A modified solid oxide fuel cell electrode and in-situ solvent thermal preparation method thereof, and a solid oxide fuel cell
By using solvothermal method to grow nanoparticles in situ on the surface of solid oxide fuel cell electrodes, the problems of increased impedance and high energy consumption of the battery in traditional methods are solved, and the battery performance improvement and process simplification is achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202011166315.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-10-27
AI Technical Summary
When a traditional solid oxide fuel cell operates at high temperatures, the increased impedance of the battery cathode leads to performance attenuation, and the traditional solution impregnation modification method is complicated and energy consumption is large, making it difficult to be suitable for industrial applications.
The modified phase nanoparticles are grown in situ on the surface of solid oxide fuel cell electrodes by solvothermal method, and the size and morphology of nanoparticles are controlled by regulating the reaction conditions to form specific single metal oxides, doped metal oxides or perovskites. catalytic material, reducing polarization impedance.
It significantly reduces the polarization impedance of the electrode, increases the output power of the battery, simplifies the preparation process, improves the controllability and operability of the process, has low energy consumption, and is suitable for industrial promotion.
Smart Images

Figure HDA0002745903130000011 
Figure HDA0002745903130000021 
Figure HDA0002745903130000022
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid oxide fuel cell electrodes, and relates to a modified solid oxide fuel cell electrode and a preparation method thereof, and a solid oxide fuel cell, and in particular to a modified solid oxide fuel cell electrode and an in-situ solvent thermal preparation method thereof, and a solid oxide fuel cell. Background Art
[0002] Solid Oxide Fuel Cell (SOFC) belongs to the third generation of fuel cells. It is an all-solid-state chemical power generation device that converts chemical energy stored in fuel and oxidant into electrical energy in an efficient and environmentally friendly manner at medium and high temperatures. Its high efficiency, pollution-free, all-solid-state structure and wide adaptability to a variety of fuel gases are the basis for its wide application. Among all fuel cells, SOFC has the highest operating temperature and belongs to high-temperature fuel cells. In recent years, distributed power stations have gradually become an important part of the world's energy supply due to their advantages such as low cost and high maintainability. Since the exhaust gas of SOFC power generation has a high temperature and high utilization value, it can provide the heat required for natural gas reforming, can also be used to produce steam, and can form a combined cycle with gas turbines, which is very suitable for distributed power generation. The combined power generation system composed of fuel cells, gas turbines, steam turbines, etc. not only has a high power generation efficiency, but also has the environmental benefits of low pollution, wide fuel adaptability, high energy conversion efficiency, all-solid-state, modular assembly, zero pollution, etc., and can directly use a variety of hydrocarbon fuels such as hydrogen, carbon monoxide, natural gas, liquefied gas, coal gas and biomass gas. In order to meet the sustainable development of social economy and ecology, reduce carbon dioxide emissions, and reduce fossil fuel consumption, the development of renewable clean energy solid oxide fuel cells has always been a hot spot in the field of technical research. It is not limited by the Carnot cycle and the energy conversion efficiency can reach more than 60%. It is small in size, low in noise, pollution-free, has a variety of available fuels, and can be used for hot spot cogeneration. It has broad application potential in centralized power generation, distributed power generation, auxiliary power supply, and cogeneration. It is of great significance in energy conservation and emission reduction, and promoting changes in the national energy structure. It also has broad application prospects as a mobile power source for ship power sources, transportation vehicle power sources, etc.
[0003] The main components of a solid oxide fuel cell monomer are electrolyte, anode or fuel electrode, cathode or air electrode and connector or bipolar plate. The working principle of solid oxide fuel cells is the same as other fuel cells, which is equivalent to the "reverse" device of water electrolysis in principle. Its single cell consists of an anode, a cathode and a solid oxide electrolyte. The anode is the place where the fuel is oxidized, and the cathode is the place where the oxidant is reduced. Both electrodes contain catalysts that accelerate the electrochemical reaction of the electrodes. When working, it is equivalent to a DC power supply, and its anode is the negative electrode of the power supply, and the cathode is the positive electrode of the power supply. However, traditional solid oxide fuel cells operate at high temperatures of 800 to 1000°C, but such high temperatures place extremely high demands on the high temperature resistance of materials. Therefore, reducing the operating temperature of solid oxide fuel cells to the medium temperature range of 600 to 800°C can greatly reduce costs, extend the service life of materials and batteries, and improve the commercial competitiveness of solid oxide fuel cells. However, as the temperature decreases, the impedance of the battery cathode will increase greatly, causing the battery performance to decay significantly. In recent years, the modification of nanoparticles on the electrode surface by solution impregnation is a commonly used modification method for battery electrodes, which can reduce the polarization impedance of the electrode without changing the material system. However, the solution impregnation method often requires repeated impregnation, which is complicated and requires sintering at a relatively high temperature after impregnation, which will damage the electrode itself, consume more energy, and take a long time.
[0004] Therefore, how to better and more conveniently modify the solid oxide fuel cell electrodes to make them suitable for industrial applications and reduce their polarization resistance without affecting the battery performance is of great practical significance and is also one of the problems that many forward-looking researchers in this field need to solve urgently. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a modified solid oxide fuel cell composite electrode and a preparation method thereof, a solid oxide fuel cell, especially an in-situ solvent thermal preparation method of a modified solid oxide fuel cell electrode. The modified solid oxide fuel cell composite electrode provided by the present invention has a specific morphological structure and is prepared by a solvent thermal method, which has a simple process, is easy to operate, and has a controllable morphology, making it more suitable for industrial promotion and application. The polarization impedance of the electrode after modification is significantly reduced, and the output power of the battery is significantly improved.
[0006] The present invention provides a modified solid oxide fuel cell electrode, comprising a solid oxide fuel cell electrode and modified phase nanoparticles composited on the solid oxide fuel cell electrode;
[0007] The material of the modified phase nanoparticles includes one or more of single metal oxides, doped metal oxides and perovskite-type catalytic materials.
[0008] Preferably, the solid oxide fuel cell electrode comprises an anode and / or a cathode of a solid oxide fuel cell;
[0009] The particle size of the modified phase nanoparticles is 10 to 300 nm;
[0010] The shape of the modified phase nanoparticles includes one or more of nanospheres, nanocubes, nanorods and nanosheets;
[0011] The composite comprises in situ growth.
[0012] Preferably, the single metal oxide includes CuO, CeO 2 、Co 3 O 4 and Ag 2 One or more of O;
[0013] The doped metal oxide includes Sm-doped CeO 2 and / or Gd-doped CeO 2 ;
[0014] The perovskite-type catalytic material includes La 2 NiO 4 ,La 1-x Sr x MnO 3 and La 1-x Sr x CoO 3 One or more of;
[0015] The mass ratio of the modified phase nanoparticles to the solid oxide fuel cell electrode with which they are composited is (1-30):100.
[0016] Preferably, the modified phase nanoparticles are uniformly dispersed and in-situ grown on the solid oxide fuel cell electrode;
[0017] The compounding on the solid oxide fuel cell electrode includes compounding on the surface of the solid oxide fuel cell electrode and in the pores of the solid oxide fuel cell electrode;
[0018] The modified phase nanoparticles can form a modified phase nanoparticle layer to coat the surface of the solid oxide fuel cell electrode and the pore surface of the solid oxide fuel cell electrode.
[0019] Preferably, the modification method includes in-situ solvent thermal modification;
[0020] By regulating the conditions of the solvothermal reaction, one or more of the size, morphology and coverage area of the modified phase nanoparticles can be regulated;
[0021] The solid oxide fuel cell comprises one or more of a cathode symmetrical cell, an anode symmetrical cell, a button cell and a flat plate structure cell.
[0022] The present invention provides a method for preparing a modified solid oxide fuel cell electrode, comprising the following steps:
[0023] 1) mixing a metal salt solution and a pH adjuster to obtain a precursor reaction solution;
[0024] 2) placing a solid oxide fuel cell or an electrode of a solid oxide fuel cell in the precursor reaction solution obtained in the above step, and evacuating the solution to obtain a reaction system;
[0025] 3) The reaction system obtained in the above steps is placed in a reaction device, and a modified solid oxide fuel cell electrode is obtained after a solvent thermal reaction.
[0026] Preferably, the solvent of the metal salt solution includes a mixed solvent of an organic solvent and water or an organic solvent;
[0027] The metal salt includes one or more of metal nitrates, metal acetates, metal oxalates and metal carbonates;
[0028] The pH regulator includes one or more of propionic acid, acetic acid, oxalic acid, ammonia water and sodium hydroxide;
[0029] The pH value of the precursor reaction solution is 3 to 12;
[0030] The precursor reaction solution also includes a surfactant.
[0031] Preferably, the organic solvent comprises one or more of ethanol, ethylene glycol, glycerol, octanol, hexanol, acetone and ether;
[0032] The surfactant includes one or more of PVP, SDBS and CTAB;
[0033] The concentration of the metal salt solution is 0.001 to 0.5 mol / L;
[0034] The volume ratio of the surfactant to the solvent is (0.001-0.3):1;
[0035] The term "placed" includes fully immersed or semi-immersed.
[0036] Preferably, the vacuum pressure of the vacuum treatment is less than or equal to 100 KPa;
[0037] The temperature of the solvent thermal reaction is 100 to 300° C.;
[0038] The solvent thermal reaction time is 0.5 to 36 hours;
[0039] The reaction device comprises a hydrothermal reaction kettle.
[0040] The present invention also provides a solid oxide fuel cell, comprising an electrode;
[0041] The electrode includes a modified solid oxide fuel cell electrode as described in any one of the above technical solutions or a modified solid oxide fuel cell electrode prepared by the preparation method as described in any one of the above technical solutions.
[0042] The present invention provides a modified solid oxide fuel cell electrode, comprising a solid oxide fuel cell electrode and modified phase nanoparticles composited on the solid oxide fuel cell electrode; the material of the modified phase nanoparticles comprises one or more of a single metal oxide, a doped metal oxide and a perovskite-type catalytic material. Compared with the prior art, the present invention is aimed at the existing solid oxide fuel cells, which usually operate at a high temperature of 800 to 1000°C, and puts forward extremely high requirements on the high temperature resistance of the material. Although the operating temperature of the solid oxide fuel cell can be reduced to a medium temperature range of 600 to 800°C, the cost can be reduced, and the service life of the material and the battery can be extended, the temperature reduction will greatly increase the impedance of the battery cathode, causing the battery performance to be greatly attenuated. Moreover, the traditional solution impregnation modification method often requires repeated impregnation, the steps are complicated, and after impregnation, it needs to be sintered at a relatively high temperature, which causes damage to the electrode itself, high energy consumption and long time consumption.
[0043] The modified solid oxide fuel cell electrode prepared by the present invention has a specific microscopic morphology and structure, and can form modified phase nanoparticles of specific single metal oxides, doped metal oxides or perovskite-type catalytic materials on the electrode surface. The polarization impedance of the electrode after modification is significantly reduced, and the output power of the battery is significantly improved. More importantly, the present invention creatively adopts a solvent thermal method for modification, and in situ grows modified phase nanoparticles on the surface of the solid oxide fuel cell. Compared with the traditional solvent thermal method, this preparation method is simple in process, easy to operate, has good morphology controllability, low reaction temperature, and low energy consumption. It is a method for preparing in-situ modified solid oxide fuel cell electrodes with strong feasibility.
[0044] The experimental results show that the present invention can grow nanoparticles of different morphologies such as nanospheres and nanocubes in situ on the electrode surface through the solvothermal method, and the size of the nanoparticles can be controlled by adjusting the reaction conditions. The modified electrode has better electrochemical performance than the blank electrode and can reduce the polarization resistance by more than 20%. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a scanning electron microscope (SEM) image of the modified solid oxide fuel cell electrode prepared in Example 1 of the present invention;
[0046] Figure 2 is the XRD diffraction spectrum of the powder separated from the solvothermal solution in Example 1 of the present invention;
[0047] Figure 3 Arrhenius curves of polarization resistance of the unmodified LSCF electrode and Example 1 of the present invention after solvent thermal treatment at different temperatures;
[0048] Figure 4 The Co prepared in the present invention 3 O 4 Scanning electron microscope (SEM) image of the surface of the modified LSCF composite electrode;
[0049] Figure 5 The Co prepared in the present invention 3 O 4 High magnification scanning electron microscopy (SEM) image of the surface of the modified LSCF composite electrode;
[0050] Figure 6 This is the XRD diffraction spectrum of the powder separated from the solvothermal solution in Example 4 of the present invention. DETAILED DESCRIPTION
[0051] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.
[0052] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0053] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure raw materials or raw materials of conventional purity used in the field of solid oxide fuel cell cathode preparation.
[0054] The present invention provides a modified solid oxide fuel cell electrode, comprising a solid oxide fuel cell electrode and modified phase nanoparticles composited on the solid oxide fuel cell electrode;
[0055] The material of the modified phase nanoparticles includes one or more of single metal oxides, doped metal oxides and perovskite-type catalytic materials.
[0056] In principle, the present invention has no particular restrictions on the selection of the solid oxide fuel cell electrode. Those skilled in the art can select and adjust it according to the actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the solid oxide fuel cell electrode preferably includes an anode and / or cathode of a solid oxide fuel cell, and more preferably an anode or cathode of a solid oxide fuel cell.
[0057] The material of the modified phase nanoparticles in the present invention includes one or more of single metal oxides, doped metal oxides and perovskite-type catalytic materials, more preferably single metal oxides, doped metal oxides or perovskite-type catalytic materials.
[0058] In principle, the present invention has no particular restrictions on the specific selection of the single metal oxide. Those skilled in the art can select and adjust according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the single metal oxide preferably includes CuO, CeO 2 、Co 3 O 4 and Ag 2 O, more preferably CuO, CeO 2 、Co 3 O 4 or Ag 2 O.
[0059] In principle, the present invention has no particular restrictions on the specific selection of the doped metal oxide. Those skilled in the art can select and adjust according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance the controllability and operability, the doped metal oxide preferably includes Sm-doped CeO 2 and / or Gd-doped CeO 2 , more preferably Sm-doped CeO 2 or Gd-doped CeO 2 .
[0060] In principle, the present invention has no particular restrictions on the specific selection of the perovskite catalyst material. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance the controllability and operability, the perovskite catalyst material preferably includes La 2 NiO 4 ,La 1-x Sr x MnO 3 and La 1-x Sr x CoO 3 One or more of, more preferably La 2 NiO 4 ,La 1-x Sr x MnO 3 or La 1- x Sr x CoO 3 .
[0061] In principle, the present invention has no particular restriction on the particle size of the modified phase nanoparticles. Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the particle size of the modified phase nanoparticles is preferably 10 to 300 nm, more preferably 60 to 250 nm, and more preferably 60 to 100 nm.
[0062] In principle, the present invention has no particular restriction on the shape of the modified phase nanoparticles. Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the shape of the modified phase nanoparticles preferably includes one or more of nanospheres, nanocubes, nanorods and nanosheets, and more preferably nanospheres, nanocubes, nanorods or nanosheets.
[0063] In principle, the present invention has no particular restriction on the mass ratio of the modified phase nanoparticles and the solid oxide fuel cell electrode with which they are composited. Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the mass ratio of the modified phase nanoparticles and the solid oxide fuel cell electrode with which they are composited is preferably (1-30):100, more preferably (5-25):100, and more preferably (10-20):100.
[0064] In principle, the present invention has no particular restrictions on the specific method of the composite, and those skilled in the art can select and adjust according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the composite preferably includes in-situ growth. More specifically, the modified phase nanoparticles are preferably uniformly dispersed and in-situ grown on the solid oxide fuel cell electrode.
[0065] In principle, the present invention has no particular restrictions on the specific state of the composite, and those skilled in the art can select and adjust according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the composite on the solid oxide fuel cell electrode preferably includes composite on the surface of the solid oxide fuel cell electrode and in the pores of the solid oxide fuel cell electrode. More specifically, the modified phase nanoparticles can preferably form a modified phase nanoparticle layer coated on the surface of the solid oxide fuel cell electrode and the pore surface of the solid oxide fuel cell electrode.
[0066] In principle, the present invention has no particular limitation on the modification method, and those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the modification method preferably includes in-situ solvent thermal modification.
[0067] The present invention is to complete and refine the overall preparation process, further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability. In the present invention, it is preferred that by regulating the conditions of the solvent thermal reaction, one or more of the size, morphology and coverage area of the modified phase nanoparticles can be regulated, and it is more preferred that the size, morphology or coverage area of the modified phase nanoparticles can be regulated.
[0068] In principle, the present invention has no particular restrictions on the specific selection of the solid oxide fuel cell. Those skilled in the art can select and adjust according to the actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology and structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the solid oxide fuel cell preferably includes one or more of a symmetrical battery for the cathode, a symmetrical battery for the anode, a button battery and a flat structure battery, and more preferably a symmetrical battery, a symmetrical battery for the anode, a button battery or a flat structure battery.
[0069] The present invention does not have any special restrictions on the definition and structure of the symmetrical battery. The structure and definition of the symmetrical battery familiar to those skilled in the art can be used. Those skilled in the art can select and adjust according to the actual application, product requirements and quality requirements. The symmetrical battery of the present invention is a half-battery commonly used for detection in the art. In the art, a symmetrical battery only includes a cathode or an anode. It is a structure proposed for the convenience of studying electrode performance and can be understood as a half-battery. Conventional batteries include a cathode and an anode and are "full batteries".
[0070] The present invention provides a method for preparing a modified solid oxide fuel cell electrode, which is characterized by comprising the following steps:
[0071] 1) mixing a metal salt solution and a pH adjuster to obtain a precursor reaction solution;
[0072] 2) placing a solid oxide fuel cell or an electrode of a solid oxide fuel cell in the precursor reaction solution obtained in the above step, and evacuating the solution to obtain a reaction system;
[0073] 3) The reaction system obtained in the above steps is placed in a reaction device, and a modified solid oxide fuel cell electrode is obtained after a solvent thermal reaction.
[0074] The selection, composition and structure of materials in the above-mentioned preparation method, as well as the corresponding preferred principles, of the present invention can preferably correspond to the selection, composition and structure, as well as the corresponding preferred principles in the aforementioned modified solid oxide fuel cell electrode, and will not be elaborated here one by one.
[0075] The present invention firstly mixes a metal salt solution and a pH regulator to obtain a precursor reaction solution.
[0076] In principle, the present invention has no particular restrictions on the specific selection of the solvent of the metal salt solution. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the solvent of the metal salt solution preferably includes a mixed solvent of an organic solvent and water or an organic solvent.
[0077] In principle, the present invention has no particular restriction on the specific selection of the organic solvent. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the organic solvent preferably includes one or more of ethanol, ethylene glycol, glycerol, octanol, hexanol, acetone and ether, and more preferably ethanol, ethylene glycol, glycerol, octanol, hexanol, acetone or ether.
[0078] In principle, the present invention has no particular restrictions on the specific selection of the metal salt. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the metal salt preferably includes one or more of metal nitrates, metal acetates, metal oxalates and metal carbonates, and more preferably metal nitrates, metal acetates, metal oxalates or metal carbonates.
[0079] In principle, the present invention has no particular restriction on the specific selection of the pH regulator. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance the controllability and operability, the pH regulator preferably includes one or more of propionic acid, acetic acid, oxalic acid, ammonia water and sodium hydroxide, and more preferably propionic acid, acetic acid, oxalic acid, ammonia water or sodium hydroxide.
[0080] In principle, the present invention has no particular restriction on the pH value of the precursor reaction solution. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the pH value of the precursor reaction solution is preferably 3-12, more preferably 5-10, and more preferably 7-8.
[0081] The present invention completes and refines the overall preparation process, further ensures the specific morphology structure of the composite material, enhances the uniform dispersion of the modified phase material, better reduces the polarization resistance of the cathode, improves the output power of the battery, simplifies the preparation process, and enhances controllability and operability. The precursor reaction solution preferably also includes a surfactant.
[0082] In principle, the present invention has no particular restriction on the specific selection of the surfactant, and those skilled in the art can select and adjust it according to actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the surfactant preferably includes one or more of PVP, SDBS and CTAB, and more preferably PVP, SDBS or CTAB.
[0083] In principle, the present invention has no particular limitation on the concentration of the metal salt solution. Those skilled in the art can select and adjust it according to actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the concentration of the metal salt solution is preferably 0.001-0.5 mol / L, more preferably 0.1-0.4 mol / L, and more preferably 0.2-0.3 mol / L.
[0084] In principle, the present invention has no particular restriction on the volume ratio of the surfactant to the solvent. Those skilled in the art can select and adjust it according to actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the volume ratio of the surfactant to the solvent is preferably (0.001-0.3):1, more preferably (0.05-0.25):1, and more preferably (0.1-0.2):1.
[0085] The present invention then places the solid oxide fuel cell or the electrode of the solid oxide fuel cell in the precursor reaction solution obtained in the above steps, and performs vacuum treatment to obtain a reaction system.
[0086] In principle, the present invention has no particular restrictions on the manner of placing, and those skilled in the art can select and adjust according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the placing preferably includes complete immersion or semi-immersion. Specifically, when selecting an electrode of a solid oxide fuel cell or a half-cell in a solid oxide fuel cell (a symmetrical cell of the cathode, a symmetrical cell of the anode), complete immersion can be selected; when selecting a button cell and a flat structure battery, complete immersion or semi-immersion can be selected, that is, only a certain electrode in the solid oxide fuel cell can be selected.
[0087] In principle, the present invention has no particular limitation on the vacuum pressure of the vacuum treatment, and those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance the controllability and operability, the vacuum pressure of the vacuum treatment is preferably less than or equal to 100KPa, more preferably less than or equal to 10KPa, and more preferably less than or equal to 1KPa.
[0088] Finally, the present invention puts the reaction system obtained in the above steps into a reaction device to carry out a solvent thermal reaction to obtain a modified solid oxide fuel cell electrode.
[0089] In principle, the present invention has no particular limitation on the temperature of the solvent thermal reaction. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance the controllability and operability, the temperature of the solvent thermal reaction is preferably 100-300°C, more preferably 120-270°C, more preferably 120-240°C, and more preferably 120-200°C.
[0090] In principle, the present invention has no particular limitation on the time of the solvent thermal reaction. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance the controllability and operability, the time of the solvent thermal reaction is preferably 0.5 to 36 hours, more preferably 0.5 to 30 hours, more preferably 0.2 to 20 hours, and more preferably 0.5 to 10 hours.
[0091] In principle, the present invention has no particular restrictions on the specific selection of the reaction device. Those skilled in the art can select and adjust it according to actual application conditions, product requirements and quality requirements. In order to further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability, the reaction device preferably includes a hydrothermal reactor.
[0092] The present invention is to complete and refine the overall preparation process, further ensure the specific morphology structure of the composite material, enhance the uniform dispersion of the modified phase material, better reduce the polarization resistance of the cathode, improve the output power of the battery, simplify the preparation process, and enhance controllability and operability. The present invention uses a solvent thermal method to in-situ grow nanoparticles on the surface of a solid oxide fuel cell. The preparation method of the modified solid oxide fuel cell electrode can specifically include the following steps:
[0093] (1) Prepare the solvent thermal solution according to the material to be modified;
[0094] (2) Immersing the battery in the solution, then evacuating the solution and performing a solvothermal reaction;
[0095] (3) The battery is taken out of the solution and cleaned with deionized water and ethanol to obtain an electrode modified with nanoparticles.
[0096] More specific:
[0097] (1) According to the materials required for the modified phase, the required metal salt is dissolved in a solvent in a certain proportion, and acid or base is added as required to adjust the pH of the solution to prepare a precursor solvothermal reaction solution; a surfactant may be further added to improve the solvothermal effect and the morphology of the nanoparticles;
[0098] (2) immersing the battery in a solvent hot solution and performing a vacuum treatment;
[0099] (3) The solution and the battery are transferred to a hydrothermal reactor for an in-situ solvothermal reaction, and the nanoparticles are grown in-situ on the electrode surface;
[0100] (4) The battery is taken out of the solution and repeatedly cleaned with ethanol and deionized water until there is no residual powder on the surface of the battery, thereby obtaining an electrode structure modified with nanoparticles.
[0101] The present invention also provides a solid oxide fuel cell, comprising an electrode;
[0102] The electrode includes the modified solid oxide fuel cell electrode described in any one of the above technical solutions or the modified solid oxide fuel cell electrode prepared by the preparation method described in any one of the above technical solutions.
[0103] The above steps of the present invention provide a modified solid oxide fuel cell electrode and its in-situ solvent thermal preparation method, and a solid oxide fuel cell. The present invention further reduces the resistance of the electrode without changing the existing commercial solid oxide fuel cell material system. It is a very feasible method for in-situ modification of solid oxide fuel cell electrodes. The present invention uses a solvent thermal method to modify nanoparticles on the surface of the solid oxide fuel cell electrode. The reaction temperature is low, the energy consumption is low, the method is simple, and the operation is convenient. The new method for modifying solid oxide fuel cell electrodes provided by the present invention grows nanoparticles in situ on the electrode surface by a solvent thermal method. The method is simple, easy to operate, and the morphology is controllable. The polarization impedance of the electrode after modification is significantly reduced, and the output power of the battery is significantly improved. Moreover, the modified solid oxide fuel cell electrode prepared by the present invention has a specific microscopic morphology and structure, and can form modified phase nanoparticles of specific single metal oxides, doped metal oxides or perovskite-type catalytic materials on the electrode surface. The polarization impedance of the electrode after modification is significantly reduced, and the output power of the battery is significantly improved.
[0104] The experimental results show that the present invention can grow nanoparticles of different morphologies such as nanospheres and nanocubes in situ on the electrode surface through the solvothermal method, and the size of the nanoparticles can be controlled by adjusting the reaction conditions. The modified electrode has better electrochemical performance than the blank electrode and can reduce the polarization resistance by more than 20%.
[0105] In order to further illustrate the present invention, a modified solid oxide fuel cell electrode and a preparation method thereof, and a solid oxide fuel cell provided by the present invention are described in detail below in combination with embodiments. However, it should be understood that these embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention. The protection scope of the present invention is not limited to the following embodiments.
[0106] Example 1
[0107] (1) 0.25 g of Ce(NO 3 ) 3 6H 2 O was dissolved in 30 mL of ethylene glycol, and then 1 mL of deionized water and 1 mL of propionic acid were added, and stirred until the solid was completely dissolved to obtain the solution required for solvothermal treatment;
[0108] (2) placing a pre-prepared symmetrical battery of the structure LSCF / GDC / YSZ / GDC / LSCF into a 50 mL polytetrafluoroethylene liner, slowly pouring the solution in step (1) into the polytetrafluoroethylene liner so that the battery is completely immersed in the solution, and then evacuating to -30 kPa;
[0109] (3) Transfer the polytetrafluoroethylene liner in step (2) to a stainless steel hydrothermal reactor and seal the reactor. Place the reactor in an oven and heat it to 150°C to 180°C for 4 hours. 2 Nanoparticles will grow in situ on the surface of LSCF electrodes;
[0110] (4) Take the symmetrical battery out of the solution and wash it repeatedly with deionized water and ethanol until it is clear to obtain CeO 2 Nanoparticle LSCF electrode.
[0111] The morphology and structure of the modified solid oxide fuel cell composite cathode prepared in Example 1 of the present invention were characterized by using a scanning electron microscope (SEM) and an X-ray powder diffractometer (XRD), and the performance was tested by measuring its impedance spectrum (EIS) using a high-performance battery testing system.
[0112] See also Figure 1 , Figure 1 The SEM images of the modified solid oxide fuel cell electrode prepared in Example 1 of the present invention are shown in Figures (a, b) and (c, d) respectively. The SEM images are shown in Figures (a, b) and (c) respectively. The SEM images are shown in Figures (c, d) and (e, f) respectively. The SEM images are shown in Figures (e, f) and (f) respectively.
[0113] Depend on Figure 1 It can be seen that the CeO prepared in Example 1 2 The surface of the modified LSCF cathode is evenly covered with many nanoparticles, which have a spherical morphology. The size and coverage area of the nanoparticles change with the temperature. The higher the reaction temperature, the larger the size of the nanoparticles and the larger the coverage area. This shows that the in-situ solvothermal method can achieve uniform modification of nanoparticles on the electrode. Moreover, the morphology and parameters of the nanoparticles can be changed by changing the parameters.
[0114] See also Figure 2 , Figure 2 This is the XRD diffraction spectrum of the powder separated from the solvothermal solution in Example 1 of the present invention.
[0115] Depend on Figure 2 As shown in the figure, all the characteristic peaks can be related to CeO 2 The PDF standard cards correspond one to one, indicating that CeO was successfully synthesized. 2 of nanoparticles.
[0116] See also Figure 3 , Figure 3 Arrhenius curves of polarization resistance of the unmodified LSCF electrode and Example 1 of the present invention after solvent thermal treatment at different temperatures.
[0117] Depend on Figure 3 It can be seen that after CeO 2 After modification, the polarization resistance of the LSCF electrode was significantly reduced. The polarization resistance of the unmodified LSCF electrode was 0.338 Ω·cm at 750 °C. 2 After hydrothermal treatment at 150℃, 165℃, and 180℃ for 4h, the polarization resistance of the modified LSCF electrode at 750℃ decreased to 0.227Ω·cm 2 、0.2095Ω·cm 2 , 0.219Ω·cm 2 , and the activation energy is significantly lower than that of the unmodified LSCF electrode.
[0118] Example 2
[0119] (1) 0.25 g of Ce(NO 3 ) 3 6H 2 O, 0.0284g Sm(NO 3 ) 3 6H 2 O was dissolved in 30 mL of ethylene glycol, and then 1 mL of deionized water and 1 mL of propionic acid were added, and stirred until the solid was completely dissolved to obtain the solution required for solvothermal treatment;
[0120] (2) placing a pre-prepared symmetrical battery of the structure LSCF / GDC / YSZ / GDC / LSCF into a 50 mL polytetrafluoroethylene liner, slowly pouring the solution in step (1) into the polytetrafluoroethylene liner so that the battery is completely immersed in the solution, and then evacuating to -30 kPa;
[0121] (3) The polytetrafluoroethylene liner in step (2) was transferred to a stainless steel hydrothermal reactor and the reactor was sealed. The reactor was placed in an oven and heated to 180°C and kept warm for 2 hours. 0.1 Ce 0.9 O 2 Nanoparticles will grow in situ on the surface of LSCF electrodes;
[0122] (4) Take the symmetrical battery out of the solution and wash it repeatedly with deionized water and ethanol until it is clear to obtain the Sm-containing 0.1 Ce 0.9 O 2 Nanoparticle LSCF electrode.
[0123] The polarization impedance of the modified solid oxide fuel cell composite electrode prepared in Example 2 of the present invention was tested using a high-performance electrochemical testing device.
[0124] The results show that the polarization resistance of the unmodified LSCF at 750°C is 0.587Ω·cm 2 After modification, the electrode polarization resistance dropped to 0.4998Ω·cm 2 .
[0125] Example 3
[0126] (1) 0.25 g of Ce(NO 3 ) 3 6H 2 O, 0.0288 g Gd(NO 3 ) 3 6H 2 O was dissolved in 30 mL of ethylene glycol, and then 1 mL of deionized water and 1 mL of propionic acid were added, and stirred until the solid was completely dissolved to obtain the solution required for solvothermal treatment;
[0127] (2) placing a pre-prepared symmetrical battery of the structure LSCF / GDC / YSZ / GDC / LSCF into a 50 mL polytetrafluoroethylene liner, slowly pouring the solution in step (1) into the polytetrafluoroethylene liner so that the battery is completely immersed in the solution, and then evacuating to -30 kPa;
[0128] (3) The polytetrafluoroethylene liner in step (2) was transferred to a stainless steel hydrothermal reactor and the reactor was sealed. The reactor was placed in an oven and heated to 180°C and kept warm for 4 hours.0.1 Ce 0.9 O 2 Nanoparticles will grow in situ on the surface of LSCF electrodes;
[0129] (4) Take the symmetrical battery out of the solution and wash it repeatedly with deionized water and ethanol until it is clear to obtain the Gd-containing 0.1 Ce 0.9 O 2 Nanoparticle LSCF electrode.
[0130] Example 4
[0131] (1) 0.65 g Co(NO 3 ) 2 6H 2 O was added to 20 mL of ethanol and stirred magnetically for 2 h to obtain solution A;
[0132] (2) Add 0.128 g of NaOH to 20 mL of ethanol and stir until the NaOH is completely dissolved to obtain solution B;
[0133] (3) While stirring, slowly drip solution B into solution A to obtain a black turbid liquid. Continue stirring for 3 h to obtain a solvothermal precursor solution.
[0134] (4) placing the previously prepared symmetrical battery of the structure of LSCF / GDC / YSZ / GDC / LSCF into a 50 mL polytetrafluoroethylene liner, slowly pouring the solution in step (3) into the polytetrafluoroethylene liner so that the battery is completely immersed in the solution, and then evacuating to -30 kPa;
[0135] (5) Transfer the polytetrafluoroethylene liner in step (2) to a stainless steel hydrothermal reactor and seal the reactor. Place the reactor in an oven and heat it to 160°C for 8 hours. 3 O 4 Nanoparticles will grow in situ on the surface of LSCF electrodes;
[0136] (6) The symmetrical battery was taken out of the solution and repeatedly washed with deionized water and ethanol until it was clear. 3 O 4 Nanoparticle LSCF electrode.
[0137] The modified solid oxide fuel cell composite electrode prepared in Example 4 of the present invention was characterized by scanning electron microscopy (SEM) for morphology and structure.
[0138] See also Figure 4 , Figure 4 The Co prepared in the present invention 3 O 4Scanning electron microscopy (SEM) image of the surface of the modified LSCF composite electrode.
[0139] Depend on Figure 4 It can be observed that a large number of nanoparticles are generated on the surface of LSCF, and the size of the nanoparticles is very uniform, about 50nm, and has good dispersion.
[0140] See also Figure 5 , Figure 5 The Co prepared in the present invention 3 O 4 High magnification scanning electron microscopy (SEM) image of the surface of the modified LSCF composite electrode.
[0141] Depend on Figure 5 It can be seen that the nanoparticles generated on the LSCF surface have a cubic structure and are evenly distributed.
[0142] See also Figure 6 , Figure 6 This is the XRD diffraction spectrum of the powder separated from the solvothermal solution in Example 4 of the present invention.
[0143] The powder obtained after centrifugation and washing of the solvent thermal solution was characterized by Figure 6 It can be seen that its characteristic peak is similar to Co 3 O 4 PDF standard cards correspond one to one, indicating that Co 3 O 4 .
[0144] The modified solid oxide fuel cell cathode prepared in Example 4 of the present invention was tested for performance by using an electrochemical impedance spectroscopy (EIS) system.
[0145] The polarization impedance test results of the high-performance electrochemical device showed that the polarization resistance of the unmodified LSCF electrode was 0.587Ω·cm at 750℃. 2 , after Co 3 O 4 After modification, the polarization resistance at 750℃ decreased to 0.335Ω·cm 2 , which has been improved significantly.
[0146] Example 5
[0147] (1) 0.25 g of Ce(NO 3 ) 3 6H 2 O was dissolved in 30 mL of ethylene glycol, and then 1 mL of deionized water and 1 mL of propionic acid were added, and stirred until the solid was completely dissolved to obtain the solution required for solvothermal treatment;
[0148] (2) placing a button cell of the structure Ni-YSZ / YSZ / GDC / LSCF prepared in advance into a 50 mL polytetrafluoroethylene liner, slowly pouring the solution in step (1) into the polytetrafluoroethylene liner so that the cell is completely immersed in the solution, and then evacuating to -30 kPa;
[0149] (3) The polytetrafluoroethylene liner in step (2) was transferred to a stainless steel hydrothermal reactor, the reactor was sealed, and the temperature was raised to 180°C in an oven and kept at this temperature for 4 hours. CeO 2 Nanoparticles will be grown in situ on both the anode and cathode surfaces simultaneously;
[0150] (4) The symmetrical battery is taken out of the solution and repeatedly washed with deionized water and ethanol until it is clear. The anode and cathode contain CeO 2 Nanoparticle-modified button battery.
[0151] Example 6
[0152] (1) 0.25 g of Ce(NO 3 ) 3 6H 2 O was dissolved in 30 mL of ethylene glycol, and then 1 mL of deionized water and 1 mL of propionic acid were added, and stirred until the solid was completely dissolved to obtain the solution required for solvothermal treatment;
[0153] (2) placing a button cell of the structure Ni-YSZ / YSZ / GDC / LSCF-GDC prepared in advance into a 50 mL polytetrafluoroethylene liner, slowly pouring the solution in step (1) into the polytetrafluoroethylene liner so that the cell is completely immersed in the solution, and then evacuating to -30 kPa;
[0154] (3) The polytetrafluoroethylene liner in step (2) was transferred to a stainless steel hydrothermal reactor and the reactor was sealed. The reactor was placed in an oven and heated to 180°C and kept warm for 4 hours. CeO 2 Nanoparticles will be grown in situ on both the anode and cathode surfaces simultaneously;
[0155] (4) The symmetrical battery is taken out of the solution and repeatedly washed with deionized water and ethanol until it is clear. The anode and cathode contain CeO 2 Nanoparticle-modified button battery.
[0156] The above is a detailed introduction to a modified solid oxide fuel cell electrode and its in-situ solvent thermal preparation method and solid oxide fuel cell provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and its core ideas of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in several ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the text of the claims, or if they include equivalent structural elements that are not substantially different from the text of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A method for preparing a modified solid oxide fuel cell electrode, It is characterized in that The following steps are involved: 1) mixing a metal salt solution and a pH adjuster to obtain a precursor reaction solution; 2) placing a solid oxide fuel cell or an electrode of a solid oxide fuel cell in the precursor reaction solution obtained in the above step, and evacuating the solution to obtain a reaction system; 3) placing the reaction system obtained in the above steps into a reaction device, and performing a solvothermal reaction to obtain a modified solid oxide fuel cell electrode; The modified solid oxide fuel cell electrode comprises a solid oxide fuel cell electrode and modified phase nanoparticles composited on the solid oxide fuel cell electrode; The material of the modified phase nanoparticles includes single metal oxides and / or doped metal oxides; The single metal oxide includes CeO 2 and / or Co 3 O 4 ; The doped metal oxide includes Sm-doped CeO 2 and / or Gd-doped CeO 2 ; The temperature of the solvent thermal reaction is 100 to 300° C.; The solvent thermal reaction time is 0.5 to 36 hours.
2. The preparation method according to claim 1, It is characterized in that The solid oxide fuel cell electrode comprises an anode and / or a cathode of a solid oxide fuel cell; The particle size of the modified phase nanoparticles is 10 to 300 nm; The shape of the modified phase nanoparticles includes one or more of nanospheres, nanocubes and nanosheets; The composite comprises in situ growth.
3. The preparation method according to claim 2, It is characterized in that The mass ratio of the modified phase nanoparticles to the solid oxide fuel cell electrode with which they are composited is (1-30):
100.
4. The preparation method according to claim 1, It is characterized in that The modified phase nanoparticles are uniformly dispersed and in-situ grown on the solid oxide fuel cell electrode.
5. The preparation method according to claim 1, It is characterized in that The compounding on the solid oxide fuel cell electrode includes compounding on the surface of the solid oxide fuel cell electrode and in the pores of the solid oxide fuel cell electrode; The modified phase nanoparticles form a modified phase nanoparticle layer that covers the surface of the solid oxide fuel cell electrode and the pore surface of the solid oxide fuel cell electrode.
6. The preparation method according to claim 1, It is characterized in that The solid oxide fuel cell comprises one or more of a cathode symmetrical cell, an anode symmetrical cell, a button cell and a flat plate structure cell.
7. The preparation method according to claim 1, It is characterized in that The solvent of the metal salt solution includes a mixed solvent of an organic solvent and water or an organic solvent; The metal salt includes one or more of metal nitrates, metal acetates, metal oxalates and metal carbonates; The pH regulator includes one or more of propionic acid, acetic acid, oxalic acid, ammonia water and sodium hydroxide; The pH value of the precursor reaction solution is 3 to 12; The precursor reaction solution also includes a surfactant.
8. The preparation method according to claim 7, It is characterized in that The organic solvent comprises one or more of ethanol, ethylene glycol, glycerol, octanol, hexanol, acetone and ether; The surfactant includes one or more of PVP, SDBS and CTAB; The concentration of the metal salt solution is 0.001 to 0.5 mol / L; The volume ratio of the surfactant to the solvent is (0.001-0.3):1; The term "placed" includes fully immersed or semi-immersed.
9. The preparation method according to claim 1, It is characterized in that The vacuum pressure of the vacuum treatment is less than or equal to 100KPa; The reaction device comprises a hydrothermal reaction kettle.
10. A solid oxide fuel cell, It is characterized in that including electrodes; The electrode comprises a modified solid oxide fuel cell electrode prepared by the preparation method according to any one of claims 1 to 9.