A method for comprehensive utilization of carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene
Through the separation and polymerization process, polydicyclopentadiene is prepared by using a mixture of cyclopentadiene and methylcyclopentadiene, which solves the problems of low utilization rate of carbon nine-carbon ten-decimal fraction and complex separation process, and achieves high efficiency of carbon Comprehensive utilization of nine-carbon ten-fraction and product performance improvement.
Patent Information
- Application Number
- CN202011178988.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-10-29
AI Technical Summary
In the prior art, the utilization route of carbon nine-carbon ten-fraction is relatively long, the separation process is complex and the economic benefits are low, making it difficult to improve the comprehensive utilization rate of carbon nine-carbon ten-fraction.
Through a series of separation and polymerization processes, polydicyclopentadiene is prepared by polymerizing a mixture of cyclopentadiene and methylcyclopentadiene, avoiding the requirement of separation purity, simplifying the process flow and improving economic benefits.
The production of a variety of products has been achieved, the comprehensive utilization rate of carbon nine-carbon ten-fraction is improved, the separation difficulty and material loss is reduced, and the obtained products are uniform and tight and have excellent mechanical properties.
Smart Images

Figure CN114426445B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of separation and recovery of petrochemical cracking by-products, and specifically relates to a method for comprehensively utilizing carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene through separation and polymerization processes. Background Art
[0002] The carbon nine carbon ten fraction is the remaining fraction after extracting and separating the C5 fraction and C6-C8 fraction from the byproducts of naphtha or light diesel cracking, accounting for about 10%-20% of the ethylene production. The C9-C10 fraction has a complex composition, with about 150 components. This fraction mainly contains aromatics above C9, styrene, methyl styrene, dicyclopentadiene (DCPD), indene, naphthalene and other components and various forms of self-polymerization and interpolymerization dimers of cyclopentadiene (CPD) and methyl cyclopentadiene (MCPD), among which methyl styrene and dicyclopentadiene have the highest content. At present, the most valuable comprehensive utilization of the carbon nine carbon ten fraction is to separate cyclopentadiene and methyl cyclopentadiene through depolymerization and separation, and then obtain dicyclopentadiene and methyl cyclopentadiene dimers as the final products through dimerization. These two dienes are widely used in the field of fine chemicals. The purity of dicyclopentadiene can reach 99%, which is used in the production of polydicyclopentadiene.
[0003] Polydicyclopentadiene (PDCPD) is a new type of engineering plastic, which is polymerized by dicyclopentadiene (DCPD) under the action of a ring-opening metathesis catalyst. It has good heat resistance, creep resistance, dimensional stability, corrosion resistance, wear resistance and other characteristics. At present, the catalyst system used to prepare polydicyclopentadiene includes tungsten-molybdenum complexes or molybdenum and ruthenium carbene catalysts, and the process used is reaction injection molding (RIM) technology, which has the advantages of fast molding speed, high efficiency and low energy consumption, and can be used to manufacture various large-scale thin-walled and complex-shaped parts.
[0004] The PDCPD material processed by RIM technology has excellent mechanical properties, thermal stability and anti-aging properties, and can be widely used in automotive parts, industrial equipment, medical devices, etc.
[0005] The RIM process conventionally uses two materials, A and B, for mixed injection in a certain proportion, using a polymerization catalyst and dicyclopentadiene as the main raw material. Different components are generally added to the polymerization raw materials to achieve different product properties.
[0006] Therefore, there are technical problems in the existing technology such as long carbon nine and carbon ten utilization routes, complex separation process, and low economic benefits. It is necessary to develop a new recycling technology to improve the comprehensive utilization rate of the carbon nine and carbon ten fractions. Summary of the invention
[0007] The present invention aims at the deficiencies of the prior art and provides a method for comprehensive utilization of the carbon nine and carbon ten fractions produced as byproducts of petroleum cracking to produce ethylene. The present invention produces a variety of products from the carbon nine and carbon ten fractions through a series of separation and polymerization reaction processes, thereby improving the comprehensive utilization rate of carbon nine and carbon ten, and through the combination of the above reaction processes and the polymerization process, a mixture of cyclopentadiene and methylcyclopentadiene is polymerized to prepare polydicyclopentadiene, thereby avoiding the requirement of separation purity and improving economic benefits.
[0008] The following are the specific technical solutions of the present invention.
[0009] The present invention provides a method for comprehensive utilization of carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene, comprising:
[0010] (1) The crude oil cracking byproduct carbon nine carbon ten fraction raw material is passed through a vacuum distillation tower, and a styrene and methyl styrene rich fraction is obtained at the top of the tower, and the bottom material enters the next processing unit; wherein the vacuum distillation tower bottom temperature is 85-120°C, the tower top temperature is 51-73°C, the reflux ratio is 3-10, and the tower top pressure is -80--90KPaG;
[0011] (2) the bottom material obtained in step (1) enters a depolymerization reactor for depolymerization reaction at 180-210° C. to obtain a fraction rich in cyclopentadiene and methylcyclopentadiene, which enters a separation tower from an upper outlet, and the bottom of the reactor is a heavy component;
[0012] (3) The upper outlet fraction obtained in step (2) enters a separation tower for separation, and a CPD-rich fraction is obtained at the top of the tower, side line 1 is a mixed fraction of CPD and MCPD, and side line 2 is a MCPD fraction; wherein the temperature of the separation tower bottom is 90-120° C., the temperature of the tower top is 35-45° C., the temperature of side line 1 is 50-70° C., the temperature of side line 2 is 65-80° C., and the reflux ratio is 3-8;
[0013] (4) a. The CPD fraction obtained from the top of step (3) is subjected to a dimerization reaction to obtain a DCPD product having a content of> 99%;
[0014] b. The CPD and MCPD mixed fraction obtained in step (3) of the side line 1 is used as a polymerization raw material after dimerization reaction, mixed with a catalyst and an antioxidant, and then enters a RIM polymerization device for RIM polymerization to prepare a polydicyclopentadiene product;
[0015] c. The MCPD fraction obtained from the side line 2 in step (3) is dimerized to obtain a DMCPD product with a content of >95%.
[0016] Furthermore, in step (1), the bottom temperature of the tower is 90 to 105° C., the top temperature of the tower is 55 to 60° C., the reflux ratio is 5 to 8, and the top pressure of the tower is -82 to -88 KPaG.
[0017] Furthermore, the depolymerization reaction temperature in step (2) is 170-190°C.
[0018] Furthermore, in step (3), the bottom temperature of the tower is 105-110°C, the top temperature of the tower is 38-42°C, the reflux ratio is 3-5, the side line 1 temperature is 55-60°C, and the side line 2 temperature is 70-75°C.
[0019] Furthermore, the dimerization reaction temperature in step (4) a is 40-110° C. and the pressure is 0.1-0.6 MPaG.
[0020] Furthermore, the dimerization reaction temperature in step (4)b is 40-110°C and the pressure is 0.1-0.6 MPaG.
[0021] Furthermore, the RIM aggregation in step (4)b includes:
[0022] A. Catalyst solution A
[0023] The catalyst is dissolved in an organic solvent to prepare a catalyst solution, wherein the molar ratio of the catalyst to the polymerization raw material liquid B is 1:5000-50000, and then an antioxidant is added, wherein the amount of the antioxidant added is 0.01%-2% of the mass of the polymerization raw material liquid B, to obtain a catalyst solution A;
[0024] B. Polymerization raw material liquid B
[0025] The polymerization raw material, i.e., a mixture of cyclopentadiene and methylcyclopentadiene, with a total content of more than 95%, is injected into a mixing tank under nitrogen protection, and the temperature is controlled at 10-30°C;
[0026] C. Mixed curing molding
[0027] Liquid A was injected into a mixing tank and mixed evenly with liquid B under nitrogen protection, and then injected into a reaction mold. The mold began to undergo a programmed temperature increase, maintaining the reaction temperature at 40-80°C for 1 hour, and the post-treatment temperature was 120-150°C for 1 hour.
[0028] D. After the mold is cooled, the product is demoulded to obtain the polymerized product.
[0029] Furthermore, the molar ratio of the catalyst to the polymerization raw material liquid B is 1:10000.
[0030] Furthermore, in the polymerization raw material, the mass ratio of cyclopentadiene to methylcyclopentadiene is 100:5-20, preferably 100:5-10.
[0031] Furthermore, the catalyst is a ruthenium-based catalyst, preferably a Grubbs second-generation catalyst; the antioxidant is a free radical scavenging antioxidant, selected from any one or a combination of tert-butylphenol, tert-butylhydroquinone, o-di-tert-butyl-p-methylphenol, etc., preferably o-di-tert-butyl-p-methylphenol.
[0032] Furthermore, in the step (C), the mold begins to undergo programmed temperature rise, maintaining the reaction temperature at 60° C. for 1 hour, and the post-treatment temperature is 140° C. for 1 hour.
[0033] Compared with the prior art, the advantages of the present invention are that while obtaining styrene, methylstyrene products, cyclopentadiene and methylcyclopentadiene products, suitable PDCPD raw materials are obtained, and the loss of materials caused by the difficulty in separating the components of the materials during the separation process is reduced, the yield of the product is improved, and the difficulty of separating the materials, especially the difficulty of separating cyclopentadiene and methylcyclopentadiene, is reduced.
[0034] The present invention selects a mixture of cyclopentadiene and methylcyclopentadiene as a RIM polymerization raw material, which reduces the separation purity requirement of the DCPD product, has a simple separation process, and the product obtained by polymerization is uniform and compact and has good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic diagram of the process flow of the present invention; wherein, a vacuum distillation tower 1, a depolymerization reactor 2, a first separation tower 3, a first dimerization reactor 4, a second dimerization reactor 5, a second separation tower 6, a RIM mixing tank 7, a RIM mold 8, and a third dimerization reactor 9. DETAILED DESCRIPTION
[0036] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0037] The catalysts used in the following examples can be obtained from commercial sources.
[0038] [Examples 1 to 5]
[0039] The process flow of Examples 1 to 5 is shown in Figure 1The raw material carbon nine carbon ten fraction W1 first enters the vacuum distillation tower 1 for vacuum distillation, and the styrene and methylstyrene fractions W2 are obtained at the top of the tower. The bottom fraction enters the depolymerization reactor 2 for depolymerization. The upper outlet is a mixture of cyclopentadiene and methylcyclopentadiene W3, and the lower part is a heavy component. W3 enters the first separation tower 3 for separation, and a cyclopentadiene mixed fraction W4 is obtained at the top of the tower. After passing through the first dimerization reactor 4, a dicyclopentadiene product W5 is obtained; the first side line is a mixed fraction W6 of cyclopentadiene and methylcyclopentadiene, which is passed through the second dimerization reactor 5 and the second separation tower 6 to obtain a polymerization raw material W7, which enters the RIM mixing tank 7 together with the catalyst, and enters the RIM mold 8 after mixing to obtain the product PDCPD; the second side line is methylcyclopentadiene, which is polymerized through the third dimerization reactor 9 to obtain the product W8; the bottom of the tower discharges the heavy component regularly.
[0040] The reaction process is as follows:
[0041] (1) The C9 and C10 raw materials are distilled through a vacuum distillation tower 1, and a styrene and methyl styrene-rich fraction is obtained at the top of the tower, and the bottom material enters the next processing unit. The bottom temperature is 85-120°C, the top temperature is 51-73°C, the reflux ratio is 3-10, and the top pressure is -80--90KPaG;
[0042] (2) The bottom material obtained in step (1) enters the depolymerization reactor 2 for depolymerization to obtain a fraction rich in cyclopentadiene and methylcyclopentadiene, which enters the separation tower from the upper outlet, and the bottom of the reactor is the heavy component. The depolymerization reaction temperature is 180-210°C;
[0043] (3) The fraction obtained in step (2) enters the separation tower 3 for separation, and a CPD-rich fraction is obtained at the top of the tower, the side line 1 is a mixture of CPD and MCPD, and the side line 2 is a MCPD fraction. The bottom temperature is 90-120°C, the top temperature is 35-45°C, the side line 1 temperature is 50-70°C, the side line 2 temperature is 65-78°C, and the reflux ratio is 3-8;
[0044] (4) a. The CPD fraction obtained from the top of step (3) is subjected to a dimerization reaction to obtain a DCPD product having a content of> 99%;
[0045] b. The CPD and MCPD mixed fraction obtained in step (3) of the side line 1 is used as a polymerization raw material after dimerization reaction, mixed with a catalyst and an antioxidant, and then enters a RIM polymerization device for RIM polymerization to prepare a polydicyclopentadiene product;
[0046] c. The MCPD fraction obtained from the side line 2 in step (3) is dimerized to obtain a DMCPD product with a content of >95%.
[0047] The RIM aggregation in step (4)b is specifically as follows:
[0048] A. Catalyst solution A
[0049] In a glove box, a certain amount of Grubbs second generation catalyst is weighed and dissolved in dichloromethane to prepare a 40 mg / ml catalyst solution, where the molar ratio of the catalyst to the polymerization raw material solution B is 1:5000-50000. 0.01%-2% (B solution weight) of antioxidant o-di-tert-butyl-p-methylphenol is added to obtain catalyst solution A;
[0050] B. Polymerization raw material liquid B
[0051] A mixture of cyclopentadiene and methylcyclopentadiene (total content greater than 95%) was metered into a mixing tank at 120 g under nitrogen protection, and the temperature was controlled at 10-30°C.
[0052] C. Mixed curing molding
[0053] Liquid A was injected into the mixer under nitrogen protection, mixed evenly with liquid B, and injected into the reaction mold. The mold began to undergo a programmed temperature increase, maintaining the reaction temperature at 60°C for 1 hour, and the post-treatment temperature was 140°C for 1 hour.
[0054] D. After the mold is cooled, the product is demoulded to obtain the polymerized product.
[0055] The raw material is the C9-C10 fraction produced as a by-product of petroleum cracking to produce ethylene. The main composition is shown in Table 1.
[0056] The process operating conditions of the vacuum distillation tower 1, the depolymerization reactor 2, the separation tower 3, and the PDCPD polymerization reaction in each embodiment are shown in Tables 2, 3, 4, and 5, respectively. The composition of materials W2, W4, W6, and W8 were analyzed by gas chromatography, and the content of the enriched components in each material is shown in Table 6. The results of the PDCPD polymerization products are shown in Table 7.
[0057] Table 1 Composition of C9 and C10 raw materials
[0058]
[0059] Table 2 Vacuum distillation tower 1 operating conditions
[0060] Tower bottom temperature (℃) Tower top temperature (℃) Tower top pressure (KPaG) Reflux ratio Example 1 95 55 -85 4 Example 2 100 56 -88 5 Example 3 105 58 -90 6 Example 4 110 61 -87 8 Example 5 120 66 -85 10
[0061] Table 3 Depolymerization reactor operating conditions
[0062] Reaction temperature (℃) Example 1 175 Example 2 180 Example 3 185 Example 4 190 Example 5 195
[0063] Table 4 Separation tower 3 operating conditions
[0064] Tower bottom temperature (℃) Tower top temperature (℃) Reflux ratio Example 1 90 35 3 Example 2 95 37 5 Example 3 100 40 6 Example 4 110 44 8 Example 5 120 45 8
[0065] Table 5 PDCPD polymerization process conditions
[0066] Example <![CDATA[n 聚合原料液 :n cat ]]> <![CDATA[m 抗氧剂 / m 聚合原料液 ]]> Example 1 50000 2% Example 2 30000 2% Example 3 20000 1% Example 4 10000 1% Example 5 5000 0.01%
[0067] Table 6 Composition of W2, W4, W6 and W8
[0068]
[0069] Table 7 Mechanical properties of PDCPD polymer
[0070]
[0071] The preferred embodiments of the present invention have been specifically described above, but the present invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A method for comprehensive utilization of the carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene, comprising: (1) The crude oil cracking byproduct carbon nine carbon ten fraction raw material is passed through a vacuum distillation tower, and a styrene and methyl styrene rich fraction is obtained at the top of the tower, and the bottom material enters the next processing unit; wherein the vacuum distillation tower bottom temperature is 85-120°C, the tower top temperature is 51-73°C, the reflux ratio is 3-10, and the tower top pressure is -80--90KPaG; (2) the bottom material obtained in step (1) enters a depolymerization reactor for depolymerization reaction at 180-210° C. to obtain a fraction rich in cyclopentadiene and methylcyclopentadiene, which enters a separation tower from an upper outlet, and the bottom of the reactor is a heavy component; (3) The upper outlet fraction obtained in step (2) enters a separation tower for separation, and a CPD-rich fraction is obtained at the top of the tower, side line 1 is a mixed fraction of CPD and MCPD, and side line 2 is a MCPD fraction; wherein the temperature of the separation tower bottom is 90-120° C., the temperature of the tower top is 35-45° C., the temperature of side line 1 is 50-70° C., the temperature of side line 2 is 65-80° C., and the reflux ratio is 3-8; (4) a. The CPD fraction obtained from the top of step (3) is subjected to a dimerization reaction to obtain a DCPD product having a content of> 99%; wherein the dimerization reaction temperature is 40 to 110°C and the pressure is 0.1 to 0.6 MPaG; b. The CPD and MCPD mixed fraction obtained in step (3) of the side line 1 is subjected to dimerization reaction as a polymerization raw material, mixed with a catalyst and an antioxidant, and then fed into a RIM polymerization device for RIM polymerization to prepare a polydicyclopentadiene product; wherein the dimerization reaction temperature is 40 to 110 ° C and the pressure is 0.1 to 0.6 MPaG; Wherein, the RIM aggregation includes: A. Catalyst solution A The catalyst is dissolved in an organic solvent to prepare a catalyst solution, wherein the molar ratio of the catalyst to the polymerization raw material liquid B is 1:5000-50000, and then an antioxidant is added, wherein the amount of the antioxidant added is 0.01%-2% of the mass of the polymerization raw material liquid B, to obtain a catalyst solution A; B. Polymerization raw material liquid B The polymerization raw material, i.e., a mixture of cyclopentadiene and methylcyclopentadiene, with a total content of more than 95%, is injected into a mixing tank under nitrogen protection, and the temperature is controlled at 10-30°C; C. Mixed curing molding Liquid A was injected into a mixing tank and mixed with liquid B under nitrogen protection, and then injected into a reaction mold. The mold began to be programmed to increase the temperature, maintaining the reaction temperature at 40-80°C for 1 hour, and the post-treatment temperature was 120-150°C for 1 hour; Wherein, in the RIM polymerization, the mass ratio of cyclopentadiene to methylcyclopentadiene in the polymerization raw material is 100:5-20; the catalyst of the RIM polymerization is Grubbs second generation catalyst; the antioxidant is selected from any one of tert-butylphenol, tert-butylhydroquinone, o-di-tert-butyl-p-methylphenol or a combination of several thereof; c. The MCPD fraction obtained from the side line 2 in step (3) is dimerized to obtain a DMCPD product with a content of >95%.
2. The method for comprehensive utilization of the carbon nine and carbon ten fractions produced as a by-product of petroleum cracking to produce ethylene according to claim 1, characterized in that: The tower bottom temperature in the step (1) is 90-105° C., the tower top temperature is 55-60° C., the reflux ratio is 5-8, and the tower top pressure is -82--88 KPaG.
3. The method for comprehensive utilization of the carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene according to claim 1, characterized in that: The depolymerization reaction temperature in step (2) is 170-190°C.
4. The method for comprehensive utilization of the carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene according to claim 1, characterized in that: In the step (3), the bottom temperature is 105-110°C, the top temperature is 38-42°C, the reflux ratio is 3-5, the side line 1 temperature is 55-60°C, and the side line 2 temperature is 70-75°C.
5. The method for comprehensive utilization of the carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene according to claim 1, characterized in that: In the RIM polymerization in step (4) b, the molar ratio of the catalyst to the polymerization raw material liquid B is 1:10000.
6. The method for comprehensive utilization of the carbon nine and carbon ten fractions produced as by-products of petroleum cracking to produce ethylene according to claim 1, characterized in that: In the step (C), the mold begins to undergo programmed temperature rise, maintaining the reaction temperature at 60° C. for 1 hour, and the post-treatment temperature is 140° C. for 1 hour.