Flash voltage booster and preparation method thereof, and electrolyte
Through flash fire voltage boosters composed of alcohol solvents and inorganic acids, the problems of poor voltage boosting ability and reduced conductivity in the existing technology are solved, and efficient voltage boosting and capacitor life extension are achieved, which is suitable for ultra-high voltage Aluminum electrolytic capacitor.
Patent Information
- Application Number
- CN202210190754.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-02-28
AI Technical Summary
When existing flash fire voltage boosters improve the voltage withstandability of the electrolyte, they usually lead to a decrease in conductivity and negatively affect the reliability and life of the capacitor. The voltage withstandability is relatively poor, making it difficult to meet the ultra-high voltage demand. .
After mixing alcohol solvents with inorganic acids and heating, organic acids, polyols and polymer substances are added, and the insulation treatment at a specific temperature and time is carried out to form a flash fire voltage booster. The specific formula includes 50%-60% alcohol solvents. Inorganic acid 10%-20%, organic acid 10%-20%, polyol 3%-5%, polymer substance 10%-20%, and add 4%-6% flash fire voltage booster to the electrolyte .
The electrolyte withstand voltage capacity has been significantly improved. Each 1% increase of flash fire voltage booster can increase the withstand voltage of 8 to 10V, and the influence on conductivity is small. The conductivity is only reduced by about 1%, which extends the capacitor's Service life.
Smart Images

Figure CN114420455B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrolytes for high-voltage electrolytic capacitors, and in particular to a flash voltage enhancer and a preparation method thereof. Background Art
[0002] Aluminum electrolytic capacitors are one of the most critical and important electronic components in electronic circuits. The development of aluminum electrolytic capacitors mainly has the following directions: 1) Development towards ultra-high voltage, the voltage has rapidly developed from the previous highest voltage of 450V to 500V, 550V, 600V, etc., or even higher in recent years; 2) Development towards wide temperature, from the original -25~+85℃ to -40~+105℃, and currently there is a trend of developing to -55~+125℃ or even +150℃; 3) Development towards high frequency, low resistance and long life, etc. The development direction of aluminum electrolytic capacitors is actually the result of the various materials or technological advances that make up aluminum electrolytic capacitors. The most critical materials are anode foil and electrolyte, especially for ultra-high voltage aluminum electrolytic capacitors, where electrolyte has become the most critical constraint.
[0003] The electrolyte for ultra-high voltage aluminum electrolytic capacitors requires high conductivity, good high temperature stability, excellent low temperature performance, long life, low saturated vapor pressure at various temperatures, and high voltage resistance. Therefore, the electrolyte is composed of many materials and the manufacturing process is complex. In particular, the conductivity and voltage resistance are negatively correlated. The higher the conductivity, the lower the voltage resistance. Conversely, the lower the conductivity, the higher the voltage resistance. In addition, the electrolyte has other characteristics. It is very difficult to improve the voltage resistance and conductivity of the electrolyte at the same time. In terms of ultra-high voltage, the electrolyte has become a bottleneck factor hindering development. For the electrolyte to develop in the direction of ultra-high voltage, the key materials are high voltage resistance electrolytes (i.e. solutes) and voltage resistance enhancement additives.
[0004] High voltage-resistant solutes are divided into inorganic solutes and organic solutes. Inorganic solutes are less in number. Although they have a high voltage resistance, the conductivity of the electrolyte is low after being added to the electrolyte, and they are not suitable for use alone. For organic solutes, as the number of carbon atoms increases, the voltage resistance of the solute also increases. However, the electrical conductivity is significantly reduced. At the same time, the solubility of organic electrolytes decreases significantly with the increase in the number of carbon atoms. Therefore, considering the electrical conductivity and relatively high voltage resistance of organic solutes, the voltage resistance is about 500V, which is still far from meeting the ultra-high voltage requirements. Therefore, in order to obtain an electrolyte with a higher voltage, it is necessary to add another type of key material, which is a voltage resistance enhancing additive (generally referred to as a flash voltage enhancer).
[0005] The voltage resistance enhancing additives in the electrolyte of high-voltage electrolytic capacitors are currently the materials or technologies that are being researched and developed by various electrolyte manufacturers and even the corresponding chemical materials research institutes. Such additives currently mainly include organic single molecule additives, organic polymer additives, organic ester additives, inorganic nano additives, etc. The above-mentioned types of voltage resistance additives have different effects on improving the voltage resistance of the electrolyte. Moreover, while improving the voltage resistance of the electrolyte, the conductivity of the electrolyte will be reduced to varying degrees. Another key issue is that each type of additive has an addition limit. After exceeding the dosage, even if the dosage of this additive is increased, the voltage resistance of the electrolyte will no longer increase, while the conductivity will still decrease proportionally. Therefore, in order to obtain a more ideal ultra-high voltage resistance electrolyte, it is generally necessary to use a variety of voltage resistance enhancing additives in combination, or to find additives with better voltage resistance enhancement effects to improve the voltage resistance effect of the electrolyte.
[0006] The existing voltage resistance enhancing additives (i.e., flash voltage enhancers) have the following main deficiencies: 1. Most of the additives have relatively poor voltage resistance enhancing capabilities; 2. They affect the conductivity of the electrolyte, that is, after adding the additives, although the voltage resistance of the electrolyte can be enhanced to a certain extent, the conductivity of the electrolyte is significantly reduced at the same time; 3. There is no correlation with the electrolyte in the electrolyte. After using the additives, there is a negative impact on the reliability and life of the capacitor. Summary of the invention
[0007] In order to solve the technical problem of poor voltage boosting capability in the prior art, the present invention provides a flash voltage booster and a preparation method thereof, and an electrolyte.
[0008] The preparation method of the flash voltage enhancer proposed by the present invention comprises:
[0009] After mixing the alcohol solvent and the inorganic acid, heating the mixture to a first temperature range and maintaining the temperature for a first time period;
[0010] Continue to add organic acid, polyol and polymer substances and mix them, and continue to keep warm for the second time;
[0011] The solution that meets the second time requirement is heated to the second temperature range, and after being heated for a third time, the solution is cooled to the third temperature range, and is heated for a fourth time, wherein the minimum value of the second temperature range is greater than the maximum value of the first temperature range;
[0012] Cool down to the operating temperature range to form a flash voltage enhancer. Continuous stirring is required during the above process.
[0013] Furthermore, by mass percentage, the alcohol solvent accounts for 50%-60%, the inorganic acid accounts for 10%-20%, the organic acid accounts for 10%-20%, the polyol accounts for 3%-5%, and the polymer substance accounts for 10%-20%; or
[0014] The alcohol solvent accounts for 50%-60%, the inorganic acid accounts for 11%-25%, the organic acid accounts for 5%-10%, the polyol accounts for 3%-5%, and the high molecular substance accounts for 10%-20%.
[0015] Furthermore, the alcohol substance includes at least one of ethylene glycol, propylene glycol and butanediol.
[0016] Furthermore, the inorganic acid includes at least one of boric acid and phosphoric acid.
[0017] Furthermore, the organic acid includes at least one of a dicarboxylic acid with a long carbon chain and a branched organic carboxylic acid.
[0018] Furthermore, the dicarboxylic acid with a long carbon chain includes at least one of azelaic acid, sebacic acid, and dodecanedioic acid.
[0019] Furthermore, the polymer substance includes at least one of polyethylene glycol, polyvinyl alcohol, and water-soluble starch.
[0020] The flash voltage booster proposed by the present invention is prepared by the flash voltage booster preparation method described in the above technical solution.
[0021] Furthermore, the alcohol solvent is ethylene glycol, the inorganic acid is boric acid, the organic acid is sebacic acid, the polyol is mannitol, and the high molecular weight substance is polyethylene glycol, wherein, calculated by mass percentage, ethylene glycol accounts for 50%-60%, boric acid accounts for 10%-20%, sebacic acid accounts for 10%-20%, mannitol accounts for 3%-5%, and polyethylene glycol accounts for 10%-20%.
[0022] Furthermore, the alcohol solvent is propylene glycol, the inorganic acid is boric acid, the organic acid is azelaic acid, the polyol is mannitol, and the polymer substance is polyvinyl alcohol, wherein, calculated by mass percentage, propylene glycol accounts for 50%-60%, boric acid accounts for 10%-20%, azelaic acid accounts for 10%-20%, mannitol accounts for 3%-5%, and polyvinyl alcohol accounts for 10%-20%.
[0023] Furthermore, the alcohol solvent is ethylene glycol, the inorganic acid is boric acid, the organic acid is dodecanedioic acid, the polyol is mannitol, and the polymer substance is water-soluble starch, wherein, calculated by mass percentage, ethylene glycol accounts for 50%-60%, boric acid accounts for 10%-20%, dodecanedioic acid accounts for 10%-20%, mannitol accounts for 3%-5%, and water-soluble starch accounts for 10%-20%.
[0024] Furthermore, the alcohol solvent is butanediol, the inorganic acid is boric acid and phosphoric acid, the organic acid is sebacic acid, the polyol is mannitol, and the polymer substance is water-soluble starch, wherein, calculated by mass percentage, butanediol accounts for 50%-60%, boric acid accounts for 10%-20%, phosphoric acid accounts for 1%-5%, sebacic acid accounts for 5%-10%, mannitol accounts for 3%-5%, and water-soluble starch accounts for 10%-20%.
[0025] The electrolyte of the high-voltage electrolytic capacitor proposed by the present invention includes the flash voltage enhancer described in the above technical solution.
[0026] Furthermore, in the electrolyte of the high-voltage electrolytic capacitor, the mass percentage of the flash voltage enhancer is 4% to 6%.
[0027] Furthermore, in terms of mass percentage, the following components are also included: the main solvent accounts for 65%-75%, the solute accounts for 10%-15%; the conventional flash voltage enhancer accounts for 10%-20%, and the others account for 3%-8%.
[0028] The ultra-high voltage aluminum electrolyte additive (i.e., flash voltage enhancer) developed by the present invention expands the types of high voltage electrolyte additives and has the following advantages over the prior art in terms of formulation design, production process, performance, etc.:
[0029] 1. The present invention has a significant effect on improving the withstand voltage of the electrolyte. For every 1% of the flash voltage enhancer added, the withstand voltage is increased by about 8 to 10V, which solves the problem that the existing additives have poor withstand voltage enhancement ability and the withstand voltage of the electrolyte is low (for existing additives, generally, the withstand voltage is less than 5V for every 1% increase).
[0030] 2. It has little effect on the conductivity of the electrolyte. Generally, for every 1% increase in content, the conductivity of the electrolyte only decreases by about 1%, which is significantly superior to the 3-5% conductivity of existing additives.
[0031] 3. The problem that the existing additives only improve the withstand voltage of the electrolyte and have a negative impact on the life of the electrolyte and even the capacitor is solved. The additive of the present invention is synthesized from a variety of high-pressure solutes and organic polymers, and is complementary to the solutes in the electrolyte. That is, during use, when the solutes in the electrolyte are slowly consumed, the solutes in the additives will be gradually released into the electrolyte, which has a supplementary effect on the electrolyte in the electrolyte, thereby extending the service life of the capacitor. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The present invention is described in detail below with reference to the embodiments and accompanying drawings, wherein:
[0033] Figure 1 This is a diagram showing the voltage resistance of an electrolyte without adding a flash voltage enhancer in the prior art.
[0034] Figure 2 This is a diagram showing the voltage resistance effect of an electrolyte to which a conventional flash voltage enhancer is added in the prior art.
[0035] Figure 3 This is a diagram showing the voltage resistance of the electrolyte to which a conventional flash voltage enhancer is added according to the present invention. DETAILED DESCRIPTION
[0036] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0037] Thus, a feature indicated in this specification will be used to illustrate one of the features of an embodiment of the present invention, rather than implying that each embodiment of the present invention must have the described feature. In addition, it should be noted that this specification describes many features. Although some features can be combined together to illustrate possible system designs, these features can also be used in other combinations that are not explicitly described. Thus, unless otherwise stated, the described combinations are not intended to be limiting.
[0038] The electrolyte of high-voltage electrolytic capacitors is mainly composed of: main solvent, solute (i.e. electrolyte), and additives. The function of the main solvent is to dissolve the electrolyte and ionize the electrolyte. The solute is the electrolyte, and its main function is to ionize anions and cations to conduct electricity under the action of the main solvent, and, under the action of voltage and current, it can continuously repair the anode foil aluminum oxide layer in the capacitor to ensure the life of the capacitor. There are many types of additives, and their functions are more complex. Among them, in high-voltage electrolytes, there is a most critical type of additive, which is the withstand voltage enhancement additive, which can also be called the flash voltage enhancer. The flash voltage enhancer plays a key role in the withstand voltage that the electrolyte and even the capacitor can withstand.
[0039] The preparation process of the additive is also very critical. After in-depth research on the additive formula ratio and preparation process, the preparation method of the flash voltage enhancer of the present invention is obtained, including:
[0040] After mixing the alcohol solvent and the inorganic acid, heating the mixture to a first temperature range and maintaining the temperature for a first time period;
[0041] Continue to add organic acid, polyol and polymer substance, stir and mix, and keep warm for the second time;
[0042] The solution that meets the second time requirement is heated to the second temperature range, and after being heated for a third time, the solution is cooled to the third temperature range, and is heated for a fourth time, wherein the minimum value of the second temperature range is greater than the maximum value of the first temperature range;
[0043] Cool down to the operating temperature range to form a flash voltage enhancer.
[0044] In a specific embodiment, after the alcohol substance and the organic acid are stirred and mixed, the mixture is heated to 70°C and kept warm for 60 minutes, and then the organic acid, polyol and polymer substance are added and stirred and mixed, and then the mixture is kept warm for 60 minutes, and then the mixture is heated to 160°C and kept warm for 240 minutes, and then the mixture is cooled to 85°C and kept warm for 60 minutes, and finally the mixture is cooled to below 60°C and can be used. Continuous stirring is required during the above process. The present invention is not limited to this specific embodiment. For example, the first temperature range can be 50-80°C, the second temperature range can be 150-170°C, the third temperature range can be 75-95°C, and the use temperature range is 0-60 degrees Celsius. The first to fourth time lengths can be ±5 minutes or 10 minutes based on the examples listed.
[0045] In one embodiment, by mass percentage, alcohol solvents account for 50%-60%, inorganic acids account for 10%-20%, organic acids account for 10%-20%, polyols account for 3%-5%, and polymer substances account for 10%-20%.
[0046] In another embodiment, by mass percentage, alcohol solvents account for 50%-60%, inorganic acids account for 11%-25%, organic acids account for 5%-10%, polyols account for 3%-5%, and polymer substances account for 10%-20%.
[0047] When choosing alcohol solvents and polyols, it is necessary to select diols or polyols with high melting points and boiling points, so that the alcohols are not easy to vaporize at high temperatures and are easy to participate in reactions. Alcohol substances include at least one of ethylene glycol, propylene glycol and butanediol. Mannitol can be selected as the polyol. Polyols can improve the pressure resistance of the electrolyte.
[0048] Acidic substances are mainly selected from types with stable structure, long life, and easy to react with alcoholic substances. Boric acid, phosphoric acid, etc. are preferred for inorganic acids. In a specific embodiment, the inorganic acid includes at least one of boric acid and phosphoric acid. Organic carboxylic acids are selected from dicarboxylic acids with long carbon chains, such as one or more of azelaic acid, sebacic acid, dodecanedioic acid, or branched organic carboxyls. In a specific embodiment, the organic acid includes at least one of azelaic acid, sebacic acid, and dodecanedioic acid. Mainly due to the characteristics of this type of acidic substance, high voltage resistance, weak acidity, and easy to participate in the reaction. That is, under certain conditions, it can react with alcoholic substances to obtain a polymer substance with higher molecular weight and voltage resistance. Moreover, when the electrolyte content in the solution is reduced due to consumption, this part of the acidic substance has a supplementary effect on the electrolyte, extending the service life of the electrolyte and the capacitor.
[0049] The selection of polymer substances mainly focuses on organic polymers with relatively large molecular weight, soluble in water or ethylene glycol, and containing more hydroxyl groups (-OH) in the molecules, which themselves have a certain effect on improving the withstand voltage of the electrolyte. In a specific embodiment, the polymer substance includes at least one of polyethylene glycol, polyvinyl alcohol, and water-soluble starch.
[0050] The flash voltage enhancer prepared by the above technical solution can specifically have the following formula ratio tables. In addition to the following formula ratio tables, those skilled in the art can also make appropriate adjustments and modifications within the scope of the above technical solution, all of which belong to the protection scope of the present invention.
[0051] In the first embodiment, the flash voltage enhancer is named Additive 1, wherein the alcohol solvent is ethylene glycol, the inorganic acid is boric acid, the organic acid is sebacic acid, the polyol is mannitol, and the polymer substance is polyethylene glycol. Calculated by mass percentage, ethylene glycol accounts for 50%-60%, boric acid accounts for 10%-20%, sebacic acid accounts for 10%-20%, mannitol accounts for 3%-5%, and polyethylene glycol accounts for 10%-20%.
[0052] In the second embodiment, the flash voltage enhancer is named Additive 2, wherein the alcohol solvent is propylene glycol, the inorganic acid is boric acid, the organic acid is azelaic acid, the polyol is mannitol, and the polymer substance is polyvinyl alcohol. Calculated by mass percentage, propylene glycol accounts for 50%-60%, boric acid accounts for 10%-20%, azelaic acid accounts for 10%-20%, mannitol accounts for 3%-5%, and polyvinyl alcohol accounts for 10%-20%.
[0053] In the third embodiment, the voltage booster is named Additive 3, wherein the alcohol solvent is ethylene glycol, the inorganic acid is boric acid, the organic acid is dodecanedioic acid, the polyol is mannitol, and the polymer substance is water-soluble starch, wherein, calculated by mass percentage, ethylene glycol accounts for 50%-60%, boric acid accounts for 10%-20%, dodecanedioic acid accounts for 10%-20%, mannitol accounts for 3%-5%, and water-soluble starch accounts for 10%-20%.
[0054] In the fourth embodiment, the voltage booster is named Additive 4, wherein the alcohol solvent is butanediol, the inorganic acids are boric acid and phosphoric acid, the organic acid is sebacic acid, the polyol is mannitol, and the polymer substance is water-soluble starch, wherein, calculated by mass percentage, butanediol accounts for 50%-60%, boric acid accounts for 10%-20%, phosphoric acid accounts for 1%-5%, sebacic acid accounts for 5%-10%, mannitol accounts for 3%-5%, and water-soluble starch accounts for 10%-20%.
[0055] The components and mass percentages of the above four specific embodiments can also be found in the following table.
[0056]
[0057] Table 1 Detailed ratio table of four specific embodiments
[0058] When the flash voltage enhancer obtained by the above technical scheme of the present invention is added to the electrolyte of a certain high-voltage electrolytic capacitor with the same existing component ratio (except the newly added flash voltage enhancer), the additive 3 has the best effect in improving the withstand voltage. For every 1% added, the voltage can be increased by 8 to 10V. With an increase of about 5%, the withstand voltage of the electrolyte is increased to more than 50V.
[0059] After specific testing experiments, it was found that the above four additives (i.e., flash voltage enhancing additives) have a more significant effect on improving the withstand voltage of the electrolyte than the existing flash voltage enhancing agents, mainly in the following two aspects: 1. The withstand voltage of the electrolyte is significantly improved. For every 1% increase in content, the withstand voltage of the electrolyte can be increased by 8 to 10V. 2. After adding the electrolyte, the service life of the electrolyte tends to be extended. The specific parameters obtained by the test are compared in Table 2 below.
[0060]
[0061] Table 2 Comparison of experimental test parameters of four flash voltage enhancement additives of the present invention
[0062] The present invention also protects an electrolyte of a high-voltage electrolytic capacitor using any one of the flash voltage enhancers in the above technical solutions, wherein the mass percentage of the flash voltage enhancer in the electrolyte of the high-voltage electrolytic capacitor is 4% to 6%.
[0063] In terms of mass percentage, the electrolyte of high-voltage electrolytic capacitors also includes the following components: the main solvent accounts for 65%-75%, the solute accounts for 10%-15%; the conventional flash voltage enhancer accounts for 10%-20%, and the others account for 3%-8%, such as inorganic nano-silicon.
[0064] After experimental test comparison of the present invention, the formula ratios of the existing formula without adding conventional flash voltage booster (the original formula in the table), the formula with added conventional flash voltage booster (the existing additives in the table), and the formula with added flash voltage booster of the present invention (the homemade additives in the table) and the obtained electrolyte parameters are shown in Tables 3 and 4 below.
[0065] Serial number Material Name Original formula Existing additives Add homemade additives 1 Main solvent 75~85 70~80 65~75 2 Solute 10~15 10~15 10~15 3 Existing additives / 10~20 10~20 4 Homemade additives 3 / / 4~6 5 other 3~8 3~8 3~8
[0066] Table 3 Ratio of three formulations
[0067] Serial number Electrolyte Conductivity (ms / cm) pH Initial flash voltage(V) 1 Original formula 1.45 6.45 490.1 2 Existing additive formulations 1.02 6.41 562.7 3 Add homemade additive formula 0.96 6.24 616.7
[0068] Table 4 Comparison of parameters of electrolytes obtained from three formulations
[0069] The electrolyte obtained by the existing formula without adding conventional flash voltage enhancer (the original formula in the table) has high conductivity and low withstand voltage of about 490V, which is only suitable for making 400-450V high-voltage aluminum electrolytic capacitors.
[0070] The electrolyte obtained by adding a formula of conventional flash voltage enhancer (the existing additives in the table) has a significantly reduced conductivity, reaching about 30%, and a significantly increased flash voltage, reaching about 560V, which is suitable for the production of 500V to 550V ultra-high voltage aluminum electrolytic capacitors.
[0071] The electrolyte obtained by adding the formula of the flash voltage enhancer of the present invention (the table shows the addition of self-made additives) has a conductivity reduced by about 5%, and the flash voltage is significantly increased again to about 616V, which is suitable for the production of 550-600V ultra-high voltage aluminum electrolytic capacitors.
[0072] Among the electrolytes obtained by the four flash voltage enhancing additives of the present invention, Additive 1 has the worst effect. According to the ratio in the last column of Table 3, when Additive 3 is replaced by Additive 1, the withstand voltage of the obtained electrolyte is improved on the basis of the existing addition, but it is still low and is not suitable for making 600V capacitors, but only suitable for making 550V. The specific formula ratios and electrolyte parameters are shown in Tables 5 and 6 below.
[0073] Serial number Material Name Add homemade additive formula 1 Solvents 65~75 2 Solute 10~15 3 Existing additives 10~20 4 Homemade additives 1 4~6 5 other 3~8
[0074] Table 5: Formula of electrolyte prepared with additive 1
[0075]
[0076] Table 6 Measured parameters of electrolyte obtained from Table 5
[0077] The high voltage referred to in the present invention refers to a voltage of 500V and above.
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a flash voltage enhancer, characterized in that: include: After mixing 50%-60% ethylene glycol and 10%-20% boric acid, the mixture is heated to a first temperature range and kept warm for a first time; the first temperature range is 50-80° C.; Continue to add 10%-20% dodecanedioic acid, 3%-5% mannitol and 10%-20% water-soluble starch, mix, and continue to keep warm for the second time; Heating the solution that meets the second time requirement to a second temperature range of 150-170° C.; After keeping warm for a third time, cooling to a third temperature range of 75-95° C., keeping warm for a fourth time, the minimum value of the second temperature range is greater than the maximum value of the first temperature range; Cool down to the operating temperature range to form a flash voltage enhancer. Continuous stirring is required during the above process.
2. A flash voltage enhancer, characterized in that: The flash voltage enhancer is prepared by the preparation method of the flash voltage enhancer as claimed in claim 1.
3. An electrolyte for a high-voltage electrolytic capacitor, characterized in that: Comprising the flash voltage enhancer as claimed in claim 2.
4. The electrolyte of the high-voltage electrolytic capacitor according to claim 3, characterized in that: In the electrolyte of the high-voltage electrolytic capacitor, the mass percentage of the flash voltage enhancer is 4% to 6%.
Citation Information
Patent Citations
Electrolyte for flame-retardant wide-temperature high-voltage aluminum electrolytic capacitor and preparation method thereof
CN102779644A
Electrolyte for driving of aluminum electrolytic capacitor and preparation method of main solute of electrolyte
CN102969161A
Flash?voltage?boosting agent used for capacitor working electrolyte and preparation method of flash?voltage?boosting agent
CN103337366A
Working electrolyte of 630 V high-voltage aluminum electrolytic capacitor and manufacturing method thereof
CN103811183A
650V-700V extra-high-voltage aluminum electrolytic capacitor, working electrolyte and preparation method thereof
CN103915258A