A graphene@hierarchical porous carbon composite material and its preparation method and application
Through the preparation of graphene@hierarchical porous carbon composite materials, the problem of insufficient charge-discharge platform and rate performance of lithium-ion capacitor anode materials has been solved, high specific capacity and excellent rate performance have been achieved, and the overall performance of lithium-ion capacitors has been improved.
Patent Information
- Application Number
- CN202011163971.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-27
AI Technical Summary
The existing negative electrode materials of graphite and porous carbon for lithium-ion capacitors have unclear charging and discharging platforms, voltage lag, and low first Coulomb efficiency during the energy storage process, which limits the improvement of device energy density and cannot match high power density cathode materials. , resulting in overall performance degradation.
Graphene@hierarchical porous carbon composite material is used as the negative electrode material of lithium ion capacitor. Through graphene surface functionalization treatment and compounding with template agent, sodium lignosulfonate precipitation and high-temperature calcination are used to prepare hierarchical porous carbon to realize battery-type materials and capacitor-type materials. Integrated construction of materials.
A lithium-ion capacitor anode material with low charge and discharge platform, high specific capacity and excellent rate performance has been realized, which improves the electrochemical performance of the device and provides a cathode material with better matching and high power density.
Abstract
Description
Technical Field
[0001] The present application relates to a graphene@hierarchical porous carbon composite material and a preparation method and application thereof, and belongs to the field of lithium ion capacitors. Background Art
[0002] As a new type of energy storage device, lithium-ion capacitors have the characteristics of high power density and long cycle life of supercapacitors and high energy density of lithium-ion batteries. They are considered to be the most promising next-generation "double-high" energy storage devices with high energy density and high power density. The positive electrode of a lithium-ion capacitor is a capacitor-type material, and the negative electrode is a battery-type material. Because the negative electrode material is an electrochemical lithium-intercalation energy storage material, the lithium-ion capacitor is provided with a higher energy density through the insertion / deintercalation of lithium ions in the bulk phase and surface charge transfer, but due to its slow kinetic reaction, it has become a "bottleneck" factor that affects the improvement of the device's power density.
[0003] At present, graphite, the commercial negative electrode material for lithium-ion capacitors, has a high platform capacity (about 300mAh / g below 0.2V), a high first coulomb efficiency (more than 90%) and excellent conductivity, but the theoretical specific capacity of graphite is low (theoretical capacity is 372mAh / g), and the rate performance and cycle stability are poor. These factors make graphite unable to match the positive electrode materials with excellent rate performance and long cycle life at high current density, resulting in a significant decline in the overall performance of the device. Porous carbon has the advantages of high specific capacity, excellent rate performance and long cycle life, and has developed rapidly in the application of negative electrode materials for lithium-ion capacitors. However, in the energy storage process, porous carbon has the disadvantages of no obvious charge and discharge platform, voltage hysteresis and low first coulomb efficiency, which limits the improvement of device energy density.
[0004] Therefore, if the respective advantages of the two carbon materials can be combined, graphene and hierarchical porous carbon can be compounded to achieve the integrated construction of battery-type materials and capacitor-type materials, the graphene@hierarchical porous carbon composite material can be used as the negative electrode material of lithium-ion capacitors, which will have better electrochemical properties. At present, there are no research reports on the use of graphene@hierarchical porous carbon composite materials as negative electrode materials for lithium-ion capacitors. Summary of the invention
[0005] According to the first aspect of the present application, a graphene@hierarchical porous carbon composite material is provided, comprising graphene and hierarchical porous carbon coated on the surface of the graphene. The material has the characteristics of low charge and discharge platform, high specific capacity and excellent rate performance.
[0006] In the present application, the hierarchical pores in the hierarchical porous carbon refer to a combination of micropores, mesopores and macropores or a combination of any two of micropores, mesopores and macropores.
[0007] According to a second aspect of the present application, a method for preparing a graphene@hierarchical porous carbon composite material is provided, comprising:
[0008] (1) mixing a dispersion liquid I containing graphene and a polycation electrolyte to obtain surface-modified graphene;
[0009] (2) mixing the dispersion II containing the surface-modified graphene and the template to obtain graphene@template;
[0010] (3) reacting the dispersion III containing the graphene@template, carbon source and precipitant, calcining and removing the template to obtain a graphene@hierarchical porous carbon composite material.
[0011] This method uses multilayer graphene as a battery-type energy storage material, performs surface functionalization on graphene, and utilizes electrostatic adsorption to achieve effective composite of the template and graphene; utilizes the alkali-soluble and acid-precipitation properties of carbon sources such as lignin sulfonates derived from papermaking black liquor to achieve precipitation of the carbon source on the surface of the graphene@template, collects the product by centrifugation, and then obtains the graphene@hierarchical porous carbon composite material through high-temperature calcination and template removal treatment.
[0012] Optionally, the polycation electrolyte in step (1) is selected from at least one of polydimethyldiallylammonium chloride, polyacrylamine hydrochloride, polyacrylamide, and polyethyleneimine.
[0013] Preferably, the number of graphene layers in step (1) is more than 3 layers and less than 10 nm.
[0014] Preferably, the graphene in step (1) is doped with at least one of fluorine and oxygen;
[0015] Preferably, the doping amount is 0.5 to 3 at %.
[0016] Preferably, in step (1), the mass fraction of the polycationic electrolyte in the dispersion liquid I is 0.2 to 2.0 wt%.
[0017] Specifically, the upper limit of the mass fraction of the polycationic electrolyte in the dispersion I is selected from 2.0wt%, 1.0wt%, 0.5wt%, and the lower limit is selected from 0.2wt%, 0.3wt%, 0.4wt%.
[0018] Preferably, in step (1), the mass concentration of the graphene in the dispersion liquid I is 0.01-2%.
[0019] Optionally, the dispersion I containing graphene and polycationic electrolyte is obtained by adding graphene into a polycationic electrolyte dispersion and mixing them.
[0020] Specifically, the specific conditions of step (1) include:
[0021] First, graphene is added into a polycation electrolyte aqueous solution and ultrasonicated for 5 to 120 minutes, and then stirred and mixed for 0.5 to 2 hours.
[0022] Optionally, the template in step (2) is selected from nano-silicon oxides of different sizes;
[0023] Preferably, the template has a diameter of 5 to 20 nm.
[0024] Optionally, the upper limit of the template diameter is selected from 7 nm, 10 nm, 15 nm, 20 nm, and the lower limit is selected from 5 nm, 7 nm, 10 nm, 15 nm.
[0025] Preferably, the mass fraction of the template in the dispersion II in step (2) is 0.2-5%.
[0026] Specifically, the upper limit of the mass fraction of the template in the dispersion II is selected from 1wt%, 1.5wt%, 3wt%, and 5wt%, and the lower limit is selected from 0.2wt%, 1wt%, 1.5wt%, and 3wt%.
[0027] Preferably, the specific conditions of step (2) include:
[0028] Carry out under stirring conditions;
[0029] The reaction temperature is room temperature °C, and the reaction time is 1 to 24 hours.
[0030] Optionally, the dispersion II containing the surface-modified graphene and the template in step (2) is obtained by the following method:
[0031] A template dispersion and a surface-modified graphene dispersion are prepared separately, and then the template dispersion is added into the surface-modified graphene dispersion to obtain the dispersion II.
[0032] Preferably, the template dispersion is added to the surface-modified graphene dispersion by dropwise addition.
[0033] Preferably, the mass ratio of the surface-modified graphene to the template is 0.01 to 0.1:1.
[0034] Preferably, the pH of the surface-modified graphene dispersion is adjusted to 4.5-5.5.
[0035] Optionally, the carbon source in step (3) is selected from at least one of sodium lignin sulfonate, ammonium lignin sulfonate, and calcium lignin sulfonate;
[0036] Preferably, the precipitant is selected from at least one of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid;
[0037] Preferably, the mass ratio of the graphene@template and the carbon source in step (3) is 1:1-50.
[0038] Specifically, the upper limit of the mass ratio of the graphene@template and the carbon source is selected from 1:10, 1:20, 1:30, 1:40, 1:50, and the lower limit is selected from 1:1, 1:10, 1:20, 1:30, 1:40.
[0039] Preferably, in step (3), the mass concentration of the graphene@template in the dispersion is 0.01 to 3%.
[0040] Preferably, the specific conditions for calcination in step (3) include:
[0041] Carry out under inert atmosphere;
[0042] The calcination temperature is 600-1000°C;
[0043] The calcination time is 0.5 to 8 hours.
[0044] In the present application, the inactive atmosphere refers to a nitrogen atmosphere or an inert atmosphere.
[0045] Optionally, the temperature is first raised to 400-500° C. and maintained for 1-3 hours, and then raised to 600-1000° C. and calcined for 1-8 hours.
[0046] Specifically, the upper limit of the calcination temperature can be selected from 700°C, 800°C, 900°C, and 1000°C, and the lower limit can be selected from 600°C, 700°C, 800°C, and 900°C.
[0047] Preferably, the removing the template agent specifically comprises: removing the template agent by etching.
[0048] Preferably, the chemical reagent for etching is selected from at least one of sodium hydroxide solution, potassium hydroxide solution and hydrofluoric acid solution.
[0049] In a specific embodiment, a method for preparing a graphene@hierarchical porous carbon lithium ion capacitor negative electrode material comprises:
[0050] Step A: adding graphene to a polycation electrolyte solution, subjecting the solution to ultrasonic treatment for 5 to 90 minutes, stirring the solution for 0 minute to 1 hour, and then centrifuging the solution. The surface-treated graphene is ultrasonically treated again for 5 to 90 minutes, and then stirred for 0 minute to 1 hour to obtain a graphene dispersion with a positively charged surface, thereby achieving functional modification of the graphene surface, and adjusting the pH thereof to 4.5 to 5.5.
[0051] Step B: taking a certain amount of silicon oxide nanosphere dispersion and adding it to the surface-modified graphene dispersion, stirring at room temperature for 1 to 24 hours; removing excess silicon oxide nanospheres by centrifugation to obtain graphene@silicon oxide.
[0052] Step C: Disperse the above graphene@silicon oxide into ultrapure water, add a certain mass of sodium lignin sulfonate and stir thoroughly until the sodium lignin sulfonate is completely dissolved; gradually add sulfuric acid solution dropwise until the sodium lignin sulfonate is completely precipitated to obtain graphene@silicon oxide@lignin sulfonic acid.
[0053] Step D: The graphene@silicon oxide@sodium lignin sulfonate obtained in step C is dried and placed in a tube furnace. In an inert atmosphere, the temperature is raised to 400°C at 2°C / min, and the temperature is continued to be raised to calcine at 600-1000°C. The reaction time is 0.5-8 hours to obtain a calcined sample.
[0054] Step E: The sample obtained in step D is treated to remove the silicon oxide nanospheres, placed in a concentrated sodium hydroxide solution and heated to 80° C., stirred for 24 to 48 hours, then filtered and washed with ultrapure water until neutral, and the product is dried to obtain a graphene@hierarchical porous carbon composite material.
[0055] According to the third aspect of the present application, a negative electrode material is provided, wherein the active material is at least one of the above-mentioned graphene@hierarchical porous carbon composite material and the graphene@hierarchical porous carbon composite material prepared by any of the above-mentioned preparation methods.
[0056] According to a third aspect of the present application, an electrode is provided, comprising:
[0057] Active material, conductive agent, binder, and current collector;
[0058] Wherein, the active material is at least one of the above-mentioned graphene@hierarchical porous carbon composite material and the graphene@hierarchical porous carbon composite material prepared by any of the above-mentioned preparation methods.
[0059] Wherein, the conductive agent is selected from at least one of Ketjen black, conductive carbon black, carbon nanotubes, and graphene;
[0060] The binder is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, and styrene-butadiene rubber;
[0061] The current collector is at least one of copper foil, foam copper, and stainless steel mesh;
[0062] Optionally, the mass ratio of the electrode active material, the conductive agent and the binder is 8:1:1.
[0063] Optionally, the loading amount of the active material in the electrode is 0.5 to 1.5 mg / cm 2 .
[0064] According to a fourth aspect of the present application, a method for preparing an electrode is provided, comprising:
[0065] A slurry containing an active material, a conductive agent, and a binder is coated on a current collector to obtain the electrode, wherein the active material is at least one of the above-mentioned graphene@hierarchical porous carbon composite materials and the graphene@hierarchical porous carbon composite materials prepared by any of the above-mentioned preparation methods.
[0066] Optionally, the compounding includes at least one of coating, rolling and extrusion.
[0067] Optionally, the mass ratio of the electrode active material, the conductive agent and the binder is 80:10:10.
[0068] The present application also provides a lithium ion capacitor half-cell, comprising:
[0069] Negative electrode, lithium sheet;
[0070] electrolyte; and
[0071] The positive electrode is at least one of the electrodes described above and the electrodes prepared by the preparation method described above.
[0072] Optionally, the electrolyte is a solution containing lithium ions;
[0073] Preferably, the electrolyte consists of a lithium source and a solvent, wherein the lithium source is LiPF 6 The solvent is composed of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate in a volume ratio of 1:1:1.
[0074] Optionally, the capacitor further includes a diaphragm, and the diaphragm is Celgard2400.
[0075] The beneficial effects of this application include:
[0076] The preparation method of the graphene@hierarchical porous carbon composite material provided in the embodiment of the present invention realizes in-situ "growth" of hierarchical porous carbon on the graphene surface through graphene surface functionalization treatment, graphene and template compounding, sodium lignin sulfonate and graphene@template compounding, and subsequent calcination treatment and template removal treatment. The preparation method of the graphene@hierarchical porous carbon provided by the present invention not only has low preparation cost and simple process, but also can realize the integrated construction of battery-type material graphene and capacitor-type material hierarchical porous carbon, which is helpful to obtain a lithium ion capacitor negative electrode material with a low charge and discharge platform, high specific capacity and excellent rate performance, so it has great promotion and application value. DETAILED DESCRIPTION
[0077] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0078] In Example 1, the fluorine-doped graphene is prepared by the electrochemical anodic stripping method described in the literature "Electrochemically Scalable Production of Fluorine-Modified Graphene for Flexible and High-Energy Ionogel-Based Microsupercapacitors", and the number of layers of the obtained fluorine-doped graphene is concentrated in 3 to 10 layers, and the fluorine doping amount is 0.5 to 3 at%;
[0079] In Example 2, the oxygen-doped graphene is provided by the Ningbo Institute of Materials Technology and Engineering, Chinese Academy of Sciences, and the number of graphene layers is concentrated in the range of 5 to 15;
[0080] In Example 3, the fluorine-doped graphene is prepared by the electrochemical anodic stripping method described in the literature "Electrochemically Scalable Production of Fluorine-Modified Graphene for Flexible and High-Energy Ionogel-Based Microsupercapacitors". The number of layers of the obtained fluorine-doped graphene is concentrated in the range of 10 to 25 layers, and the fluorine doping amount is 0.5 to 3 at%;
[0081] The oxygen-doped graphene in Example 4 is provided by Ningbo Institute of Materials Technology and Engineering, Chinese Academy of Sciences, and the number of graphene layers is concentrated in the range of 15 to 30 layers.
[0082] Example 1
[0083] 100 mg of fluorine-doped graphene was added to 200 mL of 0.2 wt% polydiallyldimethylammonium chloride aqueous solution, and then stirred for 0.5 hour after ultrasonic treatment for 1 hour to obtain dispersion I, which was then centrifuged to obtain surface-modified graphene.
[0084] The collected surface-modified graphene was added into 400 mL of water, ultrasonicated again for 0.5 hour, and then stirred for 0.5 hour to obtain a surface-modified graphene dispersion. The pH of the dispersion was adjusted to 5.0 using 1 M HCl.
[0085] 1 g of silica nanospheres with a diameter of 10 nm was prepared into a silica nanosphere dispersion with a mass concentration of 1.0 wt%, and the silica nanosphere dispersion was added dropwise into the surface-modified graphene dispersion at room temperature and continued to stir for 10 hours to obtain dispersion II, which was then centrifuged to remove excess silica nanospheres to obtain fluorine-doped graphene@silicon oxide.
[0086] The obtained graphene@silicon oxide was redispersed in 200 mL ultrapure water, and 2 g of sodium lignin sulfonate was added and stirred until it was completely dissolved to obtain a dispersion to be reacted; 2 M sulfuric acid solution was added dropwise to the dispersion to be reacted (to obtain dispersion III) and continued to stir for 1 hour until the sodium lignin sulfonate was completely precipitated and settled, and then allowed to stand for 12 hours, the supernatant was removed, and continued to stir and rapidly freeze-dried. The freeze-dried graphene@silicon oxide@sodium lignin sulfonate was placed in an argon atmosphere, and the temperature was increased to 400°C at 2°C / min, kept constant for 1 hour, and the temperature was continued to be increased, and calcined at 700°C for 1 hour, and then the calcined sample was treated with a concentrated sodium hydroxide solution at 80°C to remove silicon oxide for 48 hours, and then centrifuged, washed with deionized water until neutral, and dried in an oven at 100°C for 8 hours to obtain a graphene@hierarchical porous carbon composite material, which was recorded as product 1.
[0087] Example 2
[0088] 100 mg of oxygen-doped graphene was added to 200 mL of 0.2 wt% polyethyleneimine aqueous solution, and then stirred for 0.5 hour after ultrasonic treatment for 1 hour to obtain dispersion I, which was then centrifuged to obtain surface-modified graphene.
[0089] The collected surface-modified graphene was dispersed in 400 mL of water, and then ultrasonicated for 0.5 hour and stirred for 0.5 hour to obtain a surface-modified graphene dispersion. The pH of the dispersion was adjusted to 4.5 using 1 M HCl.
[0090] 1.5 g of silica nanospheres with a diameter of 15 nm were prepared into a silica nanosphere dispersion with a mass concentration of 0.5 wt%, and the silica nanosphere dispersion was added dropwise into the surface-modified graphene dispersion at room temperature and continued to stir for 10 hours to obtain dispersion II, which was then centrifuged to remove excess silica nanospheres to obtain graphene@silicon oxide.
[0091] The obtained graphene@silicon oxide was redispersed in 400mL ultrapure water, and 5g of ammonium lignin sulfonate was added and stirred until it was completely dissolved to obtain a dispersion to be reacted; a sulfuric acid solution with a concentration of 1M was added dropwise to the dispersion to be reacted (to obtain dispersion III) and continued to stir for 1 hour until the ammonium lignin sulfonate was completely precipitated and settled, and then allowed to stand for 12 hours, the supernatant was removed, and continued to stir and quickly freeze-dried. The freeze-dried graphene@silicon oxide@ammonium lignin sulfonate was placed in an argon atmosphere, raised to 400°C at 2°C / min, kept constant for 1 hour, and continued to increase the temperature, and calcined at 800°C for 1 hour, and then the calcined sample was treated with a concentrated sodium hydroxide solution at 80°C to remove silicon oxide for 48 hours, and then centrifuged, washed with deionized water until neutral, and dried in an oven at 100°C for 8 hours to obtain a graphene@hierarchical porous carbon composite material, which was recorded as product 2.
[0092] Example 3
[0093] 100 mg of fluorine-doped graphene was added to 200 mL of 0.5 wt% polyacrylamide aqueous solution, and then stirred for 0.5 hour after ultrasonic treatment for 1 hour to obtain dispersion liquid I, which was then centrifuged to obtain surface-modified graphene.
[0094] The collected surface-modified graphene was dispersed in 400 mL of water, and then ultrasonicated again for 0.5 hour and stirred for 0.5 hour to obtain a surface-modified graphene dispersion. The pH of the dispersion was adjusted to 5.0 using 1 M HCl.
[0095] 2 g of silica nanospheres with a diameter of 20 nm were prepared into a silica nanosphere dispersion with a mass concentration of 3.0 wt%, and the silica nanosphere dispersion was added dropwise into the surface-modified graphene dispersion at room temperature and continued to be stirred for 20 hours to obtain dispersion II, which was then centrifuged to remove excess silica nanospheres to obtain graphene@silicon oxide.
[0096] The obtained graphene @ silicon oxide was redispersed in 300 mL ultrapure water, and 5 g of sodium lignin sulfonate was added and stirred until the sodium lignin sulfonate was completely dissolved to obtain a dispersion to be reacted. A sulfuric acid solution with a mass concentration of 2 M was added dropwise to the dispersion to be reacted (to obtain dispersion III) and continued to stir for 1 hour until the sodium lignin sulfonate was completely precipitated and settled, and then allowed to stand for 12 hours, the supernatant was removed, and continued to stir and rapidly freeze-dried. The freeze-dried graphene @ silicon oxide @ sodium lignin sulfonate was placed in an argon atmosphere, raised to 400 ° C at 2 ° C / min, kept constant for 1 hour, and continued to increase the temperature, and calcined at 900 ° C for 1 hour, and then the calcined sample was treated with hydrofluoric acid solution at room temperature to remove silicon oxide for 48 hours, and then centrifuged, washed with deionized water until neutral, and dried in an oven at 100 ° C for 8 hours to obtain a graphene @ hierarchical porous carbon composite material, which was recorded as product 3.
[0097] Example 4
[0098] 150 mg of fluorine-doped graphene was added to 200 mL of 0.5 wt% polydiallyldimethylammonium chloride aqueous solution, and then ultrasonicated for 1 hour and stirred for 0.5 hour to obtain dispersion I, which was then centrifuged to obtain surface-modified graphene.
[0099] The collected surface-modified graphene was added into 400 mL of water, ultrasonicated again for 0.5 hour, and then stirred for 0.5 hour to obtain a surface-modified graphene dispersion, and the pH of the dispersion was adjusted to 5.5 with 1 M HCl.
[0100] 5 g of silica nanospheres with a diameter of 20 nm were prepared into a silica nanosphere dispersion with a mass concentration of 1.5 wt%. 100 mL of the silica nanosphere dispersion was added dropwise into the surface-modified graphene dispersion at room temperature and continued to stir for 10 hours to obtain dispersion II, which was then centrifuged to remove excess silica nanospheres to obtain graphene@silicon oxide.
[0101] The obtained graphene@silicon oxide was redispersed in 400mL ultrapure water, and 10g of calcium lignin sulfonate was added and stirred until the calcium lignin sulfonate was completely dissolved to obtain a dispersion to be reacted. A sulfuric acid solution with a mass concentration of 1M was added dropwise to the above dispersion to be reacted (to obtain dispersion III) and continued to stir for 1 hour until the calcium lignin sulfonate was completely precipitated and settled, and then allowed to stand for 12 hours, the supernatant was removed, and continued to stir and quickly freeze-dried. The freeze-dried graphene@silicon oxide@calcium lignin sulfonate was placed in an argon atmosphere, raised to 400°C at 2°C / min, kept constant for 1 hour, and continued to increase the temperature, and calcined at 1000°C for 1 hour, and then the calcined sample was treated with hydrofluoric acid solution to remove silicon oxide at room temperature for 48 hours, and then centrifuged, washed with deionized water until neutral, and dried in an oven at 120°C for 8 hours to obtain a graphene@hierarchical porous carbon composite material, which was recorded as product 4.
[0102] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a graphene@hierarchical porous carbon composite material, It is characterized in that The graphene@hierarchical porous carbon composite material comprises graphene and hierarchical porous carbon coated on the surface of the graphene; The preparation method comprises: (1) mixing a dispersion liquid I containing graphene and a polycation electrolyte to obtain surface-modified graphene; (2) mixing the dispersion II containing the surface-modified graphene and the template to obtain graphene@template; (3) reacting the dispersion III containing the graphene@template, carbon source and precipitant, calcining and removing the template to obtain a graphene@hierarchical porous carbon composite material.
2. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The polycation electrolyte in step (1) is selected from at least one of polydimethyldiallylammonium chloride, polyacrylamine hydrochloride, polyacrylamide, and polyethyleneimine.
3. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The number of graphene layers in step (1) is more than 3 layers and less than 10 layers.
4. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that In step (1), the graphene is doped with at least one of fluorine and oxygen.
5. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that In step (1), the mass fraction of the polycationic electrolyte in the dispersion I is 0.2-2.0%.
6. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that In step (1), the mass concentration of the graphene in the dispersion liquid I is 0.01-2%.
7. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The specific conditions of step (1) include: Graphene was added to the polycation electrolyte aqueous solution and ultrasonicated for 5 to 120 minutes, followed by stirring and mixing for 0.5 to 2 hours.
8. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The template in step (2) is selected from inorganic nanoparticles, and the inorganic nanoparticles include silicon oxide nanoparticles.
9. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The diameter of the template is 5-20 nm.
10. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The mass fraction of the template in the dispersion II in step (2) is 0.2-5%.
11. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that In step (2), the specific conditions of the mixing include: Carry out under stirring conditions; The mixing temperature is room temperature and the mixing time is 1 to 24 hours.
12. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that In step (2), the dispersion II containing the surface-modified graphene and the template is obtained by the following method: A template dispersion and a surface-modified graphene dispersion are prepared separately, and then the template dispersion is added into the surface-modified graphene dispersion to obtain the dispersion II.
13. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 12, It is characterized in that The template dispersion is added into the surface-modified graphene dispersion in a dropwise manner.
14. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The mass ratio of the surface modified graphene to the template agent is 0.01-0.1:
1.
15. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The carbon source in step (3) is selected from at least one of sodium lignin sulfonate, ammonium lignin sulfonate and calcium lignin sulfonate.
16. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The mass ratio of graphene@template and carbon source in step (3) is 1:1~50.
17. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The precipitant is selected from at least one of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid.
18. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that In step (3), the mass concentration of the graphene@template in the dispersion III is 0.01-3%.
19. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The specific conditions for calcination in step (3) include: Carry out under inert atmosphere; Calcination temperature is 600~1000℃; The calcination time is 0.5~8 hours.
20. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 1, It is characterized in that The removing of the template specifically comprises: The template is removed by etching.
21. The method for preparing the graphene@hierarchical porous carbon composite material according to claim 20, It is characterized in that The chemical reagent for etching is selected from at least one of sodium hydroxide solution, potassium hydroxide solution and hydrofluoric acid solution.
22. A negative electrode material, It is characterized in that The active material is a graphene@hierarchical porous carbon composite material prepared by the preparation method according to any one of claims 1 to 21.
23. An electrode, It is characterized in that include: Active substances; Conductive agent; Binder; as well as current collector; Wherein, the active material is a graphene@hierarchical porous carbon composite material prepared by the preparation method according to any one of claims 1 to 21.
24. A method for preparing an electrode, It is characterized in that include: The electrode is obtained by compounding a slurry containing an active material, a conductive agent, and a binder onto a current collector, wherein the active material is a graphene@hierarchical porous carbon composite material prepared by the preparation method according to any one of claims 1 to 21.
25. A lithium ion capacitor half-cell, It is characterized in that include: Negative electrode, lithium sheet; Electrolyte; as well as The positive electrode is one of the electrode described in claim 23 and the electrode prepared by the preparation method described in claim 24.
Citation Information
Patent Citations
Flexible graphene current collector and active material integrated electrode pole piece and preparation method thereof
CN104810504A
Carbon coated core shell structure nano-silicon / graphene composite anode material and preparation method thereof
CN107611394A
Manganese oxide / carbon nanotube / graphene negative electrode composite material and preparation method thereof
CN109037608A
Carbon nanotube-graphene composite conductive paste, preparation method therefor, and uses thereof
WO2016150174A1
Cited By
Graphene-porous carbon-hard carbon three-layer gradient structure negative electrode material and preparation method and application thereof
CN122771374A