Method of making an electrode comprising a polymer matrix entrapping an electrolyte
By using a twin-screw mixer to manufacture a polymer matrix electrode with high dynamic viscosity at low temperature, the electrolyte is captured to form an ion gel electrode, which solves the problems of liquid electrolyte leakage and low solid electrolyte conductivity, achieving higher electrochemical performance and Lower production costs.
Patent Information
- Application Number
- CN202080065408.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-17
- Filing Date
- 2020-09-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-09-16
AI Technical Summary
The liquid electrolyte in existing electrochemical batteries is prone to leakage, and the solid electrolyte has low ionic conductivity at ambient temperature, resulting in limited performance of lithium-ion batteries. Traditional methods use a large amount of solvents, which increases production costs and safety risks.
A specialized twin-screw mixer is used to manufacture paste compositions at temperatures below 100°C. The electrode ingredients are mixed by co-rotating interpenetrating screws rotating in a closed sleeve, reducing solvent use and forming a high dynamic viscosity polymer. Matrix electrode, which captures electrolyte to form an ion gel electrode.
It significantly reduces the amount of solvent used, increases the solid mass percentage of the electrode, reduces production costs and safety risks, while maintaining the electrochemical performance of lithium-ion batteries at ambient temperature and increasing the energy density of the electrode.
Smart Images

Figure BDA0003551619060000081 
Figure BDA0003551619060000091 
Figure BDA0003551619060000101
Abstract
Description
[0001] describe Technical Field
[0002] The present invention relates to a method for manufacturing an electrode comprising a polymer matrix entrapping an electrolyte, more particularly a liquid electrolyte capable of forming a gel with the polymer matrix (in this case the electrode may be referred to as an ion gel electrode), providing the electrode for incorporation in an electrochemical storage cell.
[0003] The general field of the invention can be defined as the field of energy storage devices, in particular the field of electrochemical accumulators. Prior art
[0004] The operating principle of electrochemical accumulators is that of an electrochemical cell suitable for conveying an electric current, since in each of them there is a pair of electrodes (respectively a positive electrode and a negative electrode) separated by an electrolyte, the electrodes comprising specific materials suitable for reacting according to redox reactions, whereby there is an exchange of electrons at the origin of the electric current, and an exchange of ions transmitted from one electrode to the other through the medium of the electrolyte.
[0005] Among batteries that adopt this principle, batteries that work on the principle of metal element insertion / deintercalation at the electrode (more specifically, on the electrode active material) and are called metal ion batteries (e.g., Li ions, Na ions, K ions, Ca ions, Mg ions or Al ions) have replaced other types of batteries, such as lead-acid batteries and Ni-MH batteries, especially their performance in terms of energy density. In fact, metal ion batteries, such as Li ion batteries, in particular, are able to obtain significantly greater than Ni-MH and Ni-Cd batteries (ranging from 50 to 100 Wh.kg -1 ) and lead-acid batteries (range can be 30 to 35Wh.kg -1 ) Higher weight energy density and volume energy density (greater than 180Wh.kg -1 ).
[0006] From a functional point of view, in a metal ion battery, the reaction at the origin of the generation of the electric current (i.e. when the battery is in discharge mode) involves the transport of metal cations from the negative electrode through an electrolyte that conducts metal ions, which are embedded in a network of acceptors at the positive electrode, while the electrons from the reaction at the negative electrode will supply an external circuit to which the positive and negative electrodes are connected.
[0007] More specifically, in the case of a Li-ion battery, the positive electrode may include a lithium-based phosphate material (e.g., LiFePO 4 ), optionally substituted lithiated manganese oxides (e.g. LiMn 2 O 4), LiNi based materials with x+y+z=1 x Mn y Co z O 2 (also referred to as NMC) as lithium intercalation materials, such as LiNi 0.33 Mn 0.33 Co 0.33 O 2 or LiNi 0.6 Mn 0.2 Co 0.2 O 2 , with x+y+z=1 LiNi x Co y Al z O 2 (also referred to as NCA), such as LiNi 0.8 Co 0.15 Al 0.05 O 2 .
[0008] As lithium intercalation materials, the negative electrode may include carbon-containing materials, such as graphite; silicon-based compounds, such as silicon carbide SiC or silicon oxide SiO x ; Lithiated titanium oxides, such as Li 4 Ti 5 O 12 ; lithium-germanium alloy; or a mixture of several of these lithium intercalation materials, such as a mixture including graphite and a silicon-based compound.
[0009] As mentioned above, an electrolyte is disposed between the negative electrode and the positive electrode, which allows ions (usually from a metal salt present in the electrolyte) to move from the positive electrode to the negative electrode during charging, and vice versa during discharging.
[0010] The electrolyte may be in liquid form and typically comprises one or more organic solvents (eg a mixture of carbonate solvents) in which one or more metal salts (eg one or more lithium salts when the battery is a lithium ion battery) are dissolved.
[0011] However, the use of liquid electrolytes has several disadvantages:
[0012] Problems with electrolyte leakage from batteries;
[0013] When thermal runaway occurs in a battery containing this electrolyte, there is a possibility that the liquid electrolyte chemically reacts with oxygen in the positive electrode active material, thereby possibly generating a large amount of gas, the result of which may be that the battery catches fire, or even explodes.
[0014] To overcome these drawbacks, an alternative approach consists in abandoning the use of liquid electrolytes by replacing them, for example, using the following solutions:
[0015] Lithium ion conductors in pure solid form, such as glass or ceramic, thin layers deposited by chemical vapor deposition (CVD), such as LIPON layers, or composite layers including a polymer matrix (such as polyvinylidene fluoride), and layers composed of lithiated oxides such as Li 7 La 3 Zr 2 O 12 Filling material of composition;
[0016] A dry polymer solid electrolyte composed of a polyoxyethylene (POE)-based polymer and a lithium salt, such as lithium bis(trifluorosulfonyl)imide (LiTFSI).
[0017] However, these various current solutions all have a certain number of disadvantages.
[0018] With regard to the use of glass or ceramic lithium-ion conductors, these require very complex implementation or synthesis techniques to be developed in an industrial setting, which may prove disadvantageous for the large-scale production of batteries.
[0019] Regarding solid dry polymer electrolytes, their ionic conductivity is typically less than 10 -5 S.cm -1 , while for conventional liquid electrolytes, the ionic conductivity is about 10 -3 S.cm -1 , even at ambient temperature of 10 -2 S.cm -1 It may therefore prove necessary to use a battery comprising a dry polymer electrolyte at temperatures higher than ambient temperature, for example at temperatures between 60 and 80° C., in order to promote the diffusion of lithium ions in the electrolyte.
[0020] In order to alleviate the disadvantages associated with the use of liquid electrolytes and the above-mentioned solid electrolytes, the new technology developed and explained in WO2015169835 includes capturing the liquid electrolyte in a polymer matrix to form an integral part of the positive electrode and the negative electrode (these electrodes can be called ion gel electrodes), which technology makes it possible to obtain electrochemical performance equivalent to that of a lithium-ion battery at ambient temperature, which lithium-ion battery includes a liquid electrolyte that is not captured in a polymer matrix.
[0021] These electrodes are manufactured in a conventional manner by a process comprising the following steps in sequence:
[0022] a step of making an ink (i.e. a liquid dispersion comprising suspended solid components of the electrode) by mixing the various components provided for the formation of the electrode, these components being the active material, an electron conductor additive or additives, a fluorinated (co)polymer capable of capturing a liquid electrolyte, at least one solvent for the fluorinated copolymer (e.g. acetone), a lithium salt, one or more electrolyte solvents (e.g. carbonate solvents) for dissolving the lithium salt;
[0023] Once the ink is obtained, a step of depositing it, generally by dispersing it on a substrate forming a current collector;
[0024] A step of evaporating the solvent or solvents of the fluorinated (co)polymer is optionally followed by a calendering step, wherein specific electrodes are present.
[0025] The ink manufacturing steps usually carried out in conventional mixers (such as dispersers or planetary mixers) require a high proportion of solvents, which limits the percentage of solid mass in the ink. More specifically, the percentage of solid mass relative to the total mass of the ink is usually between 35 and 49 mass%, while the mass of the liquid electrolyte (salt + electrolyte solvent) accounts for 6% to 13% of the total mass of the ink, and one or more solvents for the fluorinated (co)polymers account for 45% to 57% of the total mass of the ink.
[0026] The presence of such amounts of solvent constitutes a limiting factor for the implementation of such a process, in particular on an industrial scale, since it implies management of the effluent (here the solvent used in large quantities) both in terms of safety (in particular due to the potential flammability of the chosen solvent or solvents and / or the toxicity of the chosen solvent or solvents) and elimination of the solvent, and, moreover, such a process entails high implementation costs.
[0027] In this context, the inventors have aimed to provide a new method for manufacturing electrodes comprising a polymer matrix doped with an electrolyte, which makes it possible to limit or possibly eliminate the use of large amounts of solvents and, therefore, is cheaper and limits the disadvantages associated with the use of large amounts of solvents. Summary of the invention
[0028] To this end, the inventors have developed a method for manufacturing electrodes that no longer involves pre-manufacturing inks, but rather pre-manufacturing a paste composition that includes ingredients for entering into the composition of the electrode, and this preparation can be carried out by using a specific mixer in this step.
[0029] More specifically, according to the present invention, a method for manufacturing an electrode comprising a polymer matrix, said polymer matrix capturing an electrolyte, said method comprising the following steps:
[0030] a) the step of making a composition comprising ingredients for incorporation into an electrode;
[0031] b) forming an electrode on a substrate from the composition;
[0032] Features include:
[0033] The composition prepared in step a) is a paste-like composition which has a -1 The dynamic viscosity measured at the shear rate and ambient temperature is greater than 5000 Pa.s; and
[0034] The manufacturing step comprises introducing and mixing the ingredients provided for entering the electrode into a mixer having two co-rotating interpenetrating screws rotating in a closed sleeve, the manufacturing step being carried out at a temperature below 100°C.
[0035] Due to the use of this specific mixer, smaller amounts of solvent can be used compared to processes using conventional mixers, thus limiting the disadvantages associated with wastewater management.
[0036] First, the method of the present invention includes the step of manufacturing a paste composition including components constituting an electrode by introducing and mixing the components into a mixer having two co-rotating interpenetrating screws rotating in a closed sleeve.
[0037] The introduction of the ingredients may be simultaneous or sequential and may be carried out at different locations (e.g., introduction of solid ingredients at a first introduction zone through one or more inlets of the mixer and introduction of liquid ingredients at a second introduction zone through one or more inlets of the mixer), as described herein. Figure 3 The mixer case shown comprises:
[0038] a closed sleeve 1;
[0039] Two interpenetrating screws 3 and 5;
[0040] A first component is introduced into region 7 (designated region A);
[0041] a second component is introduced into region 9 (designated region B), and;
[0042] an outlet 11 for discharging the formed composition;
[0043] A motor 13 is connected to the screws to produce their rotation.
[0044] More specifically, the composition may include, as components constituting the electrode:
[0045] at least one electrode active material;
[0046] at least one polymer providing a formation for entry into said polymer matrix;
[0047] Electrolyte;
[0048] Optionally, at least one electronically conductive additive.
[0049] The electroactive material is a material suitable for intercalating and deintercalating metal ions in its structure, such as alkali ions (e.g., lithium ions when the battery is a lithium battery, sodium ions when the battery is a sodium-containing battery, potassium ions when the battery is a potassium battery), alkaline earth ions (e.g., magnesium ions when the battery is a magnesium battery, calcium ions when the battery is a calcium battery), metal ions (e.g., aluminum ions when the battery is an aluminum ion battery).
[0050] The nature of the active material of course depends on its purpose, i.e., whether it is for the positive electrode or the negative electrode.
[0051] Furthermore, when the method of the present invention is used to manufacture a positive electrode, as examples of the electroactive material that can be incorporated into the positive electrode of a lithium battery, there may be mentioned:
[0052] Metal chalcogenides of the formula LiMQ2, where M is at least one metal element selected from metallic elements such as Co, Ni, Fe, Mn, Cr, V, Al, and Q is a chalcogen element, such as O or S, and the preferred metal chalcogenides are those of the formula LiMO 2 where M is defined as above, for example preferably LiCoO 2 、LiNiO 2 、LiNi x Co 1-x O 2 (0 < x < 1), lithium-nickel-manganese-cobalt-based materials LiNi x Mn y Co z O 2 , (also known as the abbreviation NMC), for example LiNi 0.33 Mn 0.33 Co 0.33 O 2 , or lithium-nickel-cobalt-aluminum-based materials LiNi x Co y Al z O 2 (also known as the abbreviation NCA), such as LiNi 0,8 Co 0.15 Al 0.05 O 2 ;
[0053] Chalcogenides with a spinel structure, such as LiMn 2 O 4 ;
[0054] Formula M 1 M 2 (JO 4 ) f E 1-f A lithiated or partially lithiated material, wherein M 1 is lithium, which may be partially substituted by another alkali element with a degree of substitution less than 20%, M2 is a transition metal element in oxidation state +2 selected from Fe, Mn, Ni and combinations thereof, which may be partially substituted by one or more additional metal elements in oxidation state between +1 and +5 to a degree of substitution less than 35%, JO 4 is an oxygen-containing anion, wherein J is selected from P, S, V, Si, Nb, Mo and combinations thereof, E is a fluoride ion, a hydroxide ion or a chloride anion, and f is an oxygen-containing anion JO 4 The mole fraction is usually between 0.75 and 1 (inclusive).
[0055] More specifically, the lithiated or partially lithiated material may be based on phosphorus (which means, in other words, that the oxygen anion satisfies the formula PO 4 ) and may have an ordered or modified olivine-type structure.
[0056] Lithiated or partially lithiated materials can satisfy a specific formula Li 3-x M' y M” 2-y (JO 4 ) 3 , wherein 0≤x≤3, 0≤y≤2, M' and M" are the same or different metal elements, at least one of M' and M" is a transition metal element, JO 4 PO is preferred 4 , which may be substituted by another oxygen anion and a J portion selected from S, V, Si, Nb, Mo and combinations thereof.
[0057] The lithiated or partially lithiated material may satisfy the formula Li(Fe x Mn 1-x )PO 4 , where 0≤x≤1, preferably, x is equal to 1 (which means, in other words, that the corresponding material is LiFePO 4 ).
[0058] When the method of the present invention is used to manufacture a negative electrode, as examples of electrode active materials that can enter the negative electrode constitution of a lithium secondary battery, the modes that can be mentioned are:
[0059] Carbonaceous materials, such as graphitic carbon suitable for intercalating lithium and which may be in the form of powders, flakes, fibers or spheres (e.g. mesocarbon microbeads);
[0060] Silicon-based compounds, such as silicon carbide SiC or silicon oxide SiO x ;
[0061] Lithium metal;
[0062] Lithium alloys, such as those described in US 6203944 and / or WO 00 / 03444;
[0063] Lithiated titanium oxide, such as Li (4-x) M x Ti 5 O 12 or Li 4 M y Ti (5-y) O 12 An oxide of, wherein x and y range from 0 to 0.2, M is an element selected from Na, K, Mg, Nb, Al, Ni, Co, Zr, Cr, Mn, Fe, Cu, Zn, Si and Mo, a specific embodiment is Li 4 Ti 5 O 12 , these oxides are lithium-intercalation materials with low thermal expansion after lithium insertion;
[0064] Non-lithiated titanium oxides, such as TiO 2 ;
[0065] Formula M y Ti (5-y) O 12 An oxide of, wherein y ranges from 0 to 0.2, and M is an element selected from the group consisting of Na, K, Mg, Nb, Al, Ni, Co, Zr, Cr, Mn, Fe, Cu, Zn, Si and Mo;
[0066] Lithium-germanium alloys, such as those comprising the formula Li 4.4 Those of the crystalline phase of Ge; or
[0067] Mixtures thereof, for example, include mixtures of graphite and silicon-based compounds.
[0068] The polymer or polymers suitable for entering into the constitution of the polymer matrix are advantageously chosen from gelling polymers suitable for gelling upon contact with an electrolyte and thus capturing the electrolyte (the resulting electrode thus forms an electrode generally known as an “ion gel electrode”) and more particularly may be chosen from fluorinated polymers comprising at least one repeating unit resulting from the polymerization of a fluorinated monomer, and preferably, at least one repeating unit resulting from the polymerization of a monomer comprising at least one carboxylic acid group, optionally in the form of a salt.
[0069] It is to be understood that the repeating units resulting from the polymerization of fluorinated monomers and, if any, the repeating unit or units resulting from the polymerization of monomers comprising at least one carboxylic acid group, optionally in the form of a salt, are chemically different repeating units and in particular, the repeating unit or units resulting from the polymerization of fluorinated monomers do not comprise any carboxylic acid group, optionally in the form of a salt.
[0070] For the gel polymer, the one or more repeating units resulting from the polymerization of a fluorinated monomer may be, more specifically, one or more repeating units resulting from the polymerization of one or more olefinic monomers containing at least one fluorine atom and optionally one or more other halogen atoms, examples of this type of monomer are as follows:
[0071] C 2 -C 8 Perfluorinated olefins, such as tetrafluoroethylene and hexafluoropropylene (also known as HFP);
[0072] C 2 -C 8 Hydrogenated fluoroolefins, such as vinylidene fluoride, vinyl fluoride, 1,2-difluoroethylene and trifluoroethylene;
[0073] Formula CH 2 =CHR 1 Perfluoroalkylethylene, where R 1 It is C 1 -C 6 Perfluoroalkyl;
[0074] C containing one or more other halogen atoms (such as chlorine, bromine, iodine) 2 -C 6 Fluoroolefins, such as chlorotrifluoroethylene;
[0075] Formula CF 2 =CFOR 2 (per)fluoroalkyl vinyl ether, wherein R 2 It is C 1 -C 6 Fluorinated or perfluoroalkyl groups, such as CF 3 , C 2 F 5 , C 3 F 7 ;
[0076] Formula CF 2 =CFOR 3 The monomers, R 3 It is C 1 -C 12 Alkyl, C 1 -C 12 Alkoxy or C 1 -C 12(Per)fluoroalkoxy, for example perfluoro-2-propoxypropyl; and / or
[0077] Formula CF 2 =CFOCF 2 OR 4 The monomers, R 4 Is fluorinated or perfluorinated-C 1 -C 6 -alkyl, such as CF 2 , C 2 F 5 , C 3 F 7 or fluoro- or perfluoro-C 1 -C 6 -alkoxy, such as –C 2 F 5 -O-CF 3 .
[0078] More particularly, the gel polymer may include, as repeating units resulting from the polymerization of a fluorinated monomer, 2 -C 8 Repeating units produced by polymerization of perfluoroolefin monomers such as hexafluoropropylene, and by C 2 -C 8 Repeating units produced by polymerization of hydrogenated fluoroolefin monomers such as vinylidene fluoride.
[0079] The recurring unit or units resulting from the polymerization of monomers comprising at least one carboxylic acid group, optionally in the form of a salt, may be, more particularly, one or more recurring units resulting from the polymerization of monomers of formula (I):
[0080]
[0081] Where R 5 To R 7 are independently hydrogen or C 1 -C 3 Alkyl and R 8 is a hydrogen atom or a monovalent cation (eg, an alkali metal cation, an ammonium cation). Specific examples of such a monomer are acrylic acid or methacrylic acid.
[0082] A specific gel polymer that can be used in the context of the present invention may be a polymer comprising repeating units resulting from the polymerization of vinylidene fluoride, repeating units resulting from the polymerization of a monomer comprising at least one carboxylic acid group, such as acrylic acid and, optionally, repeating units resulting from the polymerization of a fluorinated monomer different from vinylidene fluoride, more specifically repeating units resulting from the polymerization of hexafluoropropylene.
[0083] Still more particularly, the gel polymer useful in the present invention is a gel polymer whose above-mentioned repeating unit results from polymerization:
[0084] At least 70 mol% of hydrogenated C 2 -C 8 A fluoroolefin, preferably vinylidene fluoride;
[0085] 0.1 to 15 mol% C 2 -C 8 a perfluoroolefin, preferably hexafluoropropylene; and
[0086] 0.01 to 20 mol% of the monomer of the above formula (I), preferably acrylic acid.
[0087] Furthermore, the gel polymer or polymers advantageously have an intrinsic viscosity measured in N,N-dimethylformamide at 25° C. of 0.1 to 1.0 L / g, preferably 0.25 to 0.45 L / g.
[0088] More specifically, the intrinsic viscosity is determined by the following equation based on the falling time at 25° C. of a solution obtained by dissolving the relevant polymer at a concentration of about 0.2 g / dL in a solvent (N,N-dimethylformamide) using an Ubbelohde viscometer:
[0089]
[0090] in:
[0091] η is the intrinsic viscosity (in dL / g);
[0092] c is the polymer concentration (in g / dL);
[0093] η r is the relative viscosity, which is the ratio of the solution falling time to the solvent falling time;
[0094] η sp is the specific viscosity, i.e. η r –1;
[0095] Γ is an experimental factor set to 3 for the polymer in question.
[0096] Advantageously, the electrolyte is a liquid electrolyte, more particularly, when the polymer matrix comprises one or more gel polymers, a liquid electrolyte capable of gelling in contact with the polymer matrix.
[0097] The liquid electrolyte may comprise (or even consist of) at least one organic solvent, at least one metal salt and optionally an additive belonging to the class of carbon-containing compounds (it being understood that such additives are distinct from carbonate solvents that may be included in the electrolyte).
[0098] The one or more organic solvents may be carbonate solvents, more specifically:
[0099] Cyclic carbonate solvents such as ethylene carbonate (abbreviated as EC), propylene carbonate (abbreviated as PC), butylene carbonate, vinylene carbonate, fluoroethylene carbonate, fluoropropylene carbonate and mixtures thereof;
[0100] Linear carbonate solvents such as diethyl carbonate (abbreviated as DEC), dimethyl carbonate (abbreviated as DMC), ethyl methyl carbonate (abbreviated as EMC), and mixtures thereof.
[0101] The one or more organic solvents may also be an ester solvent (such as ethyl propionate or n-propyl propionate), a nitrile solvent (such as acetonitrile), or an ether solvent (such as dimethyl ether or 1,2-dimethoxyethane).
[0102] The one or more organic solvents may also be ionic liquids, that is, compounds generally formed by the combination of positively charged cations and negatively charged anions, which are liquid at temperatures below 100° C. and atmospheric pressure.
[0103] More specifically, the ionic liquid may include:
[0104] a cation selected from the group consisting of imidazolium, pyridinium, pyrrolidinium, piperidinium, quaternary ammonium, quaternary phosphonium, pyrazolium, optionally substituted, for example, by at least one alkyl group comprising 1 to 30 carbon atoms;
[0105] Anions selected from halide anions, perfluorinated anions, borate anions.
[0106] More specifically, the cation may be selected from the following cations:
[0107] A pyrrolidinium cation of the following formula (II):
[0108]
[0109] Where R 13 and R 14 Independently of each other 1 -C 8 Alkyl, R 15 , R 16 , R 17 and R 18 are independently hydrogen or C 1 -C 30 Alkyl, preferably C 1 -C 18 Alkyl, more preferably C 1 -C 8 alkyl;
[0110] A piperidinium cation of the following formula (II):
[0111]
[0112] Where R 19 and R 20 Independently of each other 1 -C 8 Alkyl, R 21 , R 22 , R 23 , R 24 and R 25 are independently hydrogen or C 1 -C 30 Alkyl, preferably C 1 -C 18 Alkyl, more preferably C 1 -C 8 alkyl;
[0113] Quaternary ammonium cations;
[0114] Quaternary phosphonium cation;
[0115] an imidazolium cation; and
[0116] Pyrazolium cation.
[0117] In particular, the positively charged cation may be selected from the following cations:
[0118] A pyrrolidinium cation of the following formula (II-A):
[0119]
[0120] A piperidinium cation of the following formula (III-A):
[0121]
[0122] When it is a quaternary ammonium cation, it can be a tetraalkylammonium cation, a trialkylarylammonium cation or a tetraarylammonium cation, the alkyl groups, when present, are the same or different and can be straight or branched chain alkyl groups comprising from 4 to 12 carbon atoms, preferably 4-6 carbon atoms, and the aryl groups, when present, are the same or different and can be phenyl, benzyl or naphthyl. More specifically, it can be a tetraethylammonium cation, a tetrapropylammonium cation, a tetrabutylammonium cation, a trimethylbenzylammonium cation, a methyltributylammonium cation, an N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium cation, an N,N-dimethyl-N-ethyl-N-(3-methoxypropyl)ammonium cation, an N,N-dimethyl-N-ethyl-N-benzylammonium cation, an N,N-dimethyl-N-ethyl-N-phenethylammonium cation, an N-tributylammonium cation, an N-trimethyl-N-methylammonium cation, an N-trimethyl-N-butylammonium cation, an N-trimethyl-N-hexylammonium cation, an N-trimethyl-N-propylammonium cation.
[0123] When it is a quaternary phosphonium cation, it can be a tetraalkylphosphonium cation, a trialkylarylphosphonium cation or a tetraarylammonium cation, and when present, the alkyl groups are identical or different and can be alkyl, straight or branched groups, comprising 4 to 12 carbon atoms, preferably 4 to 6 carbon atoms, and the aryl groups, when present, are identical or different and can be phenyl, benzyl or naphthyl. More specifically, it can be a trihexyl (tetradecyl) phosphonium cation or a tetrabutylphosphonium cation.
[0124] When it is an imidazolium cation, it may be 1,3-dimethylimidazolium cation, 1-(4-sulfobutyl)-3-methylimidazolium cation, 1-allyl-3H-imidazolium cation, 1-butyl-3-methylimidazolium cation, 1-ethyl-3-methylimidazolium cation, 1-hexyl-3-methylimidazolium cation, 1-octyl-3-methylimidazolium cation.
[0125] In particular, the negatively charged anion may be selected from:
[0126] 4,5-dicyano-2-(trifluoromethyl)imidazole (TDI for short);
[0127] Bis(fluorosulfonyl)imide (referred to as FSI);
[0128] Formula (SO 2 CF 3 ) 2 N-bis(trifluoromethylsulfonyl)imide;
[0129] Formula PF 6 - hexafluorophosphate;
[0130] Formula BF 4 - tetrafluoroborate;
[0131] Oxalate of the following formula (IV):
[0132]
[0133] Specific ionic liquids useful according to the present invention may be composed of a cation of formula (II-A) as defined above and a cation of formula (SO 2 CF 3 ) 2 N-, PF 6 - or BF 4 - Anions of ionic liquids.
[0134] The one or more metal salts may be selected from the group consisting of salts of the formula: MeI, Me(PF 6 ) n 、Me(BF 4 ) n 、Me(ClO 4 ) n 、Me(bis(oxalato)borate) n (Can be designated as Me(BOB) n )、MeCF 3 SO 3 、Me[N(FSO 2 ) 2 ] n 、Me[N(CF 3 SO 2 ) 2 ] n ,Me[N(C 2 F 5 SO 2 ) 2 ] n 、Me[N(CF 3 SO 2 )(R F SO 2 )] n , where R F For -C 2 F 5 , -C 4 F 9 or –CF 3 OCF 2 CF 3 、Me(AsF 6 ) n 、Me[C(CF 3 SO 2 ) 3 ] n 、Me 2 S n、Me(C 6 F 3 N 4 )(C 6 F 3 N 4 is 4,5-dicyano-2-(trifluoromethyl)imidazole, when Me is Li, the salt is 4,5-dicyano-2-(trifluoromethyl)imidazole, the salt is abbreviated as LiTDI), wherein Me is a metal element, preferably Me is a transition metal element, an alkali metal element or an alkaline earth element, more preferably Me is Li (especially when the battery of the present invention is a lithium ion or lithium-air battery), Na (especially when the battery is a sodium ion battery), K (especially when the battery is a potassium ion battery), Mg (especially when the battery is a magnesium ion battery), Ca (especially when the battery is a calcium ion battery) and Al (especially when the battery is an aluminum ion battery), and n is the valence level of the metal element (usually 1, 2 or 3).
[0135] When Me is Li, the salt is preferably LiPF 6 .
[0136] The concentration of the metal salt in the liquid electrolyte is advantageously at least 0.01 M, preferably at least 0.025 M, more preferably at least 0.05 M and advantageously at most 5 M, preferably at most 2 M and more preferably, at most 1 M.
[0137] In addition, the liquid electrolyte may include at least one additive belonging to the category of carbon-containing compounds (it should be understood that this additive is different from one or more carbonate solvents or solvents included in the electrolyte, if any), such as vinylene carbonate or fluoroethylene carbonate, and the content of this additive in the electrolyte does not exceed 5wt% of the total weight of the electrolyte.
[0138] Liquid electrolytes that can be used, in particular when the electrode produced according to the method of the present invention is used in a lithium ion battery, are mixtures comprising carbonate solvents (e.g., mixtures of cyclic carbonate solvents, such as a mixture of ethylene carbonate and propylene carbonate or a mixture of cyclic carbonate solvents and linear carbonate solvents, such as a mixture of ethylene carbonate, propylene carbonate and dimethyl carbonate), lithium salts, such as LiPF 6 (e.g., 1M) and optional additives such as vinylene carbonate or fluoroethylene carbonate.
[0139] As mentioned above, the composition may include at least one electronic conductor additive, i.e. an additive capable of imparting electronic conductivity to the electrode to which it is incorporated, for example, the additive being chosen from carbonaceous materials such as carbon black, carbon nanotubes, carbon fibers (in particular vapor grown carbon fibers known by the abbreviation VGCF), graphite in powder form, graphite fibers, graphene and mixtures thereof.
[0140] In addition, the composition may include at least one solvent for the polymer (except any organic solvent for the electrolyte, as the case may be) provided to enter into the composition of the polymer matrix, the solvent being a ketone solvent (such as acetone) when the polymer or polymers are selected from the family of fluorinated polymers comprising at least one repeating unit resulting from the polymerization of a fluorinated monomer, preferably at least one repeating unit resulting from the polymerization of a monomer comprising at least one carboxylic acid group, optionally in the form of a salt. Due to the use of a specific mixer, a smaller amount of such solvent or solvents can be used relative to processes involving the use of conventional mixers.
[0141] In case the composition comprises at least one of the above mentioned solvents, the method advantageously comprises an evaporation step after the forming step, evaporating for example one or more solvents selectively selecting one or more polymers to enter the constitution of the polymer matrix, for example by in-line drying by selective evaporation.
[0142] The manufacturing step is carried out at a temperature below 100°C, preferably below 80°C, more preferably below 70°C, and preferably at a temperature greater than or equal to 5°C, more preferably greater than or equal to 10°C, and even more preferably greater than or equal to 15°C.
[0143] More specifically, the manufacturing step may be carried out at ambient temperature (i.e. the ambient temperature at which the manufacturing step takes place), without any heating element providing heat, for example a temperature in the range of 15-35° C., more specifically a temperature equal to 25° C.) or may be carried out at a temperature above ambient temperature, for example a temperature above ambient temperature but below 100° C. More specifically, the manufacturing step may be carried out at a temperature above ambient temperature but below the boiling temperature of the solvent(s) for the polymer(s) provided for the formation of the polymer matrix, when such solvent(s) are present in the composition or when such solvent(s) are absent, at a temperature above ambient temperature but below the melting temperature of the polymer(s) provided for the formation of the polymer matrix (it being understood that the temperature at which the manufacturing step is carried out is always below 100° C.).
[0144] The manufacturing steps make it possible to obtain a composition in the form of a homogeneous paste having a very high dynamic viscosity, more specifically, at 0.1 s -1 The dynamic viscosity measured at a shear rate of 1000 Pa.s and ambient temperature is greater than 5000 Pa.s, preferably greater than 6000 Pa.s, and more preferably greater than 7000 Pa.s.
[0145] It should be noted that ambient temperature is understood to mean the ambient temperature at which the dynamic viscosity measurement is performed without any heating element providing heat, for example in the temperature range of 15 to 35°C, for example a temperature equal to 25°C.
[0146] More specifically, the dynamic viscosity of the composition is measured using a Malvern brand CVO Bohlin rheometer equipped with a Peltier support and a moving cone with a diameter of 40 mm and an angle of 4°. For this purpose, the composition is deposited between the Peltier support and the moving part with a gap of 150 μm. Optionally, when the composition comprises at least one solvent for the polymer constituting the polymer matrix, a solvent trap is added to the system to avoid too rapid evaporation of the solvent. The viscosity is measured in the viscometer mode at 0.1 s -1 The shear rate and ambient temperature were measured with an integration time of 5 s.
[0147] Furthermore, under the conditions defined above (i.e., 0.1s -1 When the composition is subjected to the above-defined conditions (i.e., 0.1s -1 Very favorable results have been obtained when the shear rate and dynamic viscosity at ambient temperature are 7000 to 12000 Pa.s) in paste form).
[0148] In fact, a particularly advantageous aspect of the process of the invention is its ability to produce electrode-forming compositions having very high dynamic viscosities, which makes it possible to minimize the use of liquid electrolytes and / or organic solvents. This is an advantage over the established techniques for producing electrodes from inks produced in conventional mixers based on disperser or planetary mixer type, with dynamic viscosities measured under the conditions of the above measurements being less than 5000 Pa.s, or possibly even less than 1000 Pa.s.
[0149] When the composition comprises one or more solvents provided for incorporation into one or more polymers of the polymer matrix, the composition after the manufacturing step comprises 50-80% solid mass relative to the total mass of the composition.
[0150] More specifically, when the composition includes as a constituent component at least one electrode active material, at least one polymer provided to enter the composition of the polymer matrix, an electrolyte and optionally at least one electronic conductor additive and at least one polymer solvent, the composition further obtained in this manufacturing step advantageously has a solid weight percentage relative to the total weight of the composition, which ranges from 50-80% (compared to 35-49% for methods involving conventional mixers). In addition, these compositions may include 6 to 11% electrolyte accounting for the total weight of the composition and 11 to 42% of the polymer solvent weight accounting for the total weight of the composition (as compared to 45% to 57% for methods using conventional mixers).
[0151] According to a specific and advantageous embodiment, the composition may be free of solvents for one or more polymers or for a plurality of polymers provided to enter the composition of the polymer matrix. Under these conditions, in addition to the preparation step, the composition may comprise a solid mass of 83 to 90% relative to the total mass of the composition.
[0152] More specifically, when the composition includes as constituents at least one electrode active material, at least one polymer provided to enter a polymer matrix, an electrolyte, and optionally at least one electronic conductor additive but does not contain a solvent, in the one or more polymers, the percentage of the solid mass can be 83-90% of the total mass of the composition, and the mass of the electrolyte can be 10-17% of the total mass of the composition.
[0153] Under these conditions, the above-mentioned solvent evaporation step is not necessary.
[0154] The manufacturing steps can be carried out continuously, that is to say the introduction of the ingredients in a specific mixer and mixing them is carried out continuously, that is to say during the entire implementation of the method.
[0155] The step of forming the electrode from the composition may be performed by deposition through a die, such as a slot die, through which the composition is delivered to the substrate, the purpose of the die being to cause the composition to flow from the die from a circular geometry to a rectangular geometry to form strips on the substrate.
[0156] Beforehand, the composition may optionally be laminated before approaching the substrate in order to reduce its thickness, and the composition thus laminated may be deposited on the substrate by an operation of co-lamination with the substrate.
[0157] Before the shaping step and after the manufacturing step, the composition can be transported in another mixer, for example, in a conveying device under pressure, such as a single screw conveyor rotating in a closed sleeve and subjected to a higher pressure than the mixture used in the manufacturing step, wherein it can be provided that in this case, the shaping step is also carried out through a die arrangement, preferably, at the outlet of the other mixer, the die also having a circular geometry of the composition, with the purpose of forming strips on the substrate with a rectangular geometry.
[0158] Before introduction into another mixer, such as a single-screw conveyor, the composition can have the form of granules, which are formed at the outlet of the twin-screw mixer used in the manufacturing step, for example by passing through a circular die arranged at the outlet of the mixer to form rods, the die being equipped with a cutting system, which is arranged at the outlet of the twin-screw mixer.
[0159] After the step of forming the electrode and the optional evaporation step, the method may further comprise a step of calendering the electrode in order to increase the volumetric energy density.
[0160] The manufacturing method may be a continuous method, that is to say a method that is carried out uninterruptedly throughout the duration of its implementation, in other words, means that the electrode is manufactured uninterruptedly throughout the implementation of the method. In other words, this means that step a) and step b) are carried out simultaneously and without interruption throughout the duration of the method, in other words, this means that at each moment t of the duration of the method, a small part of the composition is subjected to the manufacturing step, while another part of the composition is subjected to the forming step. It should also be understood that in this case, all optional steps of the method (e.g. lamination step, drying step) are implemented continuously when present.
[0161] The invention will now be described with the aid of the following examples given by way of non-limiting illustration. BRIEF DESCRIPTION OF THE DRAWINGS
[0162] Figure 1 1 is a graph showing the change in voltage U (V) versus capacity C (mAh / g) of the negative electrode obtained according to the method of Example 1, wherein curve a) is the curve of the first cycle, and curve b) is the curve of the second cycle.
[0163] Figure 2 3 is a graph showing the change in voltage U (V) of the positive electrode obtained according to the method of Example 3 with capacity C (mAh / g), wherein curve a) is the curve of the first cycle, and curve b) is the curve of the second cycle.
[0164] Earlier described Figure 3 is a cross-sectional view of a specific twin-screw mixer that can be used in the process of the present invention.
[0165] Detailed description of specific embodiments
[0166] Example 1
[0167] This example illustrates the production by a continuous method according to the invention of a negative electrode comprising 55% of solid mass relative to the total mass of the electrode.
[0168] In the first stage, the ion gel electrode paste was produced by continuously introducing and mixing the components of the electrode in a mixer having two co-rotating interpenetrating screws rotating in a closed sleeve in the presence of acetone at 25°C, the introduction being carried out first by the introduction of the solid components and secondly by the introduction of the liquid components. The composition of the paste was as follows: 39.2 wt% of graphite (D 50 =20μm)13.1wt% graphite (D 50 =3.5 μm), 2.7 wt% of a copolymer constituting a polymer matrix (the copolymer is a copolymer including repeating units produced by polymerization of vinylidene fluoride (96.7 mol%), acrylic acid (0.9 mol%) and hexafluoropropylene (2.4 mol%), and having an intrinsic viscosity of 0.30 L / g in dimethylformamide at 25° C.), 37.5 wt% of anhydrous acetone and 7.5 wt% of 1 M LiPF 6 The electrolyte was added in a mixture of ethylene carbonate and propylene carbonate (1:1) containing 2 wt% of ethylene carbonate.
[0169] The dynamic viscosity of the composition was measured on a CVO Bohlin rheometer of the Malvern brand, equipped with a Peltier holder and a moving cone with a diameter of 40 mm and an angle of 4°. For this purpose, the paste was deposited between the Peltier holder and the movable part with a gap of 150 μm, a solvent trap was added to the system to avoid too rapid evaporation of the acetone, and the viscosity was measured in the viscometer mode at 0.1 s -1 The measurements were performed at a shear rate of 1000 nm and 25 °C with an integration time of 5 s.
[0170] The dynamic viscosity measurement obtained was 7200 Pa.s.
[0171] In the second stage, the electrode paste thus formed is spread on a 10 μm thick copper sheet at the outlet of a specific mixer, and then dried and rolled to form an ion gel graphite electrode. The electrode has a unit area weight of 11.3 mg / cm 2 (3.6mAh / cm 2 ), with a thickness of 90 μm. The capacity of the electrode was verified against lithium metal in a button cell.
[0172] The total measured capacity is 350 mAh / g, and the reversible capacity in the first cycle at C / 20 is 300 mAh / g. The reversible capacity in the second cycle at C / 20 is 350 mAh / g. These data are shown in Figure 2. Figure 1 As shown, it shows the change of voltage U (unit V) with capacity C (unit mAh / g), curve a) is the curve of the first cycle, and curve b) is the curve of the second cycle.
[0173] Example 2
[0174] This example illustrates the production of an ion gel electrode paste produced according to the production steps of the method of the invention and comprising 65% of solid mass relative to the total mass of the electrode.
[0175] This electrode paste is produced by continuously introducing and mixing the electrode ingredients at 25° C. in a mixer having two co-rotating interpenetrating screws rotating in a closed sleeve in the presence of acetone, the introduction being carried out firstly by the introduction of the solid ingredients and secondly by the introduction of the liquid ingredients. The composition of the paste is as follows: 46.4 wt % of graphite (D 50 =20μm)15.4wt% graphite (D 50 =3.5 μm), 3.2 wt% of a copolymer constituting a polymer matrix (the copolymer is a copolymer comprising repeating units produced by polymerization of vinylidene fluoride (96.7 mol%), acrylic acid (0.9 mol%) and hexafluoropropylene (2.4 mol%), and having an intrinsic viscosity of 0.30 L / g in dimethylformamide at 25° C.), 24.2 wt% of anhydrous acetone and 10.8 wt% of 1M LiPF 6 The electrolyte was in a mixture of ethylene carbonate, propylene carbonate and dimethyl carbonate (1:1:3) containing 2 wt% ethylene carbonate.
[0176] Due to the high dynamic viscosity (0.1s -1 The dynamic viscosity of the composition obtained using a Malvern brand CVO Bohlin rheometer cannot be measured because the shear rate is significantly greater than 10000 Pa.s).
[0177] Example 3
[0178] This example illustrates the production by a continuous process according to the invention of a positive electrode comprising 70% of solid mass relative to the total mass of the electrode.
[0179] In the first stage, the ion gel electrode paste was manufactured by continuously introducing and mixing the components of the electrode in a mixer with two co-rotating interpenetrating screws rotating in a closed sleeve in the presence of acetone at 25°C, the introduction being carried out first by the introduction of the solid components and secondly by the introduction of the liquid components. The composition of the paste was as follows: 65.8 wt% LiNi 0.33 Mn 0.33 Co 0.33 O 2 , 2.8 wt% of an electronic conductor additive, 1.4 wt% of a copolymer constituting a polymer matrix (the copolymer is a copolymer including repeating units produced by polymerization of vinylidene fluoride (96.7 mol%), acrylic acid (0.9 mol%) and hexafluoropropylene (2.4 mol%), and having an intrinsic viscosity of 0.30 L / g in dimethylformamide at 25° C.), 22.4 wt% of anhydrous acetone and 7.6 wt% of 1 M LiPF 6 The electrolyte was added in a mixture of ethylene carbonate and propylene carbonate (1:1) containing 2 wt% of ethylene carbonate.
[0180] The dynamic viscosity of the composition was measured on a CVO Bohlin rheometer of the Malvern brand, equipped with a Peltier holder and a moving cone with a diameter of 40 mm and an angle of 4°. For this purpose, the paste was deposited between the Peltier holder and the movable part with a gap of 150 μm, a solvent trap was added to the system to avoid too rapid evaporation of the acetone, and the viscosity was measured in the viscometer mode at 0.1 s -1 The measurements were performed at a shear rate of 1000 nm and 25 °C with an integration time of 5 s.
[0181] The dynamic viscosity measurement obtained was 11 000 Pa.s.
[0182] In the second stage, the electrode paste thus formed is spread on a 20 μm thick aluminum sheet at the outlet of a specific mixer, and then dried and rolled to form an ion gel graphite electrode. The electrode has a unit area weight of 19.5 mg / cm 2 (2.9mAh / cm 2 ) with a thickness of 95 μm. The capacity of the electrode was verified in a button cell against lithium metal. The total measured capacity was 170 mAh / g, and the reversible capacity was 147 mAh / g in the first cycle at C / 20. The reversible capacity was 143 mAh / g in the second cycle at C / 20. These data are shown in Figure 2 As shown, it shows the change of voltage U (unit V) with capacity C (unit mAh / g), curve a) is the curve of the first cycle, and curve b) is the curve of the second cycle.
[0183] Example 4
[0184] This example illustrates the production by a continuous method according to the invention of a positive electrode comprising 80% of solid mass relative to the total mass of the electrode.
[0185] In the first stage, the ion gel electrode paste was produced by continuously introducing and mixing the components of the electrode in a mixer with two co-rotating interpenetrating screws rotating in a closed sleeve in the presence of acetone at 25°C, the introduction being carried out first by the introduction of the solid components and secondly by the introduction of the liquid components. The composition of the paste was as follows: 75.2 wt% LiNi 0,33 Mn 0,33 Co 0,33 O 2 , 3.2 wt% of an electron conductor additive, 1.6 wt% of a copolymer constituting a polymer matrix (the copolymer is a copolymer including repeating units produced by polymerization of vinylidene fluoride (96.7 mol%), acrylic acid (0.9 mol%) and hexafluoropropylene (2.4 mol%), and having an intrinsic viscosity of 0.30 L / g in dimethylformamide at 25° C.), 11.3 wt% of anhydrous acetone and 8.7 wt% of 1 M LiPF 6 The electrolyte was added in a mixture of ethylene carbonate and propylene carbonate (1:1) containing 2 wt% of ethylene carbonate.
[0186] Due to the high dynamic viscosity (0.1s -1 The dynamic viscosity of the composition obtained using a Malvern brand CVO Bohlin rheometer cannot be measured because the shear rate is significantly greater than 10000 Pa.s).
[0187] In the second stage, the electrode paste thus produced is formed into strips through a slot die placed at the mixer outlet, and the strips are then laminated to reduce their thickness and then deposited on a current collector of aluminum by co-lamination to form an ion gel electrode.
[0188] Example 5
[0189] This example illustrates the production by a continuous method according to the invention of a positive electrode comprising 90% of solid mass relative to the total mass of the electrode.
[0190] In the first stage, the ion gel electrode paste was manufactured by continuously introducing and mixing the components of the electrode in a mixer with two co-rotating interpenetrating screws rotating in a closed sleeve in the presence of acetone at 25°C, the introduction being carried out first by the introduction of the solid components and secondly by the introduction of the liquid components. The composition of the paste was as follows: 84.6 wt% LiNi 0.33 Mn 0.33 Co 0.33 O 2, 3.6 wt% of an electronic conductor additive, 1.8 wt% of a copolymer constituting a polymer matrix (the copolymer is a copolymer comprising repeating units produced by polymerization of vinylidene fluoride (96.7 mol%), acrylic acid (0.9 mol%) and hexafluoropropylene (2.4 mol%), and having an intrinsic viscosity of 0.30 L / g in dimethylformamide at 25° C.), 10 wt% of 1M LiPF 6 The electrolyte was added in a mixture of ethylene carbonate and propylene carbonate (1:1) containing 2 wt% of ethylene carbonate.
[0191] Due to the high dynamic viscosity (0.1s -1 The dynamic viscosity of the composition obtained using a Malvern brand CVO Bohlin rheometer cannot be measured because the shear rate is significantly greater than 10000 Pa.s).
[0192] In the first stage, the electrode paste thus produced is formed into strips through a slot die placed at the mixer outlet, the strips are then laminated to reduce their thickness and then deposited on a current collector of aluminum by co-lamination to form an ion gel electrode.
Claims
1. A method for manufacturing an electrode comprising a polymer matrix, wherein the polymer matrix captures an electrolyte, the method comprising the steps of: a) a step of preparing a composition comprising as components constituting said electrode: - at least one electrode active material, at least one polymer provided for inclusion in the formation of said polymer matrix and chosen from gelling polymers suitable for gelling upon contact with said electrolyte and thus trapping said electrolyte, and - electrolytes; b) forming an electrode on a substrate from the composition; Features: - The composition prepared in step a) is a paste composition which has a -1 The dynamic viscosity measured at a shear rate and ambient temperature is greater than 5000 Pa.s; and - the manufacturing step comprises introducing and mixing the components constituting the electrode into a mixer having two co-rotating interpenetrating screws rotating in a closed sleeve, the manufacturing step being carried out at a temperature below 100°C.
2. The manufacturing method according to claim 1, wherein: The composition further includes at least one electron conductor additive as a component constituting the electrode.
3. The manufacturing method according to claim 1, wherein: The at least one polymer is chosen from fluorinated polymers comprising at least one repeating unit resulting from the polymerization of a fluorinated monomer.
4. The manufacturing method according to claim 3, wherein: The at least one polymer is selected from the fluorinated polymers further comprising at least one repeating unit resulting from the polymerization of a monomer comprising at least one carboxylic acid group.
5. The method of manufacturing according to claim 4, wherein the at least one carboxylic acid group is in the form of a salt.
6. The manufacturing method according to claim 1, wherein: The electrolyte is a liquid electrolyte including at least one organic solvent and at least one metal salt.
7. The manufacturing method according to claim 6, wherein the liquid electrolyte further comprises an additive belonging to the category of carbon-containing compounds.
8. The manufacturing method according to claim 1, wherein: The composition further comprises at least one solvent for the at least one polymer provided for entry into the composition of the polymer matrix.
9. The manufacturing method according to claim 8, further comprising, after the forming step, a step of evaporating the at least one solvent provided for entering the at least one polymer constituting the polymer matrix.
10. The manufacturing method according to claim 1, wherein: The composition is free of solvents that provide for the at least one polymer to be incorporated into the polymer matrix.
11. The manufacturing method according to any one of claims 1 to 10, wherein: The manufacturing steps are carried out continuously.
12. The manufacturing method according to claim 8 or 10, wherein: The fabrication steps are performed at ambient temperature, or at a temperature above ambient temperature but below 100°C.
13. The manufacturing method according to claim 8 or 10, wherein: When the at least one solvent for at least one polymer provided for entering the composition of the polymer matrix is present in the composition, the manufacturing step is carried out at a temperature above ambient temperature but below the boiling temperature of the at least one solvent; when the at least one solvent is not present, the manufacturing step is carried out at a temperature above ambient temperature but below the melting temperature of the at least one polymer provided for entering the composition of the polymer matrix.
14. The manufacturing method according to claim 8 or 10, wherein: When the composition comprises at least one solvent for at least one polymer provided for entering the polymer matrix, the composition after the manufacturing step comprises 50-80% solid mass relative to the total mass of the composition; or when it does not comprise a solvent for at least one polymer provided for entering the polymer matrix, the composition after the manufacturing step comprises 83-90% solid mass relative to the total mass of the composition.
Citation Information
Patent Citations
Electrode for a lithium battery
US6203944B1
Electrode material and compositions including same
WO2000003444A1
Composite electrodes
WO2015169835A1
Method for producing cathodes
CN104737332A
Composite electrodes
CN107078267A