Manufacturing method of water-decrement polyester superfine fiber synthetic leather
Through the composite spinning technology of modified polyvinyl alcohol and polyester masterbatch, combined with water-based polyurethane treatment, the problems of long production cycle and unfriendly environment of traditional microfiber synthetic leather base fabrics are solved, and efficient and environmentally friendly water-reducing polyester is achieved. The manufacturing of microfiber synthetic leather base fabrics improves product performance and economic benefits.
Patent Information
- Application Number
- CN202411202730.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-19
AI Technical Summary
The production process of traditional microfiber synthetic leather base cloth has a long cycle and is unfriendly to the environment. The use of organic solvents and alkali liquids leads to high wastewater treatment costs and high carbon emissions.
Modified polyvinyl alcohol and polyester masterbatches are melted by twin screw extruders, and non-woven fabrics are made by composite spinning, and the aqueous polyvinyl alcohol slurry is impregnated, ironed, and water-reduced treatment is carried out, using end-base The aqueous polyurethane containing the water-repellent chain segment is impregnated and finally shaped and dried to obtain a water-reduced polyester microfiber synthetic leather base cloth.
It shortens the production process, reduces equipment investment, improves the peeling performance and resilience of fibers, reduces the negative impact on the environment, and improves economic benefits and product quality.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of artificial leather, in particular to a method for manufacturing water-reduced polyester ultrafine fiber synthetic leather. Background Art
[0002] The development of synthetic leather has undergone three major technological updates. The first generation of synthetic leather uses woven fabrics with pure cotton or polyester / cotton yarn as warp and weft yarns as the base fabric after brushing. This synthetic leather has good dimensional stability and strong breathability, but its elasticity is poor, and its flatness, uniformity, and surface style are not ideal. At present, this synthetic leather is still widely used as a medium- and low-end product, but it is not competent as a high-end synthetic leather. The second generation of synthetic leather uses warp knitted fabrics of polyester fiber yarn or blended yarn as the base fabric, and the impregnation resin has developed from polyvinyl chloride (PVC) to polyurethane (PU). Due to the structural performance characteristics of warp knitted fabrics, this synthetic leather is elastic in both the longitudinal and transverse directions, and is suitable for uses such as footwear and clothing that require good stretch performance. However, knitted fabrics and woven fabrics are also woven from yarns, and it is easy to expose thread ends, which affects their simulation effect. The third generation of synthetic leather uses conventional non-woven fabrics as the base fabric, and is finished with polyurethane multi-resin. The fibers are arranged in a three-dimensional structure in the finished product without orientation, and the peel strength and folding resistance of the product are greatly improved. Compared with woven base fabric, its cross section has no wire ends and is isotropic, which has a good simulation effect. However, due to the coarse fibers used in conventional nonwoven fabrics and the low density of the base fabric structure, it cannot fully meet the requirements of high-end synthetic leather. The new generation of synthetic leather is ultrafine fiber high-simulation synthetic leather, which is made of ultrafine fiber as raw material to make needle-punched or spunlace nonwoven base fabric, and is made into high-simulation, high-density, high-performance high-end synthetic leather through special finishing such as fiber reduction, dyeing, grinding, polyurethane lamination, etc. It has the best resilience, softness, and simulation, fully meeting the high-end product needs of the domestic and foreign markets, and reflects the main direction of the development of synthetic leather technology.
[0003] Sea-island fiber is a highly functional fiber composed of "sea phase" and "island phase". It uses composite spinning technology to use two fiber-forming polymers as "sea" and "island" components respectively, and melt-spins them in different ratios. Then, the different solubility of these two components in a certain chemical solvent is used to dissolve the "sea" component and leave the "island" component. The common sea phase component is soluble polyester, and the island phase is ordinary polyester. Under a specific process, the sea component is dissolved and the island component is left, and a cluster of ultrafine fibers is obtained.
[0004] As the main component of microfiber synthetic leather, the performance of microfiber synthetic leather base fabric determines the performance of microfiber synthetic leather. Traditional microfiber synthetic leather base fabric mainly adopts polyamide (also known as nylon) or polyester (also known as polyester) and polyethylene two-component fiber melt spinning to produce sea island fiber, and then made into non-woven fabric, heated and ironed, solvent-based polyurethane impregnation, coagulation, water washing, toluene reduction, drying, oiling and other processes. The whole production process is long and the equipment investment is large. In the spinning process, organic solvents or alkali solutions are used to remove the sea component, the wastewater treatment cost is high, it is not environmentally friendly, and the carbon emission is high. Summary of the invention
[0005] Therefore, in view of the above problems, the present invention provides a method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base cloth, which solves the problems of long production cycle and environmental unfriendliness of the ultrafine fiber synthetic leather base cloth in the prior art.
[0006] To achieve the above object, the present invention adopts the following technical scheme: a method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric, comprising the following preparation steps: (1) Preparation of sea-island fibers: polyester masterbatch is used as the raw material of the island component, and modified polyvinyl alcohol masterbatch is used as the raw material of the sea component. The polyester masterbatch and the modified polyvinyl alcohol are melted through different screws of a twin-screw extruder to obtain polyester melt and modified polyvinyl alcohol melt, respectively. The polyester melt and the modified polyvinyl alcohol melt are respectively sent into a polyester melt pipeline and a modified polyvinyl alcohol melt pipeline for heating, and then extruded after being metered by a metering pump. The island component is evenly distributed into the sea component through a distribution pipeline, and then ejected through the same spinneret hole for composite spinning to obtain sea-island fibers with polyester as the island component and polyvinyl alcohol as the sea component; The melting temperature of the modified polyvinyl alcohol masterbatch is 155-165°C, and the initial thermal decomposition temperature is 260°C; The viscosity difference between polyester melt and modified polyvinyl alcohol melt is less than 10%; (2) using the sea-island fibers obtained in step (1) as raw materials, and producing a non-woven fabric by needle punching; (3) sending the nonwoven fabric into a production line and impregnating it with an aqueous polyvinyl alcohol slurry; (4) Water-based polyurethane that is ironed and impregnated with water-repellent segments; (5) Drying; (6) Water reduction: Soak the dried base fabric in hot water at 85-90°C and stir it continuously; (7) shaping and drying to obtain water-reduced polyester microfiber synthetic leather base fabric.
[0007] Furthermore: the heating temperature of the modified polyvinyl alcohol melt pipeline is 155-165°C.
[0008] Further: the weight ratio of the island component: the sea component = 70-80: 20-30.
[0009] Furthermore: in step (6) water reduction treatment, the bath ratio is 20-30:1 and the treatment time is 30-90s.
[0010] Furthermore: the mass fraction of the aqueous polyvinyl alcohol slurry in step (3) is 9-12%.
[0011] Further: The specific process of step (4) of impregnation with aqueous polyurethane treatment is: immersing the base fabric in a solution of an aqueous polyurethane emulsion containing a terminal water-repellent segment, wherein the solid content of the aqueous polyurethane emulsion is 35-40%, and a penetrant with a mass concentration of 4% is also added to the solution.
[0012] Further: The preparation method of the aqueous polyurethane containing a water-repellent segment at the end group is as follows: (1) polytetrahydrofuran, dihydroxymethylbutyric acid and acetone are mixed and stirred evenly, the temperature is raised to 55-62°C, and isophorone diisocyanate is slowly added and maintained for 2-3 hours; (2) hydroxyethyl acrylate is added and reacted at 60-65°C for 3-4 hours; (3) the temperature is lowered to 38°C, and triethylamine is added and reacted for 0.5-0.6 hours; (4) deionized water is added at 20-25°C and stirred continuously for 1-1.2 hours, the temperature is raised to 40-45°C, and acetone is evaporated at 0.05-0.06MPa.
[0013] Furthermore: the modified polyvinyl alcohol is obtained by modifying polyvinyl alcohol with a vinyl monomer, and the specific modification method is: free radical copolymerizing ethylene and vinyl acetate in a solution, and then alcoholyzing to obtain an ethylene-vinyl alcohol copolymer, wherein the vinyl content is 6-9wt%.
[0014] Furthermore: the modified polyvinyl alcohol is modified by using propylene glycol.
[0015] By adopting the above technical solution, the beneficial effects of the present invention are: 1. In the present invention, the viscosity difference between the polyester melt and the modified polyvinyl alcohol melt is less than 10%, the two melts have similar viscosities and rheological properties, and the diffusion of the low-viscosity melt to the high-viscosity melt and the subsequent pulping are avoided, and the finally obtained sea-island fiber has better stripping performance.
[0016] 2. The present invention first uses aqueous polyvinyl alcohol slurry for impregnation treatment. After water reduction treatment, the polyvinyl alcohol can be extracted, leaving pores between the polyurethane and the fiber, thereby increasing the resilience and softness of the synthetic leather.
[0017] 3. Furthermore, the weight ratio of the island component: the sea component = 70-80: 20-30. Too high an island phase ratio will cause part of the island phase to be too close to the sea phase and cause pulp adhesion, resulting in unclear interface between the sea phase and the island phase, affecting the fiber fibrillation and the quality of the ultrafine fiber. The present invention selects a suitable weight ratio of the island component: the sea component, and the sea island fiber has good fiber opening performance and high economic benefits.
[0018] 4. Further: The specific process of step (4) of impregnating with water-based polyurethane is as follows: the base fabric is impregnated with a solution of water-based polyurethane emulsion containing water-repellent segments at the end groups, the solid content of the water-based polyurethane emulsion is 35-40%, and a penetrant with a mass concentration of 4% is also added to the solution. The addition of the penetrant increases the affinity between the water-based polyurethane and the polyester fiber, which is beneficial to the penetration of the water-based polyurethane in the polyester non-woven fabric. After the addition of the penetrant, the amount of water-based polyurethane coated on the ultrafine fiber increases, and the gap between the fibers in the fabric decreases.
[0019] 5. Furthermore, the water-based polyurethane used has a structure with a water-repellent segment at the end group, which can prevent the polyurethane from swelling during the water reduction process of the non-woven fabric, thereby ensuring the smooth fiber opening process. The leather treated with the water-soluble polyurethane has better feel and resilience.
[0020] 6. The modified polyvinyl alcohol of the present invention is copolymerized and modified with vinyl monomers. Vinyl monomers can destroy the intermolecular hydrogen bonds of polyvinyl alcohol, increase its thermal decomposition temperature, inhibit its crystallization, and reduce its melting point. DETAILED DESCRIPTION
[0021] Embodiment 1
[0022] A method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric comprises the following preparation steps: (1) Preparation of sea-island fibers: polyester masterbatch is used as the raw material of the island component, and modified polyvinyl alcohol masterbatch is used as the raw material of the sea component. The polyester masterbatch and the modified polyvinyl alcohol are melted through different screws of a twin-screw extruder to obtain polyester melt and modified polyvinyl alcohol melt, respectively. The polyester melt and the modified polyvinyl alcohol melt are respectively sent into a polyester melt pipeline and a modified polyvinyl alcohol melt pipeline for heating, and then extruded after being metered by a metering pump. The island component is evenly distributed into the sea component through a distribution pipeline, and then ejected through the same spinneret hole for composite spinning to obtain sea-island fibers with polyester as the island component and polyvinyl alcohol as the sea component; The weight ratio of the island component to the sea component is 80:20; The heating temperature of the modified polyvinyl alcohol melt pipe is 165°C; the melting temperature of the modified polyvinyl alcohol masterbatch is 160°C, and the initial thermal decomposition temperature is 260°C; The viscosity difference between polyester melt and modified polyvinyl alcohol melt is less than 10%; The modified polyvinyl alcohol is obtained by modifying polyvinyl alcohol with a vinyl monomer, and the specific modification method is: free radical copolymerization of ethylene and vinyl acetate in a solution, and then alcoholysis to obtain an ethylene-vinyl alcohol copolymer, wherein the vinyl content is 6wt%; (2) using the sea-island fibers obtained in step (1) as raw materials, and producing a non-woven fabric by needle punching; (3) feeding the nonwoven fabric into a production line and impregnating it with an aqueous polyvinyl alcohol slurry, wherein the mass fraction of the aqueous polyvinyl alcohol slurry is 9%; (4) Ironing and impregnation with water-based polyurethane containing water-repellent segments at the end groups; the specific process of the impregnation treatment is: immersing the base fabric in a solution containing water-based polyurethane emulsion containing water-repellent segments at the end groups, the solid content of the water-based polyurethane emulsion is 35%, and a penetrant with a mass concentration of 4% is also added to the solution; The preparation method of the water-based polyurethane containing a water-repellent segment at the end group is as follows: (1) polytetrahydrofuran, dihydroxymethylbutyric acid and acetone are mixed and stirred evenly, the temperature is raised to 55° C., and isophorone diisocyanate is slowly added and maintained for 3 hours; (2) hydroxyethyl acrylate is added and reacted at 65° C. for 4 hours; (3) the temperature is lowered to 38° C., triethylamine is added and reacted for 0.5 hours; (4) deionized water is added at 25° C. and stirred continuously for 1 hour, the temperature is raised to 40° C., and acetone is evaporated at 0.05 MPa; (5) Drying; (6) Water reduction: soak the dried base fabric in hot water at 85°C and stir it continuously to remove polyvinyl alcohol. The bath ratio is 20:1 and the treatment time is 60 seconds. (7) shaping and drying to obtain water-reduced polyester microfiber synthetic leather base fabric.
[0023] Embodiment 2
[0024] Referring to Example 1, in this example, modified polyvinyl alcohol is modified with propylene glycol. The specific modification method is to dry the ethylene-vinyl alcohol copolymer obtained in Example 1 and ordinary polyvinyl alcohol powder, and then prepare the modified polyvinyl alcohol through a twin-screw extruder. The extrusion temperature is controlled at 190°C and the screw speed is 270r / min. Other technical schemes are the same as those in Example 1.
[0025] Embodiment 3
[0026] Referring to Example 2, in this example, the modification method of modified polyvinyl alcohol is to feed the ethylene-vinyl alcohol copolymer obtained in Example 1 into a screw extruder for melt extrusion to obtain modified polyvinyl alcohol masterbatch, and other technical schemes are the same as those in Example 1.
[0027] Embodiment 4
[0028] This embodiment is different from the embodiment 1 in the treatment process of impregnating the aqueous polyurethane containing the end group containing water-repellent segments in step (4), and the other technical schemes are the same as those of the embodiment 1.
[0029] Specifically, the process of impregnating the aqueous polyurethane in this embodiment is as follows: adding high-carbon alcohol and foaming agent to the aqueous polyurethane impregnation liquid, the amount of the high-carbon alcohol is 3% of the total amount of the impregnation liquid, and the amount of the foaming agent is 2% of the total amount of the impregnation liquid. The non-woven fabric is impregnated in the above-mentioned impregnation liquid, and is subjected to a dipping and rolling treatment, and then dried and washed with water. The foaming agent undergoes chemical foaming during the drying process, and the polyurethane is absorbed during the washing process of the high-carbon alcohol, forming through holes in the film, so that many pores are formed inside the synthetic leather. Finally, the synthetic leather obtained has better feel and air permeability.
[0030] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A method for producing a water-reduced polyester microfiber synthetic leather base fabric, characterized in that: The method comprises the following preparation steps: (1) Preparation of sea-island fibers: polyester masterbatch is used as the raw material of the island component, and modified polyvinyl alcohol masterbatch is used as the raw material of the sea component. The polyester masterbatch and the modified polyvinyl alcohol are melted through different screws of a twin-screw extruder to obtain polyester melt and modified polyvinyl alcohol melt, respectively. The polyester melt and the modified polyvinyl alcohol melt are respectively sent into a polyester melt pipeline and a modified polyvinyl alcohol melt pipeline for heating, and then extruded after being metered by a metering pump. The island component is evenly distributed into the sea component through a distribution pipeline, and then ejected through the same spinneret hole for composite spinning to obtain sea-island fibers with polyester as the island component and polyvinyl alcohol as the sea component; The melting temperature of the modified polyvinyl alcohol masterbatch is 155-165°C, and the initial thermal decomposition temperature is 260°C; The viscosity difference between polyester melt and modified polyvinyl alcohol melt is less than 10%; (2) using the sea-island fibers obtained in step (1) as raw materials, and producing a non-woven fabric by needle punching; (3) feeding the nonwoven fabric into a production line and impregnating the nonwoven fabric with an aqueous polyvinyl alcohol slurry; (4) Ironing and impregnation of water-based polyurethane containing water-repellent segments at the end groups; (5) Drying; (6) Water reduction: Soak the dried base fabric in hot water at 85-90°C and stir it continuously; (7) shaping and drying to obtain water-reduced polyester microfiber synthetic leather base fabric.
2. The method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric according to claim 1, characterized in that: The heating temperature of the modified polyvinyl alcohol melt pipeline is 155-165°C.
3. The method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric according to claim 1, characterized in that: The weight ratio of the island component: the sea component = 70-80: 20-30.
4. The method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric according to claim 1, characterized in that: In step (6) water reduction treatment, the bath ratio is 20-30:1 and the treatment time is 30-90s.
5. The method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric according to claim 1, characterized in that: The mass fraction of the aqueous polyvinyl alcohol slurry in step (3) is 9-12%.
6. The method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric according to claim 1, characterized in that: The specific process of step (4) impregnation with aqueous polyurethane containing water-repellent segments at the end groups is as follows: the base fabric is immersed in a solution containing an aqueous polyurethane emulsion, wherein the solid content of the aqueous polyurethane emulsion is 35-40%, and a penetrant with a mass concentration of 4% is also added to the solution.
7. The method for manufacturing a water-reduced polyester ultrafine fiber synthetic leather base fabric according to claim 6, characterized in that: The preparation method of the water-based polyurethane containing a water-repellent segment at the end group is as follows: (1) polytetrahydrofuran, dihydroxymethylbutyric acid and acetone are mixed and stirred evenly, the temperature is raised to 55-62° C., and isophorone diisocyanate is slowly added and maintained for 2-3 hours; (2) hydroxyethyl acrylate is added and reacted at 60-65° C. for 3-4 hours; (3) the temperature is lowered to 38° C., and triethylamine is added and reacted for 0.5-0.6 hours; (4) deionized water is added at 20-25° C. and stirred continuously for 1-1.2 hours, the temperature is raised to 40-45° C., and acetone is evaporated at 0.05-0.06 MPa.
8. The method for manufacturing a water-reduced ultrafine fiber synthetic leather base fabric according to claim 1, characterized in that: The modified polyvinyl alcohol is obtained by modifying polyvinyl alcohol with a vinyl monomer. The specific modification method is: free radical copolymerizing ethylene and vinyl acetate in a solution, and then performing alcoholysis to obtain an ethylene-vinyl alcohol copolymer, wherein the vinyl content is 6-9wt%.
9. The method for manufacturing a water-reduced ultrafine fiber synthetic leather base fabric according to claim 1, characterized in that: The modified polyvinyl alcohol is modified by using glycerol.
Citation Information
Patent Citations
Splitting method of non-woven impregnated base fabric
CN101798738A
Modified polyvinyl alcohol capable of being processed by melting and preparation method of modified polyvinyl alcohol
CN102603954A
Modified polyvinyl alcohol and preparation method thereof
CN106854255A
Waterborne polyurethane synthetic leather and preparation method thereof
CN107881798A
Novel sea-island fiber synthetic leather base cloth and production technology thereof
CN108589028A