A method for melting and treating waste circuit boards
By introducing copper ice, water quenching slag and iron-containing auxiliary materials into the waste circuit board and performing oxygen-rich smelting at high temperatures, the problem of difficulty in sufficient melting of copper components in the prior art is solved, and the copper recovery rate is significantly improved. A comprehensive recycling and treatment of multiple waste materials has been realized.
Patent Information
- Application Number
- CN202111661431.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-12-30
AI Technical Summary
The existing high-temperature smelting treatment methods are difficult to fully melt the copper components in the waste circuit board, resulting in limited copper recovery.
Preliminary pyrolysis is used to obtain the pyrolysis product of the waste circuit board, and mixed it with ice copper, water quenching slag and iron-containing auxiliary materials, and oxygen-rich smelting at 1300-1400℃. After smelting and layering, the lower layer material is derived for water-cooled ingots. , obtain a crude copper ingot.
The copper recycling rate in waste circuit boards has been significantly improved, and the comprehensive recycling and treatment of multiple waste materials has been realized, which has improved the recycling rate.
Smart Images

Figure CN114480848B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid waste recycling, in particular to a method for smelting and treating waste circuit boards. Background Art
[0002] With the continuous development of the electronics and information industry, the total amount of electronic waste has shown an expansive growth. Electronic waste not only contains a large amount of valuable metals, such as copper, tin, iron, aluminum and other precious metals, but also contains a large amount of plastics, resins, ceramics and other materials, which have a high resource recovery value, especially printed circuit boards, which are the basic products of the electronics industry and are an indispensable part of various electronic products. Printed circuit boards are mainly composed of organic reinforced resins, glass fibers, copper foils and electronic components, of which metals such as copper, gold, silver, platinum, palladium, lead, tin, nickel, iron and aluminum account for more than 95%, and have extremely high recycling value. However, due to the complex composition of circuit boards and the large number of elements, the comprehensive treatment of circuit boards is quite difficult.
[0003] In the prior art, high-temperature smelting is often used to recycle waste circuit boards. However, when the traditional smelting method is used at 1100-1400°C, since the pyrolysis products of waste circuit boards are a complex mixture of metal elements, metal oxides and other components, the metal copper and copper oxides are often difficult to fully melt and react during the actual smelting process, and are mixed and solidified with other metal components prematurely, which limits the recovery rate of copper. Therefore, a new treatment method is needed to solve the above existing problems. Summary of the invention
[0004] The object of the present invention is to provide a method for smelting and treating waste circuit boards, which is used to solve the problem that the existing high-temperature smelting process for treating waste circuit boards is difficult to fully melt the copper component, thereby limiting the copper recovery rate.
[0005] In order to solve the above technical problems, the present invention provides a method for smelting and treating waste circuit boards, comprising the following steps: preliminarily pyrolyzing the waste circuit boards to obtain pyrolysis products of the waste circuit boards; uniformly mixing the pyrolysis products of the waste circuit boards, matte, water-quenched slag, iron-containing auxiliary materials and anthracite to obtain a smelting mixture; oxygen-enriched smelting the smelting mixture at 1300-1400°C, conducting a lower layer material out after smelting and stratification, and recovering the crude copper ingot after cooling.
[0006] Preferably, the mass proportion of each component raw material in the smelting mixture is: 15-30% of circuit board pyrolysis product, 20-35% of scrap copper, 10-20% of water-quenched slag, 5-15% of iron-containing auxiliary materials, and 15-35% of anthracite.
[0007] Preferably, the copper content in the matte is 20-50%, and the iron content is 10-30%.
[0008] Preferably, the temperature of the initial pyrolysis is 250-800° C., and the pyrolysis time is 1-2 hours.
[0009] Preferably, the iron-containing auxiliary material is any one of copper sulfide slag and industrial iron mud, or a mixture of the two.
[0010] Preferably, the water-quenched slag is smelting waste slag containing silicon-calcium-iron oxides produced in the industrial smelting process of copper and lead.
[0011] Preferably, in the oxygen-enriched smelting process, the smelting time is 1.5 to 3 hours.
[0012] Preferably, during the oxygen-enriched smelting process, the oxygen concentration in the oxygen-enriched air is 50-75%, and the oxygen-carbon ratio is 1.9-2.8, where the oxygen-carbon ratio is the ratio of the volume of oxygen to the mass of carbon in the anthracite.
[0013] Preferably, the smelting mixture is subjected to oxygen-enriched smelting in an oxygen-enriched side-blown smelting pool, and after smelting and stratification, the lower layer of material is led out to a steel casting mold for water-cooled ingot casting to obtain a crude copper ingot.
[0014] Preferably, the mass percentage of metallic copper in the crude copper ingot is greater than 90%.
[0015] The beneficial effects of the present invention are as follows: Different from the prior art, the present invention provides a method for smelting and treating waste circuit boards. By introducing matte, water-quenched slag and iron-containing auxiliary materials, the pyrolysis products of the waste circuit boards are more easily and fully reacted under the condition of unchanged smelting temperature, thereby significantly improving the recovery rate of copper in the waste circuit boards; at the same time, the method realizes the comprehensive recovery and treatment of multiple waste materials, thereby significantly improving the recovery rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a process flow chart of one embodiment of the method for smelting waste circuit boards in the present invention. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] See also Figure 1 The present invention provides a method for smelting and treating waste circuit boards, comprising the following steps:
[0019] S1. Performing preliminary pyrolysis on the waste circuit boards to obtain pyrolysis products of the waste circuit boards. In this step, the preliminary pyrolysis temperature is 250-800° C. and the pyrolysis time is 1-2 hours.
[0020] S2. Evenly mix the pyrolysis products of waste circuit boards, copper matte, water-quenched slag, iron-containing auxiliary materials and anthracite to obtain a smelting mixture. In this step, the mass proportion of each component raw material in the smelting mixture is: 15-30% of circuit board pyrolysis products, 20-35% of waste copper, 10-20% of water-quenched slag, 5-15% of iron-containing auxiliary materials, and 15-35% of anthracite. Among them, the copper content in copper matte is 20-50%, and the iron content is 10-30%; the iron-containing auxiliary material is any one or a mixture of two of copper sulfide slag and industrial iron mud; the water-quenched slag is the smelting waste slag containing silicon-calcium-iron oxides produced in the process of industrial copper and lead smelting.
[0021] S3. Smelting the smelting mixture at 1300-1400°C with oxygen-enriched smelting, and after smelting and stratification, the lower layer material is discharged, and after cooling, the crude copper ingot is recovered. In this step, the smelting mixture is oxygen-enriched smelting in an oxygen-enriched side-blown smelting pool, and after smelting and stratification, the lower layer material is discharged to a cast steel mold for water-cooled ingot casting to obtain a crude copper ingot, and the mass percentage of metallic copper in the obtained crude copper ingot is greater than 90%; the oxygen-enriched smelting time is 1.5-3h, the oxygen concentration in the oxygen-enriched air is 50-75%, and the oxygen-carbon ratio is 1.9-2.8, where the oxygen-carbon ratio is the ratio of the volume of oxygen to the mass of carbon in anthracite.
[0022] The mechanism of the present invention is that the introduction of matte with lower Cu and Fe grades reduces the conditions for the melting reaction of metallic copper and copper oxide in the smelting mixture, thereby making it easier to fully react under the condition of unchanged smelting temperature, and at the same time promoting the enrichment of Cu at high temperature, thereby improving the recovery rate of copper in waste circuit boards; by introducing water-quenched slag, the slag type of the smelting mixture is adjusted to achieve a state suitable for melting reaction, and after oxygen-enriched smelting, the iron component is precipitated in the form of iron oxide and separated from the molten copper component; in addition, the method not only treats the pyrolysis products of the waste circuit boards, but also treats industrial wastes such as water-quenched slag and industrial iron mud, thereby realizing the comprehensive recovery and treatment of multiple wastes and significantly improving the recovery rate.
[0023] The treatment effect of the smelting treatment method of waste circuit boards of the present invention is analyzed below through specific examples and comparative examples. In the following examples, matte and anthracite with the same chemical composition are used. Specifically, the copper content in the matte is 40%, and the iron content is 15%; in terms of mass percentage, the fixed carbon content in the anthracite is 81.58%, the ash content is 11.58%, the volatile components are 6.3%, and the sulfur content is 0.45%.
[0024] Example 1
[0025] The steps of smelting treatment of waste circuit boards in this embodiment are as follows:
[0026] (1) The waste circuit board is subjected to preliminary pyrolysis at a temperature of 600° C. for 1 h to obtain a pyrolysis product of the waste circuit board.
[0027] (2) In terms of mass percentage, 18% of pyrolysis products of waste circuit boards, 35% of matte, 12% of water-quenched slag, 10% of industrial iron mud and 25% of anthracite are mixed evenly to obtain a smelting mixture.
[0028] (3) The smelting mixture is subjected to oxygen-enriched smelting in an oxygen-enriched side-blown smelting pool at 1350° C. The oxygen-enriched smelting time is 2 h. The oxygen concentration in the oxygen-enriched air is 50%, and the molar ratio of oxygen to carbon is 2. After smelting and stratification, the lower layer of material is discharged onto a steel casting mold for water-cooling ingot casting to obtain a crude copper ingot.
[0029] Example 2
[0030] This embodiment is based on the processing steps of Example 1, except that the ratio of each raw material in the smelting mixture is different. Specifically, the ratio of each raw material in the smelting mixture in this embodiment is: 28% pyrolysis product of waste circuit boards, 27% matte, 18% water-quenched slag, 8% industrial iron mud and 19% anthracite. Other processing steps and parameters are consistent with Example 1.
[0031] Example 3
[0032] This embodiment is based on the processing steps of Example 1, except that the ratio of each raw material in the smelting mixture is different. Specifically, the ratio of each raw material in the smelting mixture in this embodiment is: 33% pyrolysis product of waste circuit boards, 24% matte, 15% water-quenched slag, 6% industrial iron mud and 22% anthracite. Other processing steps and parameters are consistent with Example 1.
[0033] Comparative Example 1
[0034] This embodiment is based on the processing steps of Example 1, except that no matte component is added to the raw materials of the smelting mixture, other components and proportions are consistent with those of Example 1, and other processing steps and parameters are also consistent with those of Example 1.
[0035] The composition analysis of the pyrolysis products of the waste circuit boards in Examples 1 to 3 and Comparative Example 1 was performed, and the contents of specific components are shown in Table 1.
[0036] Table 1
[0037] Components Cu / % Al / % Si / % Ca / % Fe / % Zn / % Sn / % C / % Pyrolysis products of waste circuit boards 18.47 4.96 6.31 3.65 8.5 1.7 3.88 13.66
[0038] The components of the crude copper ingots obtained after the treatment in Examples 1 to 3 and Comparative Example 1 were analyzed, and the corresponding recovery rates were statistically analyzed, and the results are shown in Table 2. As can be seen from the data in Table 2, Examples 1 to 3 are all cases where matte is introduced, and the Cu content in the prepared crude copper ingots is more than 90%, and the copper recovery rate is more than 99%; while Comparative Example 1 is a case where matte is not introduced, and both the Cu content in the prepared crude copper ingot and the copper recovery rate are lower than Examples 1 to 3, which proves that the copper recovery rate can be improved after adding matte when the smelting temperature remains unchanged. In addition, by comparing the data of Examples 1 to 2 in Table 2 with the data of Example 3, it can be found that the Cu content and the copper recovery rate in the crude copper ingot prepared in Example 3 are lower than those of Examples 1 to 2. This is because the raw material components of the smelting mixture in Examples 1 to 2 are all within the aforementioned limited range, while the pyrolysis product of the circuit board in Example 3 exceeds the aforementioned limited range, which makes the content of the pyrolysis product of the circuit board in Example 3 too high and the content of matte too low. The amount of matte introduced is not enough to cooperate with the pyrolysis product of the circuit board to achieve a better effect of promoting the melting reaction. Therefore, it is explained that the raw materials in the smelting mixture need to be under the aforementioned limited ratio conditions to obtain a better copper recovery effect.
[0039] Table 2
[0040]
[0041] Different from the prior art, the present invention provides a method for smelting and treating waste circuit boards. By introducing matte, water-quenched slag and iron-containing auxiliary materials, the pyrolysis products of the waste circuit boards are more easily and fully reacted under the condition of unchanged smelting temperature, thereby significantly improving the recovery rate of copper in the waste circuit boards; at the same time, the method realizes the comprehensive recovery and treatment of multiple waste materials, significantly improving the recovery rate.
[0042] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.
[0043] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for melting and treating waste circuit boards, It is characterized in that The steps include: Performing preliminary pyrolysis on the waste circuit boards to obtain pyrolysis products of the waste circuit boards; The waste circuit board pyrolysis product, matte, water-quenched slag, iron-containing auxiliary materials and anthracite are uniformly mixed to obtain a smelting mixture; The smelting mixture is subjected to oxygen-enriched smelting at 1300-1400° C., the lower layer material is discharged after smelting and layering, and the crude copper ingot is recovered after cooling; In terms of mass percentage, the pyrolysis product of the waste circuit board includes the following components: Cu18.47%, Al4.96%, Si6.31%, Ca3.65%, Fe8.5%, Zn1.7%, Sn3.88% and C13.66%; The mass proportion of each component raw material in the smelting mixture is: 15-30% of circuit board pyrolysis product, 20-35% of matte, 10-20% of water-quenched slag, 5-15% of iron-containing auxiliary materials, and 15-35% of anthracite; The copper content in the matte is 20-50%, and the iron content is 10-30%; The iron-containing auxiliary material is any one of copper sulfide slag and industrial iron mud, or a mixture of the two; The water-quenched slag is smelting waste slag containing silicon, calcium and iron oxides produced in the process of industrial copper and lead smelting.
2. The method for smelting and treating waste circuit boards according to claim 1, It is characterized in that The temperature of the preliminary pyrolysis is 250-800°C, and the pyrolysis time is 1-2 h.
3. According to the method for smelting and treating waste circuit boards as described in claim 1, It is characterized in that In the oxygen-enriched smelting process, the smelting time is 1.5 to 3 hours.
4. The method for smelting and treating waste circuit boards according to claim 1, It is characterized in that During the oxygen-enriched smelting process, the oxygen concentration in the oxygen-enriched air is 50-75%, and the oxygen-carbon ratio is 1.9-2.8, where the oxygen-carbon ratio is the ratio of the volume of oxygen to the mass of carbon in the anthracite.
5. According to the method for smelting and treating waste circuit boards as described in claim 1, It is characterized in that The smelting mixture is oxygen-enriched smelted in an oxygen-enriched side-blown smelting pool, and after smelting and stratification, the lower layer of material is led out to a steel casting mold for water-cooled ingot casting to obtain the crude copper ingot.
6. According to the method for smelting and treating waste circuit boards as claimed in claim 5, It is characterized in that The mass percentage of metallic copper in the crude copper ingot is greater than 90%.
Citation Information
Patent Citations
Method for recovering valuable metals in copper-containing electronic wastes
CN112708766A
Method for recovering valuable metals by smelting electronic wastes and multi-metal solid wastes