A method for large-scale batch preparation of porous organic cages using high-pressure homogenization
The porous organic cage is prepared by treating organic ligands and solvents through high-pressure homogenization method, which solves the problems of long preparation time, high energy consumption and inability to continuously produce in the prior art, and realizes efficient and environmentally friendly porous organic cage preparation, which is suitable for industrialization Production.
Patent Information
- Application Number
- CN202210127476.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-11
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-02-11
AI Technical Summary
The existing preparation methods of porous organic cages have problems such as long synthesis time, complex process, high energy consumption and inability to continuously produce, making it difficult to achieve industrial production.
The commonly used organic ligand and solvent were treated by high-pressure homogenizer through a high-pressure homogenizer, combined with catalysts (such as trifluoroacetic acid and acetic acid) to prepare a porous organic cage with a pressure of 5-500Mpa and 0.01- Over 5000 minutes, followed by suction filtration and drying to obtain a porous organic cage.
High-pressure homogenization method significantly shortens the preparation time, improves yield, achieves specific surface area and thermal stability comparable to the traditional method, and has the advantages of environmental protection and energy saving, simple operation, low cost and continuous production, suitable for industrial production .
Smart Images

Figure CN114478969B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer organic porous materials, and in particular relates to a method for preparing porous organic cages in large batches by high-pressure homogenization. Background Art
[0002] Porous organic cages (POCs) are cage-type organic molecules with a three-dimensional structure formed by covalent bonds of light elements such as C, H, O, N, and B. This type of material has attracted extensive attention from scientific researchers due to its rigid skeleton structure, durable shape, molecular cavities and windows, adjustable pore structure, and large specific surface area. It has broad application prospects in adsorption separation, energy storage, sensing, detection, catalysis, gas capture, etc.
[0003] The main preparation methods for porous organic cages are currently solvothermal method, solvothermal / volatilization method, microwave radiation method, twin-screw extrusion method and dynamic flow synthesis method, among which solvothermal method and solvothermal / volatilization method are the most common.
[0004] The preparation of porous organic cages by solvothermal or solvothermal / volatilization method has good universality for POCs materials, but this method has a long synthesis time, harsh reaction conditions, high energy consumption, low product yield, and cannot be carried out in continuous batch production. Professor Yuan Daqiang's research group used the solvothermal / volatilization method to obtain a series of POCs materials (J.Am.Chem.Soc.2020,142,18060-18072; Chem.Sci.,2021,12,13307–13315). After high-temperature treatment of the reaction system, this method still requires methanol volatilization for several weeks to obtain the product, which is energy-consuming and time-consuming, and is not suitable for industrial production; the microwave method is also difficult to achieve large-scale production due to its expensive equipment, inability to scale up, and high cost; Rebecca L. Greenaway et al. proposed the use of twin-screw extrusion to prepare porous organic cages CC3. Due to limited mass transfer, the BET specific surface area of the obtained material is low, and high temperature conditions are required, which has high energy consumption and is not conducive to industrial production (Chem. Sci., 2020, 11, 6582–6589). Although the dynamic flow synthesis method can achieve large-scale preparation, it cannot be produced continuously, and high temperature conditions are required during the synthesis process, which has high energy consumption and is not conducive to the industrial production of POCs. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing porous organic cages by high pressure homogenization (HPH), which solves many problems existing in the prior art, such as long synthesis time, complex process, high energy consumption, low yield and inability to continuously produce.
[0006] In order to achieve the above-mentioned invention object, the present invention provides the following technical solutions:
[0007] A method for preparing porous organic cages in large batches by high pressure homogenization comprises the following steps:
[0008] The POCs synthesized using common organic ligands as raw materials include but are not limited to porous organic cage materials connected by imines and borate esters; the solvent used is water or an organic solvent, and the organic solvent is but is not limited to one of N,N-dimethylformamide, N,N-dimethylacetamide, dioxane, ethanol, methanol, acetonitrile, tetrahydrofuran, and mesitylene; a catalyst is used or not used during the reaction. If a catalyst is used, the catalyst includes but is not limited to trifluoroacetic acid and acetic acid, etc., which can synthesize POCs. All the reaction raw materials are mixed and homogenized by a high-pressure homogenizer to obtain a porous organic cage.
[0009] Furthermore, the ligand raw materials required for synthesizing POCs are tetraaldehyde intercyclic calix[4]arene (C4RACHO) and p-phenylenediamine or benzidine.
[0010] Furthermore, the molar ratio of the ligand to the solvent is: C4RACHO: p-phenylenediamine or benzidine: solvent = 1: 0.1-10: 50-5000.
[0011] Furthermore, the method includes the step of uniformly mixing the raw materials, and the method of uniformly mixing the raw materials includes but is not limited to one of mechanical stirring, ultrasonic treatment, and heating and dissolving.
[0012] Furthermore, the homogenization pressure of the high-pressure homogenization reaction is 5-500 MPa, and the homogenization time is 0.01-5000 min.
[0013] Furthermore, the external environment of the high-pressure homogenizer is at normal temperature and pressure, or is an inert gas atmosphere.
[0014] Furthermore, after the high-pressure homogenization reaction is completed, the product is recovered by suction filtration or centrifugation, the obtained liquid is recovered for use in the next synthesis, and the obtained solid is washed and dried to obtain a porous organic cage.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) Compared with the solvent thermal method, solvent thermal / volatilization method, and microwave method, the high pressure homogenization method of the present invention can not only shorten the one-week preparation time required by the traditional solvent thermal / volatilization method to 2 minutes under the action of cavitation effect, impact effect, and shear effect, but also obtain POCs materials with crystallinity and Brunauer-Emmett-Teller (BET) specific surface area performance equivalent to those of the solvent thermal / volatilization method. In addition, the solvent used in the high pressure homogenization method can be recycled and continuous production can be achieved. However, the microwave method cannot achieve continuous production and does not have the conditions for industrial production. Therefore, compared with the solvent thermal method, solvent thermal / volatilization method, and microwave method, the high pressure homogenization method has the advantages of environmental protection and energy saving, short reaction time, simple operation, low cost, and continuous production.
[0017] (2) Compared with the twin-screw extrusion method, the present invention has better mass transfer efficiency. Under the action of cavitation effect, impact effect and shear effect of the high-pressure homogenizer, the obtained product has the advantages of good product crystallization performance, high specific surface area, low energy consumption, and environmental protection and energy saving.
[0018] (3) Compared with the dynamic flow synthesis method, the present invention has the advantages of low product energy consumption, environmental protection and energy saving, can be produced continuously, and has better industrial application potential.
[0019] (4) The porous organic cage prepared by the method described in the present invention has the same excellent thermal stability and BET specific surface area as the traditional solvothermal method or solvothermal / volatilization method for preparing POCs materials, and solves the shortcomings of high energy consumption, poor product crystallinity, low specific surface area, and inability to produce continuously in the twin-screw extrusion method and dynamic flow synthesis method, thereby achieving high efficiency, environmental protection, energy saving, and batch continuous production of POCs materials, and has important industrialization potential. It is worth mentioning that the solvent or catalyst used in the high-pressure homogenization reaction can be recycled. The POCs material prepared by recycling the solvent and catalyst mixture still has the same excellent performance. Therefore, this method has obvious economic advantages. In summary, the method of preparing POCs materials by high-pressure homogenization is of great significance to promoting the industrial production of POCs materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is the PXRD pattern of the porous organic cage: HPH-CPOC-301-2min of Example 1;
[0021] Figure 2 This is the infrared spectrum of the porous organic cage of Example 1: HPH-CPOC-301-2min;
[0022] Figure 3 This is the thermogravimetric spectrum of the porous organic cage of Example 1: HPH-CPOC-301-2min;
[0023] Figure 4This is the nitrogen adsorption spectrum of the porous organic cage: HPH-CPOC-301-2min in Example 1;
[0024] Figure 5 is the PXRD pattern of the porous organic cage: HPH-CPOC-301 of Example 2;
[0025] Figure 6 is the PXRD pattern of the porous organic cage: HPH-CPOC-301 of Example 3;
[0026] Figure 7 is the PXRD pattern of the porous organic cage: HPH-CPOC-301 of Example 4;
[0027] Figure 8 is the PXRD pattern of the porous organic cage: HPH-CPOC-301 of Example 5;
[0028] Fig. 9 is the PXRD pattern of the porous organic cage: HPH-CPOC-301 of Example 6;
[0029] Fig.10 is the PXRD pattern of the porous organic cage: HPH-CPOC-302-2min of Example 7; DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not limited to the present invention.
[0031] Example 1
[0032] S1. At room temperature and pressure, add C4RACHO (0.5 mmol) and p-phenylenediamine (1 mmol) into a 250 mL beaker, add 80 mL (578.4 mmol) of mesitylene, and sonicate for 5 min;
[0033] S2. At room temperature and pressure, add the above suspension into a high-pressure homogenizer, and circulate the homogenization reaction at a homogenization pressure of 100 MPa for 2 minutes;
[0034] S3. After the reaction is completed, the reaction suspension is collected in a beaker, and a vacuum filtration pump is used to filter to obtain a solid product. The filtrate is collected in a clean filtration bottle. The obtained filtrate is about 80 ml of mesitylene. The filtrate is recovered and stored for later use. The obtained solid is dried at 150°C for 12 hours to obtain HPH-CPOC-301-2min prepared by a high-pressure homogenization method, and the isolated yield is 83%.
[0035] Figure 1This is the PXRD spectrum corresponding to Example 1. It can be seen from the figure that the main characteristic peak position of HPH-CPOC-301 obtained by the high-pressure homogenization method is consistent with the CPOC-301 prepared by the solvent thermal / volatilization method reported in the literature (J.Am.Chem.Soc.2020,142,18060-18072), indicating that the porous organic cage prepared by this method has an ordered crystal structure.
[0036] Figure 2 The infrared spectrum corresponding to Example 1 shows that the main infrared characteristic peaks of HPH-CPOC-301-2min obtained by high pressure homogenization and CPOC-301 prepared by solvent thermal / evaporation method are CN 1289cm -1 、C=C1582cm -1 、C=O 1615cm -1 、C=CH 2955cm -1 The positions are consistent, indicating that the porous organic cage CPOC-301 was successfully prepared by this method.
[0037] Figure 3 : This is the thermogravimetric spectrum corresponding to Example 1. It can be seen from the figure that the thermogravimetric curves of POCs obtained by the high-pressure homogenization method are basically equivalent to those of CPOC-301 prepared by the solvent thermal / volatilization method, indicating that the POC prepared by the high-pressure homogenization method has a thermal stability comparable to that of the traditional solvent thermal method.
[0038] Figure 4 The nitrogen adsorption spectrum corresponding to Example 1 is shown in the figure. It can be seen that the BET of HPH-CPOC-301-2min obtained by high pressure homogenization is 1865m 2 / g, compared with the BET (1962m 2 This result shows that the POCs prepared by high-pressure homogenization method have excellent performance comparable to that of the traditional solvent thermal / volatilization method.
[0039] Example 2
[0040] S1. At room temperature and pressure, add C4RACHO (0.5 mmol) and p-phenylenediamine (1 mmol) into a 250 mL beaker, add 80 mL (578.4 mmol) of mesitylene, and sonicate for 5 min;
[0041] S2. At room temperature and pressure, add the above suspension into a high-pressure homogenizer and circulate the homogenization reaction at a homogenization pressure of 50 MPa for 60 minutes;
[0042] S3. After the reaction is completed, the reaction suspension is collected in a beaker, and a solid product is obtained by suction filtration. The filtrate is recovered and stored for later use. The obtained solid is dried at 150°C for 12 hours to obtain HPH-CPOC-301 prepared by a high pressure homogenization method, and the isolated yield is 81%.
[0043] Figure 5 3 is the PXRD spectrum corresponding to Example 2. It can be seen from the figure that the main characteristic peak positions of HPH-CPOC-301 obtained by the high-pressure homogenization method at a homogenization pressure of 50 MPa and a homogenization time of 60 min are consistent with those of HPH-CPOC-301 obtained at a homogenization pressure of 100 MPa, and the crystallinity is good, indicating that reducing the homogenization pressure and extending the homogenization time can also obtain CPOC-301 with good crystallinity.
[0044] Example 3
[0045] S1. At room temperature and pressure, add C4RACHO (0.5 mmol) and p-phenylenediamine (1 mmol) into a 250 mL beaker, add 70 mL (506.1 mmol) of mesitylene, and use ultrasound for 5 min;
[0046] S2. At room temperature and pressure, add the above suspension into a high-pressure homogenizer, and circulate the homogenization reaction at a homogenization pressure of 100 MPa for 2 minutes;
[0047] S3. After the reaction is completed, the reaction suspension is collected in a beaker, and a solid product is obtained by suction filtration. The filtrate is recovered and stored for later use. The obtained solid is dried at 150°C for 12 hours to obtain HPH-CPOC-301 prepared by a high-pressure homogenization method, and the isolated yield is 80%.
[0048] Figure 6 3 is the PXRD spectrum corresponding to Example 3. It can be seen from the figure that when the addition amount of the solvent mesitylene is adjusted from 80 ml in Example 1 to 70 ml, HPH-CPOC-301 with good crystallinity can also be obtained, indicating that adjusting the addition amount of the solvent can obtain CPOC-301 with good crystallinity.
[0049] Example 4
[0050] S1. At room temperature and pressure, C4RACHO (0.5 mmol) and p-phenylenediamine (1 mmol) were added to a 250 mL beaker, and 80 mL (578.4 mmol) of mesitylene obtained by filtration in Example 1 was added, and ultrasonicated for 5 min;
[0051] S2. At room temperature and pressure, add the above suspension into a high-pressure homogenizer, and circulate the homogenization reaction at a homogenization pressure of 100 MPa for 2 minutes;
[0052] S3. After the reaction is completed, the reaction suspension is collected in a beaker, and a solid product is obtained by suction filtration. The filtrate is recovered and stored for later use. The obtained solid is dried at 150°C for 12 hours to obtain HPH-CPOC-301 prepared by a high-pressure homogenization method, and the isolated yield is 82%.
[0053] Figure 7 3 is the PXRD spectrum corresponding to Example 4. It can be seen from the figure that CPOC-301 with good crystallinity can still be obtained by using the solvent obtained by filtration in Example 1 to prepare CPOC-301, indicating that the solvent can be recycled.
[0054] Example 5
[0055] S1. At room temperature and pressure, C4RACHO (0.5 mmol) and p-phenylenediamine (1 mmol) were added to a 250 mL beaker, and 80 mL (578.4 mmol) of mesitylene obtained by filtration in Example 4 was added, and ultrasonicated for 5 min;
[0056] S2. At room temperature and pressure, add the above suspension into a high-pressure homogenizer, and circulate the homogenization reaction at a homogenization pressure of 100 MPa for 2 minutes;
[0057] S3. After the reaction is completed, the reaction suspension is collected in a beaker, and a solid product is obtained by suction filtration. The filtrate is recovered and stored for later use. The obtained solid is dried at 150°C for 12 hours to obtain HPH-CPOC-301 prepared by a high pressure homogenization method, and the isolated yield is 81%.
[0058] Figure 8 : This is the PXRD spectrum corresponding to Example 5. It can be seen from the figure that CPOC-301 with good crystallinity can still be obtained by recycling the homogenizing solvent twice, indicating that the solvent has good recyclability and is conducive to industrial production.
[0059] Example 6
[0060] S1. At room temperature and pressure, add C4RACHO (0.5 mmol) and p-phenylenediamine (1 mmol) into a 250 mL beaker, add 80 mL (578.4 mmol) of mesitylene, and sonicate for 5 min;
[0061] S2. To explore the effect of inert gas atmosphere on the synthesis, the feed port of the homogenizer was changed from normal temperature and pressure to inert (nitrogen) gas atmosphere conditions, and the above suspension was added to the high-pressure homogenizer, and the homogenization reaction was circulated at a homogenization pressure of 100 MPa for 2 minutes;
[0062] S3. After the reaction is completed, the reaction suspension is collected in a beaker, and a vacuum filtration pump is used to filter to obtain a solid product. The filtrate is collected in a clean filtration bottle. The obtained filtrate is about 80 ml of mesitylene. The filtrate is recovered and stored for later use. The obtained solid is dried at 150°C for 12 hours to obtain HPH-CPOC-301-2min prepared by a high-pressure homogenization method, and the isolated yield is 84%.
[0063] Fig. 9 This is the PXRD spectrum corresponding to Example 6. It can be seen from the figure that under an inert gas atmosphere, the main characteristic peak position of HPH-CPOC-301 obtained by the high-pressure homogenization method is consistent with that of CPOC-301 prepared by the solvent thermal / volatilization method reported in Example 1 and the literature (J.Am.Chem.Soc.2020,142,18060-18072), indicating that the porous organic cage prepared by this method has an ordered crystal structure.
[0064] Example 7
[0065] S1. At room temperature and pressure, add C4RACHO (0.5 mmol) and benzidine (1 mmol) into a 250 mL beaker, add 80 mL (578.4 mmol) of mesitylene, and sonicate for 5 min;
[0066] S2. At room temperature and pressure, add the above suspension into a high-pressure homogenizer, and circulate the homogenization reaction at a homogenization pressure of 100 MPa for 2 minutes;
[0067] S3. After the reaction is completed, the reaction suspension is collected in a beaker, and a vacuum filtration pump is used to filter to obtain a solid product. The filtrate is collected in a clean filtration bottle. The obtained filtrate is about 80 ml of mesitylene. The filtrate is recovered and stored for later use. The obtained solid is dried at 150°C for 12 hours to obtain HPH-CPOC-301-2min prepared by a high-pressure homogenization method, and the isolated yield is 81%.
[0068] Fig.10 This is the PXRD spectrum corresponding to Example 7. It can be seen from the figure that the main characteristic peak position of HPH-CPOC-302 obtained by the high-pressure homogenization method is basically consistent with the CPOC-302 prepared by the solvent thermal / volatilization method reported in the literature (J.Am.Chem.Soc.2020,142,18060-18072), indicating that the porous organic cage prepared by this method has an ordered crystal structure.
[0069] The present invention adopts a high-pressure homogenization method to prepare POCs materials, which greatly improves the efficiency of POCs preparation while maintaining the thermal stability and specific surface area of the POCs materials. Compared with the solvent thermal method, solvent thermal / volatilization method, and microwave method, the preparation process of the high-pressure homogenization method is green and environmentally friendly, the synthesis operation is simple, the efficiency is high, and the cost is low; compared with the twin-screw extrusion method, it has better raw material mass transfer efficiency, thereby obtaining a better degree of polymerization and specific surface area, and ensuring the performance of the resulting POCs. Compared with the dynamic flow synthesis method, it has the advantages of lower energy consumption and continuous production. In addition, this method can realize that the solvent used can be recycled for many times, and it fully meets the requirements of industrial production in terms of scale and cost. In summary, the high-pressure homogenization method provides great guarantees for the industrial production of POCs from various aspects such as production cost, green environmental protection, and product performance.
[0070] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. Those familiar with the art can easily make various modifications to these embodiments: including but not limited to modifying all ligands that can synthesize POCs, modifying the solvents used for the ligands, modifying the reaction ligand ratio, solvent ratio, catalyst dosage, etc., modifying the homogenization pressure, time, temperature, etc., and applying the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments described herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing porous organic cages in large batches by high pressure homogenization, characterized in that: The ligand raw materials required for synthesizing POCs are tetraaldehyde intercyclic calix[4]arene C4RACHO and p-phenylenediamine or benzidine, and the solvent used is water or an organic solvent, and the organic solvent is not limited to one of N,N-dimethylformamide, N,N-dimethylacetamide, dioxane, ethanol, methanol, acetonitrile, tetrahydrofuran, and mesitylene; no catalyst is used in the reaction process; The molar ratio of the ligand to the solvent is: C4RACHO: p-phenylenediamine or benzidine: solvent = 1: 0.1-10: 50-5000; The homogenization pressure of the high-pressure homogenization reaction is 5-500 MPa, and the homogenization time is 0.01-5000 min.
2. The method for preparing porous organic cages in large batches by high pressure homogenization according to claim 1, characterized in that: The method comprises the step of uniformly mixing the raw materials, wherein the method of uniformly mixing the raw materials comprises one of mechanical stirring, ultrasonic treatment and heating dissolution.
3. The method for preparing porous organic cages in large batches by high pressure homogenization according to claim 1, characterized in that: The external environment of the high-pressure homogenizer is normal temperature and pressure, or an inert gas atmosphere.
4. The method for preparing porous organic cages in large batches by high pressure homogenization according to claim 1, characterized in that: After the high-pressure homogenization reaction is completed, the product is recovered by suction filtration or centrifugation, and the obtained liquid is recovered for the next synthesis. The obtained solid is washed and dried to obtain a porous organic cage.