Electroplating seed layer construction and repair

By using high-power pulsed current and barrier layer technology in the semiconductor electroplating chamber, the problem of uneven coverage of the seed layer in high aperture ratio structures is solved, achieving a more efficient electroplating process and increasing productivity.

CN114481240BActive Publication Date: 2024-10-11APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111240314.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-23
Filing Date
2021-10-25
Publication Date
2024-10-11
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

During the semiconductor electroplating process, the characteristic structure with high aperture ratio leads to uneven coverage of the seed layer, which may form voids and insufficient conductivity. Traditional repair technology requires additional processing chambers and annealing operations, reducing yield.

Method used

High-power pulse current is used to build and repair the seed layer in the electroplating chamber. By forming a barrier layer and a copper seed layer on the substrate, a combination of pulse DC current and continuous DC current is used to control the current density and frequency. Ensure even plating and adequate coverage.

Benefits of technology

The seed layer coverage and plating uniformity are improved, yield loss is reduced, additional processing steps and annealing operations are avoided, and the efficiency and quality of electroplating operations are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114481240B_ABST
    Figure CN114481240B_ABST
Patent Text Reader

Abstract

Exemplary electroplating methods may include delivering current from a power source through a plating bath of a plating chamber for a first time period. The delivered current may be or may include a pulsed current with a duty cycle of less than or approximately 50%, and the methods may include plating a first amount of metal on a substrate within the plating bath. The substrate may define a via within the substrate. The methods may include, after the first time period, switching the power source to a continuous DC current delivery for a second time period. The methods may include plating a second amount of metal on the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of U.S. Patent Application No. 17 / 079,127, filed on October 23, 2020, entitled “ELECTROPLATING SEED LAYER BUILDUP AND REPAIR,” which is hereby incorporated by reference in its entirety. Technical Field

[0003] The present technology relates to electroplating operations in semiconductor processing. More particularly, the present technology relates to systems and methods for performing seed layer buildup in an electroplating system. Background Art

[0004] Integrated circuits are made possible by processes that create intricately patterned layers of material on a substrate surface. After forming, etching, and other processing on the substrate, metal or other conductive material is often deposited or formed to provide electrical connections between components. Because this metallization can be performed after many manufacturing operations, problems that occur during this metallization can result in expensive scrapped substrates or wafers.

[0005] Electroplating is performed in an electroplating chamber, with the target side of the wafer in a bath of liquid electrolyte, and electrical contacts on the contact ring contact a conductive layer on the surface of the wafer, such as a seed layer. Current flows from a power source through the electrolyte and the conductive layer. The metal ions in the electrolyte are plated outward onto the wafer, producing a metal layer on the wafer. When the wafer has uneven features defined across the surface, the seed layer may be incomplete or characterized by variable thickness of these features along the wafer. These variations can be challenging for electroplating operations, which benefit from a seed layer of uniform thickness and sufficient conductivity. Plating on a seed layer with thin metal or missing metal may result in voids or unevenly plated layers.

[0006] Therefore, there is a need for improved systems and methods that can be used to produce high quality devices and structures. These and other needs are addressed by the present technology. Summary of the invention

[0007] Exemplary electroplating methods may include delivering current from a power source through a plating bath of a plating chamber for a first time period. The delivered current may be or may include a pulsed current having a duty cycle of less than or approximately 50%, and the methods may include plating a first amount of metal on a substrate within the plating bath. The substrate may define a via within the substrate. The methods may include, after the first time period, switching the power source to a continuous DC current delivery for a second time period. The methods may include plating a second amount of metal on the substrate.

[0008] In some embodiments, the current delivered during the first time period can be characterized by an operational frequency of less than or about 1000 Hz. The average current density during the first time period can be less than or about 3 mA / cm 2 . The average current density during the second time period may be greater than or equal to the average current density during the first time period. The peak current during the second time period may be less than or approximately 2 amps. The peak current during the first time period may be greater than or approximately 2 amps. During the second time period, the average current density may increase over time. The via defined in the substrate may be characterized by a depth greater than or approximately 10 μm. A barrier layer may be formed along the walls of the via defined in the substrate. The barrier layer may include one or more of titanium or tantalum, and the deposited metal may be or include copper.

[0009] Some embodiments of the present technology may include electroplating methods. The methods may include delivering current from a power supply through a plating bath of a plating chamber for a first time period. The power supply may operate in pulsed DC delivery at a frequency of less than or about 750 Hz during the first time period. The methods may include plating a first amount of copper on a substrate within the plating bath. The methods may include, after the first time period, switching the power supply to continuous DC current delivery for a second time period. The methods may include plating a second amount of copper on the substrate.

[0010] In some embodiments, the on-time of each pulse during the first time period may be less than or approximately 100 ms. During the first time period, the power supply may operate at a duty cycle of less than or approximately 20%. The average current density during the first time period may be less than the average current density during the second time period. The peak current density during the first time period may be greater than the peak current density during the second time period. The peak current density during the first time period may be greater than or approximately twice the peak current density during the second time period. The substrate may define a via characterized by an aspect ratio greater than or approximately 10. The via may be lined with a barrier layer and a seed layer of copper. During the second time period, in a set of plating operations, the average current density may be ramped.

[0011] Some embodiments of the present technology may include electroplating methods. The methods may include: transmitting current from a power supply through a plating bath of a plating chamber for a first time period. The power supply may operate in pulsed DC transmission at a frequency of less than or approximately 1000 Hz and at a duty cycle of less than or approximately 50% during the first time period. The methods may include: plating a first amount of copper on a substrate in the plating bath. The substrate may define a via that is filled with a barrier layer and a seed layer of copper. The plated first amount of copper may be characterized by a thickness of less than or approximately 500 nm. After the first time period, the methods may include: converting the power supply to continuous DC current transmission for a second time period, the second time period being greater than the first time period. The average current density during the second time period may be greater than the average current density during the first time period. The methods may include: plating a second amount of copper on the substrate.

[0012] This technique can provide numerous benefits over conventional techniques. For example, the present technique can improve seed layer coverage prior to the electroplating operation, which can improve plating uniformity. Additionally, the present technique can be performed in a plating chamber, where electroplating can be performed, which can improve throughput over other techniques that attempt seed layer repair in a separate process chamber. These and other embodiments and many of their advantages and features are described in more detail in conjunction with the following description and accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] A further understanding of the nature and advantages of the disclosed embodiments may be realized by reference to the remainder of the specification and the appended drawings.

[0014] Figure 1 A schematic perspective view of an electroplating system according to some embodiments of the present technology is shown.

[0015] Figure 2 A partial cross-sectional view of an electroplating system according to some embodiments of the present technology is shown.

[0016] Figure 3 Exemplary operations in an electroplating method according to some embodiments of the present technology are shown.

[0017] Figure 4A-4B A schematic cross-sectional view of a substrate during build-up of a seed layer according to some embodiments of the present technology is shown.

[0018] Several of the drawings are included as schematic diagrams. It should be understood that these drawings are for illustration purposes and are not to be considered drawn to scale unless specifically stated to be drawn to scale. In addition, as schematic diagrams, these drawings are provided to aid understanding, may not include all aspects or information compared to what is realistically presented, and may include material that is exaggerated for illustration purposes.

[0019] In the figures, similar components and / or features may have the same numerical reference numeral. In addition, various components of the same type may be distinguished by following the reference numeral with a letter that serves to distinguish among the similar components and / or features. If only the first type of numerical reference numeral is used in the specification, the description can be applied to any of the similar components and / or features having the same first type of numerical reference numeral without regard to the letter suffix. DETAILED DESCRIPTION

[0020] Various operations are performed in semiconductor manufacturing and processing to create a large number of features throughout the substrate. As the layers of semiconductor are formed, vias, trenches and other pathways are created in the structure. These features can then be filled with conductive or metallic materials that enable current to flow through the device from one layer to another.

[0021] Electroplating operations can be performed to provide conductive material into vias and other features on the substrate. Electroplating utilizes an electrolyte bath containing ions of conductive material to electrochemically deposit the conductive material onto the substrate and into features defined on the substrate. The substrate (on which the metal is being plated) acts as a cathode. Electrical contacts such as rings or pins can enable current to flow through the system. During electroplating, the substrate can be clamped to a head and immersed in a plating bath to form the metallization. In the system described below, during processing, the substrate can also be adsorbed within a seal that can be coupled to the head.

[0022] The provided substrate may include a barrier layer formed along a feature structure, such as a barrier layer formed along the sidewall and bottom of a via, and may include a seed layer of a metal. The seed layer may provide a conductive path to promote nucleation of metal ions so as to plate out from a solution. Forming the seed layer may be performed by physical vapor deposition, which may be plasma enhanced or performed by other means, and may rely at least in part on line-of-sight access within the feature structure. For example, when a via is formed in a substrate and the via is characterized by a high aspect ratio, it may be a challenge to form a conformal seed layer, especially to form a conformal seed layer in the lower sidewall and corner area of ​​the feature structure. If the barrier layer is not exposed, then this area may be characterized by a much thinner seed layer coverage. During subsequent electroplating, these areas may not be able to fully conduct current at a plating current density, and voids may be formed in the feature structure, which may increase impedance or fail to produce a conductive path through the feature structure.

[0023] Conventional techniques have attempted to repair seed layers in high aspect ratio features. For example, the seed layer may be formed to a greater thickness during physical vapor deposition to ensure continuous coverage along the sidewalls. However, as coverage increases across the neck of the feature and the top surface of the wafer, the features may be pinched off or may have limited access to the plating fluid, which may further limit plating. Conventional repair techniques may attempt to perform a current-free process to establish a favorable surface condition in the area along the feature to form a deposition. However, these processes typically require additional processing chambers to perform the repair, and since the adhesion of the material may be poor, a subsequent annealing operation may be required followed by electroplating. If the repair also needs to be performed, this may further reduce yield.

[0024] The present technology overcomes these problems by building or repairing a seed layer into the electroplating chamber during a process operation that may be performed prior to electroplating. Such a system can utilize high power pulsing to overcome conductivity limitations throughout substrate features, which can provide sufficient seed layer thickness in all areas of the substrate. Subsequent plating can then be performed to uniformly fill the feature because the current density can be more uniform across the surface of the feature. Having described an exemplary chamber system in which various embodiments of the present technology can be performed, the remainder of the disclosure will discuss various aspects of these systems and processes of the present technology.

[0025] Figure 1 A schematic perspective view of an electroplating system 100 according to multiple embodiments of the present technology is shown, and methods and cleaning systems can be used and practiced for the electroplating system 100. The electroplating system 100 illustrates an exemplary electroplating system including a system head 110 and a bowl 115. During the electroplating operation, the wafer can be clamped to the system head 110, flipped, and extended into the bowl 115 for the electroplating operation. The electroplating system 100 can include a head elevator 120, which can be configured to both lift the head 110 and rotate the head 110, or otherwise position the head in the system, including tilting operations. The head and bowl can be attached to a deck plate 125 or to other structures that can be part of a larger system that combines multiple electroplating systems 100, which can share electrolytes and other materials. The rotor can enable the substrate to be clamped to the head to rotate within the bowl, or rotate outside the bowl in different operations. The rotor can include a contact ring that can provide conductive contact with the substrate. A seal 130, discussed further below, may be attached to the head. The seal 130 may include a sucked wafer to be processed. Figure 1 An electroplating chamber is shown that may include components to be cleaned directly on the platform. An in situ rinse system 135 is also shown with the system 100, although it should be understood that other configurations are possible, including multiple platforms where the head is moved to additional modules and seals or other component cleaning is performed.

[0026] Go to Figure 2 , Figure 2 A partial cross-sectional view of a chamber including aspects of an electroplating apparatus 200 according to some embodiments of the present technology is shown. The electroplating apparatus 200 can be combined with an electroplating system, including the electroplating system 100 described above. Figure 2, a plating bath 205 of an electroplating system is shown, shown together with a head 210 having a substrate 215 coupled to the head. In some embodiments, the substrate can be coupled to a seal 212, which is bonded to the head. A cleaning frame 220 can be coupled above the plating bath container 205 and can be configured to receive the head into the container during plating. The cleaning frame 220 can include a rim 225 extending circumferentially around an upper surface of the plating bath container 205. A rinsing channel 227 can be defined between the rim 225 and the upper surface of the plating bath container 205. For example, the rim 225 can include an inner sidewall 230, which is characterized by an inclined profile. As described above, cleaning fluid that slung off the substrate may contact the sidewall 230 and may be received in a plenum 235 extending around the rim for collecting cleaning fluid from the electroplating apparatus 200 .

[0027] In some embodiments, the electroplating apparatus 200 may additionally include one or more cleaning components. The components may include one or more nozzles for delivering fluid to or from the substrate 215 or the head 210 . Figure 2 The figure shows one of various embodiments in which the bath and substrate can be protected during cleaning operations with an improved cleaning assembly.Side cleaning nozzles 250 can extend through the edge 225 of the cleaning frame 220 in some embodiments and be directed to clean various aspects of the seal 212 along with the substrate 215 .

[0028] The chambers or systems discussed above can be used in performing exemplary methods including electroplating methods. Figure 3 , illustrating exemplary operations in method 300 according to multiple embodiments of the present technology. Method 300 may include one or more operations prior to the initiation of the method, including front-end processing, deposition, gate formation, etching, polishing, cleaning, or any other operation that may be performed prior to the operation. The method may include many optional operations that may or may not be specifically related to some embodiments of the method according to the present technology. For example, many operations are described in order to provide a broader range of processes performed, but these operations are not essential to the present technology, or as further discussed below, can be performed by alternative method systems. Method 300 may describe Figure 4A-4B The operations schematically shown in FIG. 3 will be described in conjunction with the operations of method 300. Figure 4A-4B It should be understood that these figures illustrate only partial schematic diagrams and that the substrate may include any number of additional materials and features having the various characteristics and aspects shown in the figures.

[0029] The method 300 may or may not involve a plurality of optional operations for making the semiconductor structure utilize a particular manufacturing operation. It should be understood that the method 300 may be performed on any number of semiconductor structures or substrates 405, such as Figure 4A As shown, semiconductor structure or substrate 405 includes an exemplary structure on which electroplating operations can be performed. The exemplary semiconductor structure may include a groove, a via, or other recessed feature structure that may include one or more materials. For example, the exemplary substrate may include silicon, silicon oxide, or an interlayer dielectric material that can be penetrated to form a groove, a groove, a via, or an isolation structure, and some other semiconductor substrate material. In some embodiments, the exemplary substrate may include a barrier layer 410, such as tantalum, tantalum nitride, titanium, or any other barrier material including any refractory material, which may limit the phase diffusion or interaction of the fill material with the underlying substrate. The barrier layer may also promote the deposition of a seed layer 415 in some embodiments, and the barrier layer may also be an adhesion layer that promotes the formation of the seed layer or include such an adhesion layer. The seed layer 415 may include any metal or conductive material, such as copper. Although the remaining disclosure will discuss copper electroplating operations, it should be understood that other materials may also be plated using multiple embodiments of the present technology.

[0030] As previously described, the seed layer 415 can be formed by physical vapor deposition, and the process performed can provide limited coverage along certain areas of the via, such as the sidewalls near the bottom of the groove or the bottom corner. Although deposition can be performed for a longer period of time, if the electroplating fluid is not prevented from entering the groove, this may cause pinching at the top of the groove, which is a challenge for electrodeposition. It should be understood that the structure indicated is not intended to be limiting, and any structure in various other semiconductor structures containing seed layer materials is similarly included. Other exemplary structures may include two-dimensional and three-dimensional structures common in semiconductor manufacturing, in which vias or feature structures can be formed, and seed layers can be deposited along these structures, because the present technology can build and repair seed layers in any number of structures. In addition, although high aperture ratio structures can benefit from the present technology, the present technology can also be equally applied to lower aperture ratios and any other structures.

[0031] For example, features according to the present technology may be characterized by any aperture ratio or aspect ratio of the feature, although in some embodiments the material may be characterized by a larger aperture ratio, which may be challenging for adequate seed layer coverage across the feature. For example, in some embodiments, the aperture ratio of any via or feature of the exemplary structure may be greater than or approximately 10:1, greater than or approximately 20:1, greater than or approximately 30:1, greater than or approximately 40:1, greater than or approximately 50:1, or greater. In addition, each feature may be characterized by a reduced width or diameter at the neck or opening of the feature, such as less than or approximately 10 μm, less than or approximately 8 μm, less than or approximately 6 μm, less than or approximately 5 μm, less than or approximately 4 μm, less than or approximately 3 μm, less than or approximately 2 μm, less than or approximately 1 μm, or less. This combination of high aperture ratio and minimum width may cause many conventional seed layer deposition operations to fail, which may result in void formation or incomplete filling in subsequent electroplating operations. By utilizing processes according to various embodiments of the present technology, a seed layer may be built up or repaired along features having virtually any aspect ratio prior to performing additional electroplating operations.

[0032] Method 300 can be performed in a plating system as described above, which can include a substrate that has been processed to a certain extent. For example, before the feature structure of the substrate is immersed in the plating bath, any number of processing operations can be performed to produce any number of semiconductor structures. Through holes such as through-silicon vias or any other high aperture ratio feature structures can be formed through the substrate. Pads such as barrier layer 410 can be formed along the feature structure, and pads such as barrier layer 410 can be formed conformally using any number of processes or techniques. A seed layer 415 can be formed, and the feature of the seed layer 415 can be incomplete or uneven coverage on the entire surface of the feature structure as shown in the figure. It should be understood that these figures are included only for illustration, and these figures are not considered to have any specific proportions. For example, gaps can appear within the coverage of the seed layer, or the minimum thickness can be formed in certain areas, which can be characterized by a thickness of tens of angstroms or less. If untreated, these minimum coverage areas may form gaps in the filling process.

[0033] The present technology can perform seed layer construction or repair in the electroplating chamber itself. After wetting (wetting) such as vacuum pre-wetting (pre-wet) has been performed on the entire feature structure of the substrate, the substrate can be clamped in the electroplating system as described above and arranged in a plating bath. The plating bath can be an acid bath, which can contain copper or other metal ions for plating, and can contain any number of additive materials in the bath. For example, a leveler, a suppressor, an accelerator or other materials can be included in the plating bath to promote the plating operation. These methods may include optional dwelling (dwell) in the plating bath before performing the operation of the described method 300, which can allow the bath material to diffuse in the feature structure. As described above, attempting to increase the seed layer with additional physical vapor deposition may cause the neck of the feature structure to be pinched off due to continuous deposition. However, the present technology can leverage the accelerator and suppressor in the plating bath during the execution of the method. Since lower-mobility suppressors can limit plating along the outer surface of the substrate and the neck of the feature structure, higher-mobility accelerators can fully penetrate the feature structure to promote repair. Therefore, the present technology may not be limited by line-of-sight formation or pinch-off problems similar to continuous physical vapor deposition.

[0034] Typical electroplating may be performed using a DC current applied at a particular average current density. The average current density may be kept relatively low, such as less than or about 3.0 mA / cm 2 , less than or about 2.5mA / cm 2 , less than or about 2.0mA / cm 2 , less than or about 1.5mA / cm 2 , less than or about 1.0mA / cm 2 , less than or about 0.5mA / cm 2, or less. By maintaining a low current density, the plating growth can be controlled to limit or prevent the formation of dendrites, and ensure that the additive can function within the nominal current window. Since direct current can be used, the peak current density can be substantially equal to or less than the average current density. However, this low current process may provide insufficient conductivity along the area of ​​low seed crystal coverage, which may cause several problems. For example, plating may not occur in these areas, and the current may be unevenly distributed to adjacent areas, which may affect the additive function and the plating in these areas. This may produce gaps, which may increase and close during continuous plating. The present technology can perform a repair process that can overcome the conductivity limitations associated with insufficient seed crystal layer coverage.

[0035] In operation 305, the electroplating operation can be performed by pulsing the DC power supply to deliver pulsed current to the processing chamber and the plating bath. Therefore, the power supply can be operated without pulse reversal and can therefore be operated in the forward direction throughout the operation, which can ensure that only plating is performed without de-plating. The pulse can be performed at a frequency and duty cycle to increase the peak current density during the on-time of the power supply. While operating the continuous DC power supply at higher powers may cause uneven plating that leads to dendrite growth, the present technology can limit high power operation to produce an initialization condition that can overcome the lower conductivity area caused by low seed layer coverage or gaps. This can be achieved by utilizing an average current density that is maintained at a level similar to or lower than a standard electroplating operation.

[0036] For example, the DC power supply may be pulsed at a pulse frequency greater than or about 1 Hz, and may be pulsed at a frequency greater than or about 10 Hz, greater than or about 50 Hz, greater than or about 100 Hz, greater than or about 250 Hz, greater than or about 500 Hz, greater than or about 750 Hz, greater than or about 1000 Hz, or higher. However, as the pulse frequency increases, the plating operation may more closely resemble a continuous DC power supply operation, which may cause over-plating during each on-time operation and may cause dendrite formation. Therefore, in some embodiments, the power supply may be pulsed at a frequency less than or about 1000 Hz, and the DC power supply may be pulsed at a frequency less than or about 900 Hz, less than or about 800 Hz, less than or about 700 Hz, or less. In addition, the duty cycle may be adjusted to reduce the on-time of the power supply. For example, in some embodiments, the duty cycle can be maintained at greater than or about 10%, and the duty cycle can be maintained at greater than or about 15%, greater than or about 20%, greater than or about 25%, greater than or about 30%, greater than or about 35%, greater than or about 40%, greater than or about 45%, greater than or about 50%, greater than or about 55%, greater than or about 60%, greater than or about 65%, greater than or about 70%, greater than or about 75%, or more. Again, as the duty cycle increases and the power supply operates more closely like continuous DC, ions adjacent to the seed layer may plate out quickly, causing dendrite formation. Therefore, in some embodiments, the duty cycle can be maintained at less than or about 80%, and the duty cycle can be maintained at less than or about 70%, less than or about 60%, less than or about 50%, or less.

[0037] By operating the power supply in a pulsed condition with a low duty cycle, the peak current density can be increased while keeping the average current density low enough to control plating from the bath. For example, during operation 305, the average current density can be maintained at less than or about 2.0 mA / cm 2 The average current density can be maintained at less than or about 1.5 mA / cm 2 , less than or about 1.0mA / cm 2 , less than or about 0.5mA / cm 2, or less. However, the peak current during the on-time operation can be greater than or about 0.5A, and can be greater than or about 1.0A, greater than or about 1.5A, greater than or about 2.0A, greater than or about 2.5A, greater than or about 3.0A, greater than or about 3.5A, greater than or about 4.0A, greater than or about 4.5A, greater than or about 5.0A, or more. In addition, the peak current density can be greater than or about 2 mA / cm 2 and can be greater than or approximately 5 mA / cm 2 , greater than or approximately 10mA / cm 2 , greater than or approximately 20mA / cm 2 , greater than or approximately 50mA / cm 2 , or higher. Although such high density may cause problems during continuous power operation as previously described, in some embodiments of the present technology, the on-time can be kept at less than or about 500 ms, and the on-time can be kept at less than or about 250 ms, less than or about 100 ms, less than or about 50 ms, less than or about 25 ms, less than or about 10 ms, less than or about 5 ms, less than or about 1 ms, or less, which can ensure controlled plating without dendrite growth.

[0038] Operation 305 may be performed for a first time period, during which a first amount of plating may be performed at operation 310. The first time period may be an amount of time to produce sufficient coverage, and may be greater than or about 2 minutes, greater than or about 5 minutes, greater than or about 10 minutes, or longer. Plating may be limited to less than or about 500 nm, and plating may be limited to less than or about 250 nm, less than or about 200 nm, less than or about 150 nm, less than or about 100 nm, or less, which may ensure sufficient coverage across all surfaces of the feature to be plated. It should be understood that the operation time and coverage may vary depending on aspects of the feature and the amount of buildup to be performed. Although the formation may be uniform, in some embodiments, coverage may occur preferentially in areas far from the wafer surface due to the process being performed in a plating bath, which may also be a problem with previously insufficient seeding. This may occur because a suppressor additive may limit deposition at the neck of a feature, while an accelerator additive may promote deposition further into the feature. Thus, this operation may advantageously limit pinch-off at the neck of the feature or features to be filled. Figure 4B As shown in , coverage can be increased along the bottom and corner regions of the feature while controlling formation at the neck or entrance of the feature.

[0039] After the pulsed operation has been completed, the power supply can be switched to continuous DC current delivery at operation 315, which can be performed for a second time period, during which a second amount of metal can be plated at operation 320. Therefore, pulsing can no longer be performed, but the average current density can be maintained or slightly increased, which can prevent excessive out-plating during the transition from pulsed to continuous operation. In some embodiments, the average current density during the second time period can be greater than or approximately equal to the average current density during the first time period, such as during the pulsed operation. However, the peak current or peak current density can be maintained less than the peak current or peak current density during the first time period. Thus, when the peak current can exceed 2A or more during the first time period, the peak current can be maintained at less than 2A or about 2A during the second time period, and the peak current can be maintained at less than 1.5A or about 1.5A, less than 1.0A or about 1.0A, less than 0.5A or about 0.5A, or less during the second time period. This allows plating to be performed evenly across the entire feature and can limit or prevent void formation.

[0040] The second time period may also vary according to aspects of the feature being filled, and in some embodiments, the second time period may be greater than the first time period. In addition, in some embodiments, the second time period may include a number of time sub-periods, in which the current or average current density may be ramped as equilibrium is reached in the plating, and the overall growth of these feature structures may increase as the feature structures are filled. For example, any number of ramping steps may be performed in optional operation 325, each of which increases the average current density. Each time period may be any of the aforementioned time periods, and each time period may be the same or different in some embodiments. Similarly, the current increase may be a linear increase in each sub-period, or each increase in current or current density may be greater than or less than any previous increase. In some embodiments, during each sub-period, the average current density may be equal to or greater than the average current density during the first time period. In addition, the peak current or peak current density may be less than the peak current or peak current density during the first time period. By performing pulsed operations according to multiple embodiments of the present technology, improved seed layer coverage may be ensured, which may improve via or feature filling operations while limiting or preventing void formation.

[0041] In the foregoing description, for purposes of illustration, numerous details are listed to provide an understanding of various embodiments of the present technology. However, it is apparent to those skilled in the art that some embodiments may be practiced without some of these details or with other details. For example, other substrates that may benefit from the described wet techniques may also be used with the present technology.

[0042] Several embodiments are disclosed above, and those skilled in the art will recognize that various modifications, alternative configurations, and equivalents may be used without violating the spirit of these embodiments. In addition, many well-known processes and elements are not described in order to avoid unnecessarily obscuring the present technology. Therefore, the above description should not be regarded as limiting the scope of the present technology.

[0043] Where a numerical range is provided, it is understood that each value between the upper and lower limits of the range (to the smallest part of the lower limit unit) is also explicitly disclosed, unless the context indicates otherwise. The present technology includes any narrower range between any mentioned value or unmentioned value between the range, and any other mentioned value or value between the range within the mentioned range. The upper and lower limits of these smaller ranges may be independently included in the range or excluded from the range, and under the condition of any intentionally excluded limit values ​​in the mentioned range, the present technology also includes the following each range: any or both of the upper and lower limits are included or not included in each range in these smaller ranges. Where the mentioned range includes one or both of these limits, the present technology also includes the range excluding any or both of those included limits. Where multiple values ​​are provided in a list, any range including any of these values ​​or any range based on any of these values ​​is similarly intentionally disclosed.

[0044] As used herein and in the appended claims, the singular forms "a," "an," "the," and "said" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "a material" includes a plurality of such materials and reference to "the time period" or "the time period" includes reference to one or more time periods and includes reference to equivalents thereof known to those skilled in the art, and so forth.

[0045] Furthermore, the terms “comprises,” “comprising,” and “including,” when used in this specification and the appended claims, are intended to indicate the presence of certain features, integers, components, or operations, but they do not exclude the presence or addition of one or more other features, integers, components, operations, actions, or groups.

Claims

1. An electroplating method, comprising the following steps: delivering current from a power source through a plating bath of the electroplating chamber for a first time period, wherein the delivered current comprises a pulsed current having a duty cycle of less than 50% or 50%; plating a first amount of metal on a substrate within the plating bath, wherein the substrate defines a via, the via being within the substrate; After the first time period, switching the power source to continuous DC current delivery for a second time period; and plating a second amount of metal on the substrate, Wherein a peak current density during the first time period is greater than a peak current density during the second time period.

2. The electroplating method of claim 1, wherein the current delivered during the first time period is characterized by an operating frequency of less than 1000 Hz or 1000 Hz.

3. The electroplating method of claim 1 , wherein the average current density during the first time period is less than 3 mA / cm 2 Or 3mA / cm 2 .

4. The electroplating method of claim 3, wherein the average current density during the second time period is greater than or equal to the average current density during the first time period.

5. The electroplating method of claim 4, wherein the peak current during the second time period is less than 2 amperes or is 2 amperes.

6. The electroplating method of claim 5, wherein the peak current during the first time period is greater than or equal to 2 amperes.

7. The electroplating method according to claim 1, wherein: During the second time period, the average current density increases with time.

8. The electroplating method of claim 1, wherein the via defined in the substrate is characterized by a depth greater than 10 μm or 10 μm.

9. The electroplating method of claim 1 , further comprising: A barrier layer is formed along a wall of the via defined in the substrate.

10. The electroplating method of claim 9, wherein the barrier layer comprises one or more of titanium or tantalum, and wherein the deposited metal comprises copper.

11. An electroplating method, comprising the following steps: delivering current from a power supply through a plating bath of an electroplating chamber for a first time period, wherein the power supply operates in pulsed DC delivery at a frequency of less than 750 Hz or 750 Hz during the first time period; plating a first amount of copper on a substrate in the plating bath; After the first time period, transitioning the power source to continuous DC current delivery for a second time period; and plating a second amount of copper on the substrate, Wherein a peak current density during the first time period is greater than a peak current density during the second time period.

12. The electroplating method of claim 11, wherein the on-time of each pulse during the first time period is less than 100 ms or is 100 ms.

13. The electroplating method according to claim 11, wherein: During the first time period, the power supply operates at a duty cycle of less than 20% or 20%.

14. The electroplating method of claim 11, wherein an average current density during the first time period is less than an average current density during the second time period.

15. The electroplating method of claim 11, wherein the peak current density during the first time period is greater than or is twice the peak current density during the second time period.

16. The electroplating method of claim 11, wherein the substrate defines a via, the via being characterized by an aspect ratio greater than or equal to 10.

17. The electroplating method of claim 11, wherein a via is defined in the substrate, and the via is filled with a barrier layer and a seed layer of copper.

18. The electroplating method according to claim 11, wherein: During the second time period, the average current density is increased in a set of plating operations.

19. An electroplating method, comprising the following steps: delivering current from a power supply through a plating bath of an electroplating chamber for a first time period, wherein the power supply operates in pulsed DC delivery at a frequency of less than 1000 Hz or 1000 Hz and at a duty cycle of less than 50% or 50% during the first time period; Plating a first amount of copper on a substrate in the plating bath, wherein the substrate defines a via, the via being populated with a barrier layer and a seed layer of copper, and wherein the plated first amount of copper is characterized by being less than 500 nm or having a thickness of 500 nm; after the first time period, transitioning the power source to continuous DC current delivery for a second time period, the second time period being greater than the first time period, wherein an average current density during the second time period is greater than an average current density during the first time period; and plating a second amount of copper on the substrate, Wherein a peak current density during the first time period is greater than a peak current density during the second time period.