Thermoelectric conversion element, thermoelectric conversion assembly, bonding material, and method for manufacturing thermoelectric conversion element
By using thermoelectric conversion materials containing Mg, Sb and Bi and specific bonding materials, the problem of deterioration of thermoelectric conversion components at high temperatures is solved, and the thermoelectric conversion efficiency with small resistance value is achieved, which is suitable for N-type and P-type thermoelectric conversion. Material.
Patent Information
- Application Number
- CN202080064738.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-25
- Filing Date
- 2020-11-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-11-17
AI Technical Summary
The existing thermoelectric conversion elements are prone to deterioration at high temperatures, resulting in an increase in resistance value and a decrease in thermoelectric conversion efficiency, and it is difficult to stabilize the Mg content to maintain thermoelectric characteristics.
Using thermoelectric conversion materials containing Mg, Sb and Bi, and through specific bonding materials and manufacturing methods, ensure that the Mg content does not decrease at high temperatures. Use Mg alloy as bonding material to ensure good bonding between the thermoelectric conversion layer and the metal layer. , reduce the resistance value.
The resistance value of the thermoelectric conversion element is small and stable at high temperature, avoiding the reduction of the thermoelectric conversion efficiency, and improving the heat resistance and bonding performance of the thermoelectric conversion module.
Smart Images

Figure CN114402445B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thermoelectric conversion element, a thermoelectric conversion assembly, a bonding material and a method for manufacturing the thermoelectric conversion element. Background Art
[0002] Thermoelectric conversion elements are well known. A thermoelectric conversion assembly can be used, which is formed by electrically connecting a P-type thermoelectric conversion element composed of a P-type thermoelectric conversion material and an N-type thermoelectric conversion element composed of an N-type thermoelectric conversion material. The thermoelectric conversion assembly can realize power generation based on the temperature difference caused by the influx of thermal energy. In order to facilitate the electrical connection of the thermoelectric conversion element, there is a method of pre-joining a metal part using a bonding material or the like on the end face of the thermoelectric conversion material. Such an end face is easy to handle or assemble the thermoelectric conversion element as a metal part.
[0003] Non-Patent Document 1 discloses a thermoelectric conversion element composed of a MgAgSb-based thermoelectric conversion material and a pair of Ag electrodes bonded to the material.
[0004] Patent Document 1 discloses a MgSbBiTe-based thermoelectric conversion material.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 6127281
[0008] Non-patent literature
[0009] Non-patent document 1: D. Kraemer et.al., "High thermoelectric conversion efficiency of MgAgSb-based material with hot-pressed contacts", Energy Environ. Sci., 2015, 8, 1299-1308 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The object of the present invention is to provide a thermoelectric conversion element having a small resistance value using a thermoelectric conversion material containing Mg, Sb and Bi. In addition, the object of the present invention is to provide a thermoelectric conversion module having the thermoelectric conversion element, a bonding material advantageous for manufacturing the thermoelectric conversion element, and a method for manufacturing the thermoelectric conversion element.
[0012] Methods for solving problems
[0013] The present invention provides a thermoelectric conversion element, comprising:
[0014] Thermoelectric conversion layer;
[0015] 1st metal layer;
[0016] 2nd metal layer;
[0017] A first bonding layer bonding the first surface of the thermoelectric conversion layer and the first metal layer; and
[0018] a second bonding layer bonding the second surface of the thermoelectric conversion layer to the second metal layer;
[0019] The thermoelectric conversion layer is composed of a thermoelectric conversion material containing Mg and at least one of Sb and Bi.
[0020] The first metal layer and the second metal layer are respectively composed of a metal monomer or a first alloy.
[0021] At least one of the first bonding layer and the second bonding layer is composed of a second alloy,
[0022] In the above second alloy,
[0023] The content ratio of Mg is 84 atm% or more and 89 atm% or less,
[0024] The content of Cu is 11 atm% or more and 15 atm% or less.
[0025] The content ratio of the alkaline earth metal is 0 atm % or more and 1 atm % or less.
[0026] Effects of the Invention
[0027] According to the present invention, a thermoelectric conversion element having a small resistance value is provided using a thermoelectric conversion material containing Mg, Sb and Bi. In addition, the present invention provides a thermoelectric conversion module having the thermoelectric conversion element, a bonding material advantageous for manufacturing the thermoelectric conversion element, and a method for manufacturing the thermoelectric conversion element. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram showing an example of the thermoelectric conversion element of the present invention.
[0029] Figure 2 It is a schematic diagram of the La2O3 type crystal structure of the present invention.
[0030] Figure 3A This is a graph showing an example of an X-ray diffraction pattern of a La2O3 type crystal structure.
[0031] Figure 3BThis is a graph showing the results of X-ray diffraction analysis of the thermoelectric conversion material of the present invention.
[0032] Figure 4 This is a schematic diagram showing an example of the thermoelectric conversion module of the present invention.
[0033] Figure 5 It is a schematic diagram showing a modified example of the thermoelectric conversion module of the present invention.
[0034] Figure 6 This is a schematic diagram showing one mode of use of the thermoelectric conversion module of the present invention.
[0035] Figure 7 This is a process diagram of a method for manufacturing the thermoelectric conversion element of the present invention.
[0036] Figure 8 This is a schematic diagram showing an example of a method for producing the thermoelectric conversion element of the present invention.
[0037] Fig. 9 It is a schematic diagram showing a modification of the method of manufacturing the thermoelectric conversion element of the present invention.
[0038] Fig.10 These are the results of observation of the cross-section of the thermoelectric conversion element produced in Example 1 using a scanning electron microscope (hereinafter referred to as “SEM”). DETAILED DESCRIPTION
[0039] (Knowledge that is the basis of the present invention)
[0040] Thermoelectric conversion materials containing Mg and at least one of Sb and Bi can exhibit high thermoelectric conversion characteristics at temperatures as high as 400°C. In particular, thermoelectric conversion materials of the Mg3(Sb,Bi)2 type can achieve high thermoelectric conversion performance such as a thermoelectric conversion performance index ZT=1.51 at 440°C. In this specification, (Sb,Bi) in the composition formula represents at least one of Sb and Bi. On the other hand, according to Journal of Solid State Chemistry, 2006, Vol.179, p.2252-2257, thermoelectric conversion materials containing Mg and at least one of Sb and Bi deteriorate due to decomposition of the compound when reaching 800K (527°C) or above, and there is a possibility that the thermoelectric conversion efficiency decreases. In addition, the N-type thermoelectric conversion material containing Mg and at least one of Sb and Bi can change its characteristics from N-type to P-type according to the content ratio of Mg contained in the thermoelectric conversion material. That is, with respect to N-type thermoelectric conversion materials, when the content of Mg contained in the thermoelectric conversion material decreases, the characteristics of the thermoelectric conversion material become unstable, for example, the resistance value of the thermoelectric conversion element changes, and there is a possibility that the thermoelectric conversion efficiency decreases. On the other hand, with respect to P-type thermoelectric conversion materials containing Mg and at least one of Sb and Bi, the influence of the content of Mg contained in the thermoelectric conversion material on the characteristics of the thermoelectric conversion material is small.
[0041] According to the research of the inventors, when a thermoelectric conversion element is manufactured in a manner in which the end face of the thermoelectric conversion element is a metal part, especially when an N-type thermoelectric conversion element is manufactured, the Mg content in the above-mentioned thermoelectric conversion material decreases due to the diffusion of Mg into the metal part, and research is needed to prevent the thermoelectric characteristics from being reduced.
[0042] The MgAgSb-based thermoelectric conversion element shown in Non-Patent Document 1 has a structure in which a metal component composed of an Ag electrode is bonded to its end surface. However, in Non-Patent Document 1, there is no report on the influence of Mg contained in the thermoelectric conversion element on the bonding property with the electrode. According to further research by the present inventors, it is newly found that by covering the bonding material for bonding a thermoelectric conversion material containing Mg, and at least one of Sb and Bi, and a metal component with Mg-rich, the thermoelectric conversion element can be made while maintaining the Mg content in the thermoelectric conversion material. Therefore, as the selection criteria for the bonding material, it is considered that: (i) it has heat resistance up to 400°C; (ii) it melts at a temperature that does not deteriorate the element, for example, a temperature that does not significantly exceed 500°C; and (iii) it is rich in Mg. The selection criteria of (iii) are particularly important as the selection criteria for bonding an N-type thermoelectric conversion material containing Mg, and at least one of Sb and Bi, and a metal component. On the other hand, the selection criteria of (iii), especially the selection criteria of the bonding material for bonding a P-type thermoelectric conversion material containing Mg, and at least one of Sb and Bi, to a metal part, are not necessary. However, by satisfying the selection criteria of (iii), a bonding material containing Mg, and at least one of Sb and Bi, which can be applied to both N-type thermoelectric conversion materials and P-type thermoelectric conversion materials, can be provided. The inventors of the present invention have repeatedly conducted a large number of trial and error, and gradually found a bonding material that meets the selection criteria. As a result, a thermoelectric conversion element is obtained in which, for example, the above-mentioned thermoelectric conversion material is well bonded to the metal part at a bonding temperature below 500°C and the resistance value is small.
[0043] (Embodiment of the present invention)
[0044] Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0045] (Thermoelectric conversion element)
[0046] Figure 1 An example of a thermoelectric conversion element according to an embodiment of the present invention is shown in FIG. Figure 1 The thermoelectric conversion element 10 shown in FIG. 1 includes a thermoelectric conversion layer 11, a first metal layer 14a, a second metal layer 14b, a first bonding layer 13a, and a second bonding layer 13b. The first bonding layer 13a bonds the first surface 12a of the thermoelectric conversion layer 11 to the first metal layer 14a. The second bonding layer 13b bonds the second surface 12b of the thermoelectric conversion layer 11 to the second metal layer 14b. Figure 1 The shape of the thermoelectric conversion element 10 shown in FIG. 1 is, for example, a rectangular parallelepiped. The shape of the thermoelectric conversion element 10 is not limited to a specific shape as long as it is a three-dimensional shape that can form the above-mentioned layers, and may be, for example, a cube, other prisms, or a cylinder.
[0047] [Thermoelectric conversion layer]
[0048] The thermoelectric conversion layer 11, for example, forms the middle layer of the thermoelectric conversion element 10. The thickness of the thermoelectric conversion layer 11 is not limited to a specific value, for example, it is greater than 0.5 mm and less than 50 mm. The thermoelectric conversion layer 11 is composed of a thermoelectric conversion material containing Mg, and at least one of Sb and Bi. The thermoelectric conversion material can be N-type or P-type. The composition of the N-type thermoelectric conversion material of this embodiment is, for example, represented by formula (I): Mg 3+m A a B b D 2-e E e Represented. Element A in formula (I) is at least one selected from Ca, Sr, Ba and Yb. Element B in formula (I) is at least one selected from Mn and Zn. Element D is at least one selected from Sb and Bi. Element E is at least one selected from Se and Te. The value of m in formula (I) is greater than -0.39 and less than 0.42. The value of a is greater than 0 and less than 0.12. The value of b is greater than 0 and less than 0.48. The value of e is greater than 0.001 and less than 0.06. The thermoelectric conversion material of this embodiment can, for example, adopt any composition within the range of formula (I). The thermoelectric conversion material of this embodiment is preferably a Mg3(Sb,Bi)2-based thermoelectric conversion material. Mg3(Sb,Bi)2-based thermoelectric conversion materials include Mg3(Sb,Bi)2 and materials in which a portion of the elements of Mg3(Sb,Bi)2 are replaced by other elements. In the case where a part of the elements of Mg3(Sb,Bi)2 are replaced by other elements in the Mg3(Sb,Bi)2-based thermoelectric conversion material, the content of the other elements is less than the content of Mg and less than the sum of the content of Sb and the content of Bi on a mass basis.
[0049] The thermoelectric conversion material of the present embodiment has, for example, a La 2 O 3 type crystal structure. Figure 2 Schematic diagram showing a La2O3 type crystal structure. The thermoelectric conversion material of this embodiment can be used for X-ray diffraction analysis. Figure 3B An example of the results of X-ray diffraction analysis of the thermoelectric conversion material according to the present embodiment is shown. Figure 3A A graph showing the results of X-ray diffraction analysis of a La2O3 type crystal structure having a lattice constant of 0.460 nm in the a-axis direction, a lattice constant of 0.460 nm in the b-axis direction, and a lattice constant of 0.729 nm in the c-axis direction. The diffraction peaks included in the results of X-ray diffraction analysis of the thermoelectric conversion material of the present embodiment are Figure 3A Therefore, according to Figure 3B It is understood that the thermoelectric conversion material of the present embodiment has, for example, a La 2 O 3 type crystal structure.
[0050] Based on further analysis of the X-ray diffraction measurement results, Figure 2 In the La2O3 type crystal structure shown in the figure, Mg is located at the C1 site, and at least one of Sb and Bi is located at the C2 site. The C1 site and the C2 site form a bond consisting of Figure 2 The thermoelectric conversion material of this embodiment may be a single crystal or a polycrystalline. For X-ray diffraction measurement, for example, an X-ray diffraction device Aeris research version manufactured by Spectris Corporation can be used.
[0051] In the composition of formula (I), if the element E is changed to Na or the value of e is changed to 0, the possibility that the thermoelectric conversion material has P-type characteristics increases. By such a change, a P-type thermoelectric conversion material can be obtained. Regarding the composition of the thermoelectric conversion material in this embodiment, reference can be made to Patent Gazette No. 6127281 or the corresponding U.S. Patent Publication No. 2017 / 0117453 specification.
[0052] [Metal layer]
[0053] Figure 1 The first metal layer 14a and the second metal layer 14b shown constitute, for example, the end face portion of the thermoelectric conversion element 10. The thickness of each of the first metal layer 14a and the second metal layer 14b is not limited to a specific value, for example, it is greater than 5 μm and less than 2 mm. The thickness of each layer may be the same or different. The first metal layer 14a and the second metal layer 14b are respectively composed of a metal monomer or a first alloy. The composition of the first metal layer 14a and the composition of the second metal layer 14b may be the same or different. The metal monomer or the first alloy used in the first metal layer 14a and the second metal layer 14b is not limited to a specific metal monomer or alloy. The metal monomer or the first alloy used in the first metal layer 14a and the second metal layer 14b, for example, has good compatibility with the first bonding layer 13a or the second bonding layer 13b, and has a melting point higher than the melting point of the material forming the first bonding layer 13a or the second bonding layer 13b. At least one of the first metal layer 14a and the second metal layer 14b is, for example, made of Cu or a Cu alloy, or Ag or an Ag alloy. In the first metal layer 14a and the second metal layer 14b of the present embodiment, for example, Cu or a Cu alloy with Cu as the main component, or Ag or an Ag alloy with Ag as the main component having good compatibility with the first bonding layer 13a or the second bonding layer 13b is used. The Cu alloy is, for example, brass, copper, gilding metal, phosphor bronze, montmorillonite, aluminum bronze, beryllium copper, nickel silver or white copper. The Ag alloy is, for example, an Ag-Cu alloy, an Ag-Au alloy or an Ag-Pd alloy.
[0054] Figure 1 The first bonding layer 13a shown is located between the first surface 12a of the thermoelectric conversion layer 11 and the first metal layer 14a, and the second bonding layer 13b is located between the second surface 12b of the thermoelectric conversion layer 11 and the second metal layer 14b. The thickness of each of the first bonding layer 13a and the second bonding layer 13b is not limited to a specific value, for example, it is greater than 10μm and less than 3mm. The thickness of each layer can be the same or different. At least one of the first bonding layer 13a and the second bonding layer 13b is composed of a second alloy. In the second alloy, the content of Mg is greater than 84atm% and less than 89atm%. In the second alloy, the content of Cu is greater than 11atm% and less than 15atm%. In the second alloy, the content of alkaline earth metals is greater than 0atm% and less than 1atm%. If the Mg content in the alloy is less than 84 atm% or exceeds 89 atm%, the melting point of the alloy greatly exceeds 500°C, causing degradation of the thermoelectric conversion material or reduction in bonding. However, the melting point of the second alloy is unlikely to greatly exceed 500°C, which can prevent degradation of the thermoelectric conversion material. Moreover, the bonding between the thermoelectric conversion layer 11 and the first metal layer 14a or the second metal layer 14b is likely to be high. The Mg content in the second alloy is greater than 84.3 atm%, and at least one of the first bonding layer 13a and the second bonding layer 13b is rich in Mg. From the perspective of preventing degradation of the characteristics of the thermoelectric conversion element 10 of the thermoelectric conversion layer 11 composed of an N-type thermoelectric conversion material, it is advantageous that Mg is difficult to move from the thermoelectric conversion layer 11 to the first bonding layer 13a or the second bonding layer 13b. Since at least one of the first bonding layer 13a and the second bonding layer 13b is rich in Mg, it is difficult for Mg to move from the thermoelectric conversion layer 11 to the first bonding layer 13a or the second bonding layer 13b. Therefore, the resistance value of the thermoelectric conversion element 10 is small and its resistance value is not easy to change. As a result, the characteristics of the thermoelectric conversion element 10 are not easy to deteriorate.
[0055] In the second alloy, the content ratio of Mg, the content ratio of Cu, and the content ratio of the alkaline earth metal may be as follows.
[0056] The content ratio of Mg is 84.3 atm % or more and 88.5 atm % or less.
[0057] The content rate of Cu is 10.5 atm % or more and 14.6 atm % or less.
[0058] The content ratio of the alkaline earth metal is 0.1 atm % or more and 1.1 atm % or less.
[0059] By containing an alkaline earth metal in the second alloy, the melting point of the second alloy tends to be lowered. As a result, the bonding temperature between the thermoelectric conversion layer 11 in the present embodiment and the first metal layer 14a or the second metal layer 14b can be reduced, and the thermal degradation of the thermoelectric conversion material forming the thermoelectric conversion layer 11 in the present embodiment can be suppressed. The alkaline earth metal contained in the second alloy is not limited to a specific alkaline earth metal. The second alloy may contain one alkaline earth metal or two alkaline earth metals. The alkaline earth metal contained in the second alloy is, for example, Ca. As confirmed by Example 1 described later, in the second alloy, the content ratio of Mg, the content ratio of Cu and the content ratio of Ca are preferably as described below.
[0060] Mg content: 84.590 atm% or more and 84.600 atm% or less
[0061] Cu content: 14.355 atm% or more and 14.365 atm% or less
[0062] Ca content: 1.045 atm% or more and 1.055 atm% or less
[0063] The first bonding layer 13a and the second bonding layer 13b are respectively formed of bonding materials. For example, of the first bonding layer 13a and the second bonding layer 13b, at least the bonding layer used on the high temperature side is formed of a bonding material composed of the above-mentioned second alloy. For example, when the metal layer close to the heat source is the first metal layer 14a and the metal layer close to the outside air is the second metal layer 14b, the first bonding layer 13a that is in contact with only the first metal layer 14a on the high temperature side is formed of a bonding material composed of the second alloy. In this case, the second bonding layer 13b may also be formed of, for example, a bonding material that has good compatibility between the thermoelectric conversion layer 11 and the second metal layer 14b and can suppress the change in the composition of the thermoelectric conversion layer 11. The second bonding layer 13b may also be formed of, for example, a bonding material composed of a Mg-based alloy having a melting point lower than the melting point of the second alloy. Both the first bonding layer 13a and the second bonding layer 13b may also be formed of a bonding material formed of the second alloy.
[0064] (Thermoelectric conversion components)
[0065] Figure 4 An example of the thermoelectric conversion module of this embodiment is shown in FIG. Figure 4 The thermoelectric conversion module 100 includes a P-type thermoelectric conversion element 20a and Figure 1The N-type thermoelectric conversion element 10 is shown. The P-type thermoelectric conversion element 20a and the N-type thermoelectric conversion element 10 are electrically connected in series. For example, the P-type thermoelectric conversion element 20a is electrically connected to the N-type thermoelectric conversion element 10 via an external electrode 31. The P-type thermoelectric conversion element 20a, for example, has a thermoelectric conversion layer 21, a third metal layer 24a, a fourth metal layer 24b, a third bonding layer 23a, and a fourth bonding layer 23b. The third bonding layer 23a bonds the third surface 22a of the thermoelectric conversion layer 21 and the third metal layer 24a. The fourth bonding layer 23b bonds the fourth surface 22b of the thermoelectric conversion layer 21 and the fourth metal layer 24b. The thermoelectric conversion layer 21 is composed of a P-type thermoelectric conversion material. The P-type thermoelectric conversion material is preferably a Mg3(Sb,Bi)2-based thermoelectric conversion material. An example of a P-type thermoelectric conversion material is a thermoelectric conversion material composed of Mg 2.99 Na 0.01 Sb 1.0 Bi 1.0 Mg 2.99 Na 0.01 Sb 1.5 Bi 0.5 and Mg 3.07 Sb 1.47 Bi 0.53 As a result, the difference in thermal expansion between the P-type thermoelectric conversion material and the N-type thermoelectric conversion material becomes smaller, and a thermoelectric conversion component with reduced thermal stress can be produced. The composition of the third metal layer 24a and the fourth metal layer 24b may be the same as or different from the composition of the first metal layer 14a or the composition of the second metal layer 14b. In addition, the composition of the bonding material forming the third bonding layer 23a and the fourth bonding layer 23b may be the same as or different from the composition of the bonding material forming the first bonding layer 13a or the second bonding layer 13b.
[0066] Figure 5 A modified example of the thermoelectric conversion module of this embodiment is shown in FIG. Figure 5 The thermoelectric conversion module 200 has a P-type thermoelectric conversion element 20b and Figure 1 The N-type thermoelectric conversion element 10 is shown. The P-type thermoelectric conversion element 20 b and the N-type thermoelectric conversion element 10 are electrically connected in series. For example, the P-type thermoelectric conversion element 20 b and the N-type thermoelectric conversion element 10 are electrically connected via an external electrode 31 .
[0067] The P-type thermoelectric conversion element 20b includes a thermoelectric conversion layer 21, a third metal layer 24a, and a fourth metal layer 24b. Figure 5 In the P-type thermoelectric conversion element 20b shown in FIG. 1 , the third surface 22a of the thermoelectric conversion layer 21 is directly bonded to the third metal layer 24a. Similarly, the fourth surface 22b of the thermoelectric conversion layer 21 is directly bonded to the fourth metal layer 24b. Figure 4 As in the thermoelectric conversion module 100 of the embodiment, both the P-type thermoelectric conversion element 20a and the N-type thermoelectric conversion element 10 have a bonding layer. Figure 5 As in thermoelectric conversion module 200 , only N-type thermoelectric conversion element 10 has a bonding layer.
[0068] exist Figure 6 1 shows one way of using the thermoelectric conversion assembly 100 of the present embodiment. The P-type thermoelectric conversion element 20a is electrically connected to the external electrode 33 through the fourth metal layer 24b. On the other hand, the N-type thermoelectric conversion element 10 is electrically connected to the external electrode 32 through the second metal layer 14b. The second wiring 42 is connected to the external electrode 33, and the first wiring 41 is connected to the external electrode 32. The first wiring 41 and the second wiring 42 have the function of taking out the power generated in the P-type thermoelectric conversion element 20a and the N-type thermoelectric conversion element 10 to the outside.
[0069] The thermoelectric conversion module may include the thermoelectric conversion element 10 as a P-type thermoelectric conversion element. In other words, in the thermoelectric conversion module, at least one of the N-type thermoelectric conversion element and the P-type thermoelectric conversion element may be the thermoelectric conversion element 10.
[0070] (Manufacturing method)
[0071] [Method for producing thermoelectric conversion material]
[0072] An example of a method for producing the thermoelectric conversion material of the present embodiment is shown below. However, the method for producing the thermoelectric conversion material of the present embodiment is not limited to the following example.
[0073] First, at least one of Mg powder, Sb powder and Bi powder as raw materials, and doping material A powder are put into a grinding container, and these powders are mechanically ground. The grinding atmosphere is, for example, an inert gas atmosphere. Thereby, oxidation of the raw materials can be suppressed. The inert gas is, for example, at least one of argon and helium. Through this process, for example, a powder of a precursor alloy of MgSbBiA is obtained. Next, the precursor alloy of MgSbBiA is sintered to obtain a polycrystal of MgSbBiA. During sintering, for example, a discharge plasma sintering method or a hot pressing method can be used. The obtained polycrystal can be used as a thermoelectric conversion material as it is. In addition, the obtained polycrystal can also be subjected to heat treatment. In this case, the polycrystal after heat treatment can be used as a thermoelectric conversion material.
[0074] [Thermoelectric conversion element and method for manufacturing a thermoelectric conversion module]
[0075] Figure 7 1 is a process diagram of an example of a method for manufacturing a thermoelectric conversion element according to the present embodiment. Figure 8 An example of a method for manufacturing the thermoelectric conversion element of this embodiment is shown below. However, the method for manufacturing the thermoelectric conversion element of this embodiment is not limited to the following example.
[0076] Alkaline earth metals such as Mg, Cu and Ca are weighed in a predetermined composition and melted by high frequency melting or the like to obtain the second alloy of the present embodiment. The second alloy of the present embodiment is powdered by atomization or ball milling to obtain a material for the bonding layer.
[0077] The material 14c of the first metal layer, the material 13c of the first bonding layer, the thermoelectric conversion layer 11 formed by the sintered thermoelectric conversion material, the material 13d of the second bonding layer, and the material 14d of the second metal layer are filled in the forming mold 50 in this order. Furthermore, the interior of the forming mold 50 is made an inert atmosphere. When filling the materials in the forming mold 50, the interior of the forming mold 50 may also be an inert atmosphere. As at least one of the material of the first bonding layer and the material of the second bonding layer, for example, a material of the bonding layer obtained by powdering the second alloy can be used. Thereafter, these materials are bonded by heating and pressurizing at a specified temperature to obtain a laminated body. For example, in Figure 8 The materials are pressed in the direction of the solid arrow 51 shown. Figure 8 A current corresponding to the temperature at which each material is joined is applied in the direction of the hollow arrow 52 shown. Joining is performed in this manner with sintering to obtain a laminate. Thereafter, the laminate is taken out from the forming die 50 to obtain the thermoelectric conversion element 10. For sintering, for example, a discharge plasma sintering method or a hot pressing method can be used.
[0078] In this way, the sintering of the thermoelectric conversion material and the bonding with the thermoelectric conversion layer and the metal layer are performed separately. Therefore, the sintering temperature of the thermoelectric conversion material can be higher than 500°C. When the sintering temperature is higher than 500°C, since the thermoelectric conversion material is a polycrystalline material, after the polycrystalline material is generated, if it is kept at a high temperature, the crystal grains will coarsen. That is, grain growth occurs. The thermoelectric conversion material formed by the crystal grains after grain growth has a situation where the thermoelectric properties become good.
[0079] For example, when hot pressing is used to diffuse and bond different types of metals, the bonding properties of different types of metals vary depending on the pressure and temperature in the hot pressing, making it difficult to uniformly bond different types of metals over a large area. On the other hand, according to the method for manufacturing the thermoelectric conversion element of the present embodiment, the melting point of the second alloy does not significantly exceed 500°C, and by using a bonding material composed of the second alloy, it is easy to achieve a large-area bonding. Therefore, according to the method for manufacturing the thermoelectric conversion element 10 using a bonding material composed of the second alloy, a large number of thermoelectric conversion elements 10 can be manufactured at one time, which is advantageous from the perspective of mass production. For example, 36 thermoelectric conversion elements 10 can be manufactured at one time.
[0080] like Figure 7 As shown, the predetermined temperature for joining the materials is, for example, 450° C. or higher and 500° C. or lower. By using the joining material composed of the second alloy, the materials can be joined within such a temperature range.
[0081] [Evaluation of Composition of Thermoelectric Conversion Element after Joining]
[0082] The compositions of the thermoelectric conversion layer, the bonding layer, and the metal layer in the bonded thermoelectric conversion element 10 can be evaluated by, for example, inductively coupled plasma (ICP) analysis or EDX analysis used for evaluating a sintered body of a thermoelectric conversion material.
[0083] Reference Fig. 9 Meanwhile, a modified example of the method for manufacturing the thermoelectric conversion element of this embodiment is shown below. Fig. 9 In the manufacturing method shown, the material 14c of the first metal layer, the material 13c of the first bonding layer, the material 11c of the thermoelectric conversion layer, the material 13d of the second bonding layer, and the material 14d of the second metal layer are filled in the forming mold 50 in this order. And, the interior of the forming mold 50 is made into an inert atmosphere. When each material is filled in the forming mold 50, the interior of the forming mold 50 can also be an inert atmosphere. Thereafter, each material is pressurized in the direction of the solid arrow 51, and an amount of current corresponding to the temperature at which each material is bonded is applied in the direction of the hollow arrow 52. In this way, bonding accompanied by sintering is performed to obtain a stacked body. Thereafter, the stacked body is taken out from the forming mold 50 to obtain the thermoelectric conversion element 10. In sintering, for example, a discharge plasma sintering method or a hot pressing method can be used.
[0084] According to this modification, the sintering of the thermoelectric conversion material and the bonding of the thermoelectric conversion layer and the metal layer can be performed at one time, which can simplify the manufacturing process. Figure 8 and Fig. 9 In the embodiment, each material is pressed in the upward direction and the downward direction indicated by the solid arrow 51 to join the materials. The magnitude of the pressure in the upward direction and the pressure in the downward direction is the same. Figure 8 As shown, in the case where the sintering of the thermoelectric conversion material and the bonding of the thermoelectric conversion layer and the metal layer are performed separately, and as Fig. 9 When the sintering of the thermoelectric conversion material and the bonding of the thermoelectric conversion layer and the metal layer are performed simultaneously, the magnitude of the pressurization may be the same, or the magnitude of the pressurization may be different.
[0085] Reference Figure 8 and Fig. 9 The manufacturing method described is as Figure 7 As shown in , for example, after the laminate is taken out from the forming die 50, a step of annealing the laminate may be further included. This removes residual stress and makes it easier to homogenize the thermoelectric conversion element 10. As a result, the resistance value of the thermoelectric conversion element 10 is easily reduced.
[0086] Thermoelectric conversion modules 100 and 200 can be assembled and manufactured by a known method using P-type thermoelectric conversion element 20 a or 20 b and N-type thermoelectric conversion element 10 .
[0087] The use of the thermoelectric conversion element of this embodiment is not limited to a specific use. The thermoelectric conversion element of this embodiment can be used for various uses including the use of conventional thermoelectric conversion elements.
[0088] (Example)
[0089] Hereinafter, the thermoelectric conversion material of this embodiment will be described in more detail with reference to Examples. However, the thermoelectric conversion material of this embodiment is not limited to the embodiments shown in the following Examples.
[0090] (Example 1)
[0091] [Fabrication of N-type Thermoelectric Conversion Layer]
[0092] 1.80g of Mg powder, 4.23g of Sb powder, 2.37g of Bi powder and 0.0295g of Te powder were weighed as raw materials in a glove box. The interior of the glove box was adjusted to an argon atmosphere until the thermoelectric conversion material was obtained. Then, each weighed powder was put into a ball mill container together with 30 stainless steel balls (diameter: 10mm) in the glove box. The ball mill container is made of stainless steel and has an internal volume of 80 milliliters (mL). Then, the opening of the ball mill container was sealed in the glove box.
[0093] Next, the ball mill container was taken out from the glove box and placed in a ball mill device. As the ball mill device, a planetary ball mill P-6 from Fritsch Japan Co., Ltd. was selected. A 4-hour pulverization process was performed by the operation of the ball mill device. The pulverization process formed a powder of the MgSbBiTe precursor alloy. The atomic ratio of Mg, Sb, Bi and Te in the powder of the MgSbBiTe precursor alloy was Mg:Sb:Bi:Te=3.20:1.50:0.49:0.01.
[0094] Next, the ball mill container was moved to the inside of the glove box. In the glove box, the powder was taken out from the ball mill container. About 5.3 g of the taken out powder was filled in the sintering space of a carbon mold (diameter 20 mm sintering type) and pressed using a carbon punch.
[0095] Next, the mold is housed in the chamber of a spark plasma sintering device. In Example 1, a spark plasma sintering device SPS515S manufactured by Fuji Electric Co., Ltd. (formerly SPS Semiconductors Co., Ltd.) is used. The chamber is adjusted to an argon atmosphere. Next, while applying a pressure of 50 MPa to the powder filled in the mold, an electric current is applied to the mold through the sintering device. By applying the electric current, the temperature of the mold reaches 850°C, which is the sintering temperature, and the temperature is maintained for 5 minutes. Thereafter, the current is gradually reduced to stop heating the mold. After the temperature of the mold drops to room temperature, the sintered body is taken out of the mold. The surface of the sintered body in contact with the punch press, which is a thermoelectric conversion material, is ground and then cleaned with acetone. The thickness of the sintered body is approximately 2.7 mm.
[0096] The obtained sintered body of the thermoelectric conversion material was evaluated by energy dispersive X-ray analysis (hereinafter referred to as "EDX"). As EDX, an energy dispersive X-ray spectrometer XFlash6|10 for SEM manufactured by Bruker was used. As a SEM combined with the above spectrometer, a field emission SEM (FE-SEM) SU8220 manufactured by Hitachi High-Technologies Corporation was used.
[0097] [Manufacturing of bonding materials]
[0098] A material mixed with Mg powder, Cu powder and Ca powder is used as the material of the bonding layer of Example 1. In Example 1, as shown in Table 1, 5.464g of Mg powder, 2.424g of Cu powder and 0.112g of Ca powder are weighed in a glove box as raw materials for the bonding material. The weights of the weighed Mg powder, Cu powder and Ca powder in the mixture of Mg powder, Cu powder and Ca powder, expressed in mass percentage, are shown in Table 1. Specifically, in the mixture of Mg powder, Cu powder and Ca powder, Mg is 68.30mass%, Cu is 30.30mass%, and Ca is 1.40mass%. The particle size of each powder is less than 90μm. In addition, at least one of Mg powder and Cu powder can be added to the commercially available Mg-Cu-Ca alloy powder for weighing.
[0099] [Table 1]
[0100]
[0101] Table 1 shows the weight of each powder in the mixture of Mg powder, Cu powder and Ca powder used for the preparation of the bonding material in Examples 1 to 3 in terms of mass and mass percentage. The inside of the glove box was adjusted to an argon atmosphere until the material of the bonding layer was obtained. Next, the mixture of each weighed powder was melt-heated at 480°C for 1 hour in the glove box. Thereafter, the obtained alloy was crushed in a mortar and powdered to obtain the bonding material of Example 1.
[0102] [Joining of materials]
[0103] The thermoelectric conversion material and the Cu plate cleaned with acetone were moved to the inside of the glove box. The diameter of the Cu plate was 20 mm, and the thickness of the Cu plate was 0.2 mm. In the glove box, a Cu plate, 0.25 g of the bonding material of Example 1, a thermoelectric conversion material, 0.25 g of the bonding material of Example 1, and a Cu plate were sequentially filled in the sintering space of a carbon mold, i.e., a forming mold, and powder was pressed using a punch.
[0104] Next, the mold is placed in the chamber of the spark plasma sintering device. The chamber is adjusted to an argon atmosphere. Next, while applying a pressure of 50 MPa to the filling of the mold, an electric current is applied to the mold through the sintering device. By applying the electric current, after the temperature of the mold reaches the maximum bonding temperature of 450°C, the temperature is maintained for 1 minute. After that, the current is gradually reduced to stop heating the mold. After the temperature of the mold drops to room temperature, the thermoelectric conversion element substrate is removed from the mold. The maximum bonding temperature is shown in Table 2.
[0105] [Table 2]
[0106]
[0107] Table 2 shows the contents of Mg, Cu and Ca in the bonding materials in Examples 1 to 3 in terms of atomic weight percentage. Table 2 shows the maximum values of the bonding temperatures between the thermoelectric conversion layer and the metal layer in Examples 1 to 3. The atomic weight percentages were calculated using the following formulas 1 to 3.
[0108] Formula 1: (Atomic weight percentage of Mg) = A / (A+B+C)×100
[0109] Formula 2: (Atomic weight percentage of Cu) = B / (A+B+C)×100
[0110] Formula 3: (atomic weight percentage of Ca) = C / (A+B+C)×100
[0111] A, B and C described in the above formulae 1 to 3 are as follows.
[0112] A = (mass percentage of Mg) / (atomic weight of Mg)
[0113] B = (mass percentage of Cu) / (atomic weight of Cu)
[0114] C = (mass percentage of Ca) / (atomic weight of Ca)
[0115] [Annealing treatment]
[0116] The obtained thermoelectric conversion element substrate was annealed in a furnace adjusted to an argon atmosphere. The temperature in the furnace was maintained at 470° C. for 30 minutes and then gradually cooled.
[0117] [Fabrication of N-type thermoelectric conversion element]
[0118] A 20 mm diameter thermoelectric conversion element substrate was cut into 3.5 mm square elements using a diamond cutter, and each element was cleaned with acetone. In this way, 12 N-type thermoelectric conversion elements of Example 1 were manufactured.
[0119] (Observation of the Cut Section of the Thermoelectric Conversion Element)
[0120] Fig.10 The results of SEM observation of the cross section of the thermoelectric conversion element of Example 1. The thickness of the thermoelectric conversion element of Example 1 is about 3.2 mm. In the thermoelectric conversion element of Example 1, the thermoelectric conversion layer 11 containing Mg, Sb and Bi has a thickness of about 2.7 mm, the metal layer 14 composed of the Cu plate has a thickness of about 100 μm, and the bonding layer 13 containing Mg, Cu and Ca has a thickness of about 150 μm.
[0121] (Example 2)
[0122] The raw materials of the bonding material were weighed according to the ratios shown in Table 1, and a thermoelectric conversion element of Example 2 was produced in the same manner as in Example 1 except that the maximum bonding temperature was changed to 500°C.
[0123] (Example 3)
[0124] The raw materials of the bonding material were weighed according to the ratios in Table 1, and a thermoelectric conversion element of Example 3 was produced in the same manner as in Example 1 except that the maximum bonding temperature was changed to 500°C.
[0125] (Example 4)
[0126] A thermoelectric conversion element of Example 4 was produced in the same manner as in Example 1 except that an Ag plate was used instead of the Cu plate.
[0127] (Comparative Example 1)
[0128] A thermoelectric conversion element of Comparative Example 1 was produced in the same manner as in Example 4, except that the Ag plate and the thermoelectric conversion layer were directly bonded to each other without using a bonding material.
[0129] (Example 5)
[0130] [Fabrication of P-type Thermoelectric Conversion Layer]
[0131] 11g of Mg powder, 18.4302g of Sb powder, 31.6323g of Bi powder and 0.0348g of Na powder were weighed as raw materials in a glove box. The interior of the glove box was adjusted to an argon atmosphere until the thermoelectric conversion material was obtained. Then, each weighed powder was put into a ball mill container together with 187 stainless steel balls (diameter: 10mm) in the glove box. The ball mill container is made of stainless steel and has an internal volume of 500 milliliters (mL). Then, the opening of the ball mill container was sealed in the glove box.
[0132] Next, after taking out the ball mill container from the glove box, it was set in the ball mill device. As the ball mill device, the planetary ball mill P-5 of Fritsch Japan Co., Ltd. was selected. The pulverization treatment was implemented for 5.7 hours by the operation of the ball mill device. Through the pulverization treatment, the powder of the MgSbBiNa precursor alloy was formed. The atomic number ratio of Mg, Sb, Bi and Na in the powder of the MgSbBiNa precursor alloy is Mg:Sb:Bi:Na=2.99:1.0:1.0:0.01.
[0133] Next, the ball mill container was moved to the inside of the glove box. In the glove box, the powder was taken out from the ball mill container. About 1 g of the taken out powder was filled in the sintering space of a carbon mold (diameter 10 mm sintering type) and pressed using a carbon punch.
[0134] Next, the mold was placed in a chamber of a spark plasma sintering device, and a sintered body of a P-type thermoelectric conversion material of Example 5 was obtained in the same manner as in Example 1 except that the maximum temperature was changed to 680°C.
[0135] [Manufacturing of bonding materials]
[0136] The raw materials of the bonding material were weighed in the same manner as in Example 1 according to the ratios shown in Table 3.
[0137] [Table 3]
[0138]
[0139] Table 3 shows the amount of each powder in the mixture of Mg powder, Cu powder and Ca powder used for preparing the bonding materials in Examples 5 and 6 and Comparative Example 2, expressed in terms of mass and mass percentage. The bonding material of Example 5 was obtained in the same manner as in Example 1.
[0140] [Joining of materials]
[0141] A thermoelectric conversion element substrate of Example 5 was obtained in the same manner as in Example 1 except that the P-type thermoelectric conversion material of Example 5 was used as the thermoelectric conversion material.
[0142] [Table 4]
[0143]
[0144] Table 4 shows the contents of Mg, Cu and Ca in the bonding materials of Examples 5 and 6 and Comparative Example 2 in terms of atomic weight percentage. Table 4 also shows the maximum value of the bonding temperature between the thermoelectric conversion layer and the metal layer in Examples 5 and 6 and Comparative Example 2. The atomic weight percentage is obtained by the above-mentioned formulas 1 to 3.
[0145] [Fabrication of P-type thermoelectric conversion element]
[0146] The 10 mm diameter thermoelectric conversion element substrate was cut into 3.4 mm square elements using a diamond cutter, and each element was cleaned with acetone. In this way, four P-type thermoelectric conversion elements of Example 5 were manufactured.
[0147] (Example 6)
[0148] The raw materials of the bonding material were weighed according to the ratios shown in Table 3, and a thermoelectric conversion element of Example 6 was produced in the same manner as in Example 5.
[0149] (Comparative Example 2)
[0150] The raw materials of the bonding material were weighed according to the ratios shown in Table 3, and a thermoelectric conversion element of Comparative Example 2 was produced in the same manner as in Example 5.
[0151] (Evaluation of Resistance Value R, Resistivity ρ, and Yield in N-Type Thermoelectric Conversion Element)
[0152] The resistance value R of the N-type thermoelectric conversion elements of Examples 1 to 4 was measured using a four-terminal method. Table 5 shows the results.
[0153] [Table 5]
[0154]
[0155] Table 5 shows the average values of resistance R and resistivity ρ of the thermoelectric conversion elements having resistance R of 50 mΩ or less in Examples 1 to 4. Table 5 also shows the yield rate in the production of the N-type thermoelectric conversion elements in Examples 1 to 4.
[0156] The resistivity ρ of the element is obtained by the following formula 4.
[0157] Formula 4: ρ = R × A / L
[0158] In the above formula 4,
[0159] ρ is the resistivity of the thermoelectric conversion element,
[0160] R is the resistance value of the thermoelectric conversion element,
[0161] A is the element area when the thermoelectric conversion element is viewed from above (3.5 mm×3.5 mm),
[0162] L is the thickness of the layer of the thermoelectric conversion element (3.2 mm).
[0163] The element yield rate is calculated by the following formula 5.
[0164] Formula 5: (Element yield) = {(Number of elements with a resistance value R of 50 mΩ or less) / (Number of elements produced from the thermoelectric conversion element substrate)}×100
[0165] In Examples 1 to 4, the number of elements produced from the thermoelectric conversion element substrate was 12. In Example 1, as shown in Table 5, the average value of the element resistance R was 8.1 mΩ, the average value of the element resistivity ρ was 31.0 μΩ·m, and the yield was 100.0%.
[0166] In Example 2, as shown in Table 5, the average value of the resistance value R of the element was 33.6 mΩ, the average value of the resistivity ρ of the element was 128.6 μΩ·m, and the yield rate was 16.7%.
[0167] In Example 3, as shown in Table 5, the average value of the resistance value R of the element was 13.1 mΩ, the average value of the resistivity ρ of the element was 50.1 μΩ·m, and the yield rate was 41.7%.
[0168] In Example 4, as shown in Table 5, the average value of the resistance value R of the element was 33.5 mΩ, the average value of the resistivity ρ of the element was 128.2 μΩ·m, and the yield was 75%.
[0169] In all of Examples 1 to 4 shown in Table 5, N-type thermoelectric conversion elements having a resistance value R of 50 mΩ or less can be obtained. In particular, in Example 1, a yield of 100.0% was shown, and a thermoelectric conversion element having a resistance value R of 50 mΩ or less can be obtained stably. In addition, in Example 1, the average value of the resistance value R of the element is the smallest among Examples 1 to 4, and the average value of the resistivity ρ is also the smallest.
[0170] (Evaluation of stability of element resistance)
[0171] The thermoelectric conversion element of Example 4 having a resistance value R of 12mΩ and the thermoelectric conversion element of Comparative Example 1 having a resistance value R of 262mΩ were heated in an environment of 400°C for 12 hours. The resistance value R of the thermoelectric conversion element of Comparative Example 1 was measured according to the 4-terminal method. Afterwards, the resistance value R of each thermoelectric conversion element was measured again according to the 4-terminal method. The resistance change rate was determined by dividing the resistance value R of the thermoelectric conversion element after heating by the resistance value R of the thermoelectric conversion element before heating. The results are shown in Table 6.
[0172] As shown in Table 6, in the thermoelectric conversion element of Example 4, the resistance change rate of the resistance value R of the element is small, which gives the suggestion that the resistance of the element is not easy to change at high temperatures. On the other hand, in the thermoelectric conversion element of Comparative Example 1, the resistance change rate of the resistance value R of the element is large, which gives the suggestion that the resistance of the element is easy to change at high temperatures.
[0173] [Table 6]
[0174]
[0175] (Evaluation of Resistance Value R and Resistivity ρ in P-Type Thermoelectric Conversion Element)
[0176] The resistance value R of the P-type thermoelectric conversion elements of Examples 5 and 6 and Comparative Example 2 was measured using a four-terminal method. Table 7 shows the results.
[0177] [Table 7]
[0178]
[0179] Table 7 shows the resistance values R measured by the four-terminal method and the resistivity p obtained by the above-described equation 4 for the P-type thermoelectric conversion elements of Examples 5 and 6 and Comparative Example 2.
[0180] In Example 5, as shown in Table 7, the resistance value R of the element was 27.4 mΩ, and the resistivity ρ of the element was 99.0 μΩ·m.
[0181] In Example 6, as shown in Table 7, the resistance value R of the element was 10.0 mΩ, and the resistivity ρ of the element was 36.1 μΩ·m.
[0182] In Comparative Example 2, as shown in Table 7, the resistance value R of the element was 57.0 mΩ, and the resistivity ρ of the element was 205.9 μΩ·m.
[0183] In Examples 5 and 6 shown in Table 7, P-type thermoelectric conversion elements having a resistance value R of 50 mΩ or less were obtained. On the other hand, in Comparative Example 2, a P-type thermoelectric conversion element having a resistance value R higher than 50 mΩ was obtained.
[0184] Industrial Applicability
[0185] The thermoelectric conversion element of the present invention can be used for various applications including applications of conventional thermoelectric conversion elements.
Claims
1. A thermoelectric conversion element, characterized in that: include: Thermoelectric conversion layer; 1st metal layer; 2nd metal layer; A first bonding layer bonding the first surface of the thermoelectric conversion layer and the first metal layer; and a second bonding layer bonding the second surface of the thermoelectric conversion layer to the second metal layer, The thermoelectric conversion layer is composed of a thermoelectric conversion material containing Mg and at least one of Sb and Bi. The first metal layer and the second metal layer are respectively composed of a metal monomer or a first alloy. At least one of the first bonding layer and the second bonding layer is composed of a second alloy, In the second alloy, The content ratio of Mg is 84 atm% or more and 89 atm% or less, The content of Cu is 11 atm% or more and 15 atm% or less. The content ratio of the alkaline earth metal is 0.1 atm % or more and 1 atm % or less.
2. The thermoelectric conversion element according to claim 1, characterized in that: In the second alloy, The content of Mg is 84.3 atm% or more and 88.5 atm% or less. The content of Cu is 10.5 atm% or more and 14.6 atm% or less, The content ratio of the alkaline earth metal is 0.1 atm % or more and 1.1 atm % or less.
3. The thermoelectric conversion element according to claim 1 or 2, characterized in that: The alkaline earth metal is Ca.
4. The thermoelectric conversion element according to claim 1 or 2, characterized in that: The thermoelectric conversion material is a Mg3(Sb,Bi)2 type thermoelectric conversion material.
5. The thermoelectric conversion element according to claim 1 or 2, characterized in that: The thermoelectric conversion material has a La2O3 type crystal structure.
6. The thermoelectric conversion element according to claim 1 or 2, characterized in that: The thermoelectric conversion material is N-type.
7. The thermoelectric conversion element according to claim 1 or 2, characterized in that: At least one of the first metal layer and the second metal layer is made of Cu or a Cu alloy.
8. A thermoelectric conversion component, characterized in that: include: N-type thermoelectric conversion element; and P-type thermoelectric conversion element, At least one of the N-type thermoelectric conversion element and the P-type thermoelectric conversion element is the thermoelectric conversion element according to any one of claims 1 to 7, The N-type thermoelectric conversion element and the P-type thermoelectric conversion element are electrically connected in series.
9. A bonding material, characterized in that: The content ratio of Mg is 84 atm% or more and 89 atm% or less, The content of Cu is 11 atm% or more and 15 atm% or less. The content of alkaline earth metal is 0.1 atm% or more and 1 atm% or less, Used to join thermoelectric conversion materials to metal parts.
10. A method for manufacturing a thermoelectric conversion element, characterized in that: include: A step of filling a forming die with a material for a first metal layer, a material for a first bonding layer, a material for a thermoelectric conversion layer, a material for a second bonding layer, and a material for a second metal layer in this order; The step of heating and pressurizing the material of the first metal layer, the material of the first bonding layer, the material of the thermoelectric conversion layer, the material of the second bonding layer, and the material of the second metal layer filled in the molding die at a predetermined temperature to bond them to obtain a laminated body; and The step of removing the laminate from the forming die, The material of the thermoelectric conversion layer contains Mg and at least one of Sb and Bi, The material of the first metal layer and the material of the second metal layer are respectively composed of a metal monomer or a first alloy. At least one of the material of the first bonding layer and the material of the second bonding layer is composed of a second alloy, In the second alloy, The content ratio of Mg is 84 atm% or more and 89 atm% or less, The content of Cu is 11 atm% or more and 15 atm% or less. The content ratio of the alkaline earth metal is 0.1 atm % or more and 1 atm % or less.
11. The method according to claim 10, characterized in that: The predetermined temperature is 450° C. or higher and 500° C. or lower.
12. The method according to claim 10 or 11, characterized in that: The method further includes the step of performing an annealing treatment on the stacked body after taking the stacked body out of the forming die.
Citation Information
Patent Citations
Thermoelectric conversion material
US20170117453A1
Porous region removing method and semiconductor substrate manufacturing method
US6127281A
Thermoelectric conversion element, method for manufacturing same, and thermoelectric conversion module
CN105765747A
Multi-petal thermoelectric power generation device
CN110391328A
Electrode bonding structure for thermoelectric conversion element, electrode bonding method therefor theremoelectric conversion module and production thereof
JP1998012935A