Layered oxysulfide compound composite CdS photoelectric material and preparation method and application thereof

By compounding layered oxychalene compounds with CdS to form heterostructure thin-film photoelectric materials, the problem of insufficient photoelectric performance of existing layered oxychalene compounds is solved, and a significant improvement in photoelectric performance and expansion of application prospects has been achieved.

CN114420785BActive Publication Date: 2024-11-22SHANGHAI INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111583307.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-11-22
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

The photoelectric properties of existing layered oxychalene compounds cannot meet the actual application requirements in bulk samples, and there are problems such as high device preparation cost, low environmental stability and quality defects.

Method used

By compounding layered oxychalene compounds with CdS, thin-film photoelectric materials with heterostructure are prepared, and the built-in potential at the hetero interface is used to suppress carrier recombination to improve photoelectric performance. The specific method includes depositing a CdS film on the conductive substrate, forming a composite film by spin coating of oxychalgen compound slurry and vacuum annealing, and finally using screen-printed silver paste as the back electrode.

Benefits of technology

The photoelectric performance of layered oxychalcogen compounds has been significantly improved, the photogenerating current has been increased by 360 times, and the photoelectric response time has been greatly shortened. It is suitable for applications in the field of photoelectricity, and the preparation process is simple and the overall energy consumption is low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114420785B_ABST
    Figure CN114420785B_ABST
Patent Text Reader

Abstract

The present invention relates to a composite photoelectric material, and in particular to a layered oxygen-sulfur compound composite CdS photoelectric material, a preparation method and an application thereof, comprising the following steps: S1: cleaning a conductive substrate; S2: preparing a CdS film on the cleaned conductive substrate obtained in step S1; S3: preparing an oxygen-sulfur compound slurry, and spin coating it on the CdS film obtained in step S2 and vacuum annealing; S4: screen-printing a silver paste as a back electrode on the composite film obtained in step S3 to obtain the layered oxygen-sulfur compound composite CdS photoelectric material, the structure of which is a conductive substrate, a CdS film, an oxygen-sulfur compound film and an Ag electrode from bottom to top. Compared with the prior art, the present invention prepares a thin film photoelectric material with a heterogeneous structure by combining a layered oxygen-sulfur compound with CdS, and because of the built-in potential at the heterogeneous interface, carrier recombination can be effectively suppressed, thereby achieving a significant improvement in photoelectric performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite photoelectric material, in particular to a layered oxysulfide compound composite CdS photoelectric material and a preparation method and application thereof. Background Art

[0002] In recent decades, transition metal chalcogenides (TMDCs) are a class of layered materials with a basic chemical formula of MX2, where M represents transition metal elements, including Ti, V, Ta, Mo, W, Re, etc., and X represents chalcogen atoms S, Se, Te, etc. They have attracted great attention for their wide applications in superconductors, photovoltaics, thermoelectrics, battery electrodes, photodetectors, etc. due to their excellent semiconductor optoelectronic properties, controllable band gap properties (single layer is direct band gap, multilayer is indirect band gap), adjustable band gap size (from 1.0eV for multilayer MoTe2 to 2.1eV for single layer WS2), variability from semiconductor to metallic properties (by changing the stacking phase), and strong spin-orbit coupling effects. However, so far, TMDCs with excellent optoelectronic properties are mostly limited to TMDCs with chalcopyrite structure and related derivatives, such as CdTe, CuInS2 (CIS), Cu(In x Ga 1-x )Se2(CIGS) and Cu2ZnSnS4(CZTS), but the toxicity of the elements such as As and Cd contained in them will cause great harm to the environment; In, Ga, Te and other elements are scarce, and their commercial prospects are not as good as silicon; other optoelectronic materials such as WS2 / TiO2 devices have a photocurrent of only 25nA / cm 2 Therefore, TMDCs face many challenges such as poor environment, lack of chemical composition and low efficiency.

[0003] In recent years, layered oxychalcogenides such as Bi2O2S(Se) and Bi4O4SeCl2 have been shown to have ultra-high electron mobility, suitable optical band gap and reliable environmental stability as a special quasi-two-dimensional (2D) layered material, showing great potential in high-speed and low-power devices. However, the excellent performance of most layered oxychalcogenides has only been reported in single-layer or few-layer samples, resulting in high device preparation cost, low environmental stability and inevitable quality defects.

[0004] Recently, a new layered oxychalcogenide Bi9O 7.5 Significant photoelectric properties were observed in bulk samples of S6 and FeOCuS, indicating that they have broad application prospects in the field of optoelectronics. However, the photoelectric properties of bulk samples of these materials still cannot meet the needs of practical applications, and it is urgent to explore appropriate methods or technologies to improve their photoelectric properties. Summary of the invention

[0005] Cadmium sulfide (CdS) is a II-VI group n-type wide bandgap semiconductor. Due to its high transmittance, high electron mobility and low resistivity, it is often used as an effective window layer for manufacturing super-substrate solar cell structures. CdS is not affected by charge traps induced by oxygen vacancies caused by ultraviolet light irradiation, and has been widely used in the field of composite heterojunction thin film devices.

[0006] The purpose of the present invention is to solve at least one of the above problems and to provide a layered oxysulfide compound composite CdS photoelectric material and a preparation method and application. By combining the layered oxysulfide compound with CdS to prepare a thin film photoelectric material with a heterostructure, the built-in potential exists at the heterogeneous interface, which can effectively inhibit carrier recombination, thereby achieving a significant improvement in the photoelectric performance of the layered oxysulfide compound.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] The first aspect of the present invention discloses a method for preparing a layered oxysulfide compound composite CdS photoelectric material, comprising the following steps:

[0009] S1: Cleaning the conductive substrate;

[0010] S2: preparing a CdS thin film on the cleaned conductive substrate obtained in step S1;

[0011] S3: preparing an oxygen-sulfide compound slurry, spin-coating it on the CdS film obtained in step S2, and performing vacuum annealing.

[0012] Preferably, the conductive substrate in step S1 is ITO conductive glass, FTO conductive glass or organic conductive film. The conductive substrate is a transparent conductive substrate.

[0013] Preferably, the cleaning in step S1 is ultrasonic cleaning using acetone, anhydrous ethanol and deionized water in sequence, each time for 10-15 minutes, and drying with nitrogen.

[0014] Preferably, step S2 specifically includes the following steps:

[0015] S21: Thoroughly mix thiourea, acetic acid and deionized water to obtain solution A;

[0016] S22: mixing the Cd(NO3)2 solution and aqueous ammonia to form a solution B;

[0017] S23: placing the conductive substrate in the solution A obtained in step S21, heating it to a specified temperature, and then adding the solution B obtained in step S22 into the solution A for deposition;

[0018] S24: Annealing the deposited conductive substrate obtained in step S23 to complete step S2.

[0019] Preferably, in step S21, the usage ratio of thiourea, acetic acid and deionized water is 1.903-4.3077 g: 1-2.3 mL: 75-169 mL.

[0020] Preferably, the concentration of the Cd(NO3)2 solution in step S22 is 0.2-0.3M, and the dosage ratio of the Cd(NO3)2 solution to aqueous ammonia is 0.55-0.83mL:7-16mL.

[0021] Preferably, the mixing and stirring in step S22 is performed at a speed of 100-200 rpm and for a time of 5-10 min.

[0022] Preferably, the specified temperature in step S23 is 65-90°C.

[0023] Preferably, the deposition time in step S23 is 30-90 minutes.

[0024] Preferably, the annealing in step S24 is performed in a N2 atmosphere at 300-350°C for 2-3h.

[0025] In the preparation process of CdS thin film, the chemical bath deposition method is adopted, wherein the configuration of the deposition solution and the parameters set in the synthesis process are to make the temperature of the entire solution more uniform, thereby ensuring that CdS can be uniformly deposited on the conductive substrate. At the same time, the deposited CdS thin film is annealed in N2 atmosphere, because the CdS thin film annealed in N2 has better quality, the formed film is denser and no impurities are generated.

[0026] Preferably, the oxysulfide compound slurry in step S3 is composed of an oxysulfide compound and isopropanol, and the oxysulfide compound is Bi9O 7.5 S6 or FeOCuS, the mass concentration of oxysulfide compounds is 0.3-0.7 g / mL isopropanol.

[0027] Among them, the Bi9O 7.5 S6 was prepared by the following steps:

[0028] Bi(NO3)2·5H2O, SC(NH2)2, KOH and deionized water were mixed in a ratio of 0.01mol:0.01mol:15g:10mL and stirred evenly, then transferred to the inner lining of the reactor and placed in an oven. The oven temperature was set to 150°C and the reaction time was 2-3 days. After the reaction was completed, it was naturally cooled to room temperature, washed and dried to obtain the Bi9O 7.5 S6.

[0029] Wherein, the FeOCuS is prepared by the following steps:

[0030] Iron powder, copper powder, SC(NH2)2, KOH, and deionized water were mixed in a ratio of 0.005 mol: 0.005 mol: 0.025 mol: 10 g: 10 mL and stirred evenly, then transferred to the inner lining of a reactor and placed in an oven, the oven temperature was set to 200°C, and the reaction time was 2-3 days. After the reaction was completed, the mixture was naturally cooled to room temperature, and the obtained sample was washed and dried to obtain the FeOCuS.

[0031] Preferably, the spin coating speed in step S3 is 700-2000 rpm, the time is 10-30 s, and the slurry spin coating amount is 40-80 μL. Spin coating can obtain a coating with a higher density and a more uniform coating thickness; by controlling the spin coating amount within the range of 40-80 μL, the photoelectric thin film material obtained by spin coating can also be controlled to be at a suitable thickness, so that the photoelectric thin film material obtained by spin coating can have more excellent photoelectric properties.

[0032] The isopropanol slurry of the oxysulfide compound is spin-coated on the CdS film using a coating machine. The amount of slurry used and the rotation speed used by the coating machine are directly related to the thickness of the film, and the thickness of the film formed is highly related to the photoelectric performance that the photoelectric film material can achieve. When the rotation speed and amount are controlled within the above range, the final product performance is better, and the photoelectric performance of the material prepared beyond this range will be greatly reduced. This is because as the thickness of the film increases, the light absorption capacity of the film becomes stronger and stronger, and the charge transfer performance is improved, but the thickness exceeding a certain range will hinder the electronic transmission capacity of the device and cause the device performance to decline. As mentioned above, the appropriate thickness range is 10-30μm.

[0033] Preferably, the vacuum annealing in step S3 is to heat to 200-250°C at a rate of 1-2°C / min at -0.1MPa, calcine for 1-2h, and then cool to room temperature under vacuum. If the given temperature is exceeded, the crystal structure of the oxysulfide compound will be destroyed, resulting in the decomposition of the FeOCuS sample (decomposed into Fe2O3, Cu2S, etc.). If the temperature is too low, it is not conducive to the volatilization of the organic solvent in the membrane, thereby affecting the performance of the membrane.

[0034] Preferably, the method further comprises the following steps:

[0035] S4: Screen-printing silver paste as a back electrode on the composite film obtained in step S3 to obtain the layered oxysulfide compound composite CdS photoelectric material.

[0036] The second aspect of the present invention discloses a layered oxysulfide compound composite CdS photoelectric material prepared by any of the above-described layered oxysulfide compound composite CdS photoelectric material preparation methods, wherein the structure thereof is, from bottom to top, a conductive substrate, a CdS film, an oxysulfide compound film and an Ag electrode.

[0037] The third aspect of the present invention discloses an application of the layered oxysulfide compound composite CdS photoelectric material as described above, and the application of the layered oxysulfide compound composite CdS photoelectric material in the preparation of a photoelectric device.

[0038] Preferably, the layered oxysulfide compound composite CdS photoelectric material is used in the preparation of photodetectors and photovoltaic devices.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] 1. The photoelectric thin film material obtained by compounding the layered oxysulfide compound and CdS in the present invention has a heterostructure. Since the two materials forming the heterostructure have different band gap widths, a carrier concentration difference will be generated at the interface, which will cause the wide band gap electrons to diffuse into the narrow band gap, and the narrow band gap holes to diffuse into the wide band gap, so that a space charge region will be formed at the cross section, that is, there is a built-in potential at the heterointerface. The existence of the built-in potential at the heterointerface can effectively inhibit carrier recombination, thereby making the separation of photogenerated carriers more efficient and greatly improving the photoelectric performance.

[0041] 2. In the preparation process of the present invention, a chemical bath deposition method is used to deposit a CdS film on a conductive substrate. The solution temperature is made uniform by controlling the parameters of the stirring synthesis process, so that the deposited CdS film can also achieve a uniform effect; at the same time, an annealing treatment is performed under N2 to obtain a CdS film without impurities. Further, a layer of oxygen-sulfide compound film is spin-coated on the CdS film using a glue spreader. By controlling the rotation speed and the amount of material used during the spin coating of the glue spreader, not only can the thickness of the formed film be controlled within a suitable range, but also the thickness of the formed film can be ensured to be uniform. Finally, a layered oxygen-sulfide compound composite CdS photoelectric film material is formed on the oxygen-sulfide compound film by screen printing silver paste as the back electrode, and a photoelectric film material with excellent photoelectric performance (microampere level) is obtained, which is suitable for application in the photoelectric field.

[0042] 3. The preparation method of the present invention is simple, with low overall energy consumption and mild preparation conditions. The photocurrent of the prepared photoelectric thin film material can be significantly improved compared with that of pure layered oxysulfide compounds, which can be up to 360 times that of layered oxysulfide compounds, and the photoelectric response time can also be greatly shortened, which can meet the needs in the optoelectronic field and can be further used to prepare photodetectors, photovoltaic devices and other optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 The CdS film and Bi9O prepared in Examples 1 and 2 of the present invention 7.5 XRD patterns of S6 and FeOCuS;

[0044] Figure 2 The Bi9O prepared in Example 1 of the present invention 7.5 S6 composite CdS photoelectric thin film material and pure Bi9O 7.5 IT curve of S6 material under zero bias;

[0045] Figure 3 The IT curves of the FeOCuS composite CdS photoelectric thin film material and the pure FeOCuS material prepared in Example 2 of the present invention under a bias voltage of 50 mV are shown;

[0046] Figure 4 The Bi9O prepared in Example 1 of the present invention 7.5 S6 composite CdS photoelectric thin film material and pure Bi9O 7.5 Photoelectric response time diagram of S6 material under zero bias;

[0047] Figure 5 This is a photoelectric response time diagram of the FeOCuS composite CdS photoelectric thin film material and the pure FeOCuS material prepared in Example 2 of the present invention under a bias voltage of 50 mV;

[0048] Figure 6 It is a schematic diagram of the structure of the layered oxysulfide compound composite CdS photoelectric material of the present invention;

[0049] In the figure: 1-conductive substrate; 2-CdS film; 3-oxygen sulfide compound film; 4-Ag electrode. DETAILED DESCRIPTION

[0050] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0051] Unless otherwise specified, the reagents used in the following examples may be commercially available products that can be routinely obtained by those skilled in the art.

[0052] Example 1

[0053] An oxysulfide compound Bi9O 7.5 The S6 composite CdS photoelectric thin film device has a structure from bottom to top of ITO conductive glass (conductive substrate 1), CdS thin film 2, oxygen sulfide compound thin film 3 (Bi9O 7.5 S6 film), Ag electrode 4. The preparation method is specifically:

[0054] 1. Cleaning of the conductive substrate 1:

[0055] The ITO conductive glass was first cleaned thoroughly with detergent, then ultrasonically cleaned with acetone, alcohol, and deionized water for 15 min, and then dried with nitrogen for later use.

[0056] 2. Prepare CdS thin film 2 on conductive substrate 1:

[0057] (1) Take a 250 mL beaker and a 100 mL beaker respectively, add thiourea (1.903 g), acetic acid (1 mL) and an appropriate amount of deionized water into the 250 mL beaker to make 75 mL of solution A and stir. Place the washed ITO conductive glass vertically into the wall of the large beaker and heat solution A to 75°C.

[0058] (2) Add 0.55 mL of 0.2 M Cd(NO3)2 solution and 7 mL of aqueous ammonia to a 100 mL beaker and stir at 100 rpm for 10 min to carry out complexation reaction to obtain solution B.

[0059] (3) When the temperature of solution A rises to 75°C, the two solutions are mixed and the timing is started. After 30 minutes, the conductive substrate 1 is taken out and the glass surface is cleaned with deionized water. Then, the CdS film 2 is annealed with N2 at a temperature of 350°C and a time of 2 hours.

[0060] 3. Preparation of oxysulfide compounds Bi9O 7.5 S6:

[0061] Bi(NO3)2·5H2O (0.01 mol), SC(NH2)2 (0.01 mol), KOH (15 g) and deionized water (10 mL) were mixed and stirred evenly, then transferred to a 50 mL reactor liner and placed in an oven. The oven temperature was set to 150°C and the reaction time was 3 days. After the reaction was completed and naturally cooled to room temperature, the obtained sample was washed and dried.

[0062] 4. Take Bi9O at a mass concentration of 0.6 g / mL isopropanol 7.5 S6 powder and isopropanol solution are stirred into a slurry.

[0063] 5. Take the CdS film 2 prepared in step 2, and spin-coat the slurry in step 4 on the CdS film 2 and a single ITO conductive glass (as a reference), with a spin coating amount of 80 μL, a spin coater speed of 1500 rpm, and a spin coating time of 20 s.

[0064] 6. Place the spin-coated film in a tube furnace, evacuate to -0.1 MPa, set the temperature to 200°C, keep warm for 2 hours, and heat up at a rate of 1°C / min for vacuum drying.

[0065] 7. After annealing, the film was quenched in vacuum atmosphere to room temperature, and then silver paste was screen-printed on the composite film as the back electrode to obtain Bi9O 7.5 The S6 composite CdS photoelectric thin film material has a structure from bottom to top that includes a transparent conductive substrate 1, a CdS thin film 2, a Bi9O 7.5 S6 film and Ag electrode 4, such as Figure 6 shown.

[0066] Example 2

[0067] An oxygen-sulfur compound FeOCuS composite CdS photoelectric thin film device, whose structure from bottom to top is ITO conductive glass (conductive substrate 1), CdS film 2, oxygen-sulfur compound film 3 (FeOCuS film), Ag electrode 4. The preparation method thereof is specifically:

[0068] 1. Cleaning of the conductive substrate 1:

[0069] The ITO conductive glass was first cleaned thoroughly with detergent, then ultrasonically cleaned with acetone, alcohol, and deionized water for 15 min, and then dried with nitrogen for later use.

[0070] 2. Prepare CdS thin film 2 on conductive substrate 1:

[0071] (1) Take a 250 mL beaker and a 100 mL beaker, add thiourea (1.903 g), acetic acid (1 mL) and an appropriate amount of deionized water into the 250 mL beaker to make 75 mL of solution A and stir. Place the washed ITO glass vertically on the wall of the large beaker and heat solution A to 75°C.

[0072] (2) Add 0.55 mL of 0.2 M Cd(NO3)2 solution and 7 mL of aqueous ammonia to a 100 mL beaker and stir at 100 rpm for 10 min to carry out complexation reaction to obtain solution B.

[0073] (3) When the temperature of solution A rises to 75°C, the two solutions are mixed and the timing is started. After 30 minutes, the conductive substrate 1 is taken out and the glass surface is cleaned with deionized water. Then, the CdS film 2 is annealed with N2 at a temperature of 350°C and a time of 2 hours.

[0074] 3. Preparation of oxysulfide compound FeOCuS:

[0075] Iron powder (0.005 mol), copper powder (0.005 mol), SC(NH2)2 (0.025 mol), KOH (10 g), and deionized water (10 mL) were mixed and stirred evenly, then transferred to a 50 mL reactor liner and placed in an oven. The oven temperature was set to 200 ° C and the reaction time was 3 days. After the reaction was completed, the sample was naturally cooled to room temperature and then washed and dried.

[0076] 4. Take FeOCuS powder and isopropanol solution at a mass concentration of 0.7 g / mL isopropanol and stir to form a slurry.

[0077] 5. Take the CdS film 2 prepared in step 2, and spin-coat the solution in step 4 on the CdS film 2 and a single ITO conductive glass (as a reference), with a spin coating amount of 80 μL, a spin coater speed of 1500 rpm, and a spin coating time of 20 s.

[0078] 6. Place the spin-coated sample in a tube furnace, evacuate to -0.1 MPa, set the temperature to 200°C, keep warm for 2 hours, and heat up at a rate of 1°C / min for vacuum drying.

[0079] 7. After annealing, the film is quenched in a vacuum atmosphere to room temperature, and a silver paste is screen-printed on the composite film as a back electrode to obtain a FeOCuS composite CdS photoelectric film material, whose structure from bottom to top includes a transparent conductive substrate 1, a CdS film 2, a FeOCuS film and an Ag electrode 4, as shown in FIG. Figure 6 shown.

[0080] Example 3

[0081] An oxygen-sulfur compound FeOCuS composite CdS photoelectric thin film device, whose structure from bottom to top is ITO conductive glass (conductive substrate 1), CdS film 2, oxygen-sulfur compound film 3 (FeOCuS film), Ag electrode 4. The preparation method thereof is specifically:

[0082] 1. Cleaning of the conductive substrate 1:

[0083] The ITO conductive glass was first cleaned thoroughly with detergent, then ultrasonically cleaned with acetone, alcohol, and deionized water for 10 min in sequence, and then dried with nitrogen for later use.

[0084] 2. Prepare CdS thin film 2 on conductive substrate 1:

[0085] (1) Take a 250 mL beaker and a 100 mL beaker, add thiourea (4.3077 g), acetic acid (2.3 mL) and an appropriate amount of deionized water into the 250 mL beaker to make 169 mL of solution A and stir. Place the washed ITO glass vertically on the wall of the large beaker and heat solution A to 85°C.

[0086] (2) Add 0.83 mL of 0.3 M Cd(NO3)2 solution and 16 mL of aqueous ammonia into a 100 mL beaker and stir at 150 rpm for 8 min to carry out complexation reaction to obtain solution B.

[0087] (3) When the temperature of solution A rises to 85°C, the two solutions are mixed and the timing is started. After 60 minutes, the conductive substrate 1 is taken out and the glass surface is cleaned with deionized water. Then, the CdS film 2 is annealed with N2 at a temperature of 300°C and a time of 3 hours.

[0088] 3. Preparation of oxysulfide compound FeOCuS:

[0089] Iron powder (0.005 mol), copper powder (0.005 mol), SC(NH2)2 (0.025 mol), KOH (10 g), and deionized water (10 mL) were mixed and stirred evenly, then transferred to a 50 mL reactor liner and placed in an oven. The oven temperature was set to 200 ° C and the reaction time was 2.5 days. After the reaction was completed, the sample was naturally cooled to room temperature and then washed and dried.

[0090] 4. Take FeOCuS powder and isopropanol solution at a mass concentration of 0.3 g / mL isopropanol and stir to form a slurry.

[0091] 5. Take the CdS film 2 prepared in step 2, and spin-coat the solution in step 4 on the CdS film 2 and a single ITO conductive glass (as a reference), with a spin coating amount of 80 μL, a spin coating machine speed of 800 rpm, and a spin coating time of 25 s.

[0092] 6. Place the spin-coated sample in a tube furnace, evacuate to -0.1 MPa, set the temperature to 250°C, keep warm for 1 h, and heat at a rate of 1.5°C / min for vacuum drying.

[0093] 7. After annealing, the film is quenched in a vacuum atmosphere to room temperature, and a silver paste is screen-printed on the composite film as a back electrode to obtain a FeOCuS composite CdS photoelectric film material, whose structure from bottom to top includes a transparent conductive substrate 1, a CdS film 2, a FeOCuS film and an Ag electrode 4, as shown in FIG. Figure 6 shown.

[0094] Example 4

[0095] An oxygen-sulfur compound FeOCuS composite CdS photoelectric thin film device, whose structure from bottom to top is ITO conductive glass (conductive substrate 1), CdS film 2, oxygen-sulfur compound film 3 (FeOCuS film), Ag electrode 4. The preparation method thereof is specifically:

[0096] 1. Cleaning of the conductive substrate 1:

[0097] The ITO conductive glass was first cleaned thoroughly with detergent, then ultrasonically cleaned with acetone, alcohol, and deionized water for 12 min, and then dried with nitrogen for later use.

[0098] 2. Prepare CdS thin film 2 on conductive substrate 1:

[0099] (1) Take a 250 mL beaker and a 100 mL beaker, add thiourea (2.3902 g), acetic acid (1.3 mL) and an appropriate amount of deionized water into the 250 mL beaker to make 94 mL of solution A and stir. Place the washed ITO glass vertically on the wall of the large beaker and heat the solution A to 68°C.

[0100] (2) Add 0.69 mL of 0.2 M Cd(NO3)2 solution and 9 mL of aqueous ammonia to a 100 mL beaker and stir at 200 rpm for 5 min to carry out complexation reaction to obtain solution B.

[0101] (3) When the temperature of solution A rises to 68°C, the two solutions are mixed and the timing is started. After 90 minutes, the conductive substrate 1 is taken out and the glass surface is cleaned with deionized water. Then, the CdS film 2 is annealed with N2 at a temperature of 320°C and a time of 2.5 hours.

[0102] 3. Preparation of oxysulfide compound FeOCuS:

[0103] Iron powder (0.005 mol), copper powder (0.005 mol), SC(NH2)2 (0.025 mol), KOH (10 g), and deionized water (10 mL) were mixed and stirred evenly, then transferred to a 50 mL reactor liner and placed in an oven. The oven temperature was set to 200 ° C and the reaction time was 2 days. After the reaction was completed, the sample was naturally cooled to room temperature and then washed and dried.

[0104] 4. Take FeOCuS powder and isopropanol solution at a mass concentration of 0.5 g / mL isopropanol and stir to form a slurry.

[0105] 5. Take the CdS film 2 prepared in step 2, and spin-coat the solution in step 4 on the CdS film 2 and a single ITO conductive glass (as a reference), with a spin coating amount of 80 μL, a spin coating machine speed of 1800 rpm, and a spin coating time of 15 s.

[0106] 6. Place the spin-coated sample in a tube furnace, evacuate to -0.1 MPa, set the temperature to 230°C, keep warm for 1.5 hours, and heat up at a rate of 2°C / min for vacuum drying.

[0107] 7. After annealing, the film is quenched in a vacuum atmosphere to room temperature, and a silver paste is screen-printed on the composite film as a back electrode to obtain a FeOCuS composite CdS photoelectric film material, whose structure from bottom to top includes a transparent conductive substrate 1, a CdS film 2, a FeOCuS film and an Ag electrode 4, as shown in FIG. Figure 6 shown.

[0108] Performance Testing:

[0109] The X-ray diffraction instrument was used to detect the CdS, oxysulfide compounds (Bi9O 7.5 S6 or FeOCuS) crystal structure, its XRD pattern is as follows Figure 1 As shown, all of its original diffraction peaks can correspond to the standard diffraction peak positions, indicating that the obtained samples are all pure phases.

[0110] The photoelectric properties of the oxychalcogenide compound composite CdS photoelectric thin film materials prepared in each embodiment were tested using KEITHLEY 2450, and the corresponding performances of the single Bi9O 7.5 S6 and FeOCuS thin film materials were used as controls. Figure 2 As shown, Bi9O prepared in Example 1 7.5 S6 composite CdS photoelectric thin film material and pure Bi9O 7.5 Comparison of IT curves of S6 photoelectric thin film materials under zero bias. The test uses a 55W xenon lamp as the light source, the linear scan parameter is set to 0V-0V, the limiting current is set to 20μA, and the light is turned on and off in the "Time" mode to perform a current-time curve test. 7.5 The photocurrent of S6 film is significantly improved (360 times), and the photoelectric response time is shorter (see Figure 4 ).like Figure 3 The figure shows the IT curve comparison of the FeOCuS composite CdS photoelectric thin film material prepared in Example 2 and the pure FeOCuS photoelectric thin film material under 50mV bias. The test uses a 55W xenon lamp as the light source, the linear scan parameter is set to 50mV-50mV, the limiting current is set to 120μA, and the light is turned on and off in the "Time" mode to perform the current-time curve test. The composite film has a significant increase in photocurrent compared to the single FeOCuS film (3.3 times). Figure 5It can be seen that the photoelectric response time of the composite photoelectric film is significantly reduced compared with the single FeOCuS film (from 0.99s to 0.07s). This shows that the construction of the heterojunction between the oxysulfide compound and CdS not only combines the excellent visible light capture ability of the CdS film, which greatly improves the absorption capacity of visible light, but also significantly promotes the effective separation of photogenerated charge carriers due to the synergistic effect between the two, so that the photoelectric performance of the composite film sample is significantly improved compared with the performance of the single oxysulfide compound photoelectric film.

[0111] In fact, most of the known chalcogenides with excellent photoelectric properties are limited to chalcopyrite and its derivatives (such as CdTe, Cu2ZnSnS4), whose constituent elements are highly toxic, have low reserves and high preparation costs. The two composite photoelectric films prepared by the present invention using a simple and low-cost method with the help of heterojunction construction have excellent photoelectric properties (microampere level), which is lower than WS2 / TiO2 photoelectric devices (~25nA / cm 2 ) has been significantly improved. This shows that it has broad application prospects in the field of optoelectronics.

[0112] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a layered oxysulfide compound composite CdS photoelectric material, characterized in that: The steps include: S1: Cleaning the conductive substrate; S2: preparing a CdS thin film on the cleaned conductive substrate obtained in step S1; S3: preparing an oxygen-sulfide compound slurry, spin coating it on the CdS film obtained in step S2, and vacuum annealing; In step S3: The oxysulfide compound slurry is composed of oxysulfide compound and isopropanol, and the oxysulfide compound is Bi9O 7.5 S6 or FeOCuS, the mass concentration of oxysulfide is 0.3-0.7 g / mL; The spin coating speed is 700-2000rpm, the time is 10-30s, and the slurry spin coating volume is 40-80μL; The vacuum annealing is to heat to 200-250°C at a rate of 1-2°C / min at -0.1MPa, calcine for 1-2h, and then cool to room temperature under vacuum; The photoelectric thin film material obtained by combining layered oxysulfide compounds with CdS has a heterostructure. Since the two materials forming the heterostructure have different band gap widths, a carrier concentration difference will be generated at the interface, which will cause electrons with a wide band gap to diffuse into a narrow band gap, and holes with a narrow band gap to diffuse into a wide band gap. Therefore, a space charge region will be formed at the cross section, that is, there is a built-in potential at the heterointerface.

2. The method for preparing a layered oxychalcogenide composite CdS photoelectric material according to claim 1, characterized in that: The conductive substrate described in step S1 is ITO conductive glass, FTO conductive glass or an organic conductive film.

3. The method for preparing a layered oxysulfide compound composite CdS photoelectric material according to claim 1, characterized in that: The cleaning in step S1 is to use acetone, anhydrous ethanol and deionized water for ultrasonic cleaning in sequence, each time for 10-15 minutes, and blow dry with nitrogen.

4. The method for preparing a layered oxysulfide compound composite CdS photoelectric material according to claim 1, characterized in that: Step S2 specifically includes the following steps: S21: Thoroughly mix thiourea, acetic acid and deionized water to obtain solution A; S22: mixing the Cd(NO3)2 solution and aqueous ammonia to form a solution B; S23: placing the conductive substrate in the solution A obtained in step S21, heating it to a specified temperature, and then adding the solution B obtained in step S22 into the solution A for deposition; S24: Annealing the deposited conductive substrate obtained in step S23 to complete step S2.

5. The method for preparing a layered oxychalcogenide compound composite CdS photoelectric material according to claim 4, characterized in that: Include one or more of the following: (i) in step S21, the ratio of thiourea, acetic acid and deionized water is 1.903-4.3077 g: 1-2.3 mL: 75-169 mL; (ii) in step S22, the concentration of the Cd(NO3)2 solution is 0.2-0.3M, and the ratio of the Cd(NO3)2 solution to the ammonia water is 0.55-0.83mL:7-16mL; (iii) in step S22, the mixing and stirring is performed at a speed of 100-200 rpm for 5-10 min; (iv) the temperature in step S23 is 65-90°C; (v) the deposition time in step S23 is 30-90 min; (vi) Annealing in step S24 is performed in a N2 atmosphere at 300-350°C for 2-3 hours.

6. The method for preparing a layered oxychalcogenide compound composite CdS photoelectric material according to claim 1, characterized in that: The following steps are also included: S4: Screen-printing silver paste as a back electrode on the composite film obtained in step S3 to obtain the layered oxysulfide compound composite CdS photoelectric material.

7. A layered oxysulfide compound composite CdS photoelectric material prepared by the method for preparing a layered oxysulfide compound composite CdS photoelectric material according to any one of claims 1 to 6, characterized in that: Its structure from bottom to top is a conductive substrate, a CdS film, an oxysulfide compound film and an Ag electrode.

8. An application of the layered oxysulfide compound composite CdS photoelectric material as claimed in claim 7, characterized in that: The application of the layered oxysulfide compound composite CdS photoelectric material in the preparation of photoelectric devices.