Positive electrode active material for lithium ion secondary battery and lithium ion secondary battery
By using layered rock salt type lithium-containing transition metal composite oxide particles in the positive electrode active material of lithium ion secondary batteries and forming a metal composite oxide coating layer, the problem of insufficient output characteristics and cycle characteristics has been solved, and higher performance has been achieved. Battery performance and durability for electric vehicle power supplies.
Patent Information
- Application Number
- CN202080065825.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-19
- Filing Date
- 2020-09-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-09-18
AI Technical Summary
Existing lithium-ion secondary battery cathode active materials still have room for improvement in terms of output characteristics and cycle characteristics, especially when high output and durability are required in electric vehicle applications, internal resistance and particle selectivity deteriorate. Causes problem of reduced battery capacity.
Lithium-containing transition metal composite oxide particles with a layered rock salt type crystal structure are used, and a metal composite oxide coating layer of Li and metal element M2 is formed on the surface. By controlling the particle size, particle size distribution and structural design, it forms a The composite oxide particles have a porous structure to improve the reaction area with the electrolyte and the insertion and extraction efficiency of lithium ions.
The positive electrode resistance is significantly reduced, the output characteristics and durability are improved, and it is suitable for lithium-ion secondary batteries with high energy density and high cycle characteristics, especially of industrial significance in electric vehicle power supply applications.
Smart Images

Figure CN114424369B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery composed of a lithium-nickel-containing composite oxide and a lithium ion secondary battery using the positive electrode active material for a lithium ion secondary battery as a positive electrode material. Background Art
[0002] In recent years, with the popularity of portable electronic devices such as smart phones, tablet terminals, digital cameras, and notebook computers, there is a strong desire to develop small and lightweight secondary batteries with high energy density. In addition, there is a strong desire to develop high-capacity and high-output secondary batteries as power sources for electric vehicles such as hybrid electric vehicles, plug-in hybrid electric vehicles, and battery-type electric vehicles.
[0003] As a secondary battery that meets the above requirements, there is a lithium ion secondary battery. The lithium ion secondary battery is composed of a negative electrode, a positive electrode, a non-aqueous electrolyte or a solid electrolyte, etc. As the active material used as the material of its negative electrode and positive electrode, a material that can remove and insert lithium is used. It should be noted that as a non-aqueous electrolyte, there is a non-aqueous electrolyte prepared by dissolving a lithium salt as a supporting salt in an organic solvent, and as a solid electrolyte, there is an inorganic or organic solid electrolyte that is non-flammable and has lithium ion conductivity.
[0004] Among lithium-ion secondary batteries, lithium-ion secondary batteries that use lithium-containing transition metal composite oxides with a layered rock salt type or spinel type crystal structure as the positive electrode material can obtain a voltage of 4V, so as to be a battery with high energy density, research and development and practical application are currently underway.
[0005] As a positive electrode material for lithium-ion secondary batteries, lithium cobalt composite oxide (LiCoO) which is relatively easy to synthesize has been proposed. 2 ), lithium nickel composite oxide (LiNiO 2 ), lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O 2 ), lithium manganese composite oxide (LiMn 2 O 4 ), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 O 2 ) and other lithium-containing transition metal composite oxides.
[0006] In recent years, among these lithium-containing transition metal composite oxides, lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3Co 1 / 3 O 2 The ternary positive electrode active material composed of a composite oxide (NMC) containing lithium nickel manganese cobalt containing at least nickel, manganese and cobalt as transition metals has attracted attention as a material with excellent thermal stability, high capacity, good cycle characteristics of battery capacity, low resistance and high output. The composite oxide containing lithium nickel manganese cobalt is a compound having a layered rock salt type crystal structure, similar to lithium cobalt composite oxide and lithium nickel composite oxide.
[0007] The development of lithium-containing transition metal composite oxides focuses on achieving high output by reducing their internal resistance. In particular, in the application of power sources for electric vehicles, there is a high level of demand for higher output by further reducing internal resistance.
[0008] In order to improve the output characteristics and cycle characteristics of positive electrode active materials composed of composite oxides containing lithium transition metals, such as composite oxides containing lithium nickel and composite oxides containing lithium nickel manganese cobalt, it is important to use particles with a small particle size and a narrow particle size distribution. Particles with a small particle size have a large specific surface area. When used as positive electrode active materials, they can fully ensure the reaction area with the electrolyte. Furthermore, they can form a thinner positive electrode and shorten the movement distance between the positive electrode and the negative electrode of lithium ions. Therefore, by setting particles with a small particle size, it is possible to achieve a reduction in positive electrode resistance. In addition, by using particles with a narrow particle size distribution, the voltage applied to the particles in the electrode can be uniformized, thereby suppressing the reduction in battery capacity caused by the selective degradation of the particles.
[0009] In order to further improve the output characteristics, the improvement of the particle structure of the composite oxide containing lithium transition metals is also studied and developed. For example, in order to improve the output characteristics, it is considered effective to form a space portion inside the positive electrode active material into which the electrolyte can invade. By adopting such a structure, the reaction area with the electrolyte can be increased compared to the positive electrode active material of a solid structure with the same particle size, so the positive electrode resistance can be significantly reduced. In addition, it is known that the positive electrode active material will continue the particle properties of the composite hydroxide containing transition metals as its precursor. That is, in order to obtain a positive electrode active material with a space portion, it is necessary to appropriately control the particle size, particle size distribution and particle structure of the secondary particles of the composite hydroxide containing transition metals as its precursor.
[0010] For example, in the WO2014 / 181891 Gazette and the Japanese Patent Publication No. 2018-104275 Gazette, a method for producing a composite hydroxide containing a transition metal is disclosed, characterized in that it has a nucleation process in which the pH value of an aqueous solution for nucleation containing a metal compound containing at least a transition metal and an ammonium ion donor is controlled to be greater than 12.0 and less than 14.0 for nucleation, and a particle growth process in which the pH value of an aqueous solution for particle growth containing the generated nuclei is controlled to be lower than the pH value of the nucleation process and greater than 10.5 and less than 12.0 to cause them to grow, and the initial stages of the nucleation process and the particle growth process are set to a non-oxidizing environment, and two environmental controls are performed, wherein the environmental control is switched to an oxidizing environment at a specified time in the particle growth process and then switched to a non-oxidizing environment again. According to this method, a transition metal-containing composite hydroxide composed of secondary particles with small particle size and narrow particle size distribution can be obtained, wherein the secondary particles have a central portion formed by the aggregation of plate-like or needle-like primary particles and have a stacked structure on the outside of the central portion, which is formed by alternating stacking of two low-density layers formed by the aggregation of fine primary particles and a high-density layer formed by the aggregation of plate-like primary particles.
[0011] The positive electrode active material using the transition metal-containing composite hydroxide as a precursor has a small particle size and a narrow particle size distribution, and has a porous structure with a space portion. A secondary battery using the positive electrode active material with such a porous structure can improve capacity characteristics, cycle characteristics, and output characteristics.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent document 1: WO2014 / 181891 publication.
[0015] Patent document 2: Japanese Patent Application Publication No. 2018-104275. Summary of the invention
[0016] Problems to be solved by the invention
[0017] However, there is a demand for further improvement in the output characteristics of the positive electrode active materials described in these documents.
[0018] In view of the above problems, an object of the present invention is to provide a positive electrode active material for a lithium ion secondary battery which can exhibit excellent output characteristics when used in a lithium ion secondary battery.
[0019] Means for solving problems
[0020] A positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention comprises: a lithium transition metal-containing composite oxide particle, wherein the lithium transition metal-containing composite oxide particle has a general formula (A): Li 1+u Ni x Mn y Co z M1 t O 2 The composition represented by the invention and the layered rock salt type crystal structure, wherein in the general formula (A), -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0≤t≤0.1, M1 is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W; and a coating layer, which is present on at least a portion of the surface of the lithium-transition metal-containing composite oxide particles and is composed of microparticles and / or coatings of a metal composite oxide of Li and a metal element M2, and M2 is one or more metal elements selected from Al, Ti, Zr, Nb, Mo and W.
[0021] The lithium-transition metal-containing composite oxide particles having the coating layer have a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, as determined from a particle size distribution measurement value, and a 2.0 μm or less cumulative diameter. 2 / g or more and 5.0m 2 / g or less, BET specific surface area 1.0g / cm 3 Above and 2.0g / cm 3 The tap density is less than 30 mL / 100 g and the oil absorption is less than 60 mL / 100 g.
[0022] The amount of M2 contained in the coating layer is 0.1 atomic % or more and 1.5 atomic % or less relative to the total number of atoms of Ni, Mn and Co contained in the lithium transition metal-containing composite oxide particles. In addition, the total amount of M1 and M2 in the entire positive electrode active material for lithium ion secondary batteries is preferably 10 atomic % or less relative to the total number of atoms of Ni, Mn, Co, M1 and M2.
[0023] The 50% cumulative diameter d50 of the lithium-transition metal-containing composite oxide particles having the coating layer, which is obtained from the particle size distribution measurement value, is preferably 4.0 μm or more and 6.0 μm or less.
[0024] [(d90-d10) / d50], which is an indicator of the width of the particle size distribution of the lithium-transition metal composite oxide particles having the coating layer, is preferably less than 1.0, wherein d10 is the 10% cumulative diameter calculated based on the particle size distribution measurement value, and d90 is the 90% cumulative diameter calculated based on the particle size distribution measurement value.
[0025] The value of d90 / d10 of the lithium-transition metal-containing composite oxide particles having the coating layer is preferably 1.0 or more and 2.0 or less.
[0026] Preferably, the lithium-transition metal-containing composite oxide particles are composed of secondary particles formed by agglomeration of primary particles, and the secondary particles have an agglomeration portion, one or more connecting holes connected to the peripheral portion of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connected to the connecting holes. The number of the connecting holes is preferably two or more. Preferably, the two or more space portions are connected to the connecting holes or other space portions.
[0027] Preferably, M2 contained in the coating layer is W, and the metal composite oxide is lithium tungstate.
[0028] A lithium-ion secondary battery according to one embodiment of the present invention is characterized in that the lithium-ion secondary battery has a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte (non-aqueous electrolyte secondary battery), or has a positive electrode, a negative electrode and a solid electrolyte (solid electrolyte secondary battery), and the positive electrode active material for the lithium-ion secondary battery of the present invention is used as the positive electrode active material for the positive electrode.
[0029] Effects of the Invention
[0030] For the positive electrode active material for lithium ion secondary battery of one embodiment of the present invention, by increasing the contact area with the non-aqueous electrolyte or solid electrolyte, and coating the composite oxide particles containing lithium transition metal with Li-containing metal composite oxide, the insertion and extraction of lithium ions on the interface can be further promoted, and its output characteristics can be improved. Therefore, since the lithium ion secondary battery of one embodiment of the present invention using the positive electrode active material for lithium ion secondary battery of the embodiment of the present invention is more excellent in durability and can provide high output characteristics, its industrial significance is significant, especially in the use of power supply for electric vehicles. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a SEM photograph of a cross section of secondary particles constituting the positive electrode active material for a lithium ion secondary battery of Example 1.
[0032] Figure 2 This is a SEM photograph of a cross section of secondary particles constituting the positive electrode active material for a lithium ion secondary battery of Example 2.
[0033] Figure 3 This is a SEM photograph of a cross section of secondary particles constituting the positive electrode active material for a lithium ion secondary battery of Comparative Example 1.
[0034] Figure 4 This is a schematic cross-sectional view of a 2032-type coin-shaped battery used in battery evaluation.
[0035] Figure 5 This is a measurement example of impedance evaluation.
[0036] Figure 6 This is a schematic diagram of the equivalent circuit used for analysis. DETAILED DESCRIPTION
[0037] 1. Positive electrode active material for lithium-ion secondary batteries
[0038] A positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention (hereinafter referred to as a "positive electrode active material") is characterized in that it has composite oxide particles containing a lithium transition metal (hereinafter referred to as "composite oxide particles") and a coating layer present on at least a portion of the surface of the composite oxide particles. In particular, the positive electrode active material for a lithium ion secondary battery according to this embodiment has the following requirements (1) to (6).
[0039] (1) Composite oxide particles
[0040] (1-a) Composition
[0041] The composite oxide particles have the general formula (A): Li 1+u Ni x Mn y Co z M1 t O 2 (wherein, -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0≤t≤0.1, M1 is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W) and a layered rock salt type crystal structure.
[0042] In the positive electrode active material of the present embodiment, the value of u representing the excess of lithium (Li) is in the range of -0.05 or more and 0.5 or less. Preferably, it is in the range of 0 or more and 0.50 or less, and more preferably in the range of 0 or more and 0.35 or less. By limiting the value of u to the above range, the output characteristics and battery capacity of a lithium ion secondary battery using the positive electrode active material as a positive electrode material can be improved. In contrast, when the value of u is less than -0.05, the positive electrode resistance of the secondary battery increases, and therefore, it is possible that the output characteristics cannot be improved. When the value of u is greater than 0.5, not only the initial discharge capacity is reduced, but also the positive electrode resistance is likely to increase.
[0043] Nickel (Ni) is an element that contributes to the high potential and high capacity of secondary batteries, and the value of x representing its content is in the range of more than 0.3 and less than 0.9. Preferably, it is in the range of more than 0.4 and less than 0.7, more preferably in the range of more than 0.4 and less than 0.6. When the value of x is less than 0.3, it is possible that the energy density of the secondary battery using the positive electrode active material cannot be fully improved. When the value of x is greater than 0.9, the content of other elements that improve output characteristics and durability is reduced, and it is possible that the characteristics as a positive electrode active material cannot be fully obtained.
[0044] Manganese (Mn) is an element that helps to improve thermal stability, and the value of y representing its content is in the range of 0 to 0.5. Preferably, it is in the range of 0.1 to 0.4. When the value of y is greater than 0.5, Mn dissolves from the positive electrode active material during high temperature operation, and sometimes the charge and discharge cycle characteristics deteriorate.
[0045] Cobalt (Co) is an element that helps improve charge-discharge cycle characteristics and output characteristics, and the value of z representing its content is in the range of 0 to 0.5. Preferably, it is in the range of 0.1 to 0.4. When the value of z is greater than 0.5, the initial discharge capacity of the secondary battery using the positive electrode active material is sometimes reduced.
[0046] In the positive electrode active material of the present embodiment, the additive element for further improving the durability and output characteristics of the secondary battery is basically present in the coating layer described later. However, in the positive electrode active material of the present embodiment, the following additive element M1 can also be present inside the composite oxide particles. As the additive element M1, one or more selected from magnesium (Mg), aluminum (Al), silicon (Si), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), zirconium (Zr), niobium (Nb), molybdenum (Mo), hafnium (Hf), tantalum (Ta) and tungsten (W) can be used.
[0047] The value of t representing the content of the added element M1 is in the range of 0 to 0.1. Preferably, it is in the range of 0.001 to 0.05. When the value of t is greater than 0.1, the battery capacity of the secondary battery is reduced due to the reduction of the metal elements that contribute to the redox reaction (Redox reaction). In addition, when the metal element M2 described later is also present in the coating layer, the total amount of M1 and M2 of the positive electrode active material as a whole is preferably 10 atomic % or less relative to the total number of atoms of Ni, Mn, Co, M1 and M2.
[0048] The composite oxide particles in this embodiment are preferably composed of a lithium-containing nickel-manganese-cobalt composite oxide (NMC) containing Ni, Mn, and Co as main transition metals. In this case, the composite oxide particles preferably have the general formula (B): Li 1+u Ni x Mn y Co z M1 t O 2 (-0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.7, 0.15≤y≤0.4, 0.15≤z≤0.4, 0≤t≤0.1, M1 is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W).
[0049] The compositions of the positive electrode active material and the composite oxide particles can be confirmed by performing Tewold analysis or the like on parameters obtained using inductively coupled plasma emission analysis or powder X-ray diffraction.
[0050] (1-b) Particle structure
[0051] In the positive electrode active material of the present embodiment, the composite oxide particles can be composed of primary particles or secondary particles formed by aggregation of a plurality of primary particles.
[0052] In particular, it is preferred that the composite oxide particles are composed of secondary particles formed by agglomeration of primary particles, wherein the secondary particles have an agglomeration portion, one or more communicating holes connected to the periphery of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connected to the communicating holes.
[0053] It is preferred that the two or more space portions communicate with the communicating hole or other space portions. It is also preferred that the number of the communicating holes is two or more.
[0054] Since the composite oxide particles have such a secondary particle structure, the particle properties of the positive electrode active material of the present embodiment described later can be easily achieved.
[0055] When the connecting hole of the peripheral part is not connected to the internal space part, the space part inside the particle is isolated, the electrolyte cannot fully invade the interior of the composite oxide particle (secondary particle), and sufficient reaction place cannot be ensured. Therefore, in the secondary battery using the positive electrode active material, the desired battery performance is sometimes not fully demonstrated. The two or more internal space parts can be directly connected to the connecting holes of the peripheral part respectively. Alternatively, it can also be connected to the connecting holes of the peripheral part via other connecting holes.
[0056] According to this structure, the electrolyte fully penetrates into the space inside the particle through the communicating holes in the outer periphery, and lithium can be extracted and inserted not only on the surface of the particle but also inside the particle, thereby ensuring sufficient reaction sites and significantly reducing the internal resistance of the battery.
[0057] Therefore, when a lithium ion secondary battery is constructed using a positive electrode active material having such a structure as a positive electrode material, the output characteristics can be further improved.
[0058] (2) Coating layer
[0059] The coating layer exists on at least a portion of the surface of the composite oxide particle. The coating layer is composed of fine particles and / or a coating of a metal composite oxide of Li and a metal element M2 (M2 is one or more metal elements selected from Al, Ti, Zr, Nb, Mo and W).
[0060] That is, in the positive electrode active material of this embodiment, a coating layer composed of fine particles and / or a coating of a metal composite oxide of Li and M2 exists on the surface of at least a portion of the composite oxide particle (or the secondary particle when composed of secondary particles).
[0061] The coating layer of the metal composite oxide of Li and M2 has high lithium ion conductivity and has the effect of promoting the movement of lithium ions. Therefore, by making the coating layer of the metal composite oxide of Li and M2 exist on the surface of the composite oxide particles, since a Li conduction path is formed at the interface between the composite oxide particles and the electrolyte, the reaction resistance (positive electrode resistance) of the positive electrode active material can be reduced and its output characteristics can be improved.
[0062] That is, by reducing the positive electrode resistance, the voltage lost in the secondary battery is reduced, and the voltage actually applied to the load side is relatively high, so a high output can be obtained. In addition, by increasing the voltage applied to the load side, lithium is fully inserted and removed from the positive electrode, so the battery capacity is also improved. Furthermore, since the load of the positive electrode active material during charging and discharging is also reduced due to the reduction in the positive electrode resistance, the cycle characteristics can also be improved.
[0063] The metal element M2 constituting the metal composite oxide together with Li is one or more selected from Al, Ti, Zr, Nb, Mo and W.
[0064] Among them, from the viewpoint of the effect of allowing the coating layer to exist, M2 is preferably W, and the metal composite oxide constituting the coating layer is preferably lithium tungstate.
[0065] In terms of improving the effect of the presence of the coating layer, the amount of the number of atoms of M2 in the coating layer is 0.1 atomic % or more and 1.5 atomic % or less relative to the total number of atoms of Ni, Co and Mn in the composite oxide particles (the number of atoms of M2 / (the number of atoms of Ni+the number of atoms of Co+the number of atoms of Mn)×100). It is preferably 0.1 atomic % or more and 1.0 atomic % or less, and more preferably 0.2 atomic % or more and 0.9 atomic % or less.
[0066] The composition of the coating layer can be confirmed by using inductively coupled plasma emission analysis, electron probe microanalyzer analysis, etc. The crystal structure of the coating layer can be confirmed by using powder X-ray diffraction or electron beam diffraction.
[0067] The coating layer can be in the form of particles and / or coatings of metal composite oxides of Li and M2. When the metal composite oxide of Li and M2 is composed of particles, the particle size of the particles is preferably in the range of 1 nm to 200 nm, preferably in the range of 1 nm to 100 nm. When the particle size of the particles is less than 1 nm, the particles sometimes do not have sufficient lithium ion conductivity. The upper limit of the particle size is about 200 nm. When the particle size of the particles is greater than 100 nm, due to the uneven formation of the coating of the particles, there is a tendency that the effect of reducing the reaction resistance cannot be fully obtained. Therefore, it is preferred that more than 50% of the total number of particles have a particle size in the range of 1 nm to 100 nm.
[0068] When the metal composite oxide of Li and M2 is composed of a coating, the thickness of the coating is preferably in the range of 1 nm or more and 200 nm or less. When the thickness is less than 1 nm, the coating sometimes does not have sufficient lithium ion conductivity. In addition, when the thickness is greater than 200 nm, the reaction area is reduced and the body resistance of the electrode is increased, and sometimes the effect of reducing the reaction resistance cannot be fully obtained.
[0069] Even when fine particles of a metal composite oxide of Li and M2 and a coating are present in a mixed state on the surface of the composite oxide particle, a high effect on battery characteristics can be obtained.
[0070] The coating layer of the metal composite oxide of Li and M2 can also be formed on the entire surface of the composite oxide particles. However, it is sufficient to form it on at least a portion of the composite oxide particles, or the coating layer can also be spread on the surface of the composite oxide particles. In this case, the effect of reducing the reaction resistance of the positive electrode active material can also be obtained due to the presence of the coating layer. However, it is preferred that the coating layer of the metal composite oxide of Li and M2 is uniformly present on the surface of the composite oxide particles.
[0071] The properties of the coating layer can be determined by, for example, cross-sectional observation using a field emission scanning electron microscope, cross-sectional element mapping using EDX analysis using a scanning transmission electron microscope (STEM), cross-sectional observation using a transmission electron microscope, or the like.
[0072] (3) Particle size
[0073] The composite oxide particles having a coating layer constituting the positive electrode active material of the present embodiment have a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, which is obtained from a particle size distribution measurement value.
[0074] More specifically, for the particle size of the positive electrode active material (composite oxide particles with a coating layer), the particle size d50 (when the total volume is set to 100% and the cumulative curve of the particle size distribution is obtained, the particle size of the cumulative curve is 50%), which is 50% of the total volume of all particles, is preferably 3.0 μm or more and 7.0 μm or less. d50 is preferably 4.0 μm or more and 6.5 μm or less, and more preferably 4.0 μm or more and 6.0 μm or less. If the d50 of the particles constituting the positive electrode active material is within the above range, not only can the battery capacity per unit volume of the secondary battery using the positive electrode active material be increased, but also the safety and output characteristics can be improved.
[0075] In contrast, when d50 is less than 3.0 μm, the filling property of the positive electrode active material is reduced, and the battery capacity per unit volume may not be increased. When d50 is greater than 7.0 μm, the reaction area of the positive electrode active material is reduced, and the interface with the electrolyte is reduced, so it may be difficult to improve the output characteristics.
[0076] (4) BET specific surface area
[0077] The composite oxide particles having a coating layer constituting the positive electrode active material of this embodiment have a thickness of 2.0 μm. 2 / g or more and 5.0m 2 / g or less BET specific surface area.
[0078] The BET specific surface area of the positive electrode active material of the present embodiment is an index indicating its particle properties (contact area with the electrolyte). When the positive electrode active material is composed of secondary particles having an agglomeration portion, one or more connected holes connected to the peripheral portion of the agglomeration portion, and two or more space portions present inside the agglomeration portion and connected to the connected holes, it represents the surface area of the connected holes (openings) present in the peripheral portion of the secondary particles and the microscopic cavities (space portions) inside the secondary particles.
[0079] The BET specific surface area is measured by the BET method based on nitrogen adsorption.
[0080] The BET specific surface area is preferably 2.5 m 2 / g or more and 4.5m 2 / g or less. The specific surface area of the positive electrode active material is less than 2.0m 2 When the specific surface area is greater than 5.0 m / g, the reaction area with the electrolyte cannot be sufficiently ensured in the case of constituting a secondary battery, and the output characteristics may not be sufficiently improved. 2 When the content is less than 1.34 N·g, the reaction area with the electrolyte is too large, and the durability of the secondary battery may be reduced.
[0081] (5) Tap density
[0082] The composite oxide particles having a coating layer constituting the positive electrode active material of this embodiment have a 1.0 g / cm 3 Above and 2.0g / cm 3 The following tap density.
[0083] The tap density is an index reflecting the density of the amount of solid region inside a spherical particle, for example.
[0084] Tap density less than 1.0g / cm 3 Even if the BET specific surface area is increased, the amount of solid area in the particles is small, and the durability of the secondary battery is sometimes reduced. There is no particular restriction on the upper limit of the tap density. In the present invention, when the positive electrode active material is composed of secondary particles having an agglomeration portion, one or more connecting holes connected to the peripheral portion of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connected to the connecting holes, the upper limit under normal manufacturing conditions is 2.0 g / cm 3 The tap density is preferably 1.0 g / cm 3 More preferably 1.2 g / cm 3 above.
[0085] The tap density refers to the bulk density after a sample powder collected in a container is tapped 100 times in accordance with JIS Z-2504, and can be measured using a vibration specific gravity meter.
[0086] (6) Oil absorption
[0087] The composite oxide particles having a coating layer constituting the positive electrode active material of the present embodiment have an oil absorption of 30 mL / 100 g or more and 60 mL / 100 g or less.
[0088] The oil absorption is an index that indicates the volume of the total space inside the particle (all cavities). The oil absorption is determined by following the steps described in "JIS K 6217-4:2008 (Carbon black for rubber - Basic properties - Part 4, Method for determining oil absorption (including compression specimens))". However, since the operation process is complicated, the oil absorption is usually determined using an oil absorption measuring device that is marketed in accordance with the above JIS. It should be noted that di-n-butyl phthalate (DBP) is used as the oil for measurement, and the measurement result is calculated from the oil absorption per 100g sample, so the unit is expressed in "mL / 100g".
[0089] When the oil absorption is less than 30 mL / 100 g, sufficient space cannot be formed, and sufficient BET specific surface area may not be obtained. On the other hand, when the absorption is greater than 60 mL / 100 g, there are more space inside the particles in the structure, the packing density is reduced and the filling property is reduced. When a secondary battery is formed, the battery capacity per unit volume may not be fully obtained. The oil absorption is preferably greater than 35 mL / 100 g and less than 55 mL / 100 g.
[0090] (7) Particle size distribution
[0091] Although optional, the composite oxide particles having a coating layer constituting the positive electrode active material of the present embodiment preferably have a particle size distribution width index [(d90-d10) / d50] of 1.0 or less, more preferably 0.7 or less, and further preferably 0.6 or less. Since the proportion of fine particles and coarse particles of the positive electrode active material having such a narrow particle size distribution is small, the secondary battery using the particles has excellent safety, cycle characteristics, and output characteristics.
[0092] When (d90-d10) / d50 is greater than 1.0, the proportion of fine particles and coarse particles in the positive electrode active material increases. For example, when the proportion of fine particles is large, local reaction of fine particles occurs, so the secondary battery is prone to heat, which not only reduces safety, but also sometimes leads to poor cycle characteristics due to selective degradation of fine particles. In addition, when the proportion of coarse particles is large, the reaction area between the electrolyte and the positive electrode active material cannot be fully ensured, and sometimes the output characteristics are poor.
[0093] In the case of industrial-scale production, it is not realistic to use a material with too small [(d90-d10) / d50] as a positive electrode active material. Therefore, considering cost and productivity, the lower limit of [(d90-d10) / d50] is preferably about 0.3.
[0094] It should be noted that the meaning and calculation method of d10 and d90 in the index [(d90-d10) / d50] representing the width of the particle size distribution are the same as those of the above-mentioned d50, d90 refers to the particle size at which the volume of each particle accumulated from the side with a smaller particle size is 90% of the total volume of all particles, and d10 refers to the particle size at which the volume of each particle accumulated from the side with a smaller particle size is 10% of the total volume of all particles.
[0095] (8)d90 / d10
[0096] Although optional, the composite oxide particles having a coating layer constituting the positive electrode active material of this embodiment preferably have a ratio of the d90 value obtained from the particle size distribution measurement value to the d10 value: d90 / d10 value of 1.0 to 2.0, more preferably 1.2 to 1.8.
[0097] If the d90 / d10 value of the particles constituting the positive electrode active material is within this range, not only can the battery capacity per unit volume of the secondary battery using the positive electrode active material be increased, but also the safety and output characteristics can be improved. When the d90 / d10 value is greater than 2.0, the reaction area of the positive electrode active material is reduced, and the interface with the electrolyte is reduced, so it may be difficult to improve the output characteristics.
[0098] (9) Crystallite size obtained from the X-ray diffraction pattern of the (003) plane
[0099] Although arbitrary, the composite oxide particles having a coating layer constituting the positive electrode active material of the present embodiment, when the crystallite size of the primary particles is calculated using the Scherrer equation based on the half-value width of the peak of the (003) plane based on X-ray diffraction, the crystallite size is preferably Above and The following ranges are more preferably Above and The following ranges are more preferably Above and The positive electrode active material having a crystallite diameter within the above range has extremely high crystallinity, and can reduce the positive electrode resistance of the secondary battery and improve its output characteristics.
[0100] The crystallite size of (003) surface is smaller than When the primary particles are fine, the pores between the primary particles in the positive electrode active material are too fine, and the electrolyte becomes difficult to penetrate into the positive electrode active material. Therefore, the reaction area with the electrolyte is reduced, and the output characteristics of the secondary battery are reduced. The crystallite size of the (003) plane is larger than When the primary particles become too coarse, the proportion of pores occupied by the secondary particles is extremely reduced, and the intrusion paths of the electrolyte are reduced. Therefore, the reaction area with the electrolyte is reduced, and the output characteristics of the secondary battery are reduced.
[0101] 2. Method for producing positive electrode active material for lithium ion secondary battery
[0102] The positive electrode active material according to the above embodiment of the present invention is not limited by its production method as long as it has the above-mentioned composition, crystal structure, particle structure, and particle properties.
[0103] However, by producing the positive electrode active material of the above-described embodiment by the production method described below, it is possible to easily produce the positive electrode active material having the above-described composition, crystal structure, particle structure, and particle properties.
[0104] Specifically, the positive electrode active material of the embodiment is obtained by the following process. That is, the oxidizing environment and the non-oxidizing environment in the crystallization process are switched to prepare composite hydroxide particles containing transition metals such as composite hydroxide particles containing nickel, manganese and cobalt, and the composite hydroxide particles and / or the heat-treated particles obtained by heat-treating the composite hydroxide particles are mixed with lithium compounds, and the obtained lithium mixture is calcined to obtain composite oxide particles containing lithium transition metals. Next, by mixing the composite oxide particles and the metal composite oxide of Li and M2 as the raw material of the coating layer and heat-treating them, a positive electrode active material consisting of composite oxide particles coated with the metal composite oxide of Li and M2 can be obtained.
[0105] Hereinafter, each step will be described in detail by taking as an example the case where the composite oxide particles are composite oxide particles containing lithium, nickel, manganese and cobalt.
[0106] (1) Crystallization process
[0107] Water, sodium hydroxide aqueous solution and ammonia water are supplied in appropriate amounts to the reaction tank to prepare an aqueous solution before reaction adjusted to a pH value of 11 or more and 13 or less at a liquid temperature of 25°C and an ammonium ion concentration of 9 g / L or more and 15 g / L or less. On the other hand, nickel sulfate, manganese sulfate and cobalt sulfate are preferably dissolved in water so that the molar ratio of each metal element (Ni, Co, Mn) satisfies the above formula (A), and the raw material aqueous solution is adjusted to 1.0 mol / L or more and 3.0 mol / L or less.
[0108] Then, by blowing in a gas having an oxygen concentration of less than 2% by volume such as argon or nitrogen in a non-oxidizing environment, the raw aqueous solution is supplied to the aqueous solution before the reaction to generate nuclei. At this time, preferably, sodium hydroxide aqueous solution and ammonia water are appropriately supplied to maintain the pH value and ammonium ion concentration of the aqueous solution for nucleation within the above range.
[0109] After the nucleation is completed, an acid such as sulfuric acid is added to adjust the pH value to be greater than 10 and less than 12 at a liquid temperature of 25°C and less than the pH value in the nucleation step to form an aqueous solution for particle growth. After confirming that the pH value is a specified value, the above-mentioned raw material aqueous solution is supplied to grow the nuclei (particles) generated in the nucleation step. In addition, when an aqueous solution containing a compound of the additive element M1 is prepared separately, the aqueous solution containing the compound of the additive element M1 can also be added only in the particle growth step or only in a specific stage of the particle growth step.
[0110] As the first stage of the particle growth, crystallization is continuously performed in a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less while stirring for a predetermined time using a stirrer from the start of the particle growth step.
[0111] As the second stage, while the supply of the raw material aqueous solution is continued, air or oxygen is circulated in the reaction tank using a diffuser tube having a pore size of 100 μm or more and 1 cm or less, and the reaction environment is adjusted to an oxidizing environment with an oxygen concentration of 21 volume % or more. After the start of the switching operation 1, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the oxidizing environment.
[0112] As the third stage, while the supply of the raw material aqueous solution is continued, a gas in a non-oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less, and switching operation 2 is performed. After the start of switching operation 2, crystallization is performed while maintaining the non-oxidizing environment and stirring for a predetermined time using a stirrer.
[0113] As the fourth stage, while the supply of the raw material aqueous solution is continued, the gas in the oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21 volume % or more. After the start of the switching operation 3, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the oxidizing environment.
[0114] As the fifth stage, while the supply of the raw material aqueous solution is continued, a gas in a non-oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less, and a switching operation 4 is performed. After the switching operation 4 is started, crystallization is performed while maintaining the non-oxidizing environment and stirring for a predetermined time using a stirrer.
[0115] The time of each stage in the particle growth step is second stage ≤ fourth stage < first stage ≤ third stage ≤ fifth stage. It is preferred that the crystallization time of the entire particle growth step be within 8 hours.
[0116] The particle growth process can also perform switching operations 5 and 6 in the same manner, setting the sixth stage in an oxidizing environment and the seventh stage in a non-oxidizing environment. Further, it is also possible to perform switching operations 7 and 8, setting the eighth stage in an oxidizing environment and the ninth stage in a non-oxidizing environment. It is also possible to perform switching operations 9 and 10 additionally, setting the tenth stage in an oxidizing environment and the eleventh stage in a non-oxidizing environment.
[0117] In these cases, the time of each stage in the particle growth process is also the second stage ≤ the fourth stage ≤ the sixth stage ≤ the eighth stage ≤ the tenth stage < the first stage ≤ the third stage ≤ the fifth stage ≤ the seventh stage ≤ the ninth stage ≤ the eleventh stage.
[0118] After the crystallization is completed, the obtained product is washed with water, filtered and dried, thereby obtaining predetermined nickel-manganese-cobalt-containing composite hydroxide particles.
[0119] In the particle growth step, it is preferred that the pH value and the ammonium ion concentration of the aqueous solution for particle growth be maintained within the above ranges by appropriately supplying the sodium hydroxide aqueous solution and the ammonia aqueous solution throughout the step.
[0120] The composite hydroxide particles obtained by the crystallization step have a particle structure in which a low-density layer and a high-density layer are stacked around a high-density center. By using the composite hydroxide particles having the particle structure as a precursor, it is easy to obtain composite oxide particles having a particle structure having an agglomeration portion, one or more connecting holes connected to the peripheral portion of the agglomeration portion, and one or more space portions existing inside the agglomeration portion and connected to the connecting holes.
[0121] (2) Mixing process
[0122] The mixing step is a step of mixing a lithium compound with the composite hydroxide particles and / or heat-treated particles obtained by heat-treating the composite hydroxide particles to obtain a lithium mixture.
[0123] In the mixing process, the composite hydroxide particles and / or the heat-treated particles are mixed with the lithium compound so that the ratio (Li / Me) of the sum of the number of atoms of metal atoms other than Li in the lithium mixture, specifically, Ni, Mn, Co and the added element M1 (Me) to the number of atoms of Li (Li) is 0.95 or more and 1.5 or less, preferably 1.0 or more and 1.5 or less, more preferably 1.0 or more and 1.35 or less, and further preferably 1.0 or more and 1.2 or less. That is, before and after the sintering process, since Li / Me does not change, it is necessary to mix the composite hydroxide particles and / or the heat-treated particles with the lithium compound so that the Li / Me in the mixing process is the Li / Me of the target positive electrode active material.
[0124] The lithium compound used in the mixing step is not particularly limited, but lithium hydroxide, lithium nitrate, lithium carbonate or a mixture thereof is preferably used from the perspective of availability. In particular, lithium hydroxide or lithium carbonate is preferably used in consideration of the ease of handling and quality stability.
[0125] For mixing, a common mixer can be used, for example, a vibration mixer, a Lodyga mixer, a Julia mixer, a V-blender, etc. can be used.
[0126] (3) Pre-burning process
[0127] When lithium hydroxide or lithium carbonate is used as the lithium compound, a calcination step of calcining the lithium mixture at a temperature lower than the calcination temperature described later and at 350° C. to 800° C., preferably 450° C. to 750° C., can be performed after the mixing step and before the calcination step. This allows Li to be sufficiently diffused in the composite hydroxide particles, and more uniform composite oxide particles can be obtained.
[0128] In addition, the holding time under the above temperature conditions is preferably 1 hour or more and 10 hours or less, more preferably 3 hours or more and 6 hours or less. In addition, the environment in the calcining step is preferably an oxidizing environment as in the calcining step described later, more preferably an environment with an oxygen concentration of 18 volume % or more and 100 volume % or less.
[0129] (4) Firing process
[0130] The calcining step is a step of calcining the lithium mixture obtained in the mixing step under predetermined conditions to diffuse and react Li in the composite hydroxide particles and / or the heat-treated particles to obtain composite oxide particles.
[0131] The furnace used in the sintering process is not particularly limited, as long as the lithium mixture can be heated in the atmosphere or oxygen flow. However, from the viewpoint of uniformly maintaining the environment in the furnace, an electric furnace that does not generate gas is preferably used, and any of intermittent or continuous electric furnaces can be used. In this regard, the same is true for the furnaces used in the heat treatment process and the pre-sintering process.
[0132] a) Firing temperature
[0133] The calcination temperature of the lithium mixture is set to be above 720°C and below 940°C. When the calcination temperature is less than 720°C, the composite hydroxide particles and / or heat-treated particles cannot fully react with Li, and the remaining Li, unreacted composite hydroxide particles and / or heat-treated particles remain, or the obtained positive electrode active material has insufficient crystallinity. On the other hand, when the calcination temperature is greater than 940°C, the interconnecting pores and space portions within the composite oxide particles are broken, which may lead to a decrease in the BET specific surface area of the final positive electrode active material, a decrease in oil absorption, and an increase in tap density. In addition, the particles of the positive electrode active material are violently sintered, causing abnormal grain growth, and the proportion of amorphous coarse particles increases.
[0134] By controlling the calcination temperature, the BET specific surface area, oil absorption, tap density, and 50% cumulative diameter d50 obtained from the particle size distribution measurement value can be controlled. From the viewpoint of controlling the BET specific surface area, oil absorption, tap density, and 50% cumulative diameter d50 obtained from the particle size distribution measurement value of the positive electrode active material, the calcination temperature of the lithium mixture is preferably set to 730°C or more and 920°C or less, and more preferably set to 750°C or more and 900°C or less.
[0135] The heating rate in the calcining process is preferably set to 1°C / min or more and 10°C / min or less, and more preferably set to 3°C / min or more and 8°C / min or less. Further, in the calcining process, it is more preferred to reduce the heating rate at a temperature near the melting point of the lithium compound and set it to 0.3°C / min or more and 6°C / min or less. Thus, the composite hydroxide particles and / or heat-treated particles can react with Li more uniformly.
[0136] b) Firing time
[0137] In the sintering time, the holding time under the above-mentioned sintering temperature condition is preferably set to at least 2 hours, more preferably set to more than 3 hours and less than 20 hours. When the holding time under the sintering temperature condition is less than 2 hours, Li cannot be fully diffused in the composite hydroxide particles and / or the heat-treated particles, and the remaining Li, unreacted composite hydroxide particles and / or heat-treated particles may remain or the crystallinity of the obtained positive electrode active material may be insufficient.
[0138] c) Firing environment
[0139] The environment during firing is preferably set to an oxidizing environment, more preferably set to an environment with an oxygen concentration of 18% by volume or more and 100% by volume or less, and further preferably set to an environment with an oxygen concentration of 50% by volume or more and 100% by volume or less. It is particularly preferred to set it to a mixed gas environment of oxygen and an inert gas at the above oxygen concentration. That is, firing is preferably carried out in the atmosphere or an oxygen flow. When the oxygen concentration is less than 18% by volume, the crystallinity of the positive electrode active material may be insufficient.
[0140] (5) Crushing process
[0141] In the case where the composite oxide particles obtained by the sintering process are particularly secondary particles, agglomeration or mild sintering may sometimes occur. In this case, it is preferred to crush the agglomerate or sintered body. Thus, the average particle size and particle size distribution of the obtained positive electrode active material can be adjusted to a suitable range. It should be noted that crushing refers to the operation of applying mechanical energy to an agglomerate composed of a plurality of particles generated under the action of sintering necks between particles during sintering, so as to separate them without substantially destroying the particles themselves, thereby loosening the agglomerate.
[0142] As a crushing method, a known method can be used, for example, a pin mill, a hammer mill, etc. It should be noted that at this time, it is preferable to adjust the crushing force to an appropriate range so as not to destroy the particles themselves (secondary particles themselves).
[0143] As described above, by adjusting the sintering conditions, the BET specific surface area, oil absorption, tap density and 50% cumulative diameter d50 calculated from the particle size distribution measurement value of the composite oxide particles can be controlled, and ultimately a positive electrode active material of one embodiment of the present invention having specified particle properties can be easily obtained.
[0144] (6) Coating process
[0145] The coating step is to mix and stir the composite oxide particles and the metal element M2 as a raw material of the coating layer, i.e., an oxide of one or more metals selected from Al, Ti, Zr, Nb, Mo and W, while spraying an aqueous solution or an acidic aqueous solution containing ammonium, etc., and heat-treating. By such a treatment, a coating layer composed of fine particles and / or a film of a metal composite oxide of Li and M2 is formed on at least a portion of the surface of the composite oxide particles.
[0146] In mixing and stirring, a common stirrer can be used. For example, a vibration mixer, a drum stirrer, a vacuum mixing dryer, etc. can be used. The stirring is performed under the condition that the composite oxide particles and the oxide of M2 can be fully mixed to a degree that the skeleton of the composite oxide particles is not destroyed. However, by only stirring the composite oxide particles and the oxide of M2, it is difficult for the oxide of M2, which is the raw material of the coating layer, and the lithium compound present on the surface of the composite oxide particles to react, so it is preferred to stir while spraying water, an alkaline aqueous solution or an acidic aqueous solution appropriately.
[0147] If stirring is performed at room temperature, the oxide of M2 and the lithium compound may not react sufficiently. Therefore, it is preferred to perform a heat treatment at a temperature of 100° C. to 250° C. for 1 hour or more while stirring or after stirring.
[0148] In addition, the coating layer is composed of particles and / or a film of a metal composite oxide of Li and M2 as described above. Whether to form either particles or a film or both is determined by the moisture content of the dehydrated powder. Therefore, by adjusting the moisture content of the dehydrated powder according to the composition of the metal composite oxide of Li and M2, the desired coating layer structure can be obtained.
[0149] Relative to the total number of atoms of Ni, Co and Mn contained in the mixed composite oxide powder, the amount of the metal element M2 contained in the coating layer is preferably greater than 0.1 atomic % and less than 1.5 atomic %. Thus, it is possible to have both high output characteristics and durability. When the amount of M2 contained in the coating layer is less than 0.1 atomic %, the effect of improving the output characteristics may not be fully obtained. When the amount of M2 contained in the coating layer is greater than 1.5 atomic %, there are too many metal composite oxides of Li and M2, and the Li conduction of the positive electrode active material and the electrolyte is inhibited, which may reduce the battery performance. Relative to the total number of atoms of Ni, Co and Mn contained in the composite oxide particles, the amount of M2 contained in the coating layer is more preferably greater than 0.15 atomic % and less than 1.4 atomic %.
[0150] 3. Lithium-ion secondary battery
[0151] The lithium ion secondary battery of one embodiment of the present invention can adopt the same structure as a general non-aqueous electrolyte secondary battery having components such as a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte. Alternatively, the lithium ion secondary battery of one embodiment of the present invention can adopt the same structure as a general solid electrolyte secondary battery having components such as a positive electrode, a negative electrode and a solid electrolyte. That is, as long as it is a secondary battery that is charged and discharged by the extraction and insertion of lithium ions, the present invention can be widely applied to non-aqueous electrolyte secondary batteries to all-solid lithium ion secondary batteries. It should be noted that the embodiments described below are merely examples, and the present invention can be applied to lithium ion secondary batteries that have implemented various changes and improvements according to the embodiments described in this specification.
[0152] (1) Components
[0153] a) Positive electrode
[0154] A positive electrode of a lithium ion secondary battery is produced using the positive electrode active material according to one embodiment of the present invention, for example, as follows.
[0155] First, a conductive material and a binder are mixed in the positive active material of the present embodiment, and activated carbon, viscosity adjustment and other solvents are further added as needed, and these are mixed to manufacture a positive composite material paste. At this time, each mixing ratio in the positive composite material paste is also an important factor in determining the performance of a lithium ion secondary battery. For example, when the solid content of the positive composite material from which the solvent is removed is set to 100 parts by mass, similarly to the positive electrode of a general lithium ion secondary battery, the content of the positive active material can be set to more than 60 parts by mass and less than 95 parts by mass, the content of the conductive material is set to more than 1 part by mass and less than 20 parts by mass, and the content of the binder is set to more than 1 part by mass and less than 20 parts by mass.
[0156] The obtained positive electrode composite material paste is applied to the surface of a collector made of aluminum foil, for example, and dried to disperse the solvent. As needed, it is sometimes pressed by a roller press or the like to increase the electrode density. In this way, a sheet positive electrode can be prepared. The sheet positive electrode can be cut into appropriate sizes according to the target battery and used in the preparation of a secondary battery. It should be noted that the method for manufacturing the positive electrode is not limited to the method exemplified above, and other methods can also be used.
[0157] As the conductive material, for example, carbon black materials such as graphite (natural graphite, artificial graphite, expanded graphite, etc.), acetylene black, and Ketjen black can be used.
[0158] The binder has the function of linking the active material particles to prevent them from falling off, and for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene-propylene-diene rubber, styrene-butadiene, cellulose resin or polyacrylic acid can be used.
[0159] In addition, a solvent that disperses the positive active material, the conductive material and the activated carbon and dissolves the binder can be added to the positive composite material as required. As a solvent, specifically, organic solvents such as N-methyl-2-pyrrolidone can be used. In addition, in the positive composite material, activated carbon can also be added in order to increase the double electric layer capacity.
[0160] b) Negative electrode
[0161] In the negative electrode, metallic lithium, lithium alloy, etc. can be used. In addition, the negative electrode formed by mixing a binder in a negative electrode active material capable of absorbing and desorbing lithium ions, adding a suitable solvent, and preparing a paste-like negative electrode composite material, applying the negative electrode composite material to the surface of a metal foil collector such as copper, and drying it, and compressing it as needed to increase the electrode density to form a negative electrode.
[0162] As the negative electrode active material, for example, lithium-containing materials such as metallic lithium and lithium alloys, natural graphite, artificial graphite, sintered organic compounds such as phenolic resins, and carbon material powders such as coke that can absorb and release lithium ions can be used. In this case, as the negative electrode binder, fluorine-containing resins such as PVDF, which are the same as those of the positive electrode, can be used, and as solvents for dispersing these negative electrode active materials and binders, organic solvents such as N-methyl-2-pyrrolidone can be used.
[0163] c) Spacer
[0164] The separator is sandwiched between the positive electrode and the negative electrode in the lithium ion secondary battery, and has the function of separating the positive electrode from the negative electrode and retaining the electrolyte. As such a separator, for example, a film having many micropores in a film such as polyethylene or polypropylene can be used, but there is no particular limitation as long as it has the above-mentioned function. In addition, a solid electrolyte can also be used.
[0165] d) Electrolytes
[0166] As the nonaqueous electrolyte used in the nonaqueous electrolyte secondary battery, a nonaqueous electrolytic solution prepared by dissolving a lithium salt as a supporting salt in an organic solvent or the like is used.
[0167] As the organic solvent for the non-aqueous electrolyte, one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and propylene trifluorocarbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as methyl ethyl sulfone and butane sultone; phosphorus compounds such as triethyl phosphate and trioctyl phosphate, etc. can be used alone, or two or more selected from the group consisting of the following can be used in combination.
[0168] As a supporting salt, LiPF can be used 6 , LiBF 4 、LiClO 4 、LiAsF 6 、LiN(CF 3 SO 2 ) 2 And their compound salts, etc.
[0169] Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, and the like.
[0170] Solid electrolytes used in solid electrolyte secondary batteries such as all-solid lithium ion secondary batteries have the property of withstanding high voltages. Solid electrolytes include inorganic solid electrolytes and organic solid electrolytes.
[0171] As the oxide solid electrolyte, an oxide containing oxygen (O) and having lithium ion conductivity and electronic insulation can be used, for example, Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , Li 3 PO 4 , Li 3 PO 4 N X 、LiBO 2 N X 、LiNbO 3 、LiTaO 3 , Li 2 SiO 3 , Li 4 SiO 4 -Li 3 PO 4 , Li 4 SiO 4 -Li 3 VO 4 , Li 2 OB 2 O 3 -P 2 O5 , Li 2 O-SiO 2 , Li 2 OB 2 O 3 -ZnO, Li 1+X Al X Ti 2-X (PO 4 ) 3 (0≤X≤1), Li 1+X Al X Ge 2-X (PO 4 ) 3 (0≤X≤1), LiTi 2 (PO 4 ) 3 , Li 3X La 2 / 3-X TiO 3 (0≤X≤2 / 3), Li 5 La 3 Ta 2 O 12 , Li 7 La 3 Zr 2 O 12 , Li 6 BaLa 2 Ta 2 O 12 , Li 3.6 Si 0.6 P 0.4 O 4 wait.
[0172] As the sulfide solid electrolyte, a sulfide containing sulfur (S) and having lithium ion conductivity and electronic insulation can be used, for example, Li 2 S-SiS 2 , Li 2 SP 2 S 5 、LiI-Li 2 S-SiS 2 、LiI-Li 2 SP 2 S 5 、LiI-Li 2 SB 2 S 3 , Li 3 PO 4 -Li 2 S-Si 2 S. Li 3 PO 4 -Li2 S-SiS 2 、LiPO 4 -Li 2 S-SiS、LiI-Li 2 SP 2 O 5 、LiI-Li 3 PO 4 -P 2 S 5 wait.
[0173] As an inorganic solid electrolyte other than an oxide solid electrolyte and a sulfide solid electrolyte, for example, Li 3 N, LiI, Li 3 N-LiI-LiOH, etc.
[0174] As the organic solid electrolyte, a polymer compound exhibiting ion conductivity can be used, for example, polyethylene oxide, polypropylene oxide, copolymers thereof, etc. can be used. In addition, the organic solid electrolyte can include a supporting salt (lithium salt).
[0175] In addition, when a solid electrolyte is used, the solid electrolyte may be mixed with the positive electrode material in order to ensure contact between the electrolyte and the positive electrode active material.
[0176] (2) Structure of lithium-ion secondary battery
[0177] There is no particular limitation on the composition of the lithium-ion secondary battery, and the structure composed of the positive electrode, negative electrode, separator, non-aqueous electrolyte, etc. in the non-aqueous electrolyte secondary battery can be adopted; the structure composed of the positive electrode, negative electrode, solid electrolyte, etc. in the solid electrolyte secondary battery can be adopted. In addition, there is no particular limitation on the shape of the secondary battery, and various shapes such as cylindrical and stacked can be adopted.
[0178] In the case of a non-aqueous electrolyte secondary battery, for example, the positive electrode and the negative electrode are stacked with a separator to form an electrode body, the non-aqueous electrolyte is impregnated in the obtained electrode body, and the positive electrode collector and the positive terminal connected to the outside and the negative electrode collector and the negative terminal connected to the outside are connected using a collector lead or the like, and are sealed in a battery case to complete a lithium-ion secondary battery.
[0179] (3) Characteristics of lithium-ion secondary batteries
[0180] As described above, the lithium ion secondary battery of the present embodiment uses the positive electrode active material of one embodiment of the present invention as a positive electrode material, and therefore has excellent output characteristics and durability.
[0181] (4) Applications of lithium-ion secondary batteries
[0182] As described above, the lithium ion secondary battery of the present embodiment is excellent in output characteristics and durability, and can be suitably used as a power source for electric tools and environmentally friendly vehicles that require high levels of these characteristics.
[0183] Example
[0184] An example of one embodiment of the present invention is described in detail below using examples and comparative examples. During the entire process of the nucleation step and the particle growth step, the pH value of the reaction aqueous solution is measured by a pH controller, and the supply amount of the sodium hydroxide aqueous solution is adjusted according to the measured value, so that the pH value of the reaction aqueous solution in each step is controlled to fluctuate within the range of ±0.2.
[0185] (Example 1)
[0186] a) Production of composite hydroxides
[0187] [Nucleation process]
[0188] First, 17 L of water was added to the reaction tank and stirred while the temperature in the tank was set to 40° C. At this time, nitrogen gas was circulated in the reaction tank for 1 hour to set the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less. Next, 25% by mass of sodium hydroxide aqueous solution and 25% by mass of ammonia water were appropriately supplied to the reaction tank to adjust the pH value to 12.6 at a liquid temperature of 25° C. and the ammonium ion concentration to 10 g / L, thereby forming a pre-reaction aqueous solution.
[0189] Meanwhile, nickel sulfate, manganese sulfate, and cobalt sulfate were dissolved in water so that the molar ratio of each metal element was Ni:Co:Mn=5:2:3, and a 2 mol / L raw material aqueous solution was prepared.
[0190] Then, the raw material aqueous solution was supplied to the aqueous solution before the reaction at 115 mL / min to form an aqueous solution for nucleation, and nucleation was performed for 1 minute. At this time, 25% by mass of sodium hydroxide aqueous solution and 25% by mass of ammonia water were appropriately supplied to maintain the pH value and ammonium ion concentration of the aqueous solution for nucleation within the above range.
[0191] [Particle Growth Process]
[0192] After the nucleation step is completed, the supply of all aqueous solutions is temporarily stopped, and sulfuric acid is added to adjust the pH to 11.0 at a liquid temperature of 25°C to form an aqueous solution for particle growth. After confirming that the pH value is a predetermined value, the raw material aqueous solution is supplied at the same 100 mL / min and predetermined ratio as in the nucleation step to grow the nuclei (particles) generated in the nucleation step.
[0193] As the first stage, crystallization was performed in a non-oxidizing environment with an oxygen concentration of 2% by volume or less for 35 minutes from the start of the particle growth step while stirring using a stirrer.
[0194] As the second stage, while the raw material aqueous solution was continuously supplied, air was circulated in the reaction tank using a SUS diffuser tube with a pore size of 1.0 mm to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21 volume % (switching operation 1). After switching operation 1, crystallization was performed for 20 minutes while stirring with a stirrer.
[0195] As the third stage, nitrogen was circulated in the reaction tank using a diffuser while the supply of the raw material aqueous solution was continued, and the reaction environment was adjusted to a non-oxidizing environment with an oxygen concentration of 2% by volume or less (switching operation 2). After switching operation 2 was started, crystallization was performed for 65 minutes while stirring with a stirrer.
[0196] As the fourth stage, air was circulated in the reaction tank using a diffuser while continuing to supply the raw material aqueous solution to adjust to an oxidizing atmosphere with an oxygen concentration of 21 volume % (switching operation 3). After starting switching operation 3, crystallization was performed for 40 minutes while stirring with a stirrer.
[0197] As the fifth stage, nitrogen was circulated in the reaction tank using a diffuser while the supply of the raw material aqueous solution was continued, and the reaction environment was adjusted to a non-oxidizing environment with an oxygen concentration of 2% by volume or less (switching operation 4). After the switching operation 4 was started, crystallization was performed for 110 minutes while stirring with a stirrer.
[0198] Next, the particle growth step is terminated by stopping the supply of all aqueous solutions including the raw material aqueous solution. The obtained product is washed with water, filtered, and dried to obtain composite hydroxide particles.
[0199] In the particle growth step, 25 mass % sodium hydroxide aqueous solution and 25 mass % ammonia water were appropriately supplied throughout the step to maintain the pH value and ammonium ion concentration of the aqueous solution for particle growth within the above ranges.
[0200] b) Production of positive electrode active material
[0201] The obtained composite hydroxide and lithium hydroxide were fully mixed with a vibration mixer so that Li / Me became 1.10, thereby obtaining a lithium mixture (mixing step).
[0202] The lithium mixture was heated to 920° C. at a heating rate of 1.3° C. / min in an oxygen atmosphere (oxygen concentration: 100% by volume), maintained at this temperature for 3 hours to be fired, and cooled to room temperature (firing step).
[0203] In order to eliminate aggregation or light sintering of the obtained lithium-transition metal-containing composite oxide particles, the positive electrode active material is crushed (crushing step).
[0204] Next, while using a mixing agitator to fully stir 0.8 mass % of tungsten oxide relative to the mass of the composite oxide particles containing lithium transition metals and the composite oxide particles, 10 mass % of water (pure water) relative to the mass of the composite oxide particles is sprayed on the surface of the composite oxide particles, and then, the surface is heated at 150°C for 1 hour to perform surface treatment (coating process).
[0205] c) Evaluation of positive electrode active materials
[0206] [composition]
[0207] The composition of the positive electrode active material and the W in the coating layer were analyzed using an ICP emission spectrometer (manufactured by Shimadzu Corporation, ICPE-9000). The W content was 0.4 atomic %.
[0208] [Particle size distribution]
[0209] The 50% cumulative diameter d50, 10% cumulative diameter d10 and 90% cumulative diameter d90 obtained from the particle size distribution measurement value of the positive electrode active material were measured using a laser diffraction scattering particle size analyzer (Microtrac BEL Corp., Japan, Microtrac MT3300EXII).
[0210] [BET specific surface area and tap density]
[0211] The BET specific surface area was measured using a flow-type gas adsorption specific surface area measuring apparatus (Macsorb 1200 series, manufactured by Mountech Co., Ltd.), and the tap density was measured using a tapping machine (KRS-406, manufactured by Kurachi Scientific Instruments Mfg. Co., Ltd.).
[0212] [Oil absorption]
[0213] The oil absorption of di-n-butyl phthalate (DBP) was measured using an absorption measuring device (S-500, manufactured by Asahi Soken Co., Ltd.) in accordance with "JIS K 6217-4: 2008".
[0214] [Particle structure]
[0215] A portion of the positive electrode active material was embedded in the resin, processed by cross-section polishing (manufactured by JEOL Ltd., IB-19530CP) to make the cross section observable, and then observed by SEM (FE-SEM: manufactured by JEOL Ltd., JSM-6360LA). Figure 1 As shown, it was confirmed that the positive electrode active material of Example 1 was formed by secondary particles formed by the aggregation of multiple primary particles, with about 6 connecting holes in the periphery of the secondary particles and about 10 space portions inside the secondary particles, and the connecting holes in the periphery were connected to the internal void portions.
[0216] [Identification of coating layer]
[0217] The coating layer was identified by using BL19B2 of SPring8 (large synchrotron radiation facility) to perform radioactive powder X-ray diffraction measurement and electron beam diffraction using a transmission electron microscope.
[0218] d) Manufacturing of secondary batteries
[0219] Made Figure 4 Specifically, 52.5 mg of the positive electrode active material obtained as described above, 15 mg of acetylene black and 7.5 mg of PTFE were mixed and press-molded at a pressure of 100 MPa into a shape of 11 mm in diameter and 100 μm in thickness to produce the positive electrode 1.
[0220] Then, a 2032-type coin-shaped battery using the positive electrode 1 was manufactured in a glove box in an Ar environment with a dew point of -60°C. As the negative electrode 2 of the 2032-type coin-shaped battery, lithium metal with a diameter of 14 mm and a thickness of 1 mm was used, and as the non-aqueous electrolyte, 1 M LiClO 4 An equal amount of a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) (manufactured by Ube Industries, Ltd.) was used as a supporting electrolyte. In addition, a polyethylene porous film with a film thickness of 25 μm was used as a separator 3. As described above, a 2032-type coin-shaped battery 10 having a sealing gasket 4 and a corrugated gasket 5, and having a positive electrode can 6 and a negative electrode can 7 was assembled.
[0221] e) Battery evaluation
[0222] [Positive electrode resistance]
[0223] The positive electrode resistance was measured by charging a 2032-type coin-type battery at 3.8 V using an impedance measurement method and measuring it by an AC impedance method using a frequency response analyzer and a constant current potentiostat (Solartron, 1255B). Figure 5The impedance spectrum shown in Figure 1 is shown in Figure 1. Since two semicircles are observed in the high-frequency and medium-frequency regions and a straight line is observed in the low-frequency region in the obtained impedance spectrum, it is possible to construct Figure 6 The equivalent circuit shown in the figure is used to analyze the positive electrode interface resistance. Here, Rs represents the bulk resistance, R 1 Represents the positive electrode film resistance, R ct represents electrolyte / positive electrode interface resistance, W represents Warburg component, CPE1 and CPE2 represent constant phase elements, and the positive electrode active material of Comparative Example 1 described later is used as a reference to show the resistance reduction rate of the positive electrode interface resistance relative to the reference.
[0224] The overall composition and properties of the obtained positive electrode active material and the properties of the obtained lithium ion secondary battery are shown in Table 1. In addition, these properties of Example 2, Example 3 and Comparative Example 1 are also shown in Table 1 in the same manner.
[0225] (Example 2)
[0226] A positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that the lithium mixture was heated to 890° C. and kept at that temperature for 3 hours for calcination. Figure 2 The particle structure of the obtained positive electrode active material is shown. It is confirmed that the positive electrode active material of Example 2 is formed by secondary particles formed by agglomeration of a plurality of primary particles, has about 8 connected holes in the peripheral portion of the secondary particles, has about 14 voids in the interior of the secondary particles, and the connected holes in the peripheral portion are connected to the voids in the interior.
[0227] (Example 3)
[0228] A positive electrode active material was obtained and evaluated in the same manner as in Example 2 except that the mass of tungsten oxide treated in the coating step was 0.4 mass %. The W content was 0.2 atomic %.
[0229] (Comparative Example 1)
[0230] The positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that in the crystallization process, the oxidizing environment was adjusted to an oxygen concentration of 21 volume % for crystallization until the switching operation 1 of the nucleation process and the particle growth process, and thereafter the oxygen concentration was adjusted to a non-oxidizing environment of less than 2 volume % to obtain a composite hydroxide. Figure 3 The particle structure of the obtained positive electrode active material is shown. It is confirmed that it is formed by secondary particles formed by agglomeration of multiple primary particles, has one connecting hole in the peripheral part of the secondary particle, has one space part inside the secondary particle, and is composed of a hollow structure connected by the connecting hole in the peripheral part and the internal space part.
[0231] Table 1
[0232]
[0233] It was confirmed that, when the positive electrode active materials of Examples 1 to 3 within the scope of the present invention were used in lithium ion secondary batteries, the positive electrode resistance was reduced and the output characteristics were improved compared to Comparative Example 1.
[0234] Description of Reference Numerals
[0235] 1: positive electrode (electrode for evaluation); 2: negative electrode; 3: separator; 4: sealing gasket; 5: corrugated gasket; 6: positive electrode can; 7: negative electrode can; 10: coin-type battery.
Claims
1. A positive electrode active material for a lithium ion secondary battery, in, The positive electrode active material for lithium ion secondary battery has: A lithium-transition metal-containing composite oxide particle, wherein the lithium-transition metal-containing composite oxide particle has a general formula (A): Li 1+u Ni x Mn y Co z M1 t O 2 The composition and layered rock salt type crystal structure represented by the general formula (A) are as follows: -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0≤t≤0.1, and M1 is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W; as well as a coating layer, the coating layer being present on at least a portion of the surface of the lithium-transition metal-containing composite oxide particle and being composed of fine particles and / or a coating of a metal composite oxide of Li and a metal element M2, wherein M2 is one or more metal elements selected from Al, Ti, Zr, Nb, Mo and W, The lithium-transition metal-containing composite oxide particles having the coating layer have a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, as determined from a particle size distribution measurement value, and a 2.0 μm or less cumulative diameter. 2 / g or more and 5.0m 2 / g or less, BET specific surface area 1.0g / cm 3 Above and 2.0g / cm 3 The tap density is 30 mL / 100 g or more and 60 mL / 100 g or less and the oil absorption is determined by following the procedure described in JIS K6217-4:2008. Furthermore, the amount of M2 contained in the coating layer is greater than or equal to 0.1 atomic % and less than or equal to 1.5 atomic % relative to the total number of atoms of Ni, Mn, and Co contained in the lithium-transition metal-containing composite oxide particle.
2. The positive electrode active material for lithium ion secondary battery according to claim 1, in, The 50% cumulative diameter d50 of the lithium-transition metal-containing composite oxide particles having the coating layer, which is obtained from the particle size distribution measurement value, is 4.0 μm or more and 6.0 μm or less.
3. The positive electrode active material for lithium ion secondary battery according to claim 1, in, The index [(d90-d10) / d50] representing the width of the particle size distribution of the lithium transition metal-containing composite oxide particles having the coating layer is less than 1.0, wherein d10 is the 10% cumulative diameter calculated based on the particle size distribution measurement value, and d90 is the 90% cumulative diameter calculated based on the particle size distribution measurement value.
4. The positive electrode active material for lithium ion secondary battery according to claim 2, in, The index [(d90-d10) / d50] representing the width of the particle size distribution of the lithium transition metal-containing composite oxide particles having the coating layer is less than 1.0, wherein d10 is the 10% cumulative diameter calculated based on the particle size distribution measurement value, and d90 is the 90% cumulative diameter calculated based on the particle size distribution measurement value.
5. The positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 4, in, The d90 / d10 value of the lithium transition metal-containing composite oxide particles having the coating layer is 1.0 or more and 2.0 or less, d10 being a 10% cumulative diameter obtained from the particle size distribution measurement value, and d90 being a 90% cumulative diameter obtained from the particle size distribution measurement value.
6. The positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 4, in, The lithium-transition metal-containing composite oxide particles are composed of secondary particles formed by agglomeration of primary particles, and the secondary particles have an agglomeration portion, one or more communicating holes communicating with the peripheral portion of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and communicating with the communicating holes.
7. The positive electrode active material for lithium ion secondary battery according to claim 5, in, The lithium-transition metal-containing composite oxide particles are composed of secondary particles formed by agglomeration of primary particles, and the secondary particles have an agglomeration portion, one or more communicating holes communicating with the peripheral portion of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and communicating with the communicating holes.
8. The positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 4, in, The M2 contained in the coating layer is W.
9. The positive electrode active material for lithium ion secondary battery according to claim 5, in, The M2 contained in the coating layer is W.
10. The positive electrode active material for lithium ion secondary battery according to claim 6, in, The M2 contained in the coating layer is W.
11. The positive electrode active material for lithium ion secondary battery according to claim 8, in, The metal composite oxide is lithium tungstate.
12. The positive electrode active material for lithium ion secondary battery according to claim 9, in, The metal composite oxide is lithium tungstate.
13. The positive electrode active material for lithium ion secondary battery according to claim 10, in, The metal composite oxide is lithium tungstate.
14. A lithium ion secondary battery, in, The lithium ion secondary battery comprises a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte or a positive electrode, a negative electrode and a solid electrolyte. As the positive electrode active material used for the positive electrode, the positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 13 is used.