A C5 fraction selective hydrogenation catalyst

By using alumina support and microemulsion loading technology with bimodal pore distribution structure in the selection hydrogenation catalyst of five carbon fractions, the problem of easy formation of oligomers and coking of the catalyst is solved, and the selectivity and service life of the catalyst are improved, thus achieving the realization of the catalyst. Efficient utilization of carbon five resources.

CN114471504BActive Publication Date: 2024-11-01PETROCHINA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202011159168.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-26
Publication Date
2024-11-01
Estimated Expiration
2040-10-26

AI Technical Summary

Technical Problem

The existing carbon five fraction hydrogenation catalyst is easy to generate oligomers and coke during use, resulting in a decrease in catalyst activity and shortened service life, and poor selectivity, making it difficult to effectively utilize carbon five resources.

Method used

Alumina is used as a support to prepare a catalyst with a bimodal pore distribution structure. The small pore diameter of the support is 10-25nm and the large pore diameter is 45-350nm. It contains components such as Pd, Mn, Ni, Cu, etc., and is by microemulsion and solution method. Loading, control the distribution of Ni/Cu alloy in macropores, reduce reduction temperature, reduce green oil generation and polymerization reaction.

Benefits of technology

It significantly improves the selectivity and coking resistance of the catalyst, extends the service life of the catalyst, maintains high hydrogenation activity and selectivity, and effectively utilizes the carbon five resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114471504B_ABST
    Figure CN114471504B_ABST
Patent Text Reader

Abstract

A C5 fraction selective hydrogenation catalyst, the carrier is alumina or mainly alumina, and has a bimodal pore distribution structure and a specific surface area of ​​70 to 120 m 2 / g, wherein the pore size of the small pore is 10-25nm, and the pore size of the macropore is 45-350nm; the catalyst contains at least Pd, Mn, Ni, and Cu, and based on the weight of the catalyst as 100%, the Pd content is 0.2-0.6%, the molar ratio of Mn to Pd is 3-7:1, the Ni content is 0.5-5%, and the mass ratio of Cu to Ni is 0.1-1:1, preferably 0.2-0.6:1. Ni and Cu are loaded in a microemulsion manner and distributed in the macropores of the carrier of 45-350nm; Mn is loaded by a solution method, and palladium is loaded by a solution method and a microemulsion method, that is, most of the Pd is loaded by a solution method, and a small part of the Pd is loaded by a microemulsion method, and the amount of Pd loaded by the microemulsion method is 1 / 100-1 / 200 of the Ni+Cu content. The catalyst of the present invention has a low reduction temperature in the preparation process, can be used in the selective hydrogenation process of isoprene in the C5 fraction, and has good hydrogenation activity, excellent selectivity and high coking resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a C5 fraction selective hydrogenation catalyst, in particular to a selective hydrogenation catalyst for isoprene in a cracked C5 fraction. Background Art

[0002] Cracking C5 is a byproduct of the high-temperature cracking process of petroleum hydrocarbons to produce ethylene. As of 2016, the domestic ethylene production capacity reached 17.8 million tons / year. If liquid hydrocarbons (such as naphtha and light diesel) are used as cracking raw materials, the cracking C5 yield can reach 14% to 20% of the ethylene production. The components such as isoprene, cyclopentadiene, and isoprene contained in the C5 fraction have very active chemical properties due to their special molecular structure. They can synthesize many high-value-added products and are valuable chemical raw material resources. With the rapid development of the petrochemical industry, the production capacity of ethylene is growing continuously, and the sources of cracking C5 are becoming increasingly abundant and have become a chemical resource that cannot be ignored. How to effectively utilize the considerable amount of C5 resources and increase their added value has become an urgent problem for petrochemical enterprises to solve.

[0003] The 2-methylbutene-1 and 2-methylbutene-2 ​​generated by selective hydrogenation of crude isoprene from the cracking C5 fraction separation unit can be used as raw materials for the production of isoprene petroleum resin. This utilization method is also one of the important ways for various ethylene manufacturers to comprehensively utilize the cracking C5 fraction.

[0004] For the selective hydrogenation of crude isoprene in the cracking C5 fraction, metal palladium catalysts are currently commonly used in the industry for hydrogenation. In order to ensure that 2-methylbutene-1 and 2-methylbutene-2 ​​generated by the hydrogenation of isoprene are not further hydrogenated to form alkanes, it is necessary to ensure that the catalyst has a high hydrogenation selectivity in order to obtain better economic benefits.

[0005] On the other hand, during the actual hydrogenation reaction, while the palladium catalyst catalyzes the selective hydrogenation of isoprene, unsaturated hydrocarbons such as pentene in the raw material will also polymerize on the acidic center of the catalyst to generate oligomers with a wider molecular weight, commonly known as "green oil". The green oil is then adsorbed on the catalyst surface and further forms coke, blocking the catalyst pores and preventing the reactants from diffusing to the surface of the active center of the catalyst, thereby causing the catalyst activity to decrease.

[0006] Precious metal catalysts have high activity, but they are prone to generate oligomers during use, which causes the catalyst to coke and deactivate, affecting the stability and service life of the catalyst. Patent CN200810119385.8 invented a non-precious metal supported selective hydrogenation catalyst and its preparation method and application, including a carrier and a main active component and an auxiliary active component supported on the carrier, characterized in that the main active component is Ni, the auxiliary active component is selected from at least one of Mo, La, Ag, Bi, Cu, Nd, Cs, Ce, Zn and Zr, the main active component and the auxiliary active component are both in amorphous form, with an average particle size of <10nm, the carrier is a non-oxidizing porous material; and the catalyst is prepared by microemulsion method.

[0007] Zhang Kongyuan et al. prepared Bi-modified Pd-Au / A1 for selective hydrogenation of isoprene by isovolumetric impregnation method. 2 O 3 Catalyst. The results show that the addition of Bi increases the selectivity of the catalyst for monoolefins, but at the same time the activity decreases; when the reaction temperature is 80°C, with the increase of Bi content (w = 0.1% to 0.3%), the conversion rate of isoprene decreases from 98% to 34%, the selectivity of 2-methyl-2-butene decreases from 82.3% to 68.6%, and the selectivity of 3-methyl-1-butene and 2-methyl-1-butene increases from 2.1% and 13.3% to 8.6% and 22.0%, respectively. (Zhang Kongyuan et al., Petrochemicals, 2014, VOL.43(2): P132-137.)

[0008] US5587348 uses alumina as a carrier, adds silver as a promoter to palladium, and adds fluorine chemically bonded to an alkali metal to prepare a carbon dihydrogenation catalyst with excellent performance. The catalyst has the characteristics of reducing the generation of green oil, improving ethylene selectivity, and reducing the generation of oxygen-containing compounds.

[0009] Patent CN1736589 reported a Pd / γ-Al prepared by complete adsorption impregnation method. 2 O 3 A hydrogenation catalyst is selected, and a large amount of green oil is generated during the use of the catalyst.

[0010] Patent CN200810114744.0 invented a catalyst for selective hydrogenation of unsaturated hydrocarbons and its preparation method. The catalyst uses alumina as a carrier and palladium as an active component. Rare earth and alkaline earth metals and fluorine are added to improve the catalyst's resistance to impurities and coking, but its catalyst selectivity is not ideal.

[0011] The catalysts prepared by the above methods all use catalysts with a single pore size distribution. In the fixed bed reaction process, the catalyst selectivity is poor due to the influence of internal diffusion. The carrier with a bimodal pore distribution can reduce the influence of internal diffusion while ensuring the high activity of the catalyst, and improve the catalyst selectivity. ZL971187339 discloses a hydrogenation catalyst, the carrier is a honeycomb carrier, which is a large-pore carrier, which effectively improves the selectivity of the catalyst. CN1129606 discloses a hydrocarbon conversion catalyst, the carrier catalyst includes aluminum oxide, nickel oxide, iron oxide, etc., the catalyst includes two kinds of pores, one for increasing the catalytic reaction surface, and the other is conducive to diffusion. Patent CN101433842 provides a hydrogenation catalyst, characterized in that the catalyst has a bimodal pore distribution, the most probable radius of the small pore part is 2 to 50nm, and the most probable radius of the large pore part is 100 to 500nm. Since the catalyst has a bimodal pore distribution, it has good hydrogenation activity and good selectivity, and the ethylene increment is large.

[0012] In the hydrogenation reaction of C5 fraction, the generation of green oil and the coking of catalyst are important factors affecting the service life of catalyst. The activity, selectivity and service life of catalyst constitute the overall performance of catalyst. The above-listed methods may provide a better way to improve the activity and selectivity of catalyst, but do not solve the problem of easy coking of catalyst, or solve the problem of easy generation of green oil and coking of catalyst, but do not solve the problem of selectivity. Although the carrier with macroporous structure can improve the selectivity, the larger molecules generated by polymerization and chain growth reaction are also easy to accumulate in the macropores of the carrier, causing the catalyst to coke and deactivate, affecting the service life of the catalyst.

[0013] ZL201310114077.7 discloses a hydrogenation catalyst, wherein the active components of the catalyst are Pd, Ag, and Ni, wherein Pd and Ag are loaded by aqueous solution impregnation method, and Ni is loaded by W / O microemulsion impregnation method. After adopting this method, Pd / Ag and Ni are located in pores of different pore sizes, and the green oil generated by the reaction is saturatedly hydrogenated in the macropores, and the amount of catalyst coking is reduced.

[0014] However, the reduction temperature of Ni often reaches about 500°C. At this temperature, the reduced Pd atoms are very easy to aggregate, which greatly reduces the activity of the catalyst. It is necessary to greatly increase the amount of active components to compensate for the activity loss, but this will cause a decrease in selectivity. Summary of the invention

[0015] The object of the present invention is to provide a C5 fraction selective hydrogenation catalyst, in particular a C5 fraction isoprene selective hydrogenation catalyst with good selectivity and coking resistance.

[0016] A C5 fraction selective hydrogenation catalyst, the carrier is alumina or mainly alumina, and has a bimodal pore distribution structure and a specific surface area of ​​70 to 120 m 2 / g, wherein the pore size of the small pore is 10-25nm, and the pore size of the macropore is 45-350nm; the catalyst contains at least Pd, Mn, Ni, and Cu, and based on the weight of the catalyst as 100%, the Pd content is 0.2-0.6%, preferably 0.3-0.5%, the molar ratio of Mn to Pd is 3-7:1, preferably 4-6:1, the Ni content is 0.5-5%, preferably 1.5-3.5%, and the mass ratio of Cu to Ni is 0.1-1:1, preferably 0.2-0.6:1. Ni and Cu are loaded in a microemulsion manner and distributed in the macropores of the carrier of 45-350nm; Mn is loaded by a solution method, and palladium is loaded by a solution method and a microemulsion method, and the amount of Pd loaded by the microemulsion method is 1 / 100-1 / 200 of the Ni+Cu content.

[0017] In this catalyst, the selective hydrogenation reaction of isoprene occurs in the main active center composed of Mn and Pd, Ni and Cu are impregnated in the macropores of the carrier in the form of microemulsion, and the green oil generated in the reaction undergoes saturated hydrogenation on the active center composed of Cu and Ni.

[0018] For hydrogenation reactions, it is generally necessary to reduce the hydrogenation catalyst before using it to ensure that the active components exist in a metallic state so that the catalyst has hydrogenation activity. Because during the catalyst preparation process, activation is a high-position roasting process, in which metal salts decompose into metal oxides, and the oxides form clusters, which are generally nano-sized. Different oxides need to be reduced at different temperatures due to their different chemical properties. However, for nano-sized metals, around 200°C is an important critical temperature. Above this temperature, metal particles will aggregate significantly. Therefore, lowering the reduction temperature of the active components is of great significance for hydrogenation catalysts.

[0019] The role of Cu is to form a Ni / Cu alloy during the roasting process, which not only improves the performance of the catalyst, but the inventors also found that it effectively reduces the reduction temperature of nickel during the reduction process and reduces the aggregation of Pd at high temperatures. Loading Cu and Ni together can reduce the reduction temperature of Ni, because to completely reduce NiO alone, the reduction temperature generally needs to reach 450-500°C, which will cause Pd to agglomerate. After forming a Cu / Ni alloy, its reduction temperature can be reduced by more than 100°C compared to the reduction temperature of pure Ni, reaching 350°C, thereby alleviating the agglomeration of Pd during the reduction process.

[0020] The inventor unexpectedly discovered that loading a small amount of Pd on the surface of Ni / Cu alloy can also significantly reduce the reduction temperature of Ni to below 200°C, down to 150°C.

[0021] The inventors found that the selective hydrogenation reaction of isoprene occurs in the main active center composed of Mn and Pd, and the macromolecules such as green oil generated in the reaction easily enter the macropores of the catalyst. In the macropores of the catalyst, Ni / Cu components are loaded, wherein Ni has a saturated hydrogenation function, and the green oil component undergoes a saturated hydrogenation reaction at the active center composed of Ni / Cu. Since the double bonds are saturated with hydrogenation, the green oil component can no longer undergo a polymerization reaction or the polymerization reaction rate is greatly reduced, and its chain growth reaction is terminated or delayed, and a huge molecular weight condensed ring compound cannot be formed, and it is easy to be taken out of the reactor by the material, so the coking degree of the catalyst surface will be greatly reduced, and the operating life of the catalyst will be greatly extended.

[0022] The method for controlling the positioning of the Ni / Cu alloy in the catalyst macropores in the present invention is that the Ni / Cu is loaded in the form of a microemulsion, the particle size of the microemulsion is larger than the maximum pore size of the carrier micropores, and smaller than the maximum pore size of the carrier macropores. The Ni and Cu metal salts contained in the microemulsion are difficult to enter the carrier pores with smaller sizes due to spatial resistance, so the Ni and Cu are mainly concentrated in the macropores.

[0023] In the process of loading palladium by solution method, due to the siphon effect of the small holes, the solution containing palladium enters the small holes faster. The palladium exists in the form of chloropalladate ions. Since the ions can form chemical bonds with the hydroxyl groups on the surface of the carrier, the palladium is quickly targeted. Therefore, the faster the solution enters the pores, the faster the loading speed. Therefore, in the process of impregnating Pd by solution method, it is easier to load in the small holes.

[0024] In the present invention, Pd is loaded by two methods, namely, a solution method and a microemulsion method, that is, most of the Pd is loaded by solution, and a small part of the Pd is loaded by microemulsion. When loading by microemulsion, the particle size of the microemulsion is controlled to be larger than the maximum pore size of the small pores of the carrier and smaller than the maximum pore size of the large pores of the carrier, so that the part of the Pd is mainly distributed in the large pores of the carrier. The amount of Pd loaded by the microemulsion method is 1 / 100 to 1 / 200 of the content of Ni+Cu, and the step of loading Pd by microemulsion is after the step of loading Ni and Cu by microemulsion.

[0025] The carrier used in the present invention is required to have a bimodal pore distribution structure, in particular, it should have a macropore with a pore size of 45 to 350 nm and a micropore with a pore size of 10 to 25 nm. The carrier is alumina or mainly alumina, Al 2 O 3The crystal form is preferably a θ- and α-mixed crystal form. The aluminum oxide in the catalyst carrier is preferably more than 80%, and the carrier may also contain other metal oxides such as magnesium oxide, lithium oxide, etc.

[0026] During the preparation of the catalyst, Ni / Cu loading is carried out by impregnation in the form of microemulsion, Pd loading is carried out by impregnation in the form of solution and microemulsion, and Mn loading can be carried out by solution saturation impregnation.

[0027] The present invention does not particularly limit the process of loading Ni, Cu, and Pd in ​​a microemulsion manner. As long as the microemulsion particle size is controlled to be larger than the maximum pore size of the carrier's small pores and smaller than the maximum pore size of the carrier's large pores, Ni, Cu, and Pd can be distributed in the carrier's large pores.

[0028] The present invention also recommends a method, wherein the microemulsion loading process comprises: dissolving the precursor salt in water, adding an oil phase, a surfactant and a co-surfactant, and stirring thoroughly to form a microemulsion, wherein the oil phase is an alkane or a cycloalkane, the surfactant is an ionic surfactant and / or a non-ionic surfactant, and the co-surfactant is an organic alcohol.

[0029] The types and addition amounts of the oil phase, surfactant and co-surfactant are not particularly limited in the present invention and can be determined according to the precursor salt and the pore structure of the carrier.

[0030] The oil phase recommended by the present invention is a saturated alkane or cycloalkane, preferably C 6 ~C 8 Saturated alkanes or cycloalkanes, preferably cyclohexane or n-hexane; the surfactant is an ionic surfactant and / or a nonionic surfactant, preferably a nonionic surfactant, more preferably polyethylene glycol octylphenyl ether (Triton X-100) or cetyltrimethylammonium bromide (CTAB); the co-surfactant is an organic alcohol, preferably C 4 ~C 6 Alcohols, more preferably n-butanol and / or n-pentanol.

[0031] In the microemulsion, the weight ratio of the water phase to the oil phase is preferably 1.2 to 2.5, the weight ratio of the surfactant to the oil phase is 0.3 to 0.7, and the weight ratio of the surfactant to the co-surfactant is 1 to 1.2.

[0032] The step of loading Pd with microemulsion must be after the step of loading Ni and Cu with microemulsion.

[0033] The present invention also provides a more specific catalyst, and the catalyst preparation method thereof comprises:

[0034] (1) Dissolve the precursor salts of Ni and Cu in water, add the oil phase, surfactant and co-surfactant, stir well to form a microemulsion, add the carrier to the prepared microemulsion and immerse for 0.5 to 4 hours, filter out the remaining liquid, dry at 60 to 120°C for 1 to 6 hours, and calcine at 300 to 600°C for 2 to 8 hours to obtain a semi-finished catalyst A.

[0035] (2) The precursor salt of Pd is dissolved in water and the pH is adjusted to 2.0-2.5. Then, the semi-finished catalyst A is added to the Pd salt solution, and after immersion and adsorption for 0.5-4 hours, the semi-finished catalyst is dried at 100-120° C. for 1-4 hours, and calcined at 400-550° C. for 2-6 hours to obtain the semi-finished catalyst B.

[0036] (3) The loading of Mn was carried out by a solution saturation impregnation method. After the semi-finished catalyst B was loaded with Mn, it was dried at 100-120°C for 1-4 hours and calcined at 500-550°C for 4-6 hours to obtain a semi-finished catalyst C.

[0037] (4) Dissolve the Pd precursor salt in water, add the oil phase, surfactant and co-surfactant, stir well to form a microemulsion, add the semi-finished catalyst C to the prepared microemulsion and immerse for 0.5 to 4 hours, filter out the remaining liquid, dry at 60 to 120°C for 1 to 6 hours, and calcine at 300 to 600°C for 2 to 8 hours to obtain a catalyst.

[0038] In the above preparation steps, step (1) and step (2) can be interchanged, step (3) is after step (2), and step (4) is after step (1).

[0039] The carrier in the above step (1) can be spherical, cylindrical, three-leaf clover, four-leaf clover, etc.

[0040] The precursor salts of Ni, Cu and Pd described in the above steps are soluble salts, which may be nitrates, chlorides or other soluble salts thereof.

[0041] The reduction temperature of the catalyst of the present invention is preferably 150-200°C.

[0042] The catalyst has the following characteristics: at the beginning of the hydrogenation reaction, the selective hydrogenation reaction of isoprene mainly occurs in the small pores because the palladium has high hydrogenation activity and is mainly distributed in the small pores. As the catalyst runs longer, a portion of byproducts with larger molecular weights are generated on the catalyst surface. These substances, due to their larger molecular size, enter the large pores more and have a longer residence time. Under the action of the nickel catalyst, double bond hydrogenation reactions occur to generate saturated hydrocarbons or aromatic hydrocarbons without isolated double bonds, and no substances with larger molecular weights are generated. The use of the catalyst of the present invention can greatly reduce the reduction temperature of the catalyst, which can be reduced to 150-200°C at the lowest.

[0043] The inventors have found that the initial performance of the catalyst prepared by the method is significantly improved in activity and selectivity compared with the bimodal pore distribution catalyst prepared without using microemulsion palladium.

[0044] The inventors have also found that after using the catalyst, even if the content of unsaturated hydrocarbons in the reactants is high and the amount of catalyst green oil generated is greatly increased, the catalyst still has excellent hydrogenation activity and selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The temperature-programmed reduction results (TPR) of samples prepared by the microemulsion method for loading Cu / Ni and Pd-Cu / Ni were obtained. DETAILED DESCRIPTION

[0046] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.

[0047] The catalyst of the present invention uses the following characterization methods in the preparation process: dynamic light scattering particle size analyzer, on M286572 dynamic light scattering analyzer, the particle size distribution of the Ni / Cu alloy microemulsion is analyzed; on 9510 mercury intrusion instrument and Tristar3000 automatic physical adsorption instrument of American Mack Company, the pore volume, specific surface area and pore size distribution of the carrier are measured and analyzed. On A240FS atomic absorption spectrometer, the contents of Pd, Mn, Ni and Cu in the catalyst are measured.

[0048] The present invention is further described below by way of examples, but it is not intended that the present invention is limited thereto.

[0049] Example 1

[0050] Catalyst carrier: A commercially available bimodal pore distribution cloverleaf strip alumina carrier with a diameter of 2.3-2.5 mm was used. After calcination at 980°C, the bimodal pore size distribution ranged from 13-20 nm and 80-260 nm, with a specific surface area of ​​110 m 2 Weigh 100 g of the carrier.

[0051] Catalyst 1 preparation:

[0052] (1) Weigh nickel nitrate and cupric chloride and dissolve them in 70 g of deionized water, add 29 g of cyclohexane, 8.4 g of Triton X-100, and 7.7 g of n-butanol, stir well to form a microemulsion, impregnate 100 g of the carrier calcined at high temperature into the prepared microemulsion, shake for 40 min, filter out the remaining liquid, dry at 100° C. for 4 hours, and calcine at 400° C. for 4 hours to obtain a semi-finished catalyst A.

[0053] (2) Prepare palladium chloride into an active component impregnation solution, adjust the pH to 2.4, and then impregnate the semi-finished catalyst A into the prepared palladium active component solution for 40 minutes, dry at 100° C. for 4 hours, and calcine at 500° C. for 4 hours to obtain a semi-finished catalyst B.

[0054] (3) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of semi-finished catalyst B in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 120° C. for 3 hours and calcine it at 500° C. for 5 hours to obtain semi-finished catalyst C.

[0055] (4) Palladium chloride was dissolved in 70 g of deionized water, and 29 g of cyclohexane, 8.4 g of Triton X-100, and 7.7 g of n-butanol were added. The mixture was stirred thoroughly to form a microemulsion. The semi-finished catalyst C was placed in the prepared microemulsion, shaken for 40 min, and the remaining liquid was filtered off. The mixture was dried at 80 ° C for 6 h, and calcined at 400 ° C for 6 h. The desired catalyst was obtained.

[0056] The particle size of the microemulsions prepared in steps (1) and (4) was determined to be 120 nm by dynamic light scattering.

[0057] Catalyst reduction:

[0058] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 150°C for 10 hours.

[0059] Comparative Example 1

[0060] The same carrier as in Example 1 was used, and the catalyst preparation conditions were the same as in Example 1, except that Cu was not loaded.

[0061] (1) Weigh nickel nitrate and dissolve it in 70g of deionized water, add 29g of cyclohexane, 8.4g of Triton X-100, and 7.7g of n-butanol, stir well to form a microemulsion, impregnate 100g of the carrier calcined at high temperature into the prepared microemulsion, shake for 40min, filter out the remaining liquid, dry at 100°C for 4h, and calcine at 400°C for 4h. Obtain semi-finished catalyst A1.

[0062] (2) Prepare palladium chloride into an active component impregnation solution, adjust the pH to 2.4, and then impregnate the semi-finished catalyst A1 into the prepared palladium active component solution. After impregnation for 40 minutes, dry at 100° C. for 4 hours, and calcine at 500° C. for 4 hours to obtain the semi-finished catalyst B1.

[0063] (3) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst B1 in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 120° C. for 3 hours and calcine it at 500° C. for 5 hours to obtain the semi-finished catalyst C1.

[0064] (4) Palladium chloride was dissolved in 70 g of deionized water, and 29 g of cyclohexane, 8.4 g of Triton X-100, and 7.7 g of n-butanol were added. The mixture was stirred thoroughly to form a microemulsion. The semi-finished catalyst C1 was placed in the prepared microemulsion, shaken for 40 min, and the remaining liquid was filtered off. The mixture was dried at 80 ° C for 6 h, and calcined at 400 ° C for 6 h. The desired catalyst was obtained.

[0065] The particle size of the microemulsions prepared in steps (1) and (4) was determined to be 120 nm by dynamic light scattering.

[0066] Catalyst reduction:

[0067] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 150°C for 10 hours.

[0068] Comparative Example 2

[0069] The catalyst preparation process is the same as that of Comparative Example 1, except that the catalyst reduction temperature is 360°C.

[0070] Example 2

[0071] Support: A commercially available bimodal pore distribution cloverleaf strip alumina support with a diameter of 2.3-2.5 mm was used. After calcination at 950°C, the bimodal pore size distribution ranged from 10-13 nm and 50-180 nm, with a specific surface area of ​​120 m 2 Weigh 100 g of the carrier.

[0072] Catalyst 2 preparation:

[0073] (1) Weigh nickel chloride and copper nitrate and dissolve them in 75 g of deionized water. Add 30 g of n-hexane, 5.3 g of CTAB, and 4.5 g of n-pentanol. Stir thoroughly to form a microemulsion. Weigh 100 g of the carrier calcined at high temperature and impregnate it into the prepared microemulsion. Shake for 50 min and filter out the remaining liquid. Dry at 100° C. for 5 hours and calcine at 500° C. for 4 hours. Obtain semi-finished catalyst D.

[0074] (2) Prepare palladium chloride into an active component impregnation solution, adjust the pH to 2.4, and then impregnate the semi-finished catalyst D into the prepared Pd active component solution. After impregnation for 60 minutes, dry at 100°C for 5 hours, and calcine at 400°C for 6 hours. Obtain semi-finished catalyst E.

[0075] (3) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst E in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 140° C. for 2 hours and calcine it at 500° C. for 4 hours to obtain the semi-finished catalyst F.

[0076] (4) Palladium chloride was dissolved in 75 g of deionized water, and 30 g of n-hexane, 5.3 g of CTAB, and 4.5 g of n-pentanol were added. The mixture was stirred thoroughly to form a microemulsion. The semi-finished catalyst F was placed in the prepared microemulsion, shaken for 50 min, the remaining liquid was filtered off, and the mixture was washed with deionized water. The mixture was dried at 100 ° C for 5 hours and calcined at 450 ° C for 6 hours. The desired catalyst was obtained.

[0077] The particle size of the microemulsions prepared in steps (1) and (4) was determined to be 90 nm by dynamic light scattering.

[0078] Catalyst reduction:

[0079] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 200°C for 5 hours.

[0080] Comparative Example 3

[0081] The same carrier as in Example 2 was used, and the catalyst preparation conditions were the same as in Example 2, except that Cu was loaded by the solution method.

[0082] Catalyst preparation:

[0083] (1) Weigh nickel chloride and dissolve it in 75g of deionized water. Add 30g of n-hexane, 5.3g of CTAB, and 4.5g of n-pentanol. Stir thoroughly to form a microemulsion. Weigh 100g of the carrier calcined at high temperature and impregnate it into the prepared microemulsion. Shake for 50 minutes and filter out the remaining liquid. Dry at 100°C for 5 hours and calcine at 500°C for 4 hours. This is called semi-finished catalyst D1.

[0084] (2) Prepare palladium chloride into an active component impregnation solution, adjust the pH to 2.4, and then impregnate the semi-finished catalyst D1 into the prepared Pd active component solution. After impregnation for 60 minutes, dry at 100° C. for 5 hours, and calcine at 400° C. for 6 hours to obtain the semi-finished catalyst E1.

[0085] (3) Weigh manganese nitrate and copper nitrate and dissolve them in deionized water. Impartial catalyst E1 is immersed in the prepared manganese nitrate and copper nitrate solutions and shaken. After the solution is completely absorbed, it is dried at 140° C. for 2 hours and calcined at 500° C. for 4 hours to obtain semi-finished catalyst F1.

[0086] (4) Palladium chloride was dissolved in 75 g of deionized water, and 30 g of n-hexane, 5.3 g of CTAB, and 4.5 g of n-pentanol were added. The mixture was stirred thoroughly to form a microemulsion. The semi-finished catalyst F1 was placed in the prepared microemulsion, shaken for 50 min, the remaining liquid was filtered off, and the mixture was washed with deionized water. The mixture was dried at 100 ° C for 5 hours and calcined at 450 ° C for 6 hours. The desired catalyst was obtained.

[0087] The particle size of the microemulsions prepared in steps (1) and (4) was determined to be 90 nm by dynamic light scattering.

[0088] Catalyst reduction:

[0089] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 200°C for 5 hours.

[0090] Comparative Example 4

[0091] The catalyst preparation conditions were the same as those of Comparative Example 3, except that the catalyst reduction temperature was 250°C.

[0092] Example 3

[0093] Carrier: A commercially available bimodal pore distribution cloverleaf strip alumina-magnesium oxide carrier is used, with a magnesium content of 2.5% and a diameter of 2.3-2.5 mm. After calcination at 1000°C, the bimodal pore size distribution ranges from 14-19 nm and 90-270 nm, with a specific surface area of ​​112 m 2 Weigh 100 g of the carrier.

[0094] Catalyst 3 preparation:

[0095] (1) Nickel chloride and copper nitrate were weighed and dissolved in 70 g of deionized water, 30 g of cyclohexane, 13.5 g of Triton X-100, and 12.27 g of n-butanol were added, and the mixture was stirred thoroughly to form a microemulsion. 100 g of the carrier calcined at high temperature was impregnated into the prepared microemulsion, and the mixture was shaken for 80 min. The remaining liquid was filtered off, and the mixture was dried at 120° C. for 4 hours and calcined at 600° C. for 2.5 hours. The semi-finished catalyst G was obtained.

[0096] (2) Prepare palladium nitrate into an active component impregnation solution, adjust the pH to 2.2, and then impregnate the semi-finished catalyst G into the prepared palladium active component solution for 80 minutes, dry at 120° C. for 4 hours, and calcine at 500° C. for 4 hours to obtain the semi-finished catalyst H.

[0097] (3) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst H prepared in step (2) in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 150° C. for 2 hours, and calcine it at 500° C. for 6 hours to obtain the semi-finished catalyst I.

[0098] (4) Dissolve palladium nitrate in 70g of deionized water, add 30g of cyclohexane, 13.5g of Triton X-100, and 12.27g of n-butanol, stir well to form a microemulsion, place the semi-finished catalyst I in the prepared microemulsion, shake for 30min, filter out the remaining liquid, and wash with deionized water. Dry at 120°C for 3h, and calcine at 600°C for 2h. The desired catalyst is obtained.

[0099] The particle sizes of the microemulsions prepared in steps (1) and (4) were both 100 nm as determined by dynamic light scattering.

[0100] Catalyst reduction:

[0101] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 180°C for 6 hours.

[0102] Comparative Example 5

[0103] The same carrier as in Example 3 was used, and the catalyst preparation conditions were the same as in Example 3, except that the step of loading Pd by the microemulsion method was omitted.

[0104] Catalyst preparation:

[0105] (1) Nickel chloride and copper nitrate were weighed and dissolved in 70 g of deionized water, 30 g of cyclohexane, 13.5 g of Triton X-100, and 12.27 g of n-butanol were added, and the mixture was stirred thoroughly to form a microemulsion. 100 g of the carrier calcined at high temperature was impregnated into the prepared microemulsion, and the mixture was shaken for 80 min. The remaining liquid was filtered off, and the mixture was dried at 120° C. for 4 h and calcined at 600° C. for 2.5 h. The semi-finished catalyst G1 was obtained.

[0106] (2) Prepare palladium nitrate into an active component impregnation solution, adjust the pH to 2.2, and then impregnate the semi-finished catalyst G1 into the prepared palladium active component solution for 80 minutes, dry at 120° C. for 4 hours, and calcine at 500° C. for 4 hours to obtain the semi-finished catalyst H1.

[0107] (3) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst H1 prepared in step (2) in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 150° C. for 2 hours and calcine it at 500° C. for 6 hours to obtain the desired catalyst.

[0108] The particle size of the microemulsion prepared in step (1) was 100 nm as determined by dynamic light scattering.

[0109] Catalyst reduction:

[0110] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 180°C for 6 hours.

[0111] Comparative Example 6

[0112] The catalyst preparation conditions were the same as those in Comparative Example 5, except that the catalyst reduction temperature was 350°C.

[0113] Example 4

[0114] Carrier: A commercially available bimodal pore distribution spherical alumina carrier with a diameter of 2.6 μm was used. After calcination at 1050°C, the bimodal pore size distribution range was 15-25 nm and 150-340 nm, and the specific surface area was 85 m 2 Weigh 100 g of the carrier.

[0115] Catalyst 4 preparation:

[0116] (1) Weigh nickel nitrate and cupric chloride and dissolve them in 64 g of deionized water, add 32 g of n-hexane, 17.6 g of CTAB, and 14.66 g of n-butanol, stir well to form a microemulsion, impregnate 100 g of the carrier calcined at high temperature into the prepared microemulsion, shake for 60 min, filter out the remaining liquid, dry at 90°C for 4 h, and calcine at 600°C for 2 h. This is called semi-finished catalyst J.

[0117] (2) Dissolve palladium chloride in 64 g of deionized water, add 32 g of n-hexane, 17.6 g of CTAB, and 14.66 g of n-butanol to prepare an active component impregnation solution, stir thoroughly to form a microemulsion, place the semi-finished catalyst J in the prepared microemulsion, shake for 60 min, filter out the remaining liquid, and wash with deionized water. Dry at 90°C for 4 hours and calcine at 600°C for 2 hours. This is called semi-finished catalyst K.

[0118] (3) Prepare palladium chloride into an active component impregnation solution, adjust the pH to 2.3, and then impregnate the semi-finished catalyst K into the prepared palladium active component solution. After impregnation for 80 minutes, dry at 110° C. for 6 hours, and calcine at 500° C. for 4 hours. Obtain the semi-finished catalyst L.

[0119] (4) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst L in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 100° C. for 5 hours and calcine it at 450° C. for 6 hours to obtain the desired catalyst.

[0120] The particle size of the prepared microemulsion was determined by dynamic light scattering method and was 75 nm.

[0121] Catalyst reduction:

[0122] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 190°C for 7 hours.

[0123] Comparative Example 7

[0124] The carrier and preparation conditions are the same as those in Example 4, except that there is no Ni in the comparative example.

[0125] (1) Weigh copper chloride and dissolve it in 64 g of deionized water, add 32 g of n-hexane, 17.6 g of CTAB, and 14.66 g of n-butanol, stir well to form a microemulsion, impregnate 100 g of the carrier calcined at high temperature into the prepared microemulsion, shake for 60 min, filter out the remaining liquid, dry at 90°C for 4 hours, and calcine at 600°C for 2 hours. This is called semi-finished catalyst I1.

[0126] (2) Dissolve palladium chloride in 64 g of deionized water, add 32 g of n-hexane, 17.6 g of CTAB, and 14.66 g of n-butanol to prepare an active component impregnation solution, stir thoroughly to form a microemulsion, place the semi-finished catalyst I1 in the prepared microemulsion, shake for 60 min, filter out the remaining liquid, and wash with deionized water. Dry at 90°C for 4 hours and calcine at 600°C for 2 hours. This is called semi-finished catalyst J1.

[0127] (3) Prepare palladium chloride into an active component impregnation solution, adjust the pH to 2.0, and then impregnate the semi-finished catalyst J1 into the prepared palladium active component solution for 80 minutes, dry at 110° C. for 6 hours, and calcine at 500° C. for 4 hours to obtain the semi-finished catalyst K1.

[0128] (4) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst L1 in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 100°C for 5 hours and calcine it at 450°C for 6 hours to obtain the desired catalyst.

[0129] The particle size of the prepared microemulsion was determined by dynamic light scattering method and was 75 nm.

[0130] Catalyst reduction:

[0131] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 190°C for 7 hours.

[0132] Example 5

[0133] Support: A commercially available bimodal pore distribution cylindrical alumina support with a diameter of 3m and a length of 4m was used. After calcination at 990°C, the bimodal pore size distribution range was 11-19nm and 100-300nm, and the specific surface area was 108m 2 Weigh 100 g of the carrier.

[0134] Catalyst 5 preparation:

[0135] (1) palladium chloride is prepared into an active component impregnation solution, the pH value is adjusted to 2.5, 100 g of a carrier calcined at high temperature is impregnated into the active component impregnation solution, impregnated for 30 min, dried at 90° C. for 6 h, and calcined at 500° C. for 4 h to obtain a semi-finished catalyst M.

[0136] (2) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the prepared semi-finished catalyst M in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 120° C. for 3 hours, and calcine it at 500° C. for 6 hours to obtain a semi-finished catalyst N.

[0137] (3) Weigh nickel nitrate and cupric chloride and dissolve them in 70 g of deionized water. Add 14 g of heptane, 15 g of n-hexane, 10.15 g of Triton X-100, and 9.31 g of n-hexanol. Stir well to form a microemulsion. Impregnate the semi-finished catalyst N into the prepared microemulsion and shake for 70 min. Filter out the remaining liquid, dry at 80 °C for 6 h, and calcine at 600 °C for 2 h. This is called semi-finished catalyst O.

[0138] (4) Dissolve palladium chloride in 70g of deionized water, add 14g of heptane, 15g of n-hexane, 10.15g of Triton X-100, and 9.31g of n-hexanol to prepare an active component impregnation solution, stir well to form a microemulsion, place the semi-finished catalyst O in the prepared microemulsion, shake for 100min, filter out the remaining liquid, and wash with deionized water. Dry at 100°C for 6 hours, and calcine at 450°C for 6h to obtain the desired catalyst.

[0139] The particle size of the microemulsions prepared in steps (3) and (4) was determined to be 110 nm by dynamic light scattering.

[0140] Catalyst reduction:

[0141] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 160°C for 9 hours.

[0142] Comparative Example 8

[0143] The same carrier as in Example 5 was used, and the catalyst preparation conditions were the same as in Example 5, except that the order of preparation steps (3) and (4) was reversed.

[0144] Catalyst preparation:

[0145] (1) palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2.5, 100 g of a carrier calcined at high temperature was impregnated into the active component impregnation solution, and after impregnation for 30 min, the solution was dried at 90° C. for 6 h, and calcined at 500° C. for 4 h to obtain a semi-finished catalyst L1.

[0146] (2) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the prepared semi-finished catalyst L1 in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 120° C. for 3 hours and calcine it at 500° C. for 6 hours to obtain the semi-finished catalyst M1.

[0147] (3) Dissolve palladium chloride in 70g of deionized water, add 29g of n-hexane, 10.15g of Triton X-100, and 9.31g of n-hexanol to prepare an active component impregnation solution, stir thoroughly to form a microemulsion, and immerse the prepared semi-finished catalyst M1 in the prepared sodium stannate solution, shake for 100min, filter out the remaining liquid, and wash with deionized water. Dry at 100°C for 6 hours, and calcine at 450°C for 6h to obtain the semi-finished catalyst N1.

[0148] (4) Weigh nickel nitrate and cupric chloride and dissolve them in 70 g of deionized water. Add 29 g of n-hexane, 10.15 g of Triton X-100, and 9.31 g of n-hexanol. Stir thoroughly to form a microemulsion. Impregnate the semi-finished catalyst N1 into the prepared microemulsion and shake for 70 min. Filter out the remaining liquid, dry at 80° C. for 6 h, and calcine at 600° C. for 2 h to obtain the desired catalyst.

[0149] The particle size of the microemulsions prepared in steps (3) and (4) was determined to be 110 nm by dynamic light scattering.

[0150] Catalyst reduction:

[0151] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 160°C for 9 hours.

[0152] Example 6

[0153] Carrier: A commercially available bimodal pore distribution cloverleaf strip alumina-lanthanum oxide carrier is used, with a lanthanum metal content of 2% and a diameter of 2.3-2.5 mm. After calcination at 1020°C, the bimodal pore size distribution ranges from 13-25 nm and 85-320 nm, with a specific surface area of ​​85 m2 Weigh 100 g of the carrier.

[0154] Catalyst 6 Preparation:

[0155] (1) Weigh nickel nitrate and cupric chloride and dissolve them in 68 g of deionized water. Add 31 g of n-hexane, 15.5 g of Triton X-100, and 13.47 g of n-hexanol. Stir thoroughly to form a microemulsion. Weigh 100 g of the carrier calcined at high temperature and impregnate it into the prepared microemulsion. Shake for 50 min. Filter out the remaining liquid. Dry at 110° C. for 6 h. Calcinate at 500° C. for 2 h. This is called semi-finished catalyst P.

[0156] (2) palladium chloride is prepared into an active component impregnation solution, the pH value is adjusted to 2.4, and then the semi-finished catalyst P is impregnated into the prepared palladium active component solution. After impregnation for 30 minutes, the semi-finished catalyst is dried at 80° C. for 6 hours and calcined at 500° C. for 4 hours to obtain a semi-finished catalyst Q.

[0157] (2) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the prepared semi-finished catalyst Q in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 120° C. for 3 hours, and calcine it at 500° C. for 6 hours to obtain a semi-finished catalyst R.

[0158] (4) Dissolve palladium chloride in 82g of deionized water, 38.5g of cyclohexane, 18.0g of Triton X-100, and 17.0g of n-hexanol to prepare an active component impregnation solution, stir thoroughly to form a microemulsion, place the semi-finished catalyst R in the prepared microemulsion, shake for 30 minutes, filter out the remaining liquid, and wash with deionized water. Dry at 80°C for 6 hours and calcine at 450°C for 6 hours to obtain the desired catalyst.

[0159] The particle sizes of the microemulsions prepared in steps (1) and (4) were 90 nm and 80 nm, respectively, as determined by dynamic light scattering.

[0160] Catalyst reduction:

[0161] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 170°C for 6 hours.

[0162] Comparative Example 9

[0163] The catalyst preparation conditions were the same as those in Example 6, except that the catalyst reduction temperature was 500°C.

[0164] Example 7

[0165] Support: A commercially available bimodal pore distribution cloverleaf strip alumina support with a diameter of 2.3-2.5 mm was used. After calcination at 960°C, the bimodal pore size distribution ranged from 12-17 nm and 55-210 nm, with a specific surface area of ​​115 m 2 Weigh 100 g of the carrier.

[0166] Preparation of Catalyst 7:

[0167] (1) Weigh nickel nitrate and cupric chloride and dissolve them in 33 g of deionized water, add 26 g of n-hexane, 18.0 g of CTAB, and 15.0 g of n-pentanol, stir well to form a microemulsion, impregnate 100 g of the carrier calcined at high temperature into the prepared microemulsion, shake for 110 min, filter out the remaining liquid, dry at 100° C. for 6 h, and calcine at 500° C. for 2 h. This is called semi-finished catalyst S.

[0168] (2) palladium chloride is prepared into an active component impregnation solution, the pH value is adjusted to 2.4, and then the semi-finished catalyst S is impregnated into the prepared palladium active component solution. After impregnation for 50 minutes, the semi-finished catalyst S is dried at 90° C. for 6 hours, and calcined at 500° C. for 4 hours to obtain a semi-finished catalyst T.

[0169] (3) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst T in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 130° C. for 3 hours, and calcine it at 500° C. for 5 hours to obtain the semi-finished catalyst U.

[0170] (4) Dissolve palladium chloride in 70g of deionized water, add 35g of n-hexane, 21g of CTAB, and 20g of n-pentanol to prepare an active component impregnation solution, stir thoroughly to form a microemulsion, place the semi-finished catalyst U in the prepared microemulsion, shake for 60min, filter out the remaining liquid, wash with deionized water, dry at 90°C for 6h, and calcine at 450°C for 6h. The desired catalyst is obtained.

[0171] The particle sizes of the microemulsions prepared in steps (1) and (4) were 53 nm and 70 nm, respectively, as determined by dynamic light scattering.

[0172] Catalyst reduction:

[0173] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 150°C for 10 hours.

[0174] Comparative Example 10

[0175] The same carrier as in Example 7 was used, and compared with Example 7, steps (2) and (3) were swapped during catalyst loading.

[0176] Catalyst preparation:

[0177] (1) Weigh nickel nitrate and cupric chloride and dissolve them in 33 g of deionized water, add 26 g of n-hexane, 18.0 g of CTAB, and 15.0 g of n-pentanol, stir well to form a microemulsion, impregnate 100 g of the carrier calcined at high temperature into the prepared microemulsion, shake for 110 min, filter out the remaining liquid, dry at 100° C. for 6 h, and calcine at 500° C. for 2 h. This is called semi-finished catalyst O1.

[0178] (2) Weigh manganese nitrate and dissolve it in deionized water, immerse an equal volume of the semi-finished catalyst O1 in the prepared manganese nitrate solution, shake it, and after the solution is completely absorbed, dry it at 130° C. for 3 hours and calcine it at 500° C. for 5 hours to obtain the semi-finished catalyst P1.

[0179] (3) palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2.4, and then the semi-finished catalyst P1 was impregnated into the prepared palladium active component solution. After impregnation for 50 minutes, it was dried at 90°C for 6 hours and calcined at 500°C for 4 hours to obtain the semi-finished catalyst Q1.

[0180] (4) Dissolve palladium chloride in 70g of deionized water, add 35g of n-hexane, 21g of CTAB, and 20g of n-pentanol to prepare an active component impregnation solution, stir thoroughly to form a microemulsion, place the semi-finished catalyst Q1 in the prepared microemulsion, shake for 60min, filter out the remaining liquid, wash with deionized water, dry at 90°C for 6h, and calcine at 450°C for 6h. The desired catalyst is obtained.

[0181] The particle sizes of the microemulsions prepared in steps (1) and (4) were 53 nm and 70 nm, respectively, as determined by dynamic light scattering.

[0182] Catalyst reduction:

[0183] Before use, it was placed in a fixed bed reactor and reduced in a hydrogen atmosphere at 150°C for 10 hours.

[0184] The catalyst compositions of the examples are shown in Table 1.

[0185] Table 1 Example catalyst composition

[0186]

[0187] The performance of the catalyst in the hydrogen reaction of the crude isoprene feedstock in the cracking C5 fraction separation unit is as follows:

[0188] The catalyst loading in the adiabatic fixed bed reactor is 50 mL, the filler is 50 mL, and the reaction mass space velocity is 0.8 h -1 , operating pressure: 1.0MPa, hydrogen-oil volume ratio 100:1, reactor inlet temperature 30-35°C.

[0189] The composition of the hydrogenation reaction materials is shown in Table 2.

[0190] Table 2 Main components of unsaturated hydrocarbons in crude isoprene raw materials

[0191]

[0192] The results of catalyst hydrogenation evaluation are shown in Table 3. Catalysts 1, 2, 3, 4, 5, 6, and 7 are from Examples 1, 2, 3, 4, 5, 6, and 7, respectively. Comparative catalysts 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 are from Comparative Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10, respectively.

[0193] Table 3 Evaluation results of catalysts in Examples and Comparative Examples

[0194]

[0195] It can be seen from the evaluation results of the examples and comparative examples in Table 3 that the catalyst of the present invention not only has excellent hydrogenation activity and selectivity, but also has excellent anti-coking performance, which is beneficial to the long-term stable operation of the catalyst.

[0196] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A C5 fraction selective hydrogenation catalyst, the carrier of which is alumina or mainly alumina, and has a bimodal pore distribution structure and a specific surface area of ​​70 to 120 m 2 / g, where the pore size is 10-25nm and the pore size is 45-350nm; Features The catalyst contains at least Pd, Mn, Ni and Cu, with the weight of the catalyst being 100%, the Pd content being 0.2-0.6%, the molar ratio of Mn to Pd being 3-7:1, the Ni content being 0.5-5%, and the mass ratio of Cu to Ni being 0.1-1:1, wherein Ni and Cu are loaded in a microemulsion manner and distributed in the macropores of the carrier with a size of 45-350 nm; Mn is loaded in a solution method, palladium is loaded in two methods, a solution method and a microemulsion method, most of the Pd is loaded in a solution method, and a small part of the Pd is loaded in a microemulsion manner, so that the Pd loaded in the microemulsion manner is distributed in the macropores of the carrier, and the Pd and Mn loaded in the solution method are distributed in the small pores of the carrier; During the preparation of the catalyst, the step of loading Pd by microemulsion is after the step of loading Ni and Cu by microemulsion, and the step of loading Mn by solution method is after the step of loading Pd by solution method.

2. The C5 fraction selective hydrogenation catalyst according to claim 1, It is characterized in that Based on 100% of the weight of the catalyst, the Pd content is 0.3-0.5%, the molar ratio of Mn to Pd is 4-6:1, the Ni content is 1.5-3.5%, and the mass ratio of Cu to Ni is 0.2-0.6:

1.

3. The C5 fraction selective hydrogenation catalyst according to claim 1, It is characterized in that Most of the Pd is loaded by supersaturated impregnation method; the amount of Pd loaded by microemulsion method is 1 / 100 to 1 / 200 of the Ni+Cu content.

4. The C5 fraction selective hydrogenation catalyst according to any one of claims 1 to 3, Features The microemulsion loading process includes: dissolving the precursor salt in water, adding the oil phase, surfactant and co-surfactant, and stirring thoroughly to form a microemulsion, wherein the oil phase is a saturated alkane or cycloalkane, the surfactant is an ionic surfactant and / or a non-ionic surfactant, and the co-surfactant is an organic alcohol.

5. The C5 fraction selective hydrogenation catalyst according to claim 4, Features Oil phase is C 6 ~C 8 Saturated alkane or cycloalkane; the surfactant is an ionic surfactant and / or a nonionic surfactant; the cosurfactant is C 4 ~C 6 Alcohols.

6. The C5 fraction selective hydrogenation catalyst according to claim 5, It is characterized in that The oil phase is cyclohexane or n-hexane; the surfactant is polyethylene glycol octylphenyl ether or hexadecyltrimethylammonium bromide; and the co-surfactant is n-butanol and / or n-pentanol.

7. The C5 fraction selective hydrogenation catalyst according to claim 4, Features In the microemulsion, the weight ratio of the water phase to the oil phase is 1.2-2.5, the weight ratio of the surfactant to the oil phase is 0.3-0.7, and the weight ratio of the surfactant to the co-surfactant is 1-1.

2.

8. The C5 fraction selective hydrogenation catalyst according to claim 1, Features During the preparation of the catalyst, the order of solution method loading of Pd and loading of Ni / Cu is not limited.

9. The C5 fraction selective hydrogenation catalyst according to claim 1, It is characterized in that Al 2 O 3 The crystal form is a mixed crystal form of θ and α; the mass fraction of aluminum oxide in the catalyst carrier is more than 80%.

10. The C5 fraction selective hydrogenation catalyst according to claim 1, Features The preparation process specifically includes the following steps: (1) Dissolving Ni and Cu precursor salts in water, adding an oil phase, a surfactant and a co-surfactant, and stirring thoroughly to form a microemulsion, controlling the particle size of the microemulsion to be larger than the maximum pore size of the carrier small pores but smaller than the maximum pore size of the carrier large pores, adding the carrier to the prepared microemulsion and immersing for 0.5 to 4 hours, filtering out the remaining liquid, drying at 60 to 120° C. for 1 to 6 hours, and calcining at 300 to 600° C. for 2 to 8 hours to obtain a semi-finished catalyst A; (2) dissolving a precursor salt of Pd in ​​water, adjusting the pH to 2.0-2.5, then adding the semi-finished catalyst A to the Pd salt solution, immersing and adsorbing for 0.5-4 hours, drying at 100-120° C. for 1-4 hours, and calcining at 400-550° C. for 2-6 hours to obtain a semi-finished catalyst B; (3) The loading of Mn is carried out by a solution saturation impregnation method. After the semi-finished catalyst B is loaded with Mn, it is dried at 100-120° C. for 1-4 hours and calcined at 500-550° C. for 4-6 hours to obtain a semi-finished catalyst C; (4) Dissolve the Pd precursor salt in water, add the oil phase, surfactant and co-surfactant, and stir well to form a microemulsion. Control the particle size of the microemulsion to be larger than the maximum pore size of the carrier pores but smaller than the maximum pore size of the carrier pores. Add the semi-finished catalyst C to the prepared microemulsion and immerse for 0.5 to 4 hours. Filter out the remaining liquid, dry at 60 to 120° C. for 1 to 6 hours, and calcine at 300 to 600° C. for 2 to 8 hours to obtain the catalyst.

Citation Information

Patent Citations

  • Selectively hydrogenating catalyst and preparation method thereof

    CN101433845A

  • Non-noble metal supported selective hydrogenation catalyst and preparation method and application thereof

    CN101664682A

  • Selective hydrogenation catalyst for improving coking resistance

    CN104096572A

  • Selective hydrogenation catalyst for alkyne in ethane-ethylene fraction

    CN1176291A

  • Selective hydrogenation catalyst and its application condition

    CN1736589A