A method for preparing an electrode and a method for preparing a solar cell
By using electrodes formed by electroplating and screen printing processes in solar cells, combined with silver alloys and silver-free materials, the problem of high electrode cost is solved, lower-cost and efficient electrode preparation is achieved, and the efficiency of solar cells is improved. and reliability.
Patent Information
- Application Number
- CN202210129940.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-02-11
AI Technical Summary
The electrode cost of existing solar cells is high, especially due to the use of expensive silver materials, which results in the overall cost of solar cells remaining high, hindering their promotion.
An electroplating process is used to form a secondary grid electrode on at least one side of the semiconductor substrate layer, and a screen printing process is used to form a main grid electrode on the other side. The main grid electrode is electrically connected to the secondary grid electrode, using silver alloy and non-woven fabrics. Silver-containing materials to reduce costs, while improving the morphology and reliability of the electrode through precise control of the mask layer and seed layer.
It achieves lower-cost electrode preparation, provides larger pad spots and good welding pull force, reduces the blocking of sunlight, and improves the reliability of the electrode and the efficiency of the solar cell.
Smart Images

Figure CN114420796B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to a method for preparing an electrode and a method for preparing a solar cell. Background Art
[0002] Solar cells are devices that convert solar energy directly into electrical energy based on the photovoltaic effect. At present, crystalline silicon solar cells are the mainstream of the photovoltaic industry, occupying more than 80% of the market. Heterojunction (Heterojunction withintrinsic Thin layer, referred to as HJT) cells are an important type of solar cell. The heterojunction structure is centered on an N-type single crystal silicon substrate, with a P-type amorphous silicon layer and an N-type amorphous silicon layer on both sides of the N-type single crystal silicon substrate. The heterojunction structure has excellent photoelectric properties that cannot be achieved by the PN junctions of the two semiconductors. The use of heterojunction structures to prepare cells is a very competitive solar cell technology. After the heterojunction cell is prepared, multiple cells can be interconnected to form a component, ultimately realizing the use of electrical energy.
[0003] In addition to the above-mentioned PN junction, the heterojunction solar cell also includes a transparent conductive film for collecting current and a metal grid line for current extraction, that is, transparent conductive films are formed on both sides of the P-type amorphous silicon layer and the N-type amorphous silicon layer of the heterojunction structure, and then grid lines are formed on the transparent conductive film. The metal grid lines of the prior art solar cells are printed with low-temperature conductive silver paste by screen printing, and then dried and cured to form electrodes. However, the cost of low-temperature conductive silver paste is relatively high. Taking the 166mm M6 single-chip cell as an example, the preparation of the metal grid lines requires more than 200mg of silver paste, which accounts for more than 40% of the non-silicon cost of the solar cell.
[0004] In fact, in addition to heterojunction solar cells, other types of solar cells currently also need to set grid lines as electrodes to draw out current. Grid lines are usually made of expensive silver materials, which causes the cost of solar cells to remain high, thus hindering the promotion of solar cells. It can be seen that in the field of solar cells, the cost of electrodes provided by existing technologies needs to be further reduced. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the problem that the cost of the electrode provided in the prior art needs to be further reduced, thereby providing a method for preparing an electrode and a method for preparing a solar cell.
[0006] The present invention provides a method for preparing an electrode, comprising: providing a semiconductor substrate layer, and further comprising: forming a secondary gate line electrode on at least one side of the semiconductor substrate layer by using an electroplating process; forming a main gate line electrode on the side of the semiconductor substrate layer where the secondary gate line electrode is formed by using a screen printing process, wherein the main gate line electrode is electrically connected to the secondary gate line electrode.
[0007] Optionally, before forming the secondary gate line electrode, it also includes: forming a mask layer on at least one side of the semiconductor substrate layer, the pattern of the mask layer corresponds to the area where the secondary gate line electrode does not need to be formed; forming the secondary gate line electrode is to perform an electroplating process using the mask layer as a mask to form the secondary gate line electrode on at least one side of the semiconductor substrate layer, the pattern of the secondary gate line electrode and the mask layer are complementary on one side of the semiconductor substrate layer; after forming the secondary gate line electrode and before forming the main gate line electrode, removing the mask layer.
[0008] Optionally, the process of forming the mask layer includes an inkjet printing process.
[0009] Optionally, the material of the mask layer includes paraffin.
[0010] Optionally, the material of the main grid line electrode includes silver alloy.
[0011] Optionally, the process of removing the mask layer includes a heat treatment process or a chemical stripping process.
[0012] Optionally, the temperature of the heat treatment process is 50°C to 150°C.
[0013] Optionally, when a chemical stripping process is used to remove the mask layer, a stripping solution used to remove the mask layer includes a sodium hydroxide solution or a potassium hydroxide solution.
[0014] Optionally, it also includes: before forming the mask layer, forming a whole-surface seed layer on at least one side of the semiconductor substrate layer; the step of forming the mask layer is: forming the mask layer on the side of the seed layer away from the semiconductor substrate layer using a film forming process; the step of forming the secondary gate line electrode is: electroplating the secondary gate line electrode on the surface of the seed layer exposed by the mask layer; the electrode preparation method also includes: after removing the mask layer and before forming the main gate line electrode, removing the portion of the seed layer that is not blocked by the secondary gate line electrode.
[0015] Optionally, the step of forming a seed layer includes: forming a first seed layer on the entire surface of one side of the semiconductor substrate layer, and / or forming a second seed layer on the entire surface of the other side of the semiconductor substrate layer; correspondingly, the step of forming a mask layer includes: forming a first mask layer on the surface of the first seed layer on the side away from the semiconductor substrate layer where the auxiliary gate line electrode is not required to be formed, and / or forming a second mask layer on the surface of the second seed layer on the side away from the semiconductor substrate layer where the auxiliary gate line electrode is not required to be formed; the step of electroplating the auxiliary gate line electrode on the surface of the seed layer exposed by the mask layer includes: electroplating the first auxiliary gate line electrode on the surface of the first seed layer exposed by the first mask layer, and / or electroplating the second auxiliary gate line electrode on the surface of the second seed layer exposed by the second mask layer; the step of removing the mask layer includes: forming the first auxiliary gate line electrode After that, the first mask layer is removed, and / or the second mask layer is removed after the second secondary gate line electrode is formed; the step of removing the portion of the seed layer not covered by the secondary gate line electrode includes: removing the first mask layer and then removing the portion of the first seed layer not covered by the first secondary gate line electrode, and / or removing the second mask layer and then removing the portion of the second seed layer not covered by the second secondary gate line electrode; the step of forming a main gate line electrode includes: forming a first main gate line electrode on the side of the semiconductor substrate layer where the first secondary gate line electrode is formed by a screen printing process, and / or forming a second main gate line electrode on the side of the semiconductor substrate layer where the second secondary gate line electrode is formed by a screen printing process, the first main gate line electrode is electrically connected to the first secondary gate line electrode, and the second main gate line electrode is electrically connected to the second secondary gate line electrode.
[0016] Optionally, the process of forming the seed layer includes an electroplating process.
[0017] Optionally, the material of the seed layer includes copper or nickel.
[0018] Optionally, the seed layer has a thickness of 50 nm to 150 nm.
[0019] Optionally, the process of removing the portion of the seed layer not blocked by the secondary gate line electrode comprises a chemical stripping process.
[0020] Optionally, the stripping solution in the chemical stripping process used to remove the portion of the seed layer not blocked by the secondary gate line electrode includes a sodium hydroxide solution or a potassium hydroxide solution.
[0021] Optionally, the chemical stripping process includes a spraying process.
[0022] Optionally, the step of electroplating the auxiliary gate line electrode on the surface of the seed layer exposed by the mask layer includes: electroplating the bottom auxiliary gate line electrode on the surface of the seed layer exposed by the mask layer; forming a top auxiliary gate line electrode on the surface of the bottom auxiliary gate line electrode facing away from the semiconductor substrate layer; wherein the melting point of the top auxiliary gate line electrode is lower than the melting point of the bottom auxiliary gate line electrode, and the conductivity of the bottom auxiliary gate line electrode is higher than the conductivity of the top auxiliary gate line electrode.
[0023] Optionally, the material of the bottom-layer secondary gate line electrode includes copper, and the material of the top-layer secondary gate line electrode includes tin.
[0024] Optionally, the thickness of the bottom layer auxiliary grid line electrode is 3 μm to 15 μm; the thickness of the top layer auxiliary grid line electrode is 0.3 μm to 3 μm.
[0025] Optionally, the method further includes: after removing the mask layer, forming a conductive protection layer on the side wall surface of the bottom-layer secondary gate line electrode.
[0026] Optionally, the process of forming the conductive protection layer includes a chemical plating process.
[0027] Optionally, the material of the conductive protection layer is the same as that of the top-layer secondary gate line electrode.
[0028] Optionally, the material of the conductive protective layer includes tin.
[0029] Optionally, the thickness of the conductive protective layer is 0.5 μm to 2 μm.
[0030] Optionally, after the conductive protection layer is formed, the conductive protection layer is heated so that the conductive protection layer forms a conductive covering layer covering the side wall surface and the top surface of the secondary gate line electrode.
[0031] Optionally, the conductive protection layer is formed after the portion of the seed layer not blocked by the auxiliary gate line electrode is removed; or, after the conductive protection layer is formed, the portion of the seed layer not blocked by the auxiliary gate line electrode is removed.
[0032] Optionally, a ratio of the thickness of the mask layer to the thickness of the bottom secondary gate line electrode is 1:0.95 to 1:1.05.
[0033] The present invention also provides a method for preparing a solar cell, comprising: providing a semiconductor substrate layer; forming a transparent conductive film on at least one side of the semiconductor substrate layer; and also comprising: a method for preparing an electrode provided by the present invention; wherein: the step of forming a secondary grid line electrode on at least one side of the semiconductor substrate layer by using an electroplating process comprises: forming a secondary grid line electrode on a side of a portion of the transparent conductive film away from the semiconductor substrate layer by using an electroplating process; the step of forming a main grid line electrode on at least one side of the semiconductor substrate layer by using a screen printing process comprises: forming a main grid line electrode on a side of a portion of the transparent conductive film away from the semiconductor substrate layer by using a screen printing process.
[0034] The technical solution of the present invention has the following beneficial effects:
[0035] 1. The method for preparing the electrode provided by the present invention, the main grid electrode is formed by a screen printing process, and the main grid electrode has a certain width to provide a larger pad point, provide better welding tension, and is conducive to the interconnection of components. The width of the secondary grid electrode formed by the electroplating process is narrower than that of the secondary grid electrode formed by the screen printing process, so that the secondary grid electrode blocks less sunlight. The secondary grid electrode is formed by the electroplating process, which is more conducive to forming a secondary grid electrode that does not contain silver, and can reduce the cost of the electrode.
[0036] 2. Further, before forming the mask layer, a seed layer is formed on at least one side of the semiconductor substrate layer. Since the seed layer is a whole surface and not patterned before forming the gate electrode, the seed layer is easier to form and has a higher film quality. Before forming the main gate electrode, the seed layer on the side of the auxiliary gate electrode is removed, and the seed layer does not block sunlight.
[0037] Furthermore, the process of forming the mask layer includes an inkjet printing process, so that the pattern of the mask layer has a higher precision, so that the position and morphology of the gate line electrode are better, and the inkjet printing process will not damage the seed layer.
[0038] 3. Furthermore, the melting point of the top-level auxiliary gate line electrode is lower than that of the bottom-level auxiliary gate line electrode, and the conductivity of the bottom-level auxiliary gate line electrode is higher than that of the top-level auxiliary gate line electrode; the bottom-level auxiliary gate line electrode has better conductivity and can conduct current better, and the melting point of the top-level auxiliary gate line electrode is lower, so it can be more easily welded to the welding strip in the subsequent process of forming the component, and the top-level auxiliary gate line electrode acts as an adhesive layer between the bottom-level auxiliary gate line electrode and the welding strip.
[0039] Furthermore, the material of the bottom auxiliary grid line electrode includes copper, and the material of the top auxiliary grid line electrode includes tin. The auxiliary grid line electrode avoids using a relatively expensive material such as silver, thereby reducing the cost of the electrode.
[0040] 4. Furthermore, a conductive protection layer is formed on the side wall surface of the bottom auxiliary gate line electrode. The conductive protection layer can prevent the bottom auxiliary gate line electrode from being oxidized, thereby improving the reliability of the auxiliary gate line electrode.
[0041] 5. Furthermore, the thickness of the conductive protective layer is relatively thin, and it hardly occupies the space of the semiconductor substrate layer between adjacent secondary gate electrodes, thus reducing the shielding of sunlight. Since the conductive protective layer is formed after the seed layer on the side of the secondary gate electrode is removed, it is possible to prevent the conductive protective layer from being etched and damaged during the process of removing the seed layer, thereby improving the reliability of the secondary gate electrode.
[0042] 6. Furthermore, the ratio of the thickness of the mask layer to the thickness of the underlying secondary gate line electrode is 1:0.8 to 1:1.2. The thickness of the mask layer is close to the thickness of the underlying secondary gate line electrode, thereby avoiding the poor morphology of the secondary gate line electrode caused by the mask layer being too thin, and also avoiding the waste of mask layer material caused by the mask layer being too thick.
[0043] 7. The method for preparing a solar cell provided by the present invention forms a transparent conductive film on at least one side of the semiconductor substrate layer, and the auxiliary grid line electrode is indirectly connected to the transparent conductive film through a seed layer. Therefore, the bonding force between the auxiliary grid line electrode and the transparent conductive film is better, thereby preventing the auxiliary grid line electrode from being separated from the transparent conductive film. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 A schematic diagram of a process for preparing an electrode provided in one embodiment of the present invention;
[0046] Figures 2 to 10 A schematic structural diagram of a solar cell manufacturing process provided by an embodiment of the present invention;
[0047] Figures 11 to 19 A schematic structural diagram of a solar cell manufacturing process provided by another embodiment of the present invention;
[0048] Reference numerals:
[0049] 1-semiconductor substrate layer; 1a-semiconductor substrate layer; 2-first intrinsic semiconductor layer; 2a-first intrinsic semiconductor layer; 3-second intrinsic semiconductor layer; 3a-second intrinsic semiconductor layer; 4-first conductivity type semiconductor layer; 4a-first conductivity type semiconductor layer; 5-second conductivity type semiconductor layer; 5a-second conductivity type semiconductor layer; 6-first transparent conductive film; 6a-first transparent conductive film; 7-second transparent conductive film; 7a-second transparent conductive film; 8-first seed layer; 9-second seed layer; 10-first mask layer; 10a-first mask layer ; 11-second mask layer; 12-first bottom-layer auxiliary gate electrode; 12a-first bottom-layer auxiliary gate electrode; 13-second bottom-layer auxiliary gate electrode; 14-first top-layer auxiliary gate electrode; 14a-first top-layer auxiliary gate electrode; 15-second top-layer auxiliary gate electrode; 16-first conductive protective layer; 16a-first conductive protective layer; 16b-first conductive covering layer; 16c-first conductive covering layer; 17-second conductive protective layer; 17b-second conductive covering layer; 18-first main gate electrode; 18a-second auxiliary gate electrode; 19a-first main gate electrode. DETAILED DESCRIPTION
[0050] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0052] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal connection of two components, it can be a wireless connection, or it can be a wired connection. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0053] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0054] This embodiment provides a method for preparing an electrode. Figure 1 , including the following steps:
[0055] S1: providing a semiconductor substrate layer;
[0056] S2: forming a secondary gate line electrode on at least one side of the semiconductor substrate layer by an electroplating process;
[0057] S3: forming a main gate electrode on a side of the semiconductor substrate layer where the auxiliary gate electrode is formed by a screen printing process, wherein the main gate electrode is electrically connected to the auxiliary gate electrode.
[0058] In one embodiment, before forming the auxiliary gate line electrode, it also includes: before forming the auxiliary gate line electrode, it also includes: forming a mask layer on at least one side of the semiconductor substrate layer, the pattern of the mask layer corresponds to the area where the auxiliary gate line electrode does not need to be formed; forming the auxiliary gate line electrode is to perform an electroplating process using the mask layer as a mask to form the auxiliary gate line electrode on at least one side of the semiconductor substrate layer, the pattern of the auxiliary gate line electrode and the mask layer are complementary on one side of the semiconductor substrate layer; after forming the auxiliary gate line electrode and before forming the main gate line electrode, removing the mask layer.
[0059] The process of forming the mask layer includes an inkjet printing process. In this way, the pattern of the mask layer has a high precision, so that the position and morphology of the gate electrode are better. The material of the mask layer includes paraffin. The process of removing the mask layer includes a heat treatment process or a chemical stripping process. The temperature of the heat treatment process is 50°C to 150°C, for example, 50°C, 70°C, 90°C, 110°C, 130°C or 150°C. When the chemical stripping process is used to remove the mask layer, the stripping solution used to remove the mask layer includes a sodium hydroxide solution or a potassium hydroxide solution.
[0060] In one embodiment, it also includes: before forming the mask layer, forming a seed layer on the entire surface of at least one side of the semiconductor substrate layer, the process of forming the seed layer includes an electroplating process, the material of the seed layer includes copper or nickel, preferably nickel, nickel can better prevent the diffusion of copper metal, the material of the secondary gate electrode, when electroplating the secondary gate electrode, the thickness of the seed layer is 50nm to 150nm, for example, 50nm, 80nm, 100nm, 120nm or 150nm; the step of forming the mask layer is: forming the mask layer by a film forming process on the side of the seed layer away from the semiconductor substrate layer; the step of forming the secondary gate electrode is: electroplating the secondary gate electrode on the surface of the seed layer exposed by the mask layer; after removing the mask layer and before forming the main gate electrode, removing the portion of the seed layer that is not blocked by the secondary gate electrode, retaining the seed layer under the secondary gate electrode, the process of removing the seed layer on the side of the secondary gate electrode includes a chemical stripping process, and the side of the secondary gate electrode refers to the position with the seed layer under the adjacent secondary gate electrode. Specifically, the chemical stripping process includes a spraying process, that is, spraying a stripping liquid onto the surface of the seed layer by spraying. The seed layer is relatively thin and easier to remove; while the electroplated secondary grid line electrode is relatively thick, acting as a protective layer, thereby protecting the seed layer under the secondary grid line electrode from being removed. The stripping liquid in the chemical stripping process used to remove the portion of the seed layer not covered by the secondary grid line electrode includes a sodium hydroxide solution or a potassium hydroxide solution; after removing the seed layer on the side of the secondary grid line electrode, the main grid line electrode is formed.
[0061] In this embodiment, before forming the mask layer, a seed layer is formed on the entire surface of at least one side of the semiconductor substrate layer. Since the seed layer is entire and not patterned before forming the gate electrode, the seed layer is easier to form and the film quality of the seed layer is higher. After forming the secondary gate electrode, the seed layer on the side of the secondary gate electrode is removed. This part of the seed layer does not remain in the structure of the finished battery cell and therefore does not block sunlight. In other words, the seed layer on the side of the secondary gate electrode removed here, that is, the seed layer between adjacent secondary gate electrodes, does not include the seed layer located below the secondary gate electrode. After removing the seed layer on the side of the secondary gate electrode, there is no seed layer between adjacent secondary gate electrodes.
[0062] In this embodiment, the material of the main grid line electrode includes a silver alloy. In other embodiments, the material of the main grid line electrode may also be an alloy that does not contain silver.
[0063] The step of forming a seed layer includes: forming a first seed layer on the entire surface on one side of the semiconductor substrate layer, and / or forming a second seed layer on the entire surface on the other side of the semiconductor substrate layer; in this embodiment, the first seed layer is formed on the entire surface on one side of the semiconductor substrate layer and the second seed layer is formed on the entire surface on the other side of the semiconductor substrate layer.
[0064] Correspondingly, the step of forming a mask layer includes: forming a first mask layer on the surface of the side of the first seed layer away from the semiconductor substrate layer where the auxiliary gate line electrode is not needed, and / or forming a second mask layer on the surface of the side of the second seed layer away from the semiconductor substrate layer where the auxiliary gate line electrode is not needed; that is, when only the first seed layer is formed, only the first mask layer is formed; when only the second seed layer is formed, only the second mask layer is formed; when the first seed layer and the second seed layer are formed, the first mask layer and the second mask layer are formed; in this embodiment, the first mask layer is formed on the surface of the side of the first seed layer away from the semiconductor substrate layer where the auxiliary gate line electrode is not needed, and the second mask layer is formed on the surface of the side of the second seed layer away from the semiconductor substrate layer where the auxiliary gate line electrode is not needed.
[0065] The step of electroplating the auxiliary gate line electrode on the surface of the seed layer exposed by the mask layer includes: electroplating the first auxiliary gate line electrode on the surface of the first seed layer exposed by the first mask layer, and / or electroplating the second auxiliary gate line electrode on the surface of the second seed layer exposed by the second mask layer; that is, when only the first mask layer is formed, only the first auxiliary gate line electrode is formed, when only the second mask layer is formed, only the second auxiliary gate line electrode is formed, and when the first mask layer and the second mask layer are formed, the first auxiliary gate line electrode and the second auxiliary gate line electrode are formed; in this embodiment, the first auxiliary gate line electrode is electroplated on the surface of the first seed layer exposed by the first mask layer and the second auxiliary gate line electrode is electroplated on the surface of the second seed layer exposed by the second mask layer.
[0066] The step of removing the mask layer includes: removing the first mask layer after forming the first auxiliary gate line electrode, and / or removing the second mask layer after forming the second auxiliary gate line electrode; that is, when only the first auxiliary gate line electrode is formed, only the first mask layer is removed; when only the second auxiliary gate line electrode is formed, only the second mask layer is removed; when the first auxiliary gate line electrode and the second auxiliary gate line electrode are formed, the first mask layer and the second mask layer are removed; in this embodiment, the first mask layer is removed after the first auxiliary gate line electrode is formed and the second mask layer is removed after the second auxiliary gate line electrode is formed.
[0067] The step of removing the portion of the seed layer that is not blocked by the auxiliary gate line electrode includes: removing the portion of the first seed layer that is not blocked by the first auxiliary gate line electrode after removing the first mask layer, and / or removing the portion of the second seed layer that is not blocked by the second auxiliary gate line electrode after removing the second mask layer, that is, when only the first seed layer is formed, only the first seed layer on the side of the first auxiliary gate line electrode is removed; when only the second seed layer is formed, only the second seed layer on the side of the second auxiliary gate line electrode is removed; when the first seed layer and the second seed layer are formed, the first seed layer on the side of the first auxiliary gate line electrode and the second seed layer on the side of the second auxiliary gate line electrode are removed; in this embodiment, the first seed layer on the side of the first auxiliary gate line electrode is removed after removing the first mask layer, and the second seed layer on the side of the second auxiliary gate line electrode is removed after removing the second mask layer.
[0068] The step of forming a main gate electrode on at least one side of the semiconductor substrate layer includes: forming a first main gate electrode on the side of the semiconductor substrate layer where the first sub-gate electrode is formed by a screen printing process, and / or forming a second main gate electrode on the side of the semiconductor substrate layer where the second sub-gate electrode is formed by a screen printing process, the first main gate electrode is electrically connected to the first sub-gate electrode, and the second main gate electrode is electrically connected to the second sub-gate electrode; in this embodiment, the first main gate electrode is formed on the side of the semiconductor substrate layer where the first sub-gate electrode is formed by a screen printing process, and the second main gate electrode is formed on the side of the semiconductor substrate layer where the second sub-gate electrode is formed by a screen printing process.
[0069] The step of electroplating the auxiliary grid line electrode on the surface of the seed layer exposed by the mask layer includes: electroplating the bottom auxiliary grid line electrode on the surface of the seed layer exposed by the mask layer; forming a top auxiliary grid line electrode on the surface of the bottom auxiliary grid line electrode away from the semiconductor substrate layer; the melting point of the top auxiliary grid line electrode is lower than the melting point of the bottom auxiliary grid line electrode, and the conductivity of the bottom auxiliary grid line electrode is higher than the conductivity of the top auxiliary grid line electrode. The bottom auxiliary grid line electrode has good conductivity and can conduct current well. The top auxiliary grid line electrode has a low melting point and can be easily welded to the welding strip in the subsequent process of forming the assembly. The top auxiliary grid line electrode plays the role of an adhesive layer between the bottom auxiliary grid line electrode and the welding strip.
[0070] The material of the bottom auxiliary gate electrode includes copper, and the material of the top auxiliary gate electrode includes tin. In this embodiment, the gate electrode replaces the traditional thin silver gate wire and main silver gate wire, and the gate electrode avoids using silver, a high-cost material, thereby reducing the cost of the electrode.
[0071] The thickness of the bottom auxiliary gate electrode is 3μm to 15μm, for example, 3μm, 5μm, 7μm, 9μm, 11μm, 13μm or 15μm; if the bottom auxiliary gate electrode is too thin, the conductivity of the auxiliary gate electrode will be weak; if the bottom auxiliary gate electrode is too thick, the unnecessary cost of the auxiliary gate electrode will be increased; the thickness of the top auxiliary gate electrode is 0.3μm to 3μm, for example, 0.3μm, 1μm, 1.5μm, 2μm, 2.5μm or 3μm; if the top auxiliary gate electrode is too thin, the bonding effect between the bottom auxiliary gate electrode and the welding strip will be poor; if the top auxiliary gate electrode is too thick, the unnecessary cost of the auxiliary gate electrode will be increased.
[0072] The electrode preparation method further includes: after removing the mask layer, forming a conductive protection layer on the side wall surface of the bottom auxiliary gate electrode. The conductive protection layer can prevent the bottom auxiliary gate electrode from being oxidized, thereby improving the reliability of the auxiliary gate electrode.
[0073] In the present embodiment, the material of the bottom gate electrode is copper, the material of the top gate electrode is tin, and the process for forming the conductive protective layer includes a chemical plating process. The side wall of the bottom gate electrode is subjected to an oxidation-reduction reaction by the chemical plating process. In the present embodiment, since the material of the conductive protective layer is tin, the oxidation-reduction reaction only occurs on the side wall of the bottom gate electrode, and the top gate electrode does not participate in the oxidation-reduction reaction, and therefore, only the side wall surface of the bottom gate electrode is formed with a conductive protective layer. In other words, the conductive protective layer can be realized by chemical electroplating, and the essence is to replace the exposed copper (the auxiliary gate electrode of the bottom layer) with tin (the conductive protective layer) by an oxidation-reduction reaction, and the conductive protective layer formed by the chemical plating process is relatively uniform.
[0074] The material of the conductive protection layer is the same as that of the top-layer secondary gate line electrode. Preferably, the material of the conductive protection layer includes tin.
[0075] The thickness of the conductive protection layer is 0.5 μm to 2 μm, for example, 0.5 μm, 1 μm, 1.5 μm or 2 μm.
[0076] After the conductive protective layer is formed, the conductive protective layer is heated so that the conductive protective layer flows in a molten state, and the conductive protective layer forms a conductive covering layer covering the side wall surface and the top surface of the gate electrode, so that the conductive covering layer covers the surface of the gate electrode uniformly and has a good morphology.
[0077] After removing the portion of the seed layer not blocked by the auxiliary gate electrode, the conductive protective layer is formed; or, after forming the conductive protective layer, the portion of the seed layer not blocked by the auxiliary gate electrode is removed. Preferably, after removing the portion of the seed layer not blocked by the gate electrode, the conductive protective layer is formed.
[0078] In this embodiment, the conductive protective layer is formed after the seed layer on the side of the secondary grid line electrode is removed; the conductive protective layer is thin and hardly occupies the space of the transparent conductive film between adjacent secondary grid line electrodes, thereby reducing the shielding of sunlight. Since the conductive protective layer is formed after the seed layer on the side of the secondary grid line electrode is removed, it is possible to prevent the conductive protective layer from being etched and damaged during the process of removing the seed layer, thereby improving the reliability of the secondary grid line electrode.
[0079] The ratio of the thickness of the mask layer to the thickness of the bottom auxiliary gate electrode is 1:0.95 to 1:1.05, for example, 1:0.95, 1:1 or 1:1.05. The thickness of the mask layer is substantially consistent with the thickness of the bottom auxiliary gate electrode, thereby avoiding the poor morphology of the auxiliary gate electrode caused by the low thickness of the mask layer and the waste of mask layer material caused by the high thickness of the mask layer.
[0080] The present invention provides a method for preparing an electrode, wherein the main grid electrode is formed by a screen printing process, and the main grid electrode has a certain width that can provide a larger pad point, provide a better welding tension, and is conducive to component interconnection. The width of the secondary grid electrode formed by the electroplating process is narrower than that of the secondary grid electrode formed by the screen printing process, so that the secondary grid electrode blocks less sunlight. The secondary grid electrode is formed by the electroplating process, which is more conducive to forming a secondary grid electrode that does not contain silver, and can reduce the cost of the electrode.
[0081] The following is a detailed description of the preparation of electrodes in solar cells as an example. It should be noted that in other embodiments, the preparation method of electrodes can also be applied to the preparation process of other semiconductor structures such as solar cells that need to include gate line electrodes.
[0082] The method for preparing a solar cell further includes: forming a transparent conductive film on at least one side of the semiconductor substrate layer. The step of forming a transparent conductive film on at least one side of the semiconductor substrate layer includes: forming a first transparent conductive film on one side of the semiconductor substrate layer, and / or forming a second transparent conductive film on the other side of the semiconductor substrate layer; in this embodiment, the first transparent conductive film is formed on one side of the semiconductor substrate layer and the second transparent conductive film is formed on the other side of the semiconductor substrate layer.
[0083] The auxiliary grid line electrode is indirectly connected to the transparent conductive film through the seed layer, so the auxiliary grid line electrode and the transparent conductive film have good bonding force, which prevents the auxiliary grid line electrode from being separated from the transparent conductive film.
[0084] The step of forming the auxiliary gate line electrode on at least one side of the semiconductor substrate layer by using the electroplating process is: forming the auxiliary gate line electrode on a side of a portion of the transparent conductive film away from the semiconductor substrate layer by using the electroplating process.
[0085] The step of forming a main gate electrode on the side of the semiconductor substrate layer where the auxiliary gate electrode is formed by using a screen printing process includes: forming a main gate electrode on a side of a portion of the transparent conductive film away from the semiconductor substrate layer by using a screen printing process.
[0086] The method for preparing a solar cell also includes: forming a first intrinsic semiconductor layer on one side surface of the semiconductor substrate layer; forming a first conductive type semiconductor layer on the side surface of the first intrinsic semiconductor layer facing away from the semiconductor substrate layer; forming a second intrinsic semiconductor layer on the side surface of the semiconductor substrate layer facing away from the first intrinsic semiconductor layer; forming a second conductive type semiconductor layer on the side surface of the second intrinsic semiconductor layer facing away from the semiconductor substrate layer; the conductivity type of the second conductive type semiconductor layer is opposite to that of the first conductive type semiconductor layer; forming a first transparent conductive film on the side surface of the first conductive type semiconductor layer facing away from the semiconductor substrate layer; and forming a second transparent conductive film on the side surface of the second conductive type semiconductor layer facing away from the semiconductor substrate layer.
[0087] After the secondary grid line electrode and the main grid line electrode are formed, the solar cell is cured at a low temperature, and then the photoelectric performance of the solar cell is tested.
[0088] Please refer to Figures 2 to 10 , below, a heterojunction solar cell is taken as an example of a solar cell to illustrate the structural schematic diagram of the preparation process of the solar cell provided in this embodiment.
[0089] Please refer to Figure 2 , providing a semiconductor substrate layer 1.
[0090] After the semiconductor substrate layer 1 is subjected to a texturing and cleaning treatment, a first intrinsic semiconductor layer 2 and a second intrinsic semiconductor layer 3 are deposited on both sides of the semiconductor substrate layer 1; a first conductive type semiconductor layer 4 is formed on the side of the first intrinsic semiconductor layer 2 facing away from the semiconductor substrate layer 1; a second conductive type semiconductor layer 5 is formed on the side of the second intrinsic semiconductor layer 3 facing away from the semiconductor substrate layer 1; a first transparent conductive film 6 is formed on the side of the first conductive type semiconductor layer 4 facing away from the semiconductor substrate layer 1; and a second transparent conductive film 7 is formed on the side of the second conductive type semiconductor layer 5 facing away from the semiconductor substrate layer 1.
[0091] Please refer to Figure 3 A first seed layer 8 is formed on a surface of the first transparent conductive film 6 facing away from the semiconductor substrate layer 1 , and a second seed layer 9 is formed on a surface of the second transparent conductive film 7 facing away from the semiconductor substrate layer 1 .
[0092] Please refer to Figure 4 A first mask layer 10 is formed on a surface of a portion of the first seed layer 8 that is away from the first transparent conductive film 6 by an inkjet printing process, and a second mask layer 11 is formed on a surface of a portion of the second seed layer 9 that is away from the second transparent conductive film 7 by an inkjet printing process.
[0093] Please refer to Figure 5 A first bottom auxiliary gate line electrode 12 is formed on the surface of the first seed layer 8 exposed by the first mask layer 10 through an electroplating process, and a second bottom auxiliary gate line electrode 13 is formed on the surface of the second seed layer 9 exposed by the second mask layer 11.
[0094] Please refer to Figure 6 A first top auxiliary gate electrode 14 is formed on the surface of the first bottom auxiliary gate electrode 12 away from the first seed layer 8 and a second top auxiliary gate electrode 15 is formed on the surface of the second bottom auxiliary gate electrode 13 away from the second seed layer 9 by electroplating.
[0095] Please refer to Figure 7 , remove the first mask layer 10 and the second mask layer 11. After removing the first mask layer 10 and the second mask layer 11, remove the first seed layer 8 on the side of the first bottom auxiliary gate line electrode 12, and remove the second seed layer 9 on the side of the second bottom auxiliary gate line electrode 13.
[0096] Please refer to Figure 8 A first conductive protective layer 16 is formed on the side wall surface of the first bottom auxiliary gate line electrode 12 by a chemical plating process, and the material of the first conductive protective layer 16 includes tin. A second conductive protective layer 17 is formed on the side wall surface of the second bottom auxiliary gate line electrode 13 by a chemical plating process, and the material of the second conductive protective layer 17 includes tin.
[0097] Please refer to Fig. 9 , heating the first conductive protection layer 16 and the second conductive protection layer 17, so that the first conductive protection layer 16 forms a first conductive covering layer 16b covering the entire surface of the first gate line electrode, and the second conductive protection layer 17 forms a second conductive covering layer 17b covering the entire surface of the second gate line electrode. The first conductive covering layer 16b covers the side wall surface and the top surface of the first gate line electrode, and the second conductive covering layer 17b covers the side wall surface and the top surface of the second gate line electrode.
[0098] It should be noted that, in other embodiments, it may be preferred that: after removing the first mask layer 10 and the second mask layer 11, and before removing the first seed layer 8 and the second seed layer 9, a first conductive protective layer is formed on the side wall surface of the first bottom gate electrode 12, the first conductive protective layer can prevent the first bottom auxiliary gate electrode 12 from being oxidized, and improve the reliability of the first bottom auxiliary gate electrode 12, and a second conductive protective layer is formed on the side wall surface of the second bottom gate electrode 13, the second conductive protective layer can prevent the second bottom auxiliary gate electrode 13 from being oxidized, and improve the reliability of the second bottom auxiliary gate electrode 13. In this case, when heating the first conductive protective layer and the second conductive protective layer, the step of heating the first conductive protective layer and the second conductive protective layer is set before removing the first seed layer 8 and the second seed layer 9 or after removing the first seed layer 8 and the second seed layer 9.
[0099] Please refer to Fig.10 , Fig.10 In order to illustrate the relative position relationship between the main grid line electrode and the auxiliary grid line electrode, a top view schematic diagram of a solar cell is given; through the screen printing process, a first main grid line electrode 18 is formed on the partial surface of the first transparent conductive film 6 away from the semiconductor substrate layer 1, and the first main grid line electrode 18 is connected to the first conductive covering layer 16b; a second main grid line electrode (not shown in the figure) is formed on the partial surface of the second transparent conductive film 7 away from the semiconductor substrate layer 1, and the second main grid line electrode is connected to the second conductive covering layer 17b.
[0100] It should be noted that, in other embodiments, the first conductive protective layer and the second conductive protective layer may not be heated. In this case, the first main grid electrode is connected to the first top-layer sub-grid electrode; the second main grid electrode is connected to the second top-layer sub-grid electrode. In other embodiments, the first main grid electrode may be formed by a screen printing process first, and then the second sub-grid electrode may be formed by an electroplating process.
[0101] Please refer to Figures 11 to 19 , the structural schematic diagram of the preparation process of a solar cell provided by another embodiment is described below. The difference between this embodiment and the previous embodiment is that: in the preparation process of the solar cell, only one side of the electrode in the solar cell is prepared using the preparation method of the electrode of the present invention.
[0102] Please refer to Fig.11 , providing a semiconductor substrate layer 1a.
[0103] After the semiconductor substrate layer 1a is subjected to a texturing and cleaning treatment, a first intrinsic semiconductor layer 2a and a second intrinsic semiconductor layer 3a are deposited on both sides of the semiconductor substrate layer 1a; a first conductive type semiconductor layer 4a is formed on the side of the first intrinsic semiconductor layer 2a away from the semiconductor substrate layer 1a; a second conductive type semiconductor layer 5a is formed on the side of the second intrinsic semiconductor layer 3a away from the semiconductor substrate layer 1a; a first transparent conductive film 6a is formed on the side of the first conductive type semiconductor layer 4a away from the semiconductor substrate layer 1a; and a second transparent conductive film 7a is formed on the side of the second conductive type semiconductor layer 5a away from the semiconductor substrate layer 1a. The first conductive type semiconductor layer 4a is a P-type doped semiconductor layer, and the second conductive type semiconductor layer 5a is an N-type doped semiconductor layer.
[0104] Please refer to Fig.12 A first seed layer 8a is formed on the surface of the first transparent conductive film 6a facing away from the semiconductor substrate layer 1a.
[0105] Please refer to Fig.13 A first mask layer 10a is formed on a surface of a portion of the first seed layer 8a that is away from the first transparent conductive film 6a by an inkjet printing process.
[0106] Please refer to Fig.14 A first bottom layer sub-gate line electrode 12a is formed on the surface of the first seed layer 8a exposed by the first mask layer 10a through an electroplating process.
[0107] Please refer to Fig.15 A first top-layer auxiliary gate electrode 14a is formed on the surface of the first bottom-layer auxiliary gate electrode 12a away from the first seed layer 8a by an electroplating process.
[0108] Please refer to Fig.16 , remove the first mask layer 10a, and after removing the first mask layer 10a, remove the first seed layer 8a on the side of the first bottom layer sub-gate line electrode 12a.
[0109] Please refer to Fig.17 , forming a first conductive protective layer 16a on the side wall surface of the first bottom auxiliary gate electrode 12a; forming a second auxiliary gate electrode 18a and a second main gate electrode (not shown in the figure) on the side surface of a portion of the second transparent conductive film 7a away from the second conductive type semiconductor layer 5a by screen printing. In this case, the second main gate electrode and the second auxiliary gate electrode 18a are formed simultaneously by screen printing. In other embodiments, the second auxiliary gate electrode 18a and the second main gate electrode can be formed before forming the first auxiliary gate electrode and the first main gate electrode.
[0110] Please refer to Fig.18The first conductive protective layer 16a is heated to form a first conductive covering layer 16c covering the entire surface of the first gate line electrode. The first conductive covering layer 16c covers the side wall surface and the top surface of the first gate line electrode.
[0111] It should be noted that in other embodiments, the first conductive protection layer 16 a may not be heated.
[0112] It should be noted that, in other embodiments, the first conductive protective layer may be formed on the sidewall surface of the first bottom gate electrode 12a after removing the first mask layer 10a and before removing the first seed layer 8. In this case, when the first conductive protective layer is heated, the step of heating the first conductive protective layer is arranged before removing the first seed layer 8a or after removing the first seed layer 8a.
[0113] Please refer to Fig.19 , Fig.19 In order to illustrate the relative position relationship between the main grid line electrode and the auxiliary grid line electrode, a top view schematic diagram of a solar cell is given; through the screen printing process, a first main grid line electrode 19a is formed on the surface of the first transparent conductive film 6a away from the semiconductor substrate layer 1a.
[0114] In other embodiments, the first main gate line electrode may be formed by a screen printing process first, and then the first sub-gate line electrode may be formed by an electroplating process.
[0115] In another embodiment, the first conductive type semiconductor layer is a P-type doped semiconductor layer, the second conductive type semiconductor layer is an N-type doped semiconductor layer, a second seed layer is formed on the surface of the second transparent conductive film away from the semiconductor substrate layer, and a second mask layer is formed on the surface of a portion of the second seed layer away from the second transparent conductive film by an inkjet printing process. A second bottom auxiliary gate line electrode is formed on the surface of the second mask layer exposing the second seed layer by an electroplating process; a second top auxiliary gate line electrode is formed on the surface of the second auxiliary bottom gate line electrode away from the second seed layer by an electroplating process; then, the second mask layer is removed; after removing the second mask layer, the second seed layer on the side of the second bottom auxiliary gate line electrode is removed; and a first auxiliary gate line electrode is formed on the surface of a portion of the first transparent conductive film away from the first conductive type semiconductor layer by a screen printing process. Further, it can also include: forming a second conductive protective layer on the side wall surface of the second bottom auxiliary gate line electrode; heating the second conductive protective layer so that the second conductive protective layer forms a second conductive covering layer covering the entire surface of the second gate line electrode. The second conductive covering layer covers the side wall surface and the top surface of the second gate line electrode. It should be noted that, in other embodiments, the second conductive protective layer may not be heated. It should be noted that, in other embodiments, the second conductive protective layer may be formed on the sidewall surface of the second bottom layer secondary gate line electrode after removing the second mask layer and before removing the second seed layer. In this case, when the second conductive protective layer is heated, the step of heating the second conductive protective layer is set before removing the second seed layer or after removing the second seed layer.
[0116] In the method for preparing a solar cell provided in this embodiment, the main grid electrode is formed by a screen printing process, and the main grid electrode has a certain width, which can provide a larger pad point for the solar cell, provide better welding tension, and is conducive to the interconnection of the components of the solar cell. The secondary grid electrode is formed by an electroplating process, which is more conducive to forming a secondary grid electrode that does not contain silver, which can reduce the cost of the solar cell, and the width of the secondary grid electrode formed by the electroplating process is narrower than that of the secondary grid electrode formed by the screen printing process, so that the secondary grid electrode blocks less sunlight, which is conducive to improving the efficiency of the battery.
[0117] The following is a comparison table of the test results of solar cells prepared by different methods. In the table, "Isc" represents short-circuit current, "Voc" represents open-circuit voltage, "FF" represents fill factor, "Eta" represents conversion efficiency, and "Irev2" represents leakage current.
[0118]
[0119] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing an electrode, comprising: A semiconductor substrate layer is provided, characterized in that it also includes: forming a mask layer on at least one side of the semiconductor substrate layer; Performing an electroplating process using the mask layer as a mask to form a secondary gate electrode on at least one side of the semiconductor substrate layer, wherein the pattern of the mask layer corresponds to an area where the secondary gate electrode does not need to be formed; Forming a main gate electrode on the side of the semiconductor substrate layer where the auxiliary gate electrode is formed by a screen printing process, wherein the main gate electrode is electrically connected to the auxiliary gate electrode; The step of performing an electroplating process using the mask layer as a mask to form a secondary gate line electrode on at least one side of the semiconductor substrate layer includes: Using the mask layer as a mask, electroplating the bottom sub-grid electrode using an electroplating process; Using an electroplating process to form a top-layer auxiliary gate line electrode on a side of the bottom-layer auxiliary gate line electrode away from the semiconductor substrate layer, wherein the material of the top-layer auxiliary gate line electrode is different from that of the bottom-layer auxiliary gate line electrode; removing the mask layer; Forming a conductive protective layer on the sidewall surface of the bottom auxiliary gate electrode by using a chemical plating process, wherein the material of the conductive protective layer is the same as that of the top auxiliary gate electrode; After the conductive protection layer is formed, the conductive protection layer is heated to make the conductive protection layer form a conductive covering layer covering the side wall surface and the top surface of the secondary gate line electrode.
2. The method for preparing an electrode according to claim 1, characterized in that: The auxiliary gate line electrode and the pattern of the mask layer are complementary to each other on one side of the semiconductor substrate layer.
3. The method for preparing an electrode according to claim 2, characterized in that: The process of forming the mask layer includes an inkjet printing process.
4. The method for preparing an electrode according to claim 2, characterized in that: The material of the mask layer includes paraffin.
5. The method for preparing an electrode according to claim 2, characterized in that: The material of the main grid line electrode includes silver alloy.
6. The method for preparing an electrode according to claim 2, characterized in that: The process of removing the mask layer includes a thermal treatment process or a chemical stripping process.
7. The method for preparing an electrode according to claim 6, characterized in that: The temperature of the heat treatment process is 50°C to 150°C.
8. The method for preparing an electrode according to claim 2, characterized in that: When a chemical stripping process is used to remove the mask layer, the stripping solution used to remove the mask layer includes a sodium hydroxide solution or a potassium hydroxide solution.
9. The method for preparing an electrode according to claim 2, characterized in that: Also includes: Before forming the mask layer, forming a seed layer on the entire surface of at least one side of the semiconductor substrate layer; The step of forming the mask layer is: forming the mask layer on the side of the seed layer away from the semiconductor substrate layer by using a film forming process; The step of forming the auxiliary gate line electrode is: electroplating the auxiliary gate line electrode on the surface of the seed layer exposed by the mask layer; The electrode preparation method further comprises: after removing the mask layer and before forming the main gate line electrode, removing the portion of the seed layer that is not blocked by the auxiliary gate line electrode.
10. The method for preparing an electrode according to claim 9, characterized in that: The step of forming the seed layer includes: forming a first seed layer on the entire surface of one side of the semiconductor substrate layer, and / or forming a second seed layer on the entire surface of the other side of the semiconductor substrate layer; Accordingly, the step of forming a mask layer includes: forming a first mask layer on a surface of a portion of the first seed layer that is not required to form the auxiliary gate line electrode and that is away from the semiconductor substrate layer, and / or forming a second mask layer on a surface of a portion of the second seed layer that is not required to form the auxiliary gate line electrode and that is away from the semiconductor substrate layer; The step of electroplating the auxiliary gate line electrode on the surface of the seed layer exposed by the mask layer comprises: electroplating the first auxiliary gate line electrode on the surface of the first seed layer exposed by the first mask layer, and / or electroplating the second auxiliary gate line electrode on the surface of the second seed layer exposed by the second mask layer; The step of removing the mask layer comprises: removing the first mask layer after forming the first auxiliary gate line electrode, and / or removing the second mask layer after forming the second auxiliary gate line electrode; The step of removing the portion of the seed layer not blocked by the auxiliary gate line electrode comprises: removing the portion of the first seed layer not blocked by the first auxiliary gate line electrode after removing the first mask layer, and / or removing the portion of the second seed layer not blocked by the second auxiliary gate line electrode after removing the second mask layer; The step of forming a main gate line electrode includes: forming a first main gate line electrode on a side of the semiconductor substrate layer where the first sub-gate line electrode is formed by a screen printing process, and / or forming a second main gate line electrode on a side of the semiconductor substrate layer where the second sub-gate line electrode is formed by a screen printing process, the first main gate line electrode is electrically connected to the first sub-gate line electrode, and the second main gate line electrode is electrically connected to the second sub-gate line electrode.
11. The method for preparing an electrode according to claim 9, characterized in that: The process of forming the seed layer includes an electroplating process.
12. The method for preparing an electrode according to claim 11, characterized in that: The material of the seed layer includes copper or nickel.
13. The method for preparing an electrode according to claim 11, characterized in that: The thickness of the seed layer is 50nm-150nm.
14. The method for preparing an electrode according to claim 11, characterized in that: The process of removing the portion of the seed layer not blocked by the secondary gate line electrode comprises a chemical stripping process.
15. The method for preparing an electrode according to claim 14, characterized in that: The stripping solution in the chemical stripping process used to remove the portion of the seed layer not blocked by the secondary gate line electrode includes a sodium hydroxide solution or a potassium hydroxide solution.
16. The method for preparing an electrode according to claim 14, characterized in that: The chemical stripping process includes a spray process.
17. The method for preparing an electrode according to claim 9, characterized in that: The step of electroplating a secondary gate line electrode on the surface of the seed layer exposed by the mask layer comprises: Electroplating a bottom sub-grid electrode on the surface of the seed layer exposed by the mask layer; Forming a top auxiliary gate line electrode on a side surface of the bottom auxiliary gate line electrode away from the semiconductor substrate layer; The melting point of the top-layer auxiliary gate line electrode is lower than that of the bottom-layer auxiliary gate line electrode, and the conductivity of the bottom-layer auxiliary gate line electrode is higher than that of the top-layer auxiliary gate line electrode.
18. The method for preparing an electrode according to claim 17, characterized in that: The material of the bottom auxiliary gate line electrode includes copper, and the material of the top auxiliary gate line electrode includes tin.
19. The method for preparing an electrode according to claim 17, characterized in that: The thickness of the bottom auxiliary grid line electrode is 3 μm to 15 μm; the thickness of the top auxiliary grid line electrode is 0.3 μm to 3 μm.
20. The method for preparing an electrode according to claim 1, characterized in that: The material of the conductive protection layer includes tin.
21. The method for preparing an electrode according to claim 1, characterized in that: The thickness of the conductive protection layer is 0.5 μm to 2 μm.
22. The method for preparing an electrode according to claim 17, characterized in that: After removing the portion of the seed layer not blocked by the secondary gate electrode, the conductive protection layer is formed; or after forming the conductive protection layer, the portion of the seed layer not blocked by the secondary gate electrode is removed.
23. The method for preparing an electrode according to claim 17, characterized in that: The ratio of the thickness of the mask layer to the thickness of the bottom auxiliary gate line electrode is 1:0.95 to 1:1.
05.
24. A method for preparing a solar cell, characterized in that: include: providing a semiconductor substrate layer; forming a transparent conductive film on at least one side of the semiconductor substrate layer; Also included: a method for preparing the electrode according to any one of claims 1 to 23; wherein: the step of forming a secondary gate electrode on at least one side of the semiconductor substrate layer by using an electroplating process is: forming a secondary gate electrode on a side of a portion of the transparent conductive film away from the semiconductor substrate layer by using an electroplating process; The step of forming a main grid electrode on at least one side of the semiconductor substrate layer by using a screen printing process includes: forming a main grid electrode on a side of a portion of the transparent conductive film away from the semiconductor substrate layer by using a screen printing process.
Citation Information
Patent Citations
Method for forming positive electrode of solar cell
CN102479883A
Efficient solar cell manufacturing method
CN102769070A
Silicon heterojunction solar cell with electroplating electrode and manufacturing method thereof
CN104538495A
Silicon heterojunction solar cell and preparation method thereof
CN109148616A
Solar cell, preparation method thereof and photovoltaic module
CN112993064A