizable compound.
[0045] Free radical polymerizable compounds refer to compounds or oligomers that undergo free radical polymerization reactions and solidify due to irradiation with active energy rays or heating, and specifically include compounds having ethylenically unsaturated bonds. Examples of compounds having ethylenically unsaturated bonds include (meth)acrylic compounds having one or more (meth)acryloyl groups in the molecule; vinyl compounds such as styrene, styrenesulfonic acid, vinyl acetate, vinyl propionate, and N-vinyl-2-pyrrolidone. Here, the so-called (meth)acryloyl group refers to either an acryloyl group or a methacryloyl group, and the "(meth)" when referring to (meth)acrylates, etc., has the same meaning.
[0046] The active energy ray-curable adhesive composition may contain two or more radical polymerizable compounds.
[0047] The radical polymerization initiator is preferably a photoradical polymerization initiator. A photoradical polymerization initiator is a substance that initiates a polymerization reaction of a radical polymerizable compound due to irradiation with active energy rays. Examples of the photoradical polymerization initiator include acetophenone-based initiators such as acetophenone and 3-methylacetophenone; benzophenone-based initiators such as benzophenone and 4-chlorobenzophenone; benzoin ether-based initiators such as benzoin propyl ether and benzoin ethyl ether; and thioxanthone-based initiators such as 4-isopropylthioxanthone. The active energy ray-curable adhesive composition may use two or more photoradical polymerization initiators.
[0048] The active energy ray-curable composition may contain various additives as required, such as sensitizers, ion trapping agents, antioxidants, chain transfer agents, tackifiers, thermoplastic resins, fillers, flow regulators, plasticizers, defoamers, and the like.
[0049] The first cured product layer 2 can be obtained, for example, by applying an active energy ray-curable adhesive composition on the polarizing film 1 or the first resin film 3 and curing the applied active energy ray-curable adhesive composition by irradiating the film with active energy rays.
[0050] When applying the active energy ray-curable adhesive composition, a known coating method such as a doctor blade, a wire bar, a die coater, a comma-type doctor blade coater, or a gravure coater can be used.
[0051] The light source used to cure the active energy ray-curable adhesive composition is preferably a light source having a light emission distribution at a wavelength of 400 nm or less, and examples thereof include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.
[0052] The light irradiation intensity when curing the active energy ray-curable adhesive composition can be appropriately set according to the active energy ray-curable adhesive composition, but the light irradiation intensity in the wavelength region effective for activating the polymerization initiator is preferably 0.1 to 1000 mW / cm 2 If the light irradiation intensity during the curing of the active energy ray-curable adhesive composition is too low, the time required for the reaction to fully proceed will be long. On the contrary, if the light irradiation intensity is too high, the heat radiated by the lamp and the heat released during the polymerization of the active energy ray-curable adhesive composition may cause degradation of the bonded film. The light irradiation time during the curing of the active energy ray-curable adhesive composition is not particularly limited, but it is preferred to set the cumulative light amount expressed as the product of the light irradiation intensity and the light irradiation time to 10 to 5000 mJ / cm 2 If the accumulated light intensity is too small, the generation of active species from the polymerization initiator is insufficient, and the resulting curing may be insufficient. In addition, if the accumulated light intensity is too large, the irradiation time becomes very long, which is not conducive to improving productivity.
[0053] From the viewpoint of optical properties, the average refractive index of the first cured product layer 2 is preferably 1.59 or less, more preferably 1.55 or less, further preferably 1.54 or less, particularly preferably 1.51 or less, and preferably 1.49 or more, more preferably 1.50 or more.
[0054] The average refractive index of the first cured product layer 2 can be adjusted by appropriately selecting the type of polymerizable compound contained in the active energy ray-curable adhesive composition, the content thereof, etc. For example, when the active energy ray-curable adhesive composition is a photocationic polymerizable adhesive composition, by containing a compound having a high refractive index of the compound itself, such as an alicyclic epoxy compound or an aromatic epoxy compound, the average refractive index of the first cured product layer 2 tends to be higher.
[0055] As the active energy ray-curable adhesive composition forming the first cured product layer 2 , a photocationically polymerizable adhesive composition or a photoradical polymerizable adhesive composition is preferred.
[0056] The thickness of the first cured product layer 2 is not particularly limited, but is preferably 0.1 μm or more, more preferably 0.5 μm or more, further preferably 1 μm or more, and particularly preferably 2.1 μm or more. Also, it is preferably 20 μm or less, more preferably 10 μm or less, and further preferably 5 μm or less.
[0057] <First resin film>
[0058] The first resin film 3 includes at least a film formed of a thermoplastic resin. The first resin film 3 may be formed of one layer or may be formed of two or more layers. The first resin film 3 may be, for example, a single resin film formed of a thermoplastic resin, a laminated film in which a plurality of resin films formed of thermoplastic resins are laminated, or a film in which a resin cured layer is formed on at least one surface of a resin film formed of a thermoplastic resin.
[0059] When the first resin film 3 is formed of a plurality of layers, the difference between the average refractive index of the layer in direct contact with the first cured product layer among the plurality of layers of the first resin film and the average refractive index of the first cured product layer is 0.03 or less. For example, when the first resin film 3 is a film including two layers, namely, a resin cured layer and a resin film formed of a thermoplastic resin, if the layer in direct contact with the first cured product layer is the resin cured layer, the difference in refractive index between the resin cured layer and the first cured product layer is 0.03 or less, and if the first cured product layer is in direct contact with a resin film formed of a thermoplastic resin, the difference in refractive index between the layer formed of the thermoplastic resin and the first cured product layer is 0.03 or less.
[0060] Specifically, the film formed by the thermoplastic resin can be exemplified by polyolefin resins such as polyethylene, polypropylene, and polymethylpentene; cyclic polyolefin resins having a cycloolefin or norbornene structure: fluorinated polyolefin resins such as polyvinylfluoride, polyvinylidene fluoride, and polyethylenefluoride; polyethylene naphthalate, polyethylene terephthalate, polybutylene terephthalate, and polyethylene terephthalate / isophthalate copolymers. Polyester resins such as nylon 6 and nylon 6,6; polyamides such as polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, and vinyl polymers such as vinylon; cellulose resins such as triacetyl cellulose, diacetyl cellulose, and cellophane (Japanese: セロハン); (meth) acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; and resin films formed from polystyrene, polycarbonate, polyarylate, and polyimide.
[0061] The resin film formed of the thermoplastic resin may be a film formed of a composition containing the above resin and additives. Examples of the additives include ultraviolet absorbers, antioxidants, surfactants, plasticizers, lubricants, anti-blocking agents, and the like.
[0062] The average refractive index of a resin film formed of a thermoplastic resin can be adjusted by the type of resin, the degree of polymerization of the resin, etc. Alternatively, the average refractive index can be adjusted by adding additives to the resin.
[0063] The resin film formed of a thermoplastic resin is preferably a cellulose resin film, a (meth)acrylic resin film, or a cycloolefin resin film, and more preferably a cycloolefin resin film.
[0064] When the first resin film 3 includes a resin cured layer, there is no particular limitation on the resin cured layer as long as the average refractive index difference is within a specified range, but the resin cured layer is usually a layer formed from a resin composition, and is a cured product layer of the resin composition. Specifically, a layer formed from a water-based resin composition, a layer formed from an active energy ray-curable composition, etc. can be cited.
[0065] The water-based resin composition is not particularly limited, and at least comprises a resin component, which is a composition in which the resin component is dissolved or dispersed in water. As the resin forming the water-based resin composition, for example, polyvinyl alcohol resin, polyurethane resin, polyester resin, acrylic resin with crosslinking functional groups such as oxazoline groups, etc. can be cited. In the case where the film formed by the thermoplastic resin is a cycloolefin resin film, from the viewpoint of the adhesion with the film, the resin cured layer is preferably formed by a polyurethane resin.
[0066] Typically, the polyurethane resin is a reaction product of a polyol and a polyisocyanate. Preferably, a high molecular weight polyol such as a polyacrylic polyol obtained by polymerization of a (meth)acrylate and a hydroxyl-containing monomer, a polyester polyol obtained by reaction of a polyacid and a polyol, or a polyether polyol obtained by reaction of a polyacid and a polyol is used as the polyol component.
[0067] In addition, the polyurethane resin may have an acid structure. Examples of the acid structure include acid groups such as carboxyl (-COOH) and sulfonic acid (-SO3H). In addition, the acid structure may be present in the side chain or at the end of the polyurethane resin. It should be noted that one acid structure may be used or two or more acid structures may be used in combination at any ratio. The content of the acid structure is preferably 10 mgKOH / g to 250 mgKOH / g or less in terms of the acid value in the polyurethane.
[0068] As the polyurethane resin, commercially available products may be used. For example, the “ADEKA BONTIGHTER” series manufactured by ADEKA, the “OLESTER” series manufactured by Mitsui Chemicals, the “VONDIC” series and the “HYDRAN” series manufactured by Dainippon Ink and Chemicals, the “Impranil” series manufactured by Bayer, the “POIZ” series manufactured by Kao Corporation, the “Sanprene” series manufactured by Sanyo Chemical Industries, Ltd., the “Izelax” series manufactured by Hodogaya Chemical Industries, Ltd., the “Superflex” series manufactured by Dai-ichi Kogyo Seiya, the “Neorez” series manufactured by Zeneca, the “Sancure” series manufactured by Lubrizol, and the like may be used.
[0069] In addition, the polyurethane may be used individually by 1 type, and may use 2 or more types together at any ratio.
[0070] The water-based resin composition may contain a crosslinking agent. As the crosslinking agent, a crosslinking agent capable of reacting with the crosslinking functional group of the polyurethane resin may be used without particular limitation. In the case where the polyurethane resin has a carboxyl group, a crosslinking agent containing an amino group, an oxazoline group, an epoxy group, a carbodiimide group, etc. may be used.
[0071] The water-based resin composition may contain an alkali component. As the alkali component, inorganic bases such as sodium hydroxide and potassium hydroxide can be cited; primary amine compounds, secondary amine compounds, tertiary amine compounds, hydrazide compounds, imidazoline compounds, etc. Among them, compounds having a hydrazine group (-NHNH2 group) like hydrazide compounds can appropriately improve the mechanical strength of the polyurethane resin layer, so they are preferred. As hydrazide compounds, for example, carbodihydrazide (Japanese: カルボジヒドラジド), oxalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, glycolic acid dihydrazide, polyacrylic acid dihydrazide, etc. can be cited.
[0072] The resin cured layer may be a film formed of a composition containing the above resin and additives. Examples of the additives include ultraviolet absorbers, antioxidants, surfactants, plasticizers, lubricants, anti-blocking agents, inorganic particles, and organic fine particles.
[0073] The average refractive index of the cured resin layer can be adjusted by the type of resin, the degree of polymerization of the resin, the type of crosslinking agent, etc. Alternatively, the average refractive index can be adjusted by adding an additive to the resin.
[0074] The thickness of the cured resin layer is usually 0.01 to 5 μm, preferably 0.03 to 2 μm, and more preferably 0.05 to 0.5 μm.
[0075] The first resin film 3 may or may not have a phase difference value. In addition, the first resin film 3 may have a phase difference in the plane or in the thickness direction. e and the retardation R in the thickness direction th It is defined by the following formulas (1) and (2).
[0076] R th =〔(n x +n y ) / 2-n z 〕×d (1)
[0077] R e =(n x -n y )×d (2)
[0078] (where n x is the refractive index in the slow axis direction (x-axis direction) of the film surface at a wavelength of 586 nm, n y is the refractive index in the fast axis direction (the y-axis direction orthogonal to the x-axis in the plane) of the film at a wavelength of 586 nm, n z is the refractive index in the thickness direction of the film (the z-axis direction perpendicular to the film surface) at a wavelength of 586 nm, and d is the thickness of the film.
[0079] From the viewpoint of optical properties, the average refractive index of the first resin film 3 (a layer in direct contact with the first cured layer when two or more layers are included) is preferably 1.44 to 1.57, more preferably 1.45 to 1.55, further preferably 1.48 to 1.54, and particularly preferably 1.52 to 1.53.
[0080] From the perspective of ease of operation when stacked on a polarizing film, the thickness of the first resin film 3 is preferably 6 μm or more, more preferably 12 μm or more, further preferably 20 μm or more, particularly preferably 40 μm or more, preferably 200 μm or less, more preferably 180 μm or less, further preferably 150 μm or less, particularly preferably 100 μm or less. When the first resin film 3 is formed of multiple layers, the total of the layers may be within the above range.
[0081] <Polarizing film>
[0082] The polarizing film 1 is a film having the function of extracting linear polarized light from incident natural light. As the polarizing film 1, a film in which a dichroic pigment (preferably iodine) is contained in a polyvinyl alcohol resin film and the dichroic pigment is adsorbed and oriented can be cited. The film in which the polyvinyl alcohol resin film adsorbs the dichroic pigment and orients the dichroic pigment can be manufactured using a known method, usually through a process of uniaxially stretching the polyvinyl alcohol resin film, a process of dyeing the polyvinyl alcohol resin film with a dichroic pigment to adsorb the dichroic pigment, and a process of treating the polyvinyl alcohol resin film adsorbed with the dichroic pigment with an aqueous boric acid solution. In addition, for example, a film in which the polyvinyl alcohol resin film adsorbs the dichroic pigment and orients the dichroic pigment can also be obtained using the method described in Japanese Patent Publication No. 2012-159778.
[0083] The thickness of the polarizing film 1 is preferably 3 to 30 μm, more preferably 10 to 25 μm.
[0084] The average refractive index of the polarizing film 1 is preferably the same as or larger than the average refractive index of the first cured material layer 2 .
[0085] It is preferable that the average refractive index of the polarizing film 1 is larger than the average refractive index of the first resin film 3 .
[0086] <Second cured material layer>
[0087] The polarizing plate with an adhesive layer of the present invention may include a second cured layer 4 on the surface of the polarizing film 1 opposite to the first cured layer 2. Although another layer may be present between the second cured layer 4 and the polarizing film 1, it is preferred that the second cured layer 4 and the polarizing film 1 are in direct contact.
[0088] The second cured product layer 4 is usually a layer formed of a resin composition, and is a cured product layer of the resin composition. Specifically, there can be mentioned a layer formed of an adhesive composition (adhesive layer), a layer formed of a water-based adhesive composition, a layer formed of an active energy ray-curable composition, and the like.
[0089] The resin composition forming the second cured material layer 4 may be the same as or different from the resin composition forming the first cured material layer 2 .
[0090] The second cured product layer 4 is preferably a layer formed of an active energy ray-curable composition.
[0091] <Second resin film>
[0092] The second resin film 5 is preferably a film having excellent transparency, mechanical strength, thermal stability, water barrier properties, isotropy, etc. For example, polyester polymers such as polyethylene terephthalate and polyethylene naphthalate; cellulose polymers such as diacetyl cellulose and triacetyl cellulose; acrylic polymers such as polymethyl methacrylate; styrene polymers such as polystyrene and acrylonitrile-styrene copolymer (AS resin); and polycarbonate polymers. In addition, polyethylene, polypropylene, polyolefins having a ring system or norbornene structure; polyolefin polymers such as ethylene-propylene copolymer; amide polymers such as vinyl chloride polymers, nylon, and aromatic polyamide; imide polymers, sulfone polymers, polyethersulfone polymers, polyetheretherketone polymers, polyphenylene sulfide polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl butyral polymers, arylate polymers, polyoxymethylene polymers, epoxy polymers, or blends of the above polymers can be cited.
[0093] The second resin film 5 and the first resin film 3 may be the same resin film or different resin films.
[0094] The second resin film 5 is preferably a film with low water vapor permeability. The water vapor permeability of the second resin film 5 is preferably 800 g / (m 2 ·24 hours) or less, more preferably 600g / (m 2 ·24 hours) or less, more preferably 400g / (m 2 ·24 hours) or less, particularly preferably 200g / (m 2 ·24 hours) or less, particularly preferably 100g / (m 2 If the moisture permeability of the second resin film 5 is below the above value, it is possible to prevent moisture from entering from the outside under high temperature and high humidity conditions, and prevent the movement of the dichroic pigment (iodine) contained in the polarizing film 1 from being accelerated, thereby more effectively preventing the degradation of optical properties.
[0095] The thickness of the second resin film 5 is not particularly limited, but is usually 5 to 500 μm, preferably 1 to 300 μm, more preferably 5 to 200 μm, and further preferably 10 to 100 μm.
[0096] <Adhesive layer>
[0097] The adhesive layer 6 may be a layer formed of a known adhesive composition. Examples of the adhesive composition include adhesive compositions having acrylic resins, rubber resins, polyurethane resins, silicone resins, polyvinyl ether resins, and the like as base polymers.
[0098] In addition, the adhesive composition may be an energy-ray-curable adhesive composition or a thermosetting adhesive composition.
[0099] The adhesive composition forming the adhesive layer 6 is preferably an acrylic adhesive composition having an acrylic resin as a base polymer, which is excellent in transparency, adhesive strength, reworkability, weather resistance, heat resistance, and the like.
[0100] The adhesive layer 6 can be provided by the following method: the adhesive composition is made into an organic solvent solution, applied to the first resin film 4 by a die coater, a gravure coater, etc., and dried. Alternatively, the adhesive layer 6 can be provided by a method of transferring a sheet-like adhesive composition formed on a plastic film (referred to as a release film) subjected to a demolding treatment to the first resin film 4.
[0101] The thickness of the adhesive layer 6 is not particularly limited, but is preferably in the range of 2 to 40 μm, more preferably in the range of 5 to 35 μm, and even more preferably in the range of 10 to 30 μm.
[0102] The storage modulus of the adhesive layer 6 is preferably 0.10 to 5.0 MPa at 23 to 80°C, and more preferably 0.15 to 1.0 MPa. If the storage modulus at 23 to 80°C is 0.10 MPa or more, the whitening caused by the shrinkage of the polarizing plate with an adhesive layer when the liquid crystal display panel including the polarizing plate with an adhesive layer is exposed to high temperature, etc. can be suppressed, so it is preferred. In addition, if it is 5 MPa or less, it is not easy to cause a decrease in durability due to a decrease in adhesion, so it is preferred. Here, the so-called "displaying a storage modulus of 0.10 to 5.0 MPa at 23 to 80°C" means that the storage modulus takes the value of the above range at any temperature in the range. The storage modulus usually decreases gradually with the increase in temperature, so if the storage moduli at 23°C and 80°C both fall within the above range, it can be regarded as that the adhesive layer shows the storage modulus in the above range at a temperature in the range. The storage elastic modulus of the adhesive layer can be measured using a commercially available viscoelasticity measuring device, for example, a viscoelasticity measuring device “DYNAMIC ANALYZER RDA II” manufactured by REOMETRIC Corporation.
[0103] The average refractive index of the pressure-sensitive adhesive layer 6 is preferably 1.45 to 1.49, more preferably 1.46 to 1.47.
[0104] The average refractive index of the adhesive layer 6 is preferably the same as the average refractive index of the first resin film 3, or smaller than the average refractive index of the first resin film 3. The difference between the average refractive index of the adhesive layer 6 and the average refractive index of the first resin film 3 is preferably 0.12 or less, more preferably 0.10 or less, and further preferably 0.08 or less.
[0105] The average refractive index of the pressure-sensitive adhesive layer 6 can be adjusted by changing the type of the base polymer or the type of the cross-linking agent.
[0106] The present invention also includes an image display device having a polarizing plate with an adhesive layer of the present invention and an image display panel laminated thereon. Preferably, the polarizing plate with an adhesive layer of the present invention is laminated on the visible side of the image display panel (the side opposite to the backlight in the case of a liquid crystal display panel). The image display panel may be a liquid crystal display panel or an organic EL display panel.
[0107] Example
[0108] The present invention will be described in further detail below using examples, but the present invention is not limited to these examples. It should be noted that "%" and "parts" in the examples and comparative examples represent "mass %" and "mass parts" respectively unless otherwise specified.
[0109] <Method for measuring the refractive index of active energy ray-curable adhesive>
[0110] The active energy ray curable adhesive was applied to one side of a stretched norbornene resin film (ZEONOR FILM, manufactured by ZEON Corporation) using a bar coater (manufactured by Daiichi Rika Co., Ltd.) and then irradiated with an ultraviolet ray device (manufactured by Fusion UV Systems Co., Ltd.) at a cumulative light intensity of 600 mJ / cm 2 (UV-B) UV rays were irradiated to obtain a cured product. The obtained cured product had a film thickness of about 30 μm.
[0111] The norbornene-based resin film was peeled off from the obtained cured product, and the refractive index (wavelength: 589 nm) of the cured product layer was measured under a 25° C. environment using a multi-wavelength Abbe refractometer [“DR-M2” manufactured by ATAGO Corporation].
[0112] The refractive index of the cured product of the active energy ray-curable adhesive a was 1.54, and the refractive index of the cured product of the active energy ray-curable adhesive b was 1.51.
[0113] <Manufacturing Example 1: Manufacture of Polarizing Film>
[0114] After immersing a polyvinyl alcohol film having an average degree of polymerization of about 2400, a saponification degree of 99.9 mol% or more and a thickness of 75 μm in pure water at 30° C., the film was immersed in an aqueous solution having a mass ratio of iodine / potassium iodide / water of 0.02 / 2 / 100 at 30° C. to perform iodine dyeing (iodine dyeing step). The polyvinyl alcohol film that had undergone the iodine dyeing step was immersed in an aqueous solution having a mass ratio of potassium iodide / boric acid / water of 12 / 5 / 100 at 56.5° C. to perform boric acid treatment (boric acid treatment step).
[0115] The polyvinyl alcohol film after the boric acid treatment step was washed with pure water at 8°C and dried at 65°C to obtain a polarizer in which iodine was adsorbed and oriented in the polyvinyl alcohol. At this time, stretching was performed in the iodine dyeing step and the boric acid treatment step. The total stretching ratio in the stretching was 5.3 times, and the thickness of the obtained polarizer was 27 μm.
[0116] <Production Example 1: Production of Polarizing Plate>
[0117] The resin films used for producing the polarizing plate are shown below.
[0118] Film A: 80 μm film made of (meth)acrylic resin
[0119] Film B: 50 μm film made of cycloolefin resin with an average refractive index of 1.53 (in-plane retardation Re=50 nm, retardation in the thickness direction Rth=135 nm)
[0120] Film C: A film in which a cured resin layer X having a thickness of 50 nm and an average refractive index of 1.57 is formed on one surface of a cycloolefin-based resin film (film B).
[0121] A corona discharge treatment is applied to one side of the film A, and an active energy ray-curable curable composition b is applied to the corona discharge treated surface so that the thickness after curing is about 3.5 μm. Then, the polarizer prepared in Manufacturing Example 1 is bonded to the coated surface. Then, a corona discharge treatment is applied to one side of the film B, and an active energy ray-curable curable composition a is applied to the corona discharge treated surface so that the thickness after curing is about 2.5 μm. The polarizer with the film A prepared above is overlapped on the coated surface with the polarizer side, and a laminating roller is used to press and bond to obtain a laminate. For the obtained laminate, an ultraviolet irradiation device with a conveyor belt is used from the film B side [the lamp uses a "D bulb" made by Fusion UV Systems] so that the cumulative light amount is 400 mJ / cm 2 The polarizing plate is prepared by irradiating ultraviolet rays in the manner of UVB to cure the adhesive layers on both sides. The structure of the obtained polarizing plate is film A (second resin film) / cured material layer of curable composition b (second cured material layer) / polarizing film / cured material layer of curable composition a (first cured material layer) / film B (first resin film), and the absolute value of the refractive index difference between the first cured material layer and the first resin film is 0.01.
[0122] Example 1: Preparation of a polarizing plate with an adhesive layer
[0123] An organic solvent solution of an acrylic adhesive was applied to a release-treated surface of a 38 μm thick polyethylene terephthalate film using a die coater and dried to prepare a sheet-like adhesive layer with a release film. The thickness of the adhesive layer was 20 μm.
[0124] The release film was peeled off from the produced sheet-like adhesive layer, and the refractive index of the adhesive layer (wavelength 589 nm) was measured using a multi-wavelength Abbe refractometer ["DR-M2" manufactured by ATAGO Corporation] at 25° C. The refractive index of the adhesive layer was 1.47.
[0125] <Production of polarizing plate with adhesive layer>
[0126] The surface of the film B (first resin film) of the polarizing plate was subjected to a corona treatment, and the surface (adhesive surface) of the sheet-like adhesive prepared in Preparation Example 2 on the opposite side to the release film was laminated using a laminator, and then aged for 7 days at a temperature of 23° C. and a relative humidity of 65%, thereby obtaining a polarizing plate with an adhesive layer having an adhesive layer. The laminated body has a structure in which a release film is laminated on the adhesive layer.
[0127] <Production of a single piece>
[0128] Use a cutting device (super cutter "PN1-600" manufactured by Ogino Seiki Mfg. Co., Ltd.) to cut the above-mentioned polarizing plate with an adhesive layer so that the length of the polarizing plate with adhesive in the stretching direction (MD) of the polarizer from the film A side is 50 mm, and the length of the polarizer in the direction intersecting the stretching direction (TD) is 50 mm.
[0129] <Evaluation of light leakage at the end>
[0130] After peeling off the release film from the obtained polarizing plate with an adhesive layer, the adhesive layer is bonded to the center of a 0.7 mm thick glass substrate ["Eagle XG" manufactured by Corning] to obtain a laminate. The obtained laminate is placed on a backlight so that the 10 mm (MD) × 50 mm (TD) polarizing plate portion of the 50 mm × 50 mm is exposed from the bright part of the backlight. Then, the polarizing plate (40 mm × 50 mm) in the bright part of the backlight and the entire bright part of the backlight are covered with a black acrylic plate. Turn on the power of the backlight and tilt it from 85° ( Figure 3 The edge of the polarizing plate was visually checked at an angle of θ=85°. The results were determined according to the following criteria. The results are shown in Table 1.
[0131] <Light leakage judgment criteria>
[0132] ○: Light leakage is hardly observed.
[0133] △: Light leakage is slightly observed.
[0134] ×: Light leakage is strongly observed.
[0135] Example 2: Production of polarizing plate
[0136] A polarizing plate with an adhesive layer was prepared in the same manner as in Example 1 except that the curable composition b was used as the composition for forming the first cured product layer, and the same evaluation was performed.
[0137] Example 3: Production of polarizing plate
[0138] A corona discharge treatment is applied to one side of the film A, and an active energy ray-curable curable composition b is applied to the corona discharge treated surface so that the thickness after curing is about 3.5 μm. Then, the polarizer prepared in Manufacturing Example 1 is bonded to the coated surface. Then, a corona discharge treatment is applied to the cycloolefin resin film surface of the film C, and an active energy ray-curable curable composition b is applied to the corona discharge treated surface so that the thickness after curing is about 2.5 μm. The polarizer with the film A prepared above is overlapped on the coated surface with the polarizer side, and a laminating roller is used to press and bond to obtain a laminate. The obtained laminate is irradiated with an ultraviolet ray with a conveyor belt from the film C side [the lamp uses a "D bulb" made by Fusion UV Systems] so that the cumulative light amount is 400 mJ / cm 2 The polarizing plate is prepared by irradiating ultraviolet rays in the manner of UVB to cure the adhesive layers on both sides. The obtained polarizing plate is composed of film A (second resin film) / cured material layer of curable composition b (second cured material layer) / polarizing film / cured material layer of curable composition b (first cured material layer) / film C (cycloolefin resin film / resin cured layer X), and the absolute value of the refractive index difference between the first cured material layer and the cycloolefin resin film is 0.02.
[0139] An adhesive layer was formed on the surface of the cured resin layer X and evaluated in the same manner as in Example 1. Table 1 shows the results.
[0140] Example 4: Production of polarizing plate
[0141] A polarizing plate was produced in the same manner as in Example 3 except that the resin cured layer X surface of the film C was subjected to corona discharge treatment and the active energy ray-curable curable composition a was applied to the corona discharge treated surface so as to have a thickness of about 2.5 μm after curing.
[0142] The structure of the obtained polarizing plate is film A (second resin film) / cured layer of curable composition b (second cured layer) / polarizing film / cured layer of curable composition a (first cured layer) / film C (resin cured layer X / cycloolefin resin film), and the absolute value of the refractive index difference between the first cured layer and the resin cured layer X is 0.03.
[0143] An adhesive layer was formed on the surface of the cycloolefin-based resin film in the same manner as in Example 1 and evaluated. Table 1 shows the results.
[0144] Comparative Example 1: Production of polarizing plate
[0145] Except that the active energy ray curable composition a is replaced by the active energy ray curable composition b, a polarizing plate with an adhesive layer is prepared in the same manner as in Example 4, and the same evaluation is performed. The structure of the obtained polarizing plate with an adhesive layer is film A (second resin film) / curable composition b's cured layer (second cured layer) / polarizing film / curable composition b's cured layer (first cured layer) / film C (resin cured layer X / cycloolefin resin film) / adhesive layer, and the absolute value of the refractive index difference between the first cured layer and the resin cured layer is 0.06. The results are shown in Table 1.
[0146] [Table 1]
[0147]
[0148] The polarizing plate with an adhesive layer of the present invention can suppress light leakage even when it is observed at an angle of approximately 85° relative to the surface of the polarizing plate. Therefore, when the polarizing plate with an adhesive layer of the present invention is installed in a display device in which the height of the frame provided in the display device is reduced or the frame is omitted, light leakage can be suppressed even if the end of the polarizing plate is exposed.
[0149] Industrial Applicability
[0150] The polarizing plate with an adhesive layer of the present invention is useful because light leakage from the edge of the polarizing plate is small even when incorporated in a display device with a narrow frame width, a display device with a reduced frame height, or a display device without a frame.
[0151] Description of Reference Numerals
[0152] 1 polarizing film, 2 first cured layer, 3 first resin film, 4 second cured layer, 5 second resin film, 6 adhesive layer, 7 image display panel, 10 polarizing plate, 20 polarizing plate with adhesive layer, 30 image display device, θ is an angle relative to the front surface of the polarizing plate.
Claims
1. A polarizing plate with an adhesive layer, comprising, in order, a polarizing film, a first cured layer, a first resin film, and an adhesive layer. The polarizing film is in direct contact with the first cured material layer. The first cured product layer is in direct contact with the first resin film, The first resin film is in direct contact with the adhesive layer, The absolute value of the difference between the average refractive index of the first cured product layer and the average refractive index of the first resin film is 0.03 or less, The thickness of the first resin film is 20 μm or more, The thickness of the first cured product layer is 10 μm or less. The difference between the average refractive index of the first resin film and the average refractive index of the adhesive layer is 0.08 or less.
2. The polarizing plate according to claim 1, in, The first cured product layer is a cured product of the active energy ray-curable adhesive composition.
3. The polarizing plate according to claim 1, in, The refractive index of the first cured product layer is 1.55 or less.
4. The polarizing plate according to claim 2, in, The refractive index of the first cured product layer is 1.55 or less.
5. The polarizing plate according to any one of claims 1 to 4, in, The first resin film includes a film formed of a thermoplastic resin.
6. The polarizing plate according to any one of claims 1 to 4, in, The polarizing film includes a second resin film on a surface opposite to the first cured material layer via a second cured material layer. 7 . An image display device comprising an image display panel and the polarizing plate with a pressure-sensitive adhesive layer according to claim 1 , which is disposed on a viewing side of the image display panel.