Polyimide resin composition, polyimide varnish and polyimide film
By introducing a sulfonyl diamine monomer and an oxazole-based cross-linking agent into the polyimide resin, a polyimide resin composition is formed, which solves the risk of reduced optical properties and damage to the polyimide film during the peeling process. High problem, achieving high colorless transparency, optical isotropy and excellent peeling performance.
Patent Information
- Application Number
- CN202080070656.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-11
- Filing Date
- 2020-10-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-08
AI Technical Summary
The existing technology has problems such as reduced optical properties, high risk of damage, complex processes, and poor stability during the peeling process of polyimide films. In particular, it is difficult to achieve excellent performance in maintaining colorless transparency and optical isotropy.
A composition containing a polyimide resin and a cross-linking agent containing specific structural units is used to introduce a sulfonyl-based diamine monomer and an oxazole-based cross-linking agent into the polyimide resin to form a polyimide resin with excellent optical properties and peelability. High-performance polyimide resin compositions for the preparation of polyimide varnishes and films.
It achieves high colorless transparency, optical isotropy and excellent peelability of the polyimide film, reduces residual stress and damage risk, and improves the heat resistance and mechanical strength of the film.
Smart Images

Figure BDA0003585175500000031 
Figure BDA0003585175500000041 
Figure BDA0003585175500000042
Abstract
Description
Technical Field
[0001] The invention relates to a polyimide resin composition, a polyimide varnish and a polyimide film. Background Art
[0002] Polyimide resins are being studied for various uses in the fields of electrical and electronic components. For example, in order to make devices lighter and more flexible, it is expected that glass substrates used in image display devices such as liquid crystal displays and OLED displays will be replaced with plastic substrates, and research on polyimide films suitable as such plastic substrates is being promoted.
[0003] In an image display device, when light emitted from a display element is emitted through a plastic substrate, the plastic substrate is required to be colorless and transparent. Furthermore, when light passes through a phase difference film or a polarizing plate (for example, a liquid crystal display, a touch panel, etc.), in addition to being colorless and transparent, high optical isotropy (i.e., low Rth) is also required.
[0004] Moreover, when a polyimide film is used as a substrate, the target electronic circuit is made on the polyimide film through various processes such as a sputtering process and an etching process for making an oxide semiconductor film such as an indium tin oxide (ITO) film, depending on the purpose. When the target electronic circuit is made on the polyimide film, the flatness of the polyimide film must be ensured. For this reason, the polyimide film is closely attached to a hard support such as a glass plate, and can be peeled off from the support after cooling.
[0005] As a method for making a polyimide film adhere to a support, in addition to a method of adding an adhesive to the polyimide itself, there is also known a method of interposing a layer called a release layer between the polyimide film and the support to ensure adhesion during the process.
[0006] In addition, as a method of peeling a polyimide film from a support, for example, the following method is known.
[0007] Method (1) obtains a structure including a polyimide resin / support body, and then irradiates the support body with laser to ablate the polyimide resin interface, thereby peeling the polyimide resin (see, for example, Patent Document 1). The types of lasers include solid (YAG) lasers and gas (UV excimer) lasers, and a spectrum of 308 nm or the like is used.
[0008] Method (2) is to form a release layer on the support before coating the resin composition on the support, and then obtain a structure including polyimide resin film / release layer / support, and mechanically release the polyimide resin film (for example, see Patent Document 2). As the release layer, there are methods using Parylene (registered trademark, manufactured by Parylene Japan KK) and tungsten oxide; methods using a vegetable oil-based, silicone-based, fluorine-based, or alkyd-based release agent, etc. In addition, the laser irradiation described in the above (1) is sometimes used in combination.
[0009] In addition, Patent Document 3 discloses the following method: fixing a resin substrate on a supporting substrate by means of an adhesive layer, forming an electronic component on the resin substrate, and peeling an electronic device including the electronic component and the resin substrate from the supporting substrate, wherein the adhesive layer is composed mainly of a material whose adhesive strength with the supporting substrate is reduced by contact with moisture.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application No. 2007-512568
[0013] Patent Document 2: Japanese Patent Application Publication No. 2010-067957
[0014] Patent Document 3: Japanese Patent Application Publication No. 2016-021384 Summary of the invention
[0015] Problem that the invention aims to solve
[0016] The method (1) requires an expensive laser irradiation device and may damage the resin substrate formed on the base during laser irradiation. The method (2) may limit the combination of the release layer and the polyimide in order to achieve the best performance.
[0017] In the method of Patent Document 3, when forming an electronic component, in order to prevent the adhesive layer from contacting with moisture and thus not reducing the adhesive force, a sealing layer must be formed to seal the exposed part of the adhesive layer. On the other hand, when the electronic device is peeled off after the electronic component is formed, in order to make the adhesive layer contact with moisture, the sealing layer must be removed before peeling. Therefore, the method of Patent Document 3 is a complicated process as a whole. Furthermore, in order to contact with moisture, it must be set in a high humidity environment with a humidity of more than 90%, which has the problem of difficulty in controlling the moisture content and ensuring stable peelability. Furthermore, the polyimide used in Patent Document 3 uses phenylenediamine with strong intramolecular charge transfer interaction, so it is easy to color, resulting in low transparency, and the polymer molecules are in a structure that is easy to arrange, so the optical isotropy is low.
[0018] As described above, according to the above method, optical properties such as colorless transparency and optical isotropy of the film tend to decrease due to damage, addition of a release layer, and properties of the polymer, and the yield also tends to deteriorate.
[0019] Thus, a polyimide resin is required which can maintain the high colorless transparency and optical properties such as optical isotropy of the obtained polyimide film and can easily and stably peel the polyimide film from a glass substrate or a silicon substrate.
[0020] Therefore, an object of the present invention is to provide a polyimide resin composition capable of forming a film having excellent colorless transparency and optical isotropy and excellent releasability from a substrate, and a polyimide varnish and a polyimide film comprising the polyimide resin composition.
[0021] Solutions for solving problems
[0022] The present inventors have found that a polyimide resin composition containing a polyimide resin including a combination of specific structural units and a specific crosslinking agent can solve the above-mentioned problems, and have thus completed the invention.
[0023] That is, the present invention relates to the following <1> to <11>.
[0024] <1> A polyimide resin composition comprises: a polyimide resin and a cross-linking agent having at least two oxazole groups.
[0025] The polyimide resin is a polyimide resin having a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from diamine.
[0026] The structural unit B includes a structural unit (B-1) derived from a diamine having a sulfonyl group in its structure and a structural unit (B-2) derived from a compound represented by the following formula (b-2).
[0027]
[0028] (In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii), p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4. When p is 0, m1 is an integer of 1 to 4.)
[0029]
[0030] (In formula (b-2-i), m3 is an integer of 0 to 5; in formula (b-2-ii), m4 is an integer of 0 to 5. It should be noted that when m1+m2+m3+m4 is 1 or more and p is 2, 2 Xs and 2 m2 to m4 are independently selected.)
[0031] <2> According to the above <1> The polyimide resin composition, wherein the structural unit (B-2) is a structural unit (B-21) derived from a compound represented by the following formula (b-21).
[0032]
[0033] <3> According to the above <1> or <2> The polyimide resin composition, wherein the structural unit (B-1) is at least one selected from the group consisting of a structural unit (B-11) derived from a compound represented by the following formula (b-11), a structural unit (B-12) derived from a compound represented by the following formula (b-12), and a structural unit (B-13) derived from a compound represented by the following formula (b-13).
[0034]
[0035] <4> According to the above <1> ~ <3> The polyimide resin composition described in any one of the preceding claims, wherein the structural unit A comprises at least one selected from the group consisting of a structural unit (A-1) derived from a compound represented by the following formula (a-1) and a structural unit (A-2) derived from a compound represented by the following formula (a-2).
[0036]
[0037] <5> According to the above <1> ~ <4> The polyimide resin composition described in any one of the preceding claims, wherein the structural unit B further includes a structural unit (B-3) derived from a compound represented by the following formula (b-3).
[0038]
[0039] (In formula (b-3), Z 1 and Z 2 Each independently represents a divalent aliphatic group or a divalent aromatic group which may contain an oxygen atom, and R 1 and R 2 Each independently represents a monovalent aromatic group or a monovalent aliphatic group, R 3 and R 4 Each independently represents a monovalent aliphatic group, R 5 and R 6Each independently represents a monovalent aliphatic group or a monovalent aromatic group, m and n each independently represent an integer greater than 1, and the sum of m and n represents an integer of 2 to 1000. 1 and R 2 At least one of them represents a monovalent aromatic group. )
[0040] <6> According to the above <1> ~ <5> The polyimide resin composition described in any one of the preceding claims, wherein the structural unit B further includes a structural unit (B-4) derived from a compound represented by the following formula (b-4).
[0041]
[0042] <7> According to the above <1> ~ <6> The polyimide resin composition described in any one of the preceding claims, wherein the crosslinking agent is a compound including an aromatic ring or an aromatic heterocyclic ring to which at least two oxazole groups are bonded.
[0043] <8> According to the above <1> ~ <7> The polyimide resin composition described in any one of the preceding claims, wherein the crosslinking agent is a compound including a benzene ring to which at least two oxazolyl groups are bonded.
[0044] <9> According to the above <1> ~ <8> The polyimide resin composition described in any one of the preceding claims, wherein the crosslinking agent is 1,3-bis(4,5-dihydro-2-oxazolyl)benzene.
[0045] <10> A polyimide varnish, which is the above <1> ~ <9> The polyimide resin composition described in any one of the above is dissolved in an organic solvent.
[0046] <11> A polyimide film, which is the above <1> ~ <9> The polyimide resin in any one of the polyimide resin compositions is cross-linked by the cross-linking agent.
[0047] Effects of the Invention
[0048] According to the present invention, a thin film which is excellent in colorlessness, transparency, and optical isotropy and further has excellent releasability from a substrate can be formed. DETAILED DESCRIPTION
[0049] [Polyimide resin composition]
[0050] The polyimide resin composition of the present invention comprises: a polyimide resin and a crosslinking agent. The polyimide resin and the crosslinking agent in the present invention are described below.
[0051] It should be noted that the reason why the polyimide resin composition of the present invention maintains colorless transparency, optical properties such as optical isotropy, and has excellent peeling properties is unclear, but it is believed that the stacking between imides is hindered by the curved polymer molecular structure derived from the diamine monomer having a sulfonyl group on the main chain, and the optical properties such as optical isotropy are excellent, and the residual stress of the obtained polyimide film can be reduced, so the peeling properties are excellent.
[0052] <Polyimide resin>
[0053] The polyimide resin contained in the polyimide resin composition of the present invention has a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from a diamine, and the structural unit B includes: a structural unit (B-1) derived from a diamine having a sulfonyl group in the structure, and a structural unit (B-2) derived from a compound represented by the following formula (b-2).
[0054]
[0055] (In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii), p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4. When p is 0, m1 is an integer of 1 to 4.)
[0056]
[0057] (In formula (b-2-i), m3 is an integer of 0 to 5; in formula (b-2-ii), m4 is an integer of 0 to 5. It should be noted that when m1+m2+m3+m4 is 1 or more and p is 2, 2 Xs and 2 m2 to m4 are independently selected.)
[0058] (Structural unit A)
[0059] The structural unit A is a structural unit derived from tetracarboxylic dianhydride which occupies the polyimide resin.
[0060] As structural unit A, it is preferred to include at least one selected from the group consisting of a structural unit (A-1) derived from a compound represented by the following formula (a-1) and a structural unit (A-2) derived from a compound represented by the following formula (a-2), and it is more preferred to include structural unit (A-2). By including structural unit (A-2), colorless transparency and optical isotropy can be improved, and residual stress can also be reduced.
[0061] On the other hand, it is more preferable to contain the structural unit (A-1) particularly from the viewpoint of colorless transparency and heat resistance.
[0062]
[0063] The compound represented by formula (a-1) is norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride. By including the structural unit (A-1), the structural unit A can improve the colorless transparency and heat resistance of the film.
[0064] The ratio of the structural unit (A-1) in the structural unit A is preferably 40 mol% or more, more preferably 50 mol% or more, and further preferably 60 mol% or more. The upper limit of the ratio of the structural unit (A-1) is not particularly limited, that is, 100 mol%. The structural unit A may be composed only of the structural unit (A-1).
[0065] The compound represented by formula (a-2) is 1,2,4,5-cyclohexanetetracarboxylic dianhydride. By including the structural unit (A-2), the structural unit A can improve the colorless transparency and optical isotropy of the film and further reduce the residual stress.
[0066] The ratio of the structural unit (A-2) in the structural unit A is preferably 50 mol% or more, more preferably 70 mol% or more, and further preferably 85 mol% or more. The upper limit of the ratio of the structural unit (A-2) is not particularly limited, that is, 100 mol%. The structural unit A may be composed only of the structural unit (A-2).
[0067] When the structural unit A contains the structural unit (A-1) and the structural unit (A-2), the total ratio of the structural units (A-1) and (A-2) in the structural unit A is preferably 50 mol% or more, more preferably 70 mol% or more, further preferably 90 mol% or more, and particularly preferably 99 mol% or more. The upper limit of the total ratio of the structural units (A-1) and (A-2) is not particularly limited, that is, 100 mol%. The structural unit A may be composed only of the structural unit (A-1) and the structural unit (A-2).
[0068] The structural unit A may contain structural units other than the structural units (A-1) and (A-2).
[0069] The structural unit A may contain a structural unit (A-3) derived from silicone modified with acid anhydrides at both ends in addition to the structural units (A-1) and (A-2).
[0070] As the silicone modified with anhydride at both ends, a compound represented by the following formula (a-3) is preferred.
[0071]
[0072] (In formula (a-3),
[0073] R 31 ~R 36 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms,
[0074] L 31 and L 32 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms,
[0075] Z 31 and Z 32 are each independently a trivalent hydrocarbon group having 1 to 20 carbon atoms,
[0076] n3 is 1 to 200. )
[0077] R in formula (a-3) 31 ~R 36 Each independently is a monovalent hydrocarbon group having 1 to 20 carbon atoms.
[0078] Examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms include alkyl groups having 1 to 20 carbon atoms, cycloalkyl groups having 3 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms, aralkyl groups having 7 to 20 carbon atoms, and alkenyl groups having 2 to 20 carbon atoms.
[0079] As the alkyl group having 1 to 20 carbon atoms, an alkyl group having 1 to 10 carbon atoms is preferred, and examples thereof include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, and hexyl. As the cycloalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms is preferred, and examples thereof include cyclopentyl and cyclohexyl. As the aryl group having 6 to 20 carbon atoms, an aryl group having 6 to 10 carbon atoms is preferred, and examples thereof include phenyl and naphthyl. As the aralkyl group having 7 to 20 carbon atoms, an aralkyl group having 7 to 10 carbon atoms is preferred, and examples thereof include benzyl and phenethyl. As the alkenyl group having 2 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms is preferred, and examples thereof include vinyl, allyl, propenyl, isopropenyl, and butenyl.
[0080] R in formula (a-3) 31 ~R 36Each is independently preferably selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, and an alkenyl group having 2 to 20 carbon atoms; more preferably selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 10 carbon atoms, and an alkenyl group having 2 to 10 carbon atoms; further preferably selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an alkenyl group having 2 to 10 carbon atoms; particularly preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, phenyl, naphthyl, vinyl, allyl, propenyl, isopropenyl, and butenyl; most preferably selected from the group consisting of methyl, ethyl, phenyl, and vinyl.
[0081] L in formula (a-3) 31 and L 32 Each independently represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms.
[0082] Examples of the divalent hydrocarbon group having 1 to 20 carbon atoms include an alkylene group having 1 to 20 carbon atoms, a cycloalkylene group having 3 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms.
[0083] The alkylene group having 1 to 20 carbon atoms is preferably an alkylene group having 1 to 10 carbon atoms, and examples thereof include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group.
[0084] The cycloalkylene group having 3 to 20 carbon atoms is preferably a cycloalkylene group having 3 to 10 carbon atoms, and examples thereof include cyclobutylene, cyclopentylene, cyclohexylene, and cycloheptylene.
[0085] The arylene group having 6 to 20 carbon atoms is preferably an arylene group having 6 to 10 carbon atoms, and examples thereof include a phenylene group and a naphthylene group.
[0086] L 31 and L 32 Each is independently preferably selected from the group consisting of a single bond, an alkylene group having 1 to 20 carbon atoms, a cycloalkylene group having 3 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms; more preferably selected from the group consisting of a single bond, an alkylene group having 1 to 10 carbon atoms, a cycloalkylene group having 3 to 10 carbon atoms, and an arylene group having 6 to 10 carbon atoms; further preferably selected from the group consisting of a single bond, an alkylene group having 1 to 10 carbon atoms, and an arylene group having 6 to 10 carbon atoms; particularly preferably selected from the group consisting of a single bond, a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a phenylene group, and a naphthyl group; most preferably selected from the group consisting of a single bond, a methylene group, an ethylene group, a propylene group, and a phenylene group.
[0087] Z in formula (a-3) 31 and Z 32Each is independently a trivalent hydrocarbon group having 1 to 20 carbon atoms.
[0088] Z in formula (a-3) 31 and Z 32 Each is preferably independently selected from the group consisting of a group represented by the following formula (a-3-i), a group represented by the following formula (a-3-ii), a group represented by the following formula (a-3-iii), and a group represented by the following formula (a-3-iv).
[0089]
[0090] The group represented by formula (a-3-i) is a succinic acid residue, the group represented by formula (a-3-ii) is a phthalic acid residue, the group represented by formula (a-3-iii) is a 2,3-norbornene dicarboxylic acid residue, and the group represented by formula (a-3-iv) is a 5-norbornene-2,3-dicarboxylic acid residue. It should be noted that in formulas (a-3-i) to (a-3-iv), "*" represents a bonding position.
[0091] n3 in formula (a-3) is 1 to 200. n3 is preferably 3 to 150, more preferably 5 to 120.
[0092] Examples of commercially available products of silicone modified with anhydrides at both ends include "X22-168AS", "X22-168A", "X22-168B", and "X22-168-P5-8" manufactured by Shin-Etsu Chemical Co., Ltd. and "DMS-Z21" manufactured by Gelest Corporation.
[0093] When the structural unit A contains the structural unit (A-3), the ratio of the structural unit (A-3) in the structural unit A is preferably 1 to 50 mol%, more preferably 2 to 40 mol%, and further preferably 3 to 30 mol%.
[0094] By further including the structural unit (A-3), the structural unit A can improve the colorless transparency while maintaining the residual stress of the film at a low level.
[0095] Structural units other than structural units (A-1) and (A-2) arbitrarily included in structural unit A are not limited to structural unit (A-3). There are no particular limitations on the tetracarboxylic dianhydride that provides such an arbitrary structural unit, and examples thereof include aromatic tetracarboxylic dianhydrides such as pyromellitic dianhydride, 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 4,4'-(hexafluoroisopropylidene)phthalic anhydride; alicyclic tetracarboxylic dianhydrides such as 1,2,3,4-cyclobutanetetracarboxylic dianhydride (excluding compounds represented by formula (a-1) or (a-2)); and aliphatic tetracarboxylic dianhydrides such as 1,2,3,4-butanetetracarboxylic dianhydride.
[0096] It should be noted that, in the present specification, aromatic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing one or more aromatic rings, alicyclic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing one or more alicyclic rings and no aromatic ring, and aliphatic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing neither an aromatic ring nor an alicyclic ring.
[0097] The structural units other than the structural units (A-1) and (A-2) optionally contained in the structural unit A may be one type or two or more types.
[0098] (Structural unit B)
[0099] Structural unit B is a structural unit derived from diamine that occupies the polyimide resin, and includes a structural unit (B-1) derived from a diamine having a sulfonyl group in the structure and a structural unit (B-2) derived from a compound represented by the following formula (b-2).
[0100]
[0101] (In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii), p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4. When p is 0, m1 is an integer of 1 to 4.)
[0102]
[0103] (In formula (b-2-i), m3 is an integer of 0 to 5; in formula (b-2-ii), m4 is an integer of 0 to 5. It should be noted that when m1+m2+m3+m4 is 1 or more and p is 2, 2 Xs and 2 m2 to m4 are independently selected.)
[0104] In addition, in formula (b-2-i) and (b-2-ii), "*" represents a bonding position.
[0105] The structural unit (B-1) derived from a diamine having a sulfonyl group in the structure is preferably at least one selected from the group consisting of a structural unit (B-11) derived from a compound represented by the following formula (b-11), a structural unit (B-12) derived from a compound represented by the following formula (b-12), and a structural unit (B-13) derived from a compound represented by the following formula (b-13).
[0106]
[0107] The compound represented by formula (b-11) is bis(3-aminophenyl)sulfone (3,3'-DDS), the compound represented by formula (b-12) is bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), and the compound represented by formula (b-13) is bis[4-(3-aminophenoxy)phenyl]sulfone (BAPS-M).
[0108] The polyimide resin used in the composition of the present invention contains a structural unit derived from at least one diamine selected from the group consisting of compounds represented by formula (b-11), formula (b-12) and formula (b-13), so that the colorless transparency and optical isotropy of the obtained polyimide film are improved.
[0109] When the structural unit (B-1) contains the structural unit (B-12), it is preferably used in combination with the structural unit (B-13) from the viewpoint of optical isotropy. That is, from the viewpoint of optical isotropy, the structural unit (B-1) preferably contains the structural unit (B-12) and the structural unit (B-13).
[0110] It is believed that the use of a diamine having a sulfonyl group affects the bendability of the polymer molecular chain and affects the peelability of the polyimide film. It is further believed that the sulfonyl group in the diamine hinders the movement of charges within the molecule and hinders the conjugation of electrons, thereby improving the colorless transparency and optical isotropy of the polyimide film.
[0111] Specific examples of the compound represented by formula (b-2) include compounds represented by any of the following formulae (b-21) to (b-27).
[0112]
[0113] Specific examples of the compound represented by the formula (b-21) include a compound represented by the following formula (b-211), that is, 3,5-diaminobenzoic acid.
[0114]
[0115] The structural unit (B-2) is preferably a structural unit (B-21) derived from a compound represented by the formula (b-21), and more preferably a structural unit (B-211) derived from a compound represented by the formula (b-211).
[0116] When the structural unit B contains the structural unit (B-2), the heat resistance and chemical resistance of the film are improved.
[0117] The ratio of the structural unit (B-1) in the structural unit B is preferably 15 to 95 mol %, more preferably 20 to 95 mol %, further preferably 50 to 90 mol %, further preferably 70 to 85 mol % from the viewpoint of heat resistance.
[0118] The ratio of the structural unit (B-2) in the structural unit B is preferably 5 to 85 mol%, more preferably 5 to 80 mol%, further preferably 10 to 50 mol%, and further preferably 15 to 30 mol%.
[0119] The molar ratio of the structural unit (B-1) to the structural unit (B-2) in the structural unit B [(B-1) / (B-2)] is preferably 15 / 85 to 95 / 5, and from the viewpoint of reducing residual stress and improving elongation, it is more preferably 15 / 85 to 70 / 30, further preferably 15 / 85 to 50 / 50, and further preferably 15 / 85 to 40 / 60.
[0120] The total ratio of the structural units (B-1) and (B-2) in the structural unit B is preferably 50 mol% or more, more preferably 70 mol% or more, and further preferably 90 mol% or more. The upper limit of the total ratio of the structural units (B-1) and (B-2) is not particularly limited, that is, 100 mol%. The structural unit B may be composed only of the structural unit (B-1) and the structural unit (B-2).
[0121] The structural unit B preferably includes a structural unit (B-3) derived from a compound represented by the following formula (b-3). When the structural unit B includes the structural unit (B-3), the colorless transparency and optical isotropy of the film are improved, and the residual stress is reduced.
[0122]
[0123] In formula (b-3), Z 1 and Z 2 Each independently represents: a divalent aliphatic group or a divalent aromatic group which may contain an oxygen atom, R 1 and R 2 Each independently represents a monovalent aromatic group or a monovalent aliphatic group, R 3 and R 4 Each independently represents a monovalent aliphatic group, R 5 and R 6 Each independently represents a monovalent aliphatic group or a monovalent aromatic group, m and n each independently represent an integer greater than 1, and the sum of m and n represents an integer of 2 to 1000. 1 and R 2 At least one of them represents a monovalent aromatic group.
[0124] In addition, in formula (b-3), two or more different repeating units described in parallel by [] may be repeated in any form and order, such as random, alternating or block.
[0125] In formula (b-3), Z 1 and Z 2 The divalent aliphatic group or divalent aromatic group in the formula (a) may be substituted with a fluorine atom. Examples of the divalent aliphatic group include a divalent saturated or unsaturated aliphatic group having 1 to 20 carbon atoms and an aliphatic group containing an oxygen atom. The divalent aliphatic group preferably has 3 to 20 carbon atoms.
[0126] Examples of the divalent saturated aliphatic group include alkylene groups having 1 to 20 carbon atoms, such as methylene, ethylene, propylene, trimethylene, tetramethylene, hexamethylene, octamethylene, decamethylene, and dodecamethylene.
[0127] Examples of the divalent unsaturated aliphatic group include an alkylene group having 2 to 20 carbon atoms, such as a vinylene group, a propenylene group, and an alkylene group having an unsaturated double bond at a terminal.
[0128] Examples of the aliphatic group containing an oxygen atom include an alkyleneoxy group and an aliphatic group having an ether bond.
[0129] Examples of the divalent aromatic group include an arylene group having 6 to 20 carbon atoms and an aralkylene group having 7 to 20 carbon atoms. 1 and Z 2 Specific examples of the arylene group having 6 to 20 carbon atoms include o-phenylene, m-phenylene, p-phenylene, 4,4′-biphenylene, and 2,6-naphthylene.
[0130] As Z in formula (b-3) 1 and Z 2 , particularly preferably trimethylene and p-phenylene, more preferably trimethylene.
[0131] In formula (b-3), R 1 ~R 6 The monovalent aliphatic group in the formula (a) may be a monovalent saturated or unsaturated aliphatic group. As the monovalent saturated aliphatic group, an alkyl group having 1 to 22 carbon atoms may be mentioned, such as methyl, ethyl, propyl, etc. As the monovalent unsaturated aliphatic group, an alkenyl group having 2 to 22 carbon atoms may be mentioned, such as vinyl, propenyl, etc. These groups may be substituted with fluorine atoms.
[0132] As R of formula (b-3) 1 , R 2 , R 5 and R 6Examples of the monovalent aromatic group in include an aryl group having 6 to 20 carbon atoms, an aryl group having 7 to 30 carbon atoms and substituted with an alkyl group, and an aralkyl group having 7 to 30 carbon atoms. The monovalent aromatic group is preferably an aryl group, and more preferably a phenyl group.
[0133] R in formula (b-3) 1 and R 2 At least one of them represents a monovalent aromatic group, preferably R 1 and R 2 are all monovalent aromatic groups, and R 1 and R 2 All are phenyl.
[0134] As R in formula (b-3) 3 and R 4 , preferably an alkyl group having 1 to 6 carbon atoms, more preferably a methyl group.
[0135] As R in formula (b-3) 5 and R 6 , preferably a monovalent aliphatic group, more preferably a methyl group.
[0136] As described above, among the compounds represented by formula (b-3), the compounds represented by the following formula (b-31) are preferred.
[0137]
[0138] (In formula (b-31), m and n have the same meanings as m and n in formula (b-3), and the preferred ranges are also the same.)
[0139] In formula (b-3), m represents the number of repetitions of siloxane units to which at least one monovalent aromatic group is bonded, and n represents the number of repetitions of siloxane units to which a monovalent aliphatic group is bonded.
[0140] In formula (b-3), m and n each independently represent an integer greater than 1, and the sum of m and n (m+n) represents an integer of 2 to 1000. The sum of m and n preferably represents an integer of 3 to 500, more preferably represents an integer of 3 to 100, and even more preferably represents an integer of 3 to 50.
[0141] The ratio of m / n in formula (b-3) is preferably 5 / 95 to 50 / 50, more preferably 10 / 90 to 40 / 60, further preferably 20 / 80 to 30 / 70.
[0142] The functional group equivalent (amine equivalent) of the compound represented by formula (b-3) is preferably 150 to 5000 g / mol, more preferably 400 to 4000 g / mol, and further preferably 500 to 3000 g / mol.
[0143] In addition, the functional group equivalent means the mass of the compound represented by formula (b-3) per 1 mol of the functional group (amino group).
[0144] Among the compounds represented by formula (b-3), commercially available products include "X-22-9409", "X-22-1660B", "X-22-161AS", "X-22-161A", and "X-22-161B" manufactured by Shin-Etsu Chemical Co., Ltd.
[0145] The ratio of the structural unit (B-3) in the structural unit B is preferably 1 to 25 mol%, more preferably 2 to 20 mol%, further preferably 3 to 15 mol%, further preferably 5 to 15 mol%, further preferably 7 to 15 mol%.
[0146] The structural unit B preferably includes a structural unit (B-4) derived from a compound represented by the following formula (b-4).
[0147] By including the structural unit (B-4) in the structural unit B, the colorless transparency of the film is improved.
[0148]
[0149] The ratio of the structural unit (B-4) in the structural unit B is preferably 1 to 50 mol%, more preferably 5 to 45 mol%, further preferably 5 to 40 mol%, further preferably 10 to 40 mol%, further preferably 10 to 30 mol%.
[0150] The structural unit B may contain structural units other than the structural units (B-1) to (B-4). The diamines providing such structural units are not particularly limited, and examples thereof include 1,4-phenylenediamine, p-phenylenediamine, 1,5-diaminonaphthalene, 2,2'-dimethylbiphenyl-4,4'-diamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminobenzanilide, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine, α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, N,N'-bis(4-aminophenyl)-1,4-diisopropylbenzene, and N,N'-bis(4-aminophenyl)-1,4-diisopropylbenzene. ) terephthalamide, 4,4'-bis(4-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane, and 9,9-bis(4-aminophenyl)fluorene (excluding compounds represented by any of formulas (b-1) to (b-4)); alicyclic diamines such as 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane; and aliphatic diamines such as ethylenediamine and hexamethylenediamine (excluding compounds represented by formula (b-1) and compounds represented by formula (b-3)).
[0151] In this specification, aromatic diamine refers to a diamine containing one or more aromatic rings, alicyclic diamine refers to a diamine containing one or more alicyclic rings and no aromatic ring, and aliphatic diamine refers to a diamine containing neither an aromatic ring nor an alicyclic ring.
[0152] The structural unit other than the structural units (B-1) to (B-4) optionally contained in the structural unit B may be one kind or two or more kinds.
[0153] From the viewpoint of mechanical strength of the obtained polyimide film, the number average molecular weight of the polyimide resin is preferably 5000 to 100000. The number average molecular weight of the polyimide resin can be determined, for example, from a standard polymethyl methacrylate (PMMA) conversion value measured by gel permeation chromatography.
[0154] The polyimide resin may contain structures other than the polyimide chain (structure formed by imide bonding of the structural unit A and the structural unit B). Examples of structures other than the polyimide chain that may be contained in the polyimide resin include structures containing amide bonds.
[0155] The polyimide resin preferably contains a polyimide chain (a structure formed by imide bonding of structural unit A and structural unit B) as a main structure. Therefore, the ratio of the polyimide chain in the polyimide resin is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 90% by mass or more, and particularly preferably 99% by mass or more.
[0156] The polyimide resin composition of the present invention including the above-mentioned polyimide resin can form a film having colorless transparency, excellent optical isotropy and excellent releasability, and the preferred physical property values of the film are as follows.
[0157] When the film is made into a film with a thickness of 10 μm, the total light transmittance is preferably 88% or more, more preferably 89% or more, and further preferably 90% or more.
[0158] When used as a film having a thickness of 10 μm, the yellowness index (YI) is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.0 or less.
[0159] The residual stress is preferably 25.0 MPa or less, more preferably 24.0 MPa or less, and further preferably 22.0 MPa or less.
[0160] When a film having a thickness of 10 μm is formed, the absolute value of the thickness retardation (Rth) is preferably 100 nm or less, more preferably 60 nm or less, and further preferably 35 nm or less. Within this range, the optical isotropy is excellent.
[0161] Furthermore, the film that can be formed using the polyimide resin described above is also excellent in heat resistance and mechanical properties, and has the following suitable physical property values.
[0162] The glass transition temperature (Tg) is preferably 250°C or higher, more preferably 270°C or higher, and further preferably 280°C or higher.
[0163] The tensile modulus is preferably 2.0 GPa or more, more preferably 2.5 GPa or more, and further preferably 2.6 GPa or more.
[0164] The tensile elongation is preferably 5% or more, more preferably 6% or more, further preferably 7% or more, and further preferably 10% or more.
[0165] When the tensile modulus and the tensile elongation are within the above ranges, the releasability of the film from the substrate during processing becomes good.
[0166] It should be noted that the above-mentioned physical property values in the present invention can be specifically measured by the methods described in the Examples.
[0167] <Method for producing polyimide resin>
[0168] In the present invention, the polyimide resin can be produced by reacting a tetracarboxylic acid component containing a compound providing the structural unit A and a diamine component containing a compound providing the structural unit (B-1) and a compound providing the structural unit (B-2).
[0169] As the compound providing the structural unit A, the compound represented by formula (a-1), the compound represented by formula (a-2), etc. can be cited, but it is not limited thereto, and the derivatives thereof can be provided within the scope of providing the same structural unit. As the derivative, tetracarboxylic acids corresponding to the tetracarboxylic dianhydrides represented by formula (a-1) and formula (a-2) (i.e., norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid) and alkyl esters of the tetracarboxylic acids can be cited. Among them, the tetracarboxylic dianhydrides represented by formula (a-1) and formula (a-2) are preferred.
[0170] The tetracarboxylic acid component preferably contains 40 mol% or more, more preferably 50 mol% or more, and further preferably 60 mol% or more of the compound providing the structural unit (A-1). The upper limit of the content of the compound providing the structural unit (A-1) is not particularly limited, that is, 100 mol%. The tetracarboxylic acid component may be composed only of the compound providing the structural unit (A-1).
[0171] The tetracarboxylic acid component preferably contains 50 mol% or more, more preferably contains 70 mol% or more, and further preferably contains 85 mol% or more of the compound providing the structural unit (A-2). The upper limit of the content of the compound providing the structural unit (A-2) is not particularly limited, that is, 100 mol%. The tetracarboxylic acid component can be composed only of the compound providing the structural unit (A-2).
[0172] When the tetracarboxylic acid component includes a compound providing a structural unit (A-1) and a compound providing a structural unit (A-2), the tetracarboxylic acid component preferably includes 50 mol% or more, more preferably 70 mol% or more, further preferably 90 mol% or more, and particularly preferably 99 mol% or more of the compound providing a structural unit (A-1) and the compound providing a structural unit (A-2). The upper limit of the compound providing a structural unit (A-1) and the compound providing a structural unit (A-2) is not particularly limited, that is, 100 mol%. The tetracarboxylic acid component may be composed only of a compound providing a structural unit (A-1) and a compound providing a structural unit (A-2).
[0173] The tetracarboxylic acid component may contain compounds other than the compound providing the structural unit (A-1) and the compound providing the structural unit (A-2).
[0174] The tetracarboxylic acid component may further contain a compound providing a structural unit (A-3) in addition to the compound providing a structural unit (A-1) and the compound providing a structural unit (A-2).
[0175] As the compound providing the structural unit (A-3), an anhydride-modified silicone at both ends (e.g., a compound represented by formula (a-3)) can be cited, but it is not limited thereto and can be a derivative thereof within the scope of providing the same structural unit. As the derivative, a tetracarboxylic acid corresponding to the anhydride-modified silicone at both ends and an alkyl ester of the tetracarboxylic acid can be cited. As the compound providing the structural unit (A-3), an anhydride-modified silicone at both ends (i.e., a dianhydride) is preferred.
[0176] When the tetracarboxylic acid component contains a compound providing structural unit (A-3), the tetracarboxylic acid component preferably contains 1 to 50 mol%, more preferably 2 to 40 mol%, and further preferably 3 to 30 mol% of the compound providing structural unit (A-3).
[0177] The compounds arbitrarily included in the tetracarboxylic acid component except the compound providing the structural unit (A-1) and the compound providing the structural unit (A-2) are not limited to the compound providing the structural unit (A-3). As such arbitrary compounds, the above-mentioned aromatic tetracarboxylic dianhydride, alicyclic tetracarboxylic dianhydride, and aliphatic tetracarboxylic dianhydride, and their derivatives (tetracarboxylic acids, alkyl esters of tetracarboxylic acids, etc.) can be cited.
[0178] The compound other than the compound providing the structural unit (A-1) and the compound providing the structural unit (A-2) which is optionally contained in the tetracarboxylic acid component may be one kind or two or more kinds.
[0179] As the compound providing the structural unit (B-1), the compound shown in formula (b-11), the compound shown in formula (b-12), and the compound shown in formula (b-13) can be cited, but it is not limited thereto, and its derivative can be provided within the scope of providing the same structural unit. As the derivative, the diisocyanate corresponding to the diamine shown in formula (b-11), the diisocyanate corresponding to the diamine shown in formula (b-12), and the diisocyanate corresponding to the diamine shown in formula (b-13) can be cited. Among them, the diamine shown in formula (b-11), formula (b-12) and formula (b-13) are preferred.
[0180] Similarly, as a compound providing structural unit (B-2), a compound shown in formula (b-2) can be cited, but it is not limited thereto, and its derivative can be provided within the scope of providing the same structural unit. As the derivative, a diisocyanate corresponding to the diamine shown in formula (b-2) can be cited. As a compound providing structural unit (B-2), a compound shown in formula (b-2) (i.e., diamine) is preferred.
[0181] The diamine component preferably contains 15 to 95 mol %, more preferably 20 to 95 mol %, further preferably 50 to 90 mol %, and further preferably 70 to 85 mol % of the compound providing the structural unit (B-1).
[0182] The diamine component preferably contains 5 to 85 mol%, more preferably 5 to 80 mol%, further preferably 10 to 50 mol%, and further preferably 15 to 30 mol% of the compound providing the structural unit (B-2).
[0183] The total content of the diamine component is preferably 50 mol% or more, more preferably 70 mol% or more, further preferably 90 mol% or more, and particularly preferably 99 mol% or more of the compound providing the structural unit (B-1) and the compound providing the structural unit (B-2). The upper limit of the total content of the compound providing the structural unit (B-1) and the compound providing the structural unit (B-2) is not particularly limited, that is, 100 mol%. The diamine component may be composed only of the compound providing the structural unit (B-1) and the compound providing the structural unit (B-2).
[0184] The diamine component may contain compounds other than the compound providing the structural unit (B-1) and the compound providing the structural unit (B-2).
[0185] The diamine component may further contain a compound providing a structural unit (B-3) in addition to the compound providing a structural unit (B-1) and the compound providing a structural unit (B-2).
[0186] As the compound providing the structural unit (B-3), the compound shown in formula (b-3) can be cited, but it is not limited thereto, and its derivative can be provided within the scope of providing the same structural unit. As the derivative, a diisocyanate corresponding to the diamine shown in formula (b-3) can be cited. As the compound providing the structural unit (B-3), the compound shown in formula (b-3) (i.e., diamine) is preferred.
[0187] The diamine component preferably contains 1 to 25 mol%, more preferably 2 to 20 mol%, further preferably 3 to 15 mol%, further preferably 5 to 15 mol%, further preferably 7 to 15 mol% of the compound providing the structural unit (B-3).
[0188] The diamine component may further contain a compound providing a structural unit (B-4) in addition to the compound providing a structural unit (B-1) and the compound providing a structural unit (B-2).
[0189] As the compound providing the structural unit (B-4), the compound shown in formula (b-4) can be cited, but it is not limited thereto, and its derivative can be provided within the scope of providing the same structural unit. As the derivative, the diisocyanate corresponding to the diamine shown in formula (b-4) can be cited. As the compound providing the structural unit (B-4), the compound shown in formula (b-4) (i.e., diamine) is preferred.
[0190] The diamine component preferably contains 1 to 50 mol%, more preferably 5 to 45 mol%, further preferably 5 to 40 mol%, further preferably 10 to 40 mol%, further preferably 10 to 30 mol% of the compound providing the structural unit (B-4). In addition, from the viewpoint of reducing the residual stress, it is preferably 1 to 50 mol%, more preferably 10 to 50 mol%, further preferably 20 to 40 mol%.
[0191] The compounds arbitrarily contained in the diamine component other than the compound providing the structural unit (B-1) and the compound providing the structural unit (B-2) are not limited to the compound providing the structural unit (B-3) and the compound providing the structural unit (B-4). Such arbitrary compounds include the above-mentioned aromatic diamines, alicyclic diamines, and aliphatic diamines, and their derivatives (diisocyanates, etc.).
[0192] The compound other than the compound providing the structural unit (B-1) and the compound providing the structural unit (B-2) which is optionally contained in the diamine component may be one kind or two or more kinds.
[0193] In the present invention, the charging amount ratio of the tetracarboxylic acid component and the diamine component used for producing the polyimide resin is preferably 0.9 to 1.1 mol of the diamine component relative to 1 mol of the tetracarboxylic acid component.
[0194] In addition, in the present invention, when manufacturing the polyimide resin, in addition to the aforementioned tetracarboxylic acid component and diamine component, an end-capping agent can also be used. As the end-capping agent, monoamines or dicarboxylic acids are preferred. The amount of the introduced end-capping agent is preferably 0.0001 to 0.1 moles, particularly preferably 0.001 to 0.06 moles, relative to 1 mole of the tetracarboxylic acid component. As monoamine end-capping agents, for example, methylamine, ethylamine, propylamine, butylamine, benzylamine, 4-methylbenzylamine, 4-ethylbenzylamine, 4-dodecylbenzylamine, 3-methylbenzylamine, 3-ethylbenzylamine, aniline, 3-methylaniline, 4-methylaniline, etc. are recommended. Among these, benzylamine and aniline can be suitably used. As dicarboxylic acid end-capping agents, dicarboxylic acids are preferred, and a part of them can be ring-closed. For example, phthalic acid, phthalic anhydride, 4-chlorophthalic acid, tetrafluorophthalic acid, 2,3-benzophenone dicarboxylic acid, 3,4-benzophenone dicarboxylic acid, cyclohexane-1,2-dicarboxylic acid, cyclopentane-1,2-dicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, etc. are recommended. Among these, phthalic acid and phthalic anhydride can be preferably used.
[0195] There is no restriction|limiting in particular about the method for making the said tetracarboxylic acid component and a diamine component react, A well-known method can be used.
[0196] As specific reaction methods, the following methods can be cited: method (1), adding a tetracarboxylic acid component, a diamine component, and a reaction solvent to a reactor, stirring at room temperature to 80°C for 0.5 to 30 hours, and then heating to carry out an imidization reaction; method (2), adding a diamine component and a reaction solvent to a reactor to dissolve them, adding a tetracarboxylic acid component, stirring at room temperature to 80°C for 0.5 to 30 hours as needed, and then heating to carry out an imidization reaction; method (3), adding a tetracarboxylic acid component, a diamine component, and a reaction solvent to a reactor, and immediately heating to carry out an imidization reaction; etc.
[0197] The reaction solvent used in the production of the polyimide resin may be any solvent as long as it does not inhibit the imidization reaction and can dissolve the generated polyimide, and examples thereof include aprotic solvents, phenolic solvents, etheric solvents, carbonate solvents, and the like.
[0198] Specific examples of aprotic solvents include amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone (NMP), N-methylcaprolactam, 1,3-dimethylimidazolidinone, and tetramethylurea; lactone solvents such as γ-butyrolactone (GBL) and γ-valerolactone; phosphorus-containing amide solvents such as hexamethylphosphoramide and hexamethylphosphinetriamide; sulfur-containing solvents such as dimethyl sulfone, dimethyl sulfoxide, and cyclopentane; ketone solvents such as acetone, cyclohexanone, and methylcyclohexanone; amine solvents such as picoline and pyridine; and ester solvents such as (2-methoxy-1-methylethyl)acetate.
[0199] Specific examples of the phenolic solvent include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol.
[0200] Specific examples of the ether solvent include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, and 1,4-dioxane.
[0201] Specific examples of the carbonate-based solvent include diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, and propylene carbonate.
[0202] Among the above reaction solvents, amide solvents or lactone solvents are preferred. In addition, the above reaction solvents may be used alone or in combination of two or more.
[0203] In the imidization reaction, it is preferred to use a Dean-Stark water trap apparatus or the like to carry out the reaction while removing water generated during the production. By carrying out such an operation, the degree of polymerization and the imidization ratio can be further increased.
[0204] In the above-mentioned imidization reaction, a known imidization catalyst can be used. Examples of the imidization catalyst include a base catalyst and an acid catalyst.
[0205] Examples of the base catalyst include organic base catalysts such as pyridine, quinoline, isoquinoline, α-methylpyridine, β-methylpyridine, 2,4-lutidine, 2,6-lutidine, trimethylamine, triethylamine (TEA), tripropylamine, tributylamine, triethylenediamine, imidazole, N,N-dimethylaniline, and N,N-diethylaniline; and inorganic base catalysts such as potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium hydrogen carbonate, and sodium hydrogen carbonate.
[0206] Examples of the acid catalyst include crotonic acid, acrylic acid, trans-3-hexenoic acid, cinnamic acid, benzoic acid, methylbenzoic acid, hydroxybenzoic acid, terephthalic acid, benzenesulfonic acid, p-toluenesulfonic acid, and naphthalenesulfonic acid. The imidization catalysts described above may be used alone or in combination of two or more.
[0207] Among the above, from the viewpoint of operability, it is preferred to use a base catalyst, more preferably to use an organic base catalyst, further preferably to use triethylamine, and particularly preferably to use a combination of triethylamine and triethylenediamine.
[0208] From the viewpoint of reaction rate and suppression of gelation, the temperature of the imidization reaction is preferably 120 to 250° C., more preferably 160 to 200° C. The reaction time is preferably 0.5 to 10 hours from the start of distillation of generated water.
[0209] <Cross-linking agent>
[0210] In the present invention, the crosslinking agent has at least two oxazolyl groups. That is, the crosslinking agent in the present invention is a polyfunctional oxazoline compound having two or more oxazolyl groups (oxazoline rings) in the molecule.
[0211] Oxazolyl group is reactive with carboxyl group, and when carboxyl group and oxazolyl group react, an amide ester bond is formed as shown below. This reaction is particularly easy to proceed when heated to 80°C or higher.
[0212]
[0213] The polyimide resin contained in the polyimide resin composition of the present invention has a carboxyl group, so when the polyimide resin composition of the present invention is heated, the polyimide resins are cross-linked with each other by the cross-linking agent to form a cross-linked polyimide resin. For this reason, the chemical resistance of the film is improved.
[0214] The cross-linking agent is not particularly limited as long as it is a polyfunctional oxazoline compound having two or more oxazolyl groups in the molecule. Specific examples thereof include 1,3-bis(4,5-dihydro-2-oxazolyl)benzene, 1,4-bis(4,5-dihydro-2-oxazolyl)benzene, 2,2'-bis(2-oxazoline), "K-2010E", "K-2020E", "K-2030E" manufactured by Nippon Shokubai Co., Ltd., 2,6-bis(4-isopropyl-2-oxazolin-2-yl)pyridine, 2,6-bis(4-phenyl-2-oxazolin-2-yl)pyridine, 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), and 2,2'-isopropylidenebis(4-tert-butyl-2-oxazoline).
[0215] The cross-linking agent is preferably a compound containing an aromatic ring or aromatic heterocyclic ring to which at least two oxazolyl groups are bonded, more preferably a compound containing a benzene ring or pyridine ring to which at least two oxazolyl groups are bonded, further preferably a compound containing a benzene ring to which at least two oxazolyl groups are bonded, and particularly preferably 1,3-bis(4,5-dihydro-2-oxazolyl)benzene.
[0216] The cross-linking agent may be used alone or in combination of two or more.
[0217] The polyimide resin composition of the present invention preferably contains a polyimide resin and a crosslinking agent in such a manner that the molar ratio of the oxazole group in the crosslinking agent to the carboxyl group in the polyimide resin (oxazole group / carboxyl group) is in the range of 1 / 8 to 1 / 0.5. The molar ratio is more preferably 1 / 6 to 1 / 1, and further preferably 1 / 4 to 1 / 2.
[0218] It should be noted that the above-mentioned molar ratio refers to the molar ratio of the oxazole group contained in the cross-linking agent to the carboxyl group contained in the compound providing the structural unit (B-2) used in the production of the polyimide resin, which is calculated based on the added amount of the cross-linking agent and the added amount of the compound providing the structural unit (B-2).
[0219] [Polyimide varnish]
[0220] A preferred embodiment of the polyimide resin composition of the present invention includes a polyimide resin composition (hereinafter also referred to as “polyimide varnish”) containing an organic solvent in addition to the polyimide resin and the crosslinking agent, and in which the polyimide resin is dissolved.
[0221] The organic solvent is not particularly limited as long as it can dissolve the polyimide resin, and it is preferred to use the above-mentioned compounds as reaction solvents used in the production of the polyimide resin alone or in combination of two or more.
[0222] The polyimide varnish may be one obtained by adding a crosslinking agent to a solution obtained by dissolving a polyimide resin obtained by a polymerization method in a reaction solvent, or one obtained by adding a diluting solvent and a crosslinking agent to the solution.
[0223] The polyimide varnish preferably contains 5 to 40% by mass, more preferably 7 to 30% by mass, and further preferably 8 to 20% by mass of a polyimide resin. The viscosity of the polyimide varnish is preferably 50 to 5000 Pa·s, more preferably 100 to 4000 Pa·s, and further preferably 300 to 3500 Pa·s. The viscosity of the polyimide varnish is a value measured at 25° C. using an E-type viscometer.
[0224] In addition, the polyimide varnish of the present invention may contain various additives such as inorganic fillers, adhesion promoters, release agents, flame retardants, ultraviolet stabilizers, surfactants, leveling agents, defoaming agents, fluorescent brighteners, crosslinking agents, polymerization initiators, and photosensitizers within the range that the required properties of the polyimide film are not impaired.
[0225] The method for producing the polyimide varnish of the present invention is not particularly limited, and a known method can be applied.
[0226] [Polyimide film]
[0227] The polyimide film of the present invention is formed by crosslinking the polyimide resin contained in the polyimide resin composition of the present invention with the crosslinking agent. That is, the polyimide film of the present invention comprises: a crosslinked product of polyimide resins mutually crosslinked by a crosslinking agent, i.e., a crosslinked polyimide resin. Therefore, the polyimide film of the present invention has excellent heat resistance, colorless transparency and chemical resistance, and further has low residual stress. The suitable physical property values of the polyimide film of the present invention are as described above.
[0228] In the method for producing the polyimide film of the present invention, there is no particular restriction as long as the process of cross-linking is performed at a temperature (preferably above 80°C, more preferably above 100°C, and further preferably above 150°C) at which the cross-linking reaction between the polyimide resin and the cross-linking agent is performed. For example, the following method can be cited: the polyimide varnish is coated on a smooth support such as a glass plate, a metal plate, a plastic, or formed into a film, and then heated. By this heat treatment, the cross-linking reaction between the polyimide resin and the cross-linking agent in the polyimide varnish can be performed while removing organic solvents such as reaction solvents and dilution solvents contained in the polyimide varnish. A release agent can be pre-coated on the surface of the aforementioned support as needed.
[0229] As a heat treatment, the following method is preferred. That is, it is preferred that, first, the organic solvent is evaporated at a temperature below 120°C, and then dried at a temperature above the boiling point of the organic solvent to manufacture a polyimide film. In addition, it is preferred to dry under a nitrogen atmosphere. The pressure of the drying atmosphere can be reduced pressure, normal pressure, or pressurized. Drying is performed at two stages of temperature, so that a film with a smooth and defect-free film surface can be obtained. In addition, the drying temperature of the second stage is not particularly limited, preferably 200-450°C, more preferably 300-430°C, and particularly preferably 350-400°C. By drying within this temperature range, the transparency / yellowness of the film becomes good, and good solvent resistance is obtained.
[0230] The polyimide film of the present invention can also be produced using a polyamic acid varnish in which a polyamic acid and a cross-linking agent are dissolved in an organic solvent.
[0231] The polyamic acid contained in the polyamic acid varnish is a precursor of the polyimide resin in the present invention, and is a product of a polyaddition reaction of a tetracarboxylic acid component containing a compound providing the structural unit A, and a diamine component containing a compound providing the structural unit (B-1) and a compound providing the structural unit (B-2). The polyamic acid is imidized (dehydrated and ring-closed) to obtain a polyimide resin.
[0232] As the organic solvent contained in the polyamic acid varnish, the organic solvent contained in the polyimide varnish of the present invention can be used.
[0233] In the present invention, the polyamic acid varnish may be a polyamic acid solution itself obtained by subjecting a tetracarboxylic acid component containing a compound providing the structural unit A and a diamine component containing a compound providing the structural unit (B-1) and a compound providing the structural unit (B-2) in a reaction solvent for addition polymerization, or may be a polyamic acid solution obtained by further adding a diluting solvent.
[0234] In the method for making polyimide film using polyamic acid varnish, as long as the process of crosslinking is carried out at a temperature (preferably above 80°C, more preferably above 100°C, and further preferably above 150°C) included in the crosslinking reaction of polyimide resin and crosslinking agent, there is no particular restriction, and known methods can be adopted. For example, polyamic acid varnish is applied on a smooth support such as a glass plate, a metal plate, a silicon wafer, plastics, or is formed into a film shape, and the organic solvents such as the reaction solvent and the diluting solvent contained in the varnish are removed by heating to obtain the polyamic acid film, and the polyamic acid in the polyamic acid film is imidized by heating, and then the polyimide resin is reacted with the crosslinking agent and crosslinked, thereby the polyimide film can be manufactured.
[0235] The heating temperature when the polyamic acid varnish is dried to obtain a polyamic acid film is preferably 50 to 120° C. The heating temperature when the polyamic acid is imidized by heating is preferably 200 to 400° C.
[0236] In addition, the imidization method is not limited to thermal imidization, and chemical imidization may also be applied.
[0237] The thickness of the polyimide film of the present invention can be appropriately selected depending on the application, and is preferably in the range of 1 to 250 μm, more preferably 5 to 100 μm, and even more preferably 10 to 80 μm. When the thickness is 1 to 250 μm, it can be practically used as a self-supporting film.
[0238] The thickness of the polyimide film can be easily controlled by adjusting the solid content concentration and viscosity of the polyimide varnish.
[0239] The polyimide film of the present invention is suitable for use as a film for various components such as color filters, flexible displays, semiconductor components, optical components, etc. The polyimide film of the present invention is particularly suitable for use as a substrate for image display devices such as liquid crystal displays and OLED displays.
[0240] Example
[0241] Hereinafter, the present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0242] The solid content concentration of the varnishes obtained in Examples and Comparative Examples and various physical properties of the thin films were measured by the methods shown below.
[0243] (1) Solid content concentration
[0244] The solid content concentration of the varnish was determined by heating a sample at 320° C. for 120 minutes in a small electric furnace “MMF-1” manufactured by AS ONE Corporation and calculating the solid content concentration from the difference in mass of the sample before and after heating.
[0245] (2) Film thickness
[0246] The film thickness was measured using a micrometer manufactured by Mitutoyo Co., Ltd.
[0247] (3) Total light transmittance, yellowness index (YI)
[0248] The total light transmittance and YI were measured in accordance with JIS K7105:1997 using a color / turbidity simultaneous measuring device "COH7700" manufactured by Nippon Denshoku Industries Co., Ltd.
[0249] (4) Haze
[0250] The measurement was performed in accordance with JIS K7361-1 using a color / turbidity simultaneous measuring device "COH400" manufactured by Nippon Denshoku Industries Co., Ltd.
[0251] (5)b *
[0252] b * The color and turbidity were measured in accordance with JIS Z8781:2013 using a color / turbidity simultaneous measuring device "COH7700" manufactured by Nippon Denshoku Industries, Ltd.
[0253] (6) In-plane retardation (Re)
[0254] The in-plane retardation (Re) was measured using an ellipsometer "M-220" manufactured by JASCO Corporation. The in-plane phase difference value at a measurement wavelength of 590 nm was measured.
[0255] (7)Thickness Retardation (Rth)
[0256] The thickness phase difference (Rth) was measured using an ellipsometer "M-220" manufactured by JASCO Corporation. The value of the thickness phase difference at a measurement wavelength of 590 nm was measured. It should be noted that Rth is represented by the following formula when the maximum value of the refractive index in the plane of the polyimide film is set to nx, the minimum value is set to ny, the refractive index in the thickness direction is set to nz, and the thickness of the film is set to d.
[0257] Rth=[{(nx+ny) / 2}-nz]×d
[0258] (8) Peel force
[0259] The peeling force of the interface between the polyimide film and the glass was measured using a tensile testing machine "STROGRAPH EII-L05" manufactured by Toyo Seiki Co., Ltd. The test piece used was a polyimide film formed on a glass plate of size 10 mm × 100 mm. The test piece with one end of the film peeled off in advance was placed horizontally on the device, and the end of the film was clamped with a chuck. The stress when the peeled film and the glass were stretched at an angle of approximately 90° was used as the peeling force. It should be noted that the tensile test speed was set to 50 mm / minute.
[0260] (9) Glass transition temperature (Tg)
[0261] Using a thermomechanical analyzer "TMA / SS6100" manufactured by Hitachi High-Tech Science Corporation, the temperature was raised to a sufficient temperature to remove the residual stress under the conditions of a sample size of 2 mm×20 mm, a load of 0.1 N, and a heating rate of 10°C / min in the tensile mode, and then cooled to room temperature after the residual stress was removed. Thereafter, the elongation of the test piece was measured under the same conditions as the treatment for removing the residual stress, and the inflection point of the elongation was determined as the glass transition temperature.
[0262] (10) 1% weight loss temperature (Td 1%)
[0263] The 1% weight loss temperature is as follows: About 10 mg of a sample is used as an object, and a thermogravimetric analyzer ("TG / DTA6200" manufactured by Seiko Instruments Inc.) is used.
[0264] The temperature at which the sample weight decreases by 1% by weight relative to 100% by weight of the sample at 100°C is measured when the temperature is increased from room temperature to 450°C at a heating rate of 10°C / min.
[0265] The temperature was increased under the conditions of an air atmosphere with an air gas flow rate of 50 mL / min and under the conditions of a nitrogen atmosphere with a nitrogen gas flow rate of 100 mL / min.
[0266] (11) Residual stress
[0267] Using the residual stress measuring device "FLX-2320" manufactured by KLA Tencor, a polyimide varnish or polyamic acid varnish was applied to a 4-inch silicon wafer with a thickness of 525μm±25μm and pre-baked using a spin coater. After that, a heat curing treatment was performed at 350-400°C for 30 minutes in a nitrogen atmosphere using a hot air dryer to produce a silicon wafer with a polyimide film having a thickness of 8-15μm after curing. The warpage of the wafer was measured using the aforementioned residual stress measuring device to evaluate the residual stress generated between the silicon wafer and the polyimide film.
[0268] (12) Chemical resistance 1 (PGMEA)
[0269] A solvent was added dropwise to the polyimide film formed on the glass plate at room temperature to confirm whether the film surface changed. Propylene glycol monomethyl ether acetate (PGMEA) was used as the solvent.
[0270] The evaluation criteria of solvent resistance were as follows.
[0271] ○: No change on the film surface.
[0272] △: Cracks slightly occurred on the film surface.
[0273] ×: Cracks occurred on the film surface, or the film surface was dissolved.
[0274] (13) Chemical resistance 2 (acid resistance)
[0275] The polyimide film formed on the glass plate was immersed in a mixed acid solution (a mixed solution of H3PO4 (70 mass%) + HNO3 (10 mass%) + CH3COOH (5 mass%) + H2O (15 mass%)) heated to 40°C for 4 minutes, and then washed with water. After washing with water, the water was wiped off and the film was heated on a hot plate at 240°C for 50 minutes and dried. The b was measured before and after the test. * , find its change (Δb * ). The table shows the b after the test. * and Δb * It should be noted that b * The measurement was performed in a state where a polyimide film was formed on a glass plate (state of glass plate + polyimide film).
[0276] (14) Tensile modulus and tensile elongation (tensile breaking strain)
[0277] The tensile modulus and tensile elongation (tensile breaking strain) were measured in accordance with JIS K7161: 2014 and JIS K7127: 1999 using a tensile tester "STROGRAPH VG-1E" manufactured by Toyo Seiki Co., Ltd. The chuck distance was 50 mm, the test piece size was 10 mm×70 mm, and the test speed was 20 mm / min.
[0278] The tetracarboxylic acid component and the diamine component used in the Examples and Comparative Examples, and the abbreviations thereof are as follows.
[0279] <Diamine>
[0280] 3,3'-DDS: 3,3'-bis(aminophenyl)sulfone (manufactured by Seika Co., Ltd.; compound represented by formula (b-11))
[0281] BAPS: bis[4-(4-aminophenoxy)phenyl]sulfone (manufactured by Seika Co., Ltd.; compound represented by formula (b-12))
[0282] BAPS-M: bis[4-(3-aminophenoxy)phenyl]sulfone (manufactured by Seika Co., Ltd.; compound represented by formula (b-13))
[0283] 3,5-DABA: 3,5-diaminobenzoic acid (manufactured by Japan Junryo Pharmaceutical Co., Ltd.; compound represented by formula (b-2))
[0284] X-22-9409: Silicone oil modified with amino groups at both ends "X-22-9409" (manufactured by Shin-Etsu Chemical Co., Ltd.; compound represented by formula (b-3))
[0285] 6FODA: 4,4'-diamino-2,2'-bistrifluoromethyl diphenyl ether (manufactured by ChinaTech Chemical (Tianjin) Co., Ltd.; compound represented by formula (b-4))
[0286] <Tetracarboxylic acid component>
[0287] CpODA: Norbornane-2-spiro-α-cyclopentanone-α′-spiro-2″-norbornane-5,5″,6,6″-tetracarboxylic dianhydride (manufactured by JX Energy Co., Ltd.; compound represented by formula (a-1))
[0288] HPMDA: 1,2,4,5-cyclohexanetetracarboxylic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.; compound represented by formula (a-2))
[0289] <Cross-linking agent>
[0290] 1,3-PBO: 1,3-bis(4,5-dihydro-2-oxazolyl)benzene (manufactured by Mikuni Pharmaceutical Industry Co., Ltd.)
[0291] <Other>
[0292] GBL: γ-butyrolactone (manufactured by Mitsubishi Chemical Corporation)
[0293] TEA: triethylamine (manufactured by Kanto Chemical Co., Ltd.)
[0294] Example 1
[0295] In a 300 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and a glass end cap, 28.793 g (0.066 mol) of BAPS-M, 3.372 g (0.022 mol) of 3,5-DABA, and 125.425 g of GBL were added, and the mixture was stirred at a temperature of 70° C. in the system, at a rotation speed of 200 rpm under a nitrogen atmosphere to obtain a solution.
[0296] To this solution, 35.026 g (0.089 mol) of CpODA and 35.026 g of GBL were added simultaneously, and 0.784 g of TEA was added as an imidization catalyst. The reaction system was heated in a hooded heater to raise the temperature to 200° C. over about 30 minutes. The components removed by distillation were collected, the rotation speed was adjusted according to the increase in viscosity, and the temperature in the reaction system was maintained at 200° C. and refluxed for 4 hours.
[0297] Then, GBL was added to a solid content concentration of 20% by mass, and the temperature in the reaction system was cooled to 100° C., followed by stirring for about 1 hour for homogenization. Then, 0.755 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and stirred for 30 minutes for homogenization to obtain a polyimide varnish.
[0298] The obtained polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating and dried on a hot plate at 120° C. for 15 minutes. Thereafter, the solvent was evaporated by heating in a hot air dryer at 260° C. in the atmosphere for 60 minutes to obtain a 10 μm thick film.
[0299] Example 2
[0300] In a 300 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and a glass end cap, 15.007 g (0.045 mol) of 6FODA, 5.564 g (0.022 mol) of 3,3'-DDS, 6.791 g (0.045 mol) of 3,5-DABA, 13.670 g (0.011 mol) of X-22-9409, and 127.679 g of GBL were added, and the mixture was stirred at a temperature of 70° C. in the system, at a rotation speed of 200 rpm under a nitrogen atmosphere to obtain a solution.
[0301] To this solution, 27.368 g (0.122 mol) of HPMDA and 31.920 g of GBL were added simultaneously, and 0.730 g of TEA was added as an imidization catalyst. The reaction system was heated in a hooded heater to raise the temperature to 200° C. over about 30 minutes. The components removed by distillation were collected, the rotation speed was adjusted according to the increase in viscosity, and the temperature in the reaction system was maintained at 200° C. and refluxed for 4 hours.
[0302] Then, GBL was added so that the solid content concentration became 20 mass %, and the temperature in the reaction system was cooled to 100° C., and then stirred for about 1 hour for homogenization. Then, 1.492 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and stirred for 30 minutes for homogenization to obtain a polyimide varnish.
[0303] The obtained polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating and dried on a hot plate at 120° C. for 15 minutes. Thereafter, the solvent was evaporated by heating in a hot air dryer at 260° C. in the atmosphere for 60 minutes to obtain a 10 μm thick film.
[0304] Example 3
[0305] In a 300 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and a glass end cap, 13.853 g (0.041 mol) of 6FODA, 8.921 g (0.021 mol) of BAPS-M, 6.269 g (0.041 mol) of 3,5-DABA, 13.610 g (0.011 mol) of X-22-9409, and 127.099 g of GBL were added, and the mixture was stirred at a temperature of 70° C. in the system, at a rotation speed of 200 rpm under a nitrogen atmosphere to obtain a solution.
[0306] To this solution, 25.436 g (0.113 mol) of HPMDA and 31.775 g of GBL were added simultaneously, and 0.678 g of TEA was further added as an imidization catalyst. The reaction system was heated in a hooded heater to raise the temperature to 200° C. over about 30 minutes. The components removed by distillation were collected, the rotation speed was adjusted according to the increase in viscosity, and the temperature in the reaction system was maintained at 200° C. and refluxed for 4 hours.
[0307] Then, GBL was added to a solid content concentration of 20 mass %, and the temperature in the reaction system was cooled to 100° C., followed by stirring for about 1 hour for homogenization. Then, 1.384 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and stirred for 30 minutes for homogenization to obtain a polyimide varnish.
[0308] The obtained polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating and dried on a hot plate at 120° C. for 15 minutes. Thereafter, the solvent was evaporated by heating in a hot air dryer at 260° C. in the atmosphere for 60 minutes to obtain a 10 μm thick film.
[0309] Example 4
[0310] In a 300 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and a glass end cap, BAPS 14.512 g (0.034 mol), 3,3'-DDS 8.363 g (0.034 mol), 3,5-DABA 2.552 g (0.017 mol), X-22-9409 6.616 g (0.005 mol) and GBL 125.448 g were added, and the mixture was stirred at a temperature of 70° C. in the system, at a rotation speed of 200 rpm under a nitrogen atmosphere to obtain a solution.
[0311] To this solution, 35.161 g (0.089 mol) of CpODA and 31.362 g of GBL were added simultaneously, and 0.619 g of TEA was further added as an imidization catalyst. The reaction system was heated in a hooded heater to raise the temperature to 200° C. over about 30 minutes. The components removed by distillation were collected, the rotation speed was adjusted according to the increase in viscosity, and the temperature in the reaction system was maintained at 200° C. and refluxed for 4 hours.
[0312] Then, GBL was added so that the solid content concentration became 20 mass %, and the temperature in the reaction system was cooled to 100° C., and then stirred for about 1 hour for homogenization. Then, 0.571 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and stirred for 30 minutes for homogenization to obtain a polyimide varnish.
[0313] The obtained polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating and dried on a hot plate at 120° C. for 15 minutes. Thereafter, the solvent was evaporated by heating in a hot air dryer at 260° C. in the atmosphere for 60 minutes to obtain a 10 μm thick film.
[0314] Example 5
[0315] In a 300 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and a glass end cap, BAPS 17.235 g (0.040 mol), BAPS-M 17.252 g (0.040 mol), 3,5-DABA 3.031 g (0.020 mol), X-22-9409 6.771 g (0.005 mol) and GBL 126.514 g were added, and the mixture was stirred at a temperature of 70° C. in the system, at a rotation speed of 200 rpm under a nitrogen atmosphere to obtain a solution.
[0316] To this solution, 23.486 g (0.105 mol) of HPMDA and 31.629 g of GBL were added simultaneously, and 0.731 g of TEA was added as an imidization catalyst. The reaction system was heated in a hooded heater to raise the temperature to 200° C. over about 30 minutes. The components removed by distillation were collected, the rotation speed was adjusted according to the increase in viscosity, and the temperature in the reaction system was maintained at 200° C. and refluxed for 4 hours.
[0317] Then, GBL was added so that the solid content concentration became 20 mass %, and the temperature in the reaction system was cooled to 100° C., and then stirred for about 1 hour for homogenization. Then, 0.672 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and stirred for 30 minutes for homogenization to obtain a polyimide varnish.
[0318] The obtained polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating and dried on a hot plate at 120° C. for 15 minutes. Thereafter, the solvent was evaporated by heating in a hot air dryer at 260° C. in the atmosphere for 60 minutes to obtain a 10 μm thick film.
[0319] The obtained film was subjected to the above-mentioned evaluation. The results are shown in Table 1.
[0320] [Table 1]
[0321] Table 1
[0322]
[0323] As shown in Table 1, the polyimide films of Examples 1 to 5 were good in colorless transparency and optical isotropy, and also excellent in peelability from the substrate.
Claims
1. A polyimide resin composition comprising: a polyimide resin, and a cross-linking agent having at least two oxazole groups, The polyimide resin is a polyimide resin having a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from diamine, The structural unit B includes a structural unit (B-1) derived from a diamine having a sulfonyl group in its structure and a structural unit (B-2) derived from a compound represented by the following formula (b-2). The structural unit (B-1) is at least one selected from the group consisting of a structural unit (B-12) derived from a compound represented by the following formula (b-12) and a structural unit (B-13) derived from a compound represented by the following formula (b-13), The ratio of the structural unit (B-1) in the structural unit B is 15 to 95 mol%. In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii), p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4, in, When p is 0, m1 is an integer from 1 to 4. In formula (b-2-i), m3 is an integer from 0 to 5; in formula (b-2-ii), m4 is an integer from 0 to 5; it should be noted that when m1+m2+m3+m4 is greater than 1 and p is 2, 2 Xs and 2 m2 to m4 are selected independently.
2. The polyimide resin composition according to claim 1, in, The structural unit (B-2) is a structural unit (B-21) derived from a compound represented by the following formula (b-21), 3. The polyimide resin composition according to claim 1 or 2, in, The structural unit A comprises at least one selected from the group consisting of a structural unit (A-1) derived from a compound represented by the following formula (a-1) and a structural unit (A-2) derived from a compound represented by the following formula (a-2), 4. The polyimide resin composition according to claim 1 or 2, in, The structural unit B further includes a structural unit (B-3) derived from a compound represented by the following formula (b-3), In formula (b-3), Z 1 and Z 2 Each independently represents a divalent aliphatic group or a divalent aromatic group which may contain an oxygen atom, and R 1 and R 2 Each independently represents a monovalent aromatic group or a monovalent aliphatic group, and R 3 and R 4 Each independently represents a monovalent aliphatic group, R 5 and R 6 Each independently represents a monovalent aliphatic group or a monovalent aromatic group, m and n each independently represent an integer greater than 1, and the sum of m and n represents an integer of 2 to 1000, wherein R 1 and R 2 At least one of them represents a monovalent aromatic group.
5. The polyimide resin composition according to claim 1 or 2, in, The structural unit B further includes a structural unit (B-4) derived from a compound represented by the following formula (b-4), 6. The polyimide resin composition according to claim 1 or 2, in, The cross-linking agent is a compound including an aromatic ring or an aromatic heterocyclic ring to which at least two oxazolyl groups are bonded.
7. The polyimide resin composition according to claim 1 or 2, in, The cross-linking agent is a compound including a benzene ring to which at least two oxazole groups are bonded.
8. The polyimide resin composition according to claim 1 or 2, in, The cross-linking agent is 1,3-bis(4,5-dihydro-2-oxazolyl)benzene. 9 . A polyimide varnish, wherein the polyimide resin composition according to claim 1 is dissolved in an organic solvent. 10 . A polyimide film, wherein the polyimide resin in the polyimide resin composition according to claim 1 is cross-linked by the cross-linking agent.