Membranes with hydrophobically modified cellulose fibers and oil
By using hydrophobically modified cellulose fibers and oil with an SP value of less than 10 to prepare a dispersion, the resulting film reduces oil mobility on fluids, solving the problem of poor antifouling effect caused by easy oil movement in the prior art, and achieving high efficiency and durability in antifouling.
Patent Information
- Application Number
- CN202210228454.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-03-07
- Filing Date
- 2018-03-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2038-03-06
AI Technical Summary
In the prior art, the oil that forms the surface film tends to migrate to the flow material, resulting in a short-lasting effect in preventing dirt adhesion, especially when the flow material contains oily components.
A dispersion was prepared using hydrophobically modified cellulose fibers and oil with an SP value of less than 10. The dispersion was then coated onto a molded body to form a film. The strong affinity between the hydrophobically modified cellulose fibers and the oil was utilized to reduce the mobility of the oil to the fluid.
It achieves long-term maintenance of the anti-fouling effect of fluids, improves the lubricating surface properties and durability of the membrane, reduces oil mobility, and maintains a highly efficient antifouling effect.
Smart Images

Figure BDA0003536476410000121 
Figure BDA0003536476410000201 
Figure BDA0003536476410000241
Abstract
Description
[0001] This application is a divisional application of an invention patent application with an application date of March 6, 2018, application number 201880013968.4, and invention name “Membrane with hydrophobically modified cellulose fibers and oil”. Technical Field
[0002] The present invention relates to a membrane having hydrophobically modified cellulose fibers and oil. Background Art
[0003] In the field of packaging containers for cosmetics or foods, etc., surface films that prevent objects or dirt from adhering have been developed. Recently, a water-slippery or oil-slippery film is known, which is characterized by having a porous polymer film and a lubricant liquid impregnated in the pores of the porous polymer film, wherein the porous polymer film has a skeleton of a network structure formed by fibrous polymers entangled with each other in three-dimensional directions, and has a continuous pore structure as its gaps (Patent Document 1), and in Patent Document 1, fluorine oil or silicone oil is exemplified as the lubricant liquid (Claim 7).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-011375 Summary of the invention
[0007] The present invention relates to the following [1] to [4].
[0008] [1] A film having:
[0009] Hydrophobically modified cellulose fibers in which a modifying group is bonded to one or more groups selected from anionic groups and hydroxyl groups of the cellulose fibers, and an oil having an SP value of 10 or less.
[0010] [2] A molded article comprising the film according to [1] above.
[0011] [3] A method for forming a film on a formed body, comprising:
[0012] Step 1 of preparing a dispersion containing hydrophobically modified cellulose fibers and an oil having an SP value of 10 or less; and
[0013] Step 2 of applying the dispersion prepared in step 1 onto a molded body.
[0014] [4] A dispersion for a film, comprising:
[0015] Hydrophobically modified cellulose fibers in which a modifying group is bonded to one or more groups selected from anionic groups and hydroxyl groups of the cellulose fibers, and an oil having an SP value of 10 or less. DETAILED DESCRIPTION
[0016] Regarding the technology of Patent Document 1, there is a possibility that the oil constituting the surface film migrates to the object, resulting in the loss of the effect of the surface film on preventing the adhesion of dirt, etc. This phenomenon is particularly significant when the object (fluid) contains an oily component.
[0017] The present invention relates to a film in which the oil constituting the surface film has low mobility toward a flowing object and can maintain the effect of preventing the flowing object from attaching to the film for a long time. Furthermore, the present invention relates to a molded body in which a high effect of preventing the flowing object from attaching to the film can be maintained for a long time. Furthermore, the present invention relates to a method for forming the film on a molded body. Furthermore, the present invention relates to a dispersion for the film.
[0018] Regarding the film of the present invention, the oil constituting the surface film has low mobility toward the flowing object, and the effect of preventing the flowing object from attaching can be maintained for a long time. Furthermore, the molded body of the present invention can maintain a high effect of preventing the flowing object from attaching for a long time because it has the film of the present invention. Furthermore, by the method of forming a film on a molded body of the present invention, such a film can be formed on the molded body.
[0019] [membrane]
[0020] The film of the present invention contains specific hydrophobic modified cellulose fibers and oil having an SP value of 10 or less. Here, the so-called film means a film that does not flow at room temperature and maintains its shape. As for the surface hardness of the film, the following film is preferred: for example, when measured using a microhardness meter, the Martens hardness (HM) calculated according to the following formula is 0.1 (N / mm 2 Specifically, the Martens hardness of the film was measured according to the method described in the following examples.
[0021] HM=F / (26.43×hmax 2 )
[0022] F: Test force (N)
[0023] hmax: Maximum value of the pressing depth (mm)
[0024] The mechanism by which the membrane of the present invention exerts the effect that the oil constituting the surface membrane has a low mobility toward the flowing object and can maintain the anti-attachment effect against the flowing object for a long time is not clear, but it is speculated as follows. It is believed that the hydrophobicity of the oil with an SP value of less than 10 is higher than that of the oil with an SP value of more than 10, so the affinity of the oil with an SP value of less than 10 and the hydrophobic modified cellulose fiber becomes stronger. As a result, it is speculated that the oil with an SP value of less than 10 will not easily separate from the hydrophobic modified cellulose fiber, so even when the flowing object contains an oily component, it is not easy to move to the flowing object.
[0025] The higher the smoothness of the film of the present invention, the higher the synovial surface property, and therefore it is preferred. Specifically, as the arithmetic mean roughness of the film, from the viewpoint of cost-effectiveness, it is preferably 0.3 μm or more, more preferably 0.5 μm or more, and further preferably 0.8 μm or more, while from the viewpoint of synovial surface property, it is preferably 40 μm or less, more preferably 35 μm or less, and further preferably 30 μm or less. In addition, the arithmetic mean roughness of the film can be measured according to the method described in the following examples.
[0026] The thickness of the film of the present invention is not particularly limited. From the perspective of film durability, it is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more. From the perspective of economic efficiency, it is preferably 2000 μm or less, more preferably 1200 μm or less, further preferably 500 μm or less, and further preferably 100 μm or less. Furthermore, the thickness of the film can be set to a desired value by using a coating tool such as an applicator to set the coating thickness or adjusting the ratio of the solvent in the dispersion.
[0027] <Synovial surface membrane>
[0028] The membrane of the present invention preferably exhibits the synovial surface properties disclosed in the document (Technology of super water-repellent, super oil-repellent, and synovial surface / Publisher: Motoki Hiroshi / Publisher: Science & Technology Co., Ltd. / Published on January 28, 2016). In this specification, a membrane exhibiting this synovial surface property is also referred to as a "synovial surface membrane."
[0029] The surface properties of the synovial fluid can be measured, for example, by the method described in the paper (Nature 2011, vol477, p443-447). Specifically, at room temperature 20°C, a 2 μL droplet (20°C) is added to the surface of the synovial fluid, and after standing for 10 seconds, the surface is tilted at a speed of 1° / s, and the angle at which the droplet starts to flow (hereinafter also referred to as the sliding angle) is measured, thereby evaluating the surface properties of the synovial fluid. For example, when dodecane is used as the droplet in the above-mentioned measurement method, from the perspective of expressing the surface properties of the synovial fluid, the sliding angle on the synovial fluid surface film is preferably 80° or less, more preferably 50° or less, and further preferably 40° or less.
[0030] Since the membrane of the present invention has a high effect of inhibiting the adhesion of flowing substances, it can be used as a slippery surface membrane for modifying a solid surface into a slippery surface, for example.
[0031] Examples of uses of the film of the present invention include inner materials of packaging containers for cosmetics, foods, and the like, transportation pipes, ship bottoms, and covering materials for electric wires.
[0032] One feature of the film of the present invention is that the film has a high adhesion inhibition effect on flowing objects. Specifically, the sliding speed is preferably 1.5 cm / minute or more, more preferably 2.0 cm / minute or more, and further preferably 2.5 cm / minute or more. Furthermore, from the perspective of the durability of the adhesion inhibition effect on flowing objects, the sliding speed at the fifth measurement is preferably 1.5 cm / minute or more, more preferably 2.0 cm / minute or more, and further preferably 2.5 cm / minute or more. Furthermore, the sliding speed can be measured according to the method described in the following examples.
[0033] One feature of the film of the present invention is that the mobility of oil with an SP value of 10 or less to the flowing object is small. The small mobility allows the film to be maintained for a longer period of time, and as a result, the adhesion inhibition effect is also exerted for a longer period of time. Specifically, the lubricating oil mobility is preferably 10.0% or less, more preferably 7.5% or less, further preferably 5.0% or less, and further preferably 0%. The lubricating oil mobility can be measured according to the method described in the following examples.
[0034] <Flowing Animal>
[0035] The so-called fluid in the present invention refers to an object such as cosmetics or food that is a packaging object or a coating object. The fluid that can be suppressed from attaching by the film of the present invention is not particularly limited. From the perspective of easily showing the effect of the present invention, the viscosity of the fluid is preferably 0.1 mPa·s or more, more preferably 0.5 mPa·s or more, and further preferably 0.8 mPa·s or more. From the same perspective, it is preferably 100,000 mPa·s or less, more preferably 80,000 mPa·s or less, and further preferably 50,000 mPa·s or less. In addition, the viscosity of the fluid can be measured by an E-type viscometer (25°C, 1 rpm, after 1 minute, standard conical rotor, rotor code: 01).
[0036] In addition, from the viewpoint of easily showing the effect of the present invention, the surface tension of the fluid is preferably 15 mN / m or more, more preferably 18 mN / m or more, and further preferably 20 mN / m or more. From the same viewpoint, it is preferably 75 mN / m or less. Furthermore, the surface tension of the fluid can be measured by the plate method (Wilhelmy method).
[0037] <Hydrophobic modified cellulose fiber>
[0038] The so-called hydrophobically modified cellulose fiber in the present invention is formed by bonding a modifying group to one or more groups selected from the anionic groups and hydroxyl groups of the cellulose fiber, and exhibiting dispersibility in oils with an SP value of 10 or less. The so-called dispersibility in oils with an SP value of 10 or less refers to the following situation: when the viscosity of the mixed liquid of oil and the target hydrophobically modified cellulose fiber is measured using an E-type viscometer (25°C, 1 rpm, after 1 minute, standard conical rotor, rotor code: 01), a thickening is observed. As the hydrophobically modified cellulose in the present invention, for example, the following is preferably used: the liquid prepared in a manner such that the concentration of cellulose fibers in squalane, which is a representative example of oils with an SP value of 10 or less, becomes 0.5% by mass, and the viscosity of the dispersion after micronization becomes 50 mPa·s or more. Furthermore, the micronization treatment can be carried out by the following method.
[0039] From the viewpoint of the performance of the synovial surface, the crystallinity of the hydrophobically modified cellulose fiber is preferably 10% or more. In addition, from the viewpoint of the availability of raw materials, it is preferably 90% or less. Furthermore, in the present specification, the crystallinity of cellulose is the cellulose I type crystallinity calculated by using the diffraction intensity value of the X-ray diffraction method, which can be measured according to the method described in the following examples. Furthermore, the so-called cellulose I type means the crystal form of natural cellulose, and the so-called cellulose I type crystallinity means the ratio of the amount of crystalline region in the whole cellulose. The presence or absence of a cellulose I type crystal structure can be determined by the presence of a peak at 2θ=22.6° in the X-ray diffraction measurement.
[0040] The preferred ranges of the average fiber diameter, average fiber length and average aspect ratio of the hydrophobically modified cellulose fibers are the same as the preferred ranges of the average fiber diameter, average fiber length and average aspect ratio of the microcellulose fibers described below from the viewpoint of the synovial surface property and the inhibition of the migration of oil to the fluid. In addition, they can be obtained according to the measurement method described in the following Examples.
[0041] The amount of hydrophobic modified cellulose fibers in the membrane of the present invention is not particularly limited. From the viewpoint of the slippery surface properties and durability of the membrane, it is preferably 1% by mass or more, more preferably 3% by mass or more, and further preferably 4% by mass or more. From the same viewpoint, it is preferably 40% by mass or less, more preferably 35% by mass or less, and further preferably 30% by mass or less.
[0042] As hydrophobic modified cellulose fibers, for example, there can be listed: hydrophobic modified cellulose fibers (A) in which a modifying group is bonded to the anionic group of cellulose fibers having anionic groups (hereinafter also referred to as "anionic modified cellulose fibers"), or hydrophobic modified cellulose fibers (B) in which a modifying group is bonded to the hydroxyl groups on the surface of the cellulose fibers in the form of ether bonds (hereinafter also referred to as "etherified cellulose fibers"). From the viewpoint of further exerting the effect of the present invention, the hydrophobic modified cellulose fibers (A) are preferred.
[0043] (Cellulose Fiber)
[0044] Cellulose fibers as a raw material of the hydrophobically modified cellulose fibers are preferably natural cellulose fibers from an environmental perspective, and examples thereof include wood pulps such as coniferous tree pulp and broadleaf tree pulp, cotton pulps such as cotton linter and cotton lint, non-wood pulps such as straw pulp and bagasse pulp, bacterial cellulose, etc., and any one of them may be used alone or in combination of two or more.
[0045] The average fiber diameter of the raw material cellulose fiber is not particularly limited. From the viewpoint of handleability and cost, it is preferably 1 μm or more, more preferably 5 μm or more, and further preferably 15 μm or more. On the other hand, it is preferably 300 μm or less, more preferably 100 μm or less, and further preferably 60 μm or less.
[0046] In addition, the average fiber length of the raw material cellulose fiber is not particularly limited, but from the viewpoint of availability and cost, it is preferably 100 μm or more, more preferably 500 μm or more, and further preferably 1,000 μm or more, and further preferably 5,000 μm or less, more preferably 4,000 μm or less, and further preferably 3,000 μm or less. The average fiber diameter and average fiber length of the raw material cellulose fiber can be measured according to the method described in the following Examples.
[0047] <Hydrophobic modified cellulose fiber (A)>
[0048] The hydrophobically modified cellulose fibers (A) in the present invention refer to cellulose fibers in which a compound for introducing a modifying group is bonded to an anionic group of an anionic modified cellulose fiber.
[0049] (Anionic modified cellulose fiber)
[0050] Examples of the anionic groups contained in the anion-modified cellulose fibers include carboxyl groups, sulfonic acid groups, and phosphoric acid groups, and from the perspective of the efficiency of introduction into the cellulose fibers, carboxyl groups are preferred. Examples of the ions that are the counterparts of the anionic groups in the anion-modified cellulose fibers (counter ions) include metal ions such as sodium ions, potassium ions, calcium ions, and aluminum ions generated in the presence of a base during production, or protons generated by replacing these metal ions with an acid.
[0051] (Anionic group content)
[0052] The anionic group content in the anion-modified cellulose fiber used in the present invention is preferably 0.1 mmol / g or more, more preferably 0.4 mmol / g or more, further preferably 0.6 mmol / g or more, and further preferably 0.8 mmol / g or more from the viewpoint of introducing the modifying group. In addition, from the viewpoint of improving the operability, it is preferably 3 mmol / g or less, more preferably 2 mmol / g or less, and further preferably 1.8 mmol / g or less. Furthermore, the so-called "anionic group content" means the total amount of anionic groups in the cellulose constituting the cellulose fiber, and specifically, it can be measured according to the method described in the following examples.
[0053] In addition, the preferred ranges of the average fiber diameter, average fiber length and average aspect ratio of the anionically modified cellulose fibers are the same as those of the hydrophobically modified cellulose fibers described above, and are the same as those of the average fiber diameter and average fiber length of the microfibers described below. In addition, they can be obtained according to the measurement method described in the following Examples.
[0054] (Step of introducing anionic groups)
[0055] The anionically modified cellulose fibers used in the present invention can be obtained by subjecting target cellulose fibers to an oxidation treatment or an anionic group-adding treatment to introduce at least one anionic group to perform anionic modification.
[0056] Examples of the cellulose fibers to be anion-modified include raw cellulose fibers. From the viewpoint of dispersibility, it is preferred to use cellulose fibers having an average fiber length of 1 μm to 1,000 μm obtained by short-fiberizing the raw cellulose fibers by alkali hydrolysis or acid hydrolysis.
[0057] The following describes in more detail the case where (i) carboxyl groups are introduced into cellulose fibers as anionic groups and (ii) sulfonic acid groups or phosphoric acid groups are introduced into cellulose fibers as anionic groups.
[0058] (i) Introducing carboxyl groups as anionic groups into cellulose fibers
[0059] Examples of methods for introducing carboxyl groups as anionic groups into cellulose fibers include a method of oxidizing hydroxyl groups of cellulose to convert them into carboxyl groups, and a method of reacting hydroxyl groups of cellulose with at least one selected from a compound having a carboxyl group, an acid anhydride of a compound having a carboxyl group, and derivatives thereof.
[0060] (Oxidized cellulose fiber)
[0061] In this specification, cellulose fibers having carboxyl groups are referred to as "oxidized cellulose fibers". Oxidized cellulose fibers can be produced, for example, by applying the following method: using 2,2,6,6-tetramethyl-1-piperidinyl-N-oxyl radical (TEMPO) as a catalyst, and then using an oxidant such as sodium hypochlorite, a bromide such as sodium bromide, etc., to oxidize the hydroxyl groups of the cellulose fibers into carboxyl groups. In more detail, the method described in Japanese Patent Publication No. 2011-140632 can be referred to, and an additional oxidation treatment or reduction treatment can be performed to prepare oxidized cellulose fibers from which the aldehyde groups are removed. Oxidized cellulose fibers are preferred from the viewpoint of inhibiting the migration of oil to the fluid compared to other anion-modified cellulose fibers.
[0062] (ii) Introducing sulfonic acid groups or phosphoric acid groups as anionic groups into cellulose fibers
[0063] Examples of a method for introducing sulfonic acid groups as anionic groups into cellulose fibers include a method of adding sulfuric acid to cellulose fibers and heating the fibers.
[0064] Examples of methods for introducing phosphoric acid groups as anionic groups into cellulose fibers include a method of mixing a powder or aqueous solution of phosphoric acid or a phosphoric acid derivative with dry or wet cellulose fibers, or a method of adding an aqueous solution of phosphoric acid or a phosphoric acid derivative to a dispersion of cellulose fibers, etc. When these methods are used, dehydration treatment and heat treatment are usually performed after mixing or adding a powder or aqueous solution of phosphoric acid or a phosphoric acid derivative.
[0065] (Modifying group)
[0066] In this specification, the bonding of the modifying group in the hydrophobically modified cellulose fiber (A) means a state in which the modifying group is bonded to the anionic group, preferably the carboxyl group, on the surface of the cellulose fiber in the form of an ionic bond and / or a covalent bond. As the bonding mode on the anionic group, there can be listed: ionic bonding and covalent bonding. As the covalent bond here, for example, there can be listed: amide bond, ester bond, carbamate bond, among which, from the viewpoint of inhibiting the movement of oil to the flowing object, amide bond is preferred. From the viewpoint of inhibiting the movement of oil to the flowing object, the hydrophobically modified cellulose fiber (A) in the present invention is preferably a substance obtained by bonding the compound for introducing the modifying group to the existing carboxyl group on the surface of the cellulose fiber in the form of an ionic bond and / or an amide bond.
[0067] (Compound for introducing a modifying group)
[0068] As the compound for introducing the modifying group, as long as it is capable of introducing the following modifying group, according to the bonding mode, for example, the following substances can be used. In the case of ionic bond, it can be any of primary amine, secondary amine, tertiary amine, quaternary ammonium compound, and phosphonium compound. Among them, from the viewpoint of dispersibility, preferred primary amine, secondary amine, tertiary amine, and quaternary ammonium compound. In addition, as the anion component of the above-mentioned ammonium compound or phosphonium compound, from the viewpoint of reactivity, preferably cite: halogen ions such as chloride ion or bromide ion, hydrogen sulfate ion, perchlorate ion, tetrafluoroborate ion, hexafluorophosphate ion, trifluoromethanesulfonate ion, hydroxyl ion, and more preferably cite hydroxyl ion. In the case of covalent bond, according to the substituted functional group, the following substances can be used.
[0069] Regarding the modification of the carboxyl group, in the case of an amide bond, it may be any of a primary amine and a secondary amine. In the case of an ester bond, it may be an alcohol, such as butanol, octanol, and dodecanol. In the case of a urethane bond, it may be an isocyanate compound.
[0070] As the modifying group in the hydrophobically modified cellulose fiber (A), a hydrocarbon group or the like can be used. These can be bonded (introduced) to the cellulose fiber alone or in combination of two or more.
[0071] (Hydrocarbon)
[0072] Examples of the hydrocarbon group include a chain saturated hydrocarbon group, a chain unsaturated hydrocarbon group, a cyclic saturated hydrocarbon group, and an aromatic hydrocarbon group. From the viewpoint of suppressing side reactions and from the viewpoint of stability, a chain saturated hydrocarbon group, a cyclic saturated hydrocarbon group, and an aromatic hydrocarbon group are preferred. The number of carbon atoms in the hydrocarbon group is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more from the viewpoint of synovial surface properties. From the same viewpoint, it is preferably 30 or less, more preferably 24 or less, and further preferably 18 or less.
[0073] The chain saturated hydrocarbon group may be straight chain or branched. Regarding the carbon number of the chain saturated hydrocarbon group, from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the fluid, the carbon number in one modifying group is preferably 1 or more, more preferably 2 or more, further preferably 3 or more, further preferably 6 or more, further preferably 8 or more. In addition, from the same viewpoint, it is preferably 30 or less, more preferably 24 or less, further preferably 18 or less, further preferably 16 or less. In addition, the carbon number of the hydrocarbon group mentioned below means the carbon number in one modifying group.
[0074] Specific examples of the chain saturated hydrocarbon group include, for example, methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, isobutyl, pentyl, tert-pentyl, isopentyl, hexyl, isohexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, dodecyl, tridecyl, tetradecyl, octadecyl, docosyl, octacosyl, etc., and from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the flowing object, propyl, isopropyl, butyl, sec-butyl, tert-butyl, isobutyl, pentyl, tert-pentyl, isopentyl, hexyl, isohexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, dodecyl, tridecyl, tetradecyl, octadecyl, docosyl, octacosyl, etc. are preferred. These groups may be introduced alone or in any combination.
[0075] The chain unsaturated hydrocarbon group may be straight-chain or branched. The carbon number of the chain unsaturated hydrocarbon group is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more from the viewpoint of operability. In addition, from the viewpoint of easy availability, it is preferably 30 or less, more preferably 18 or less, further preferably 12 or less, and further preferably 8 or less.
[0076] Specific examples of the chain unsaturated hydrocarbon group include vinyl, propenyl, butenyl, isobutenyl, isoprenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, dodecenyl, tridecenyl, tetradecenyl, and octadecenyl. In terms of the surface properties of the synovial fluid and the inhibition of the migration of oil to the fluid, vinyl, propenyl, butenyl, isobutenyl, isoprenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, and dodecenyl are preferred. These may be introduced alone or in any ratio.
[0077] The carbon number of the cyclic saturated hydrocarbon group is preferably 3 or more, more preferably 4 or more, and further preferably 5 or more from the viewpoint of operability. In addition, from the viewpoint of availability, it is preferably 20 or less, more preferably 16 or less, further preferably 12 or less, and further preferably 8 or less.
[0078] Specific examples of the cyclic saturated hydrocarbon group include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, cyclododecyl, cyclotridecyl, cyclotetradecyl, cyclooctadecyl, and cyclooctadecyl. From the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the flowing object, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, and cyclododecyl are preferred. These groups may be introduced alone or in any ratio.
[0079] The aromatic hydrocarbon group is, for example, selected from an aryl group and an aralkyl group. In the case of the aryl group and the aralkyl group, the aromatic ring itself may be substituted or unsubstituted.
[0080] The total carbon number of the aryl group may be 6 or more, and is preferably 24 or less, more preferably 20 or less, further preferably 14 or less, further preferably 12 or less, further preferably 10 or less, from the viewpoint of synovial surface properties and inhibition of oil migration to the fluid.
[0081] The total carbon number of the aralkyl group is 7 or more, preferably 8 or more from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the fluid, and preferably 24 or less, more preferably 20 or less, further preferably 14 or less, further preferably 13 or less, further preferably 11 or less from the same viewpoint.
[0082] Examples of the aryl group include phenyl, naphthyl, anthracenyl, phenanthrenyl, biphenyl, triphenyl, terphenyl, and groups in which these groups are substituted with the following substituents, and these groups may be introduced alone or in any ratio. Among them, phenyl, biphenyl, and terphenyl are preferred from the viewpoint of the surface properties of the synovial fluid and the inhibition of the migration of oil to the fluid.
[0083] Examples of the aralkyl group include benzyl, phenethyl, phenylpropyl, phenylpentyl, phenylhexyl, phenylheptyl, phenyloctyl, and aromatic groups of these groups substituted with the following substituents, and the like, each of which may be introduced alone or in any ratio. Among them, benzyl, phenethyl, phenylpropyl, phenylpentyl, phenylhexyl, and phenylheptyl are preferred from the viewpoint of the surface properties of the synovial fluid and the inhibition of the migration of oil to the fluid.
[0084] The primary amine, secondary amine, tertiary amine, quaternary ammonium compound, phosphonium compound, acid anhydride, and isocyanate compound used for introducing the above-mentioned hydrocarbon group may be a commercially available product or may be prepared by a known method.
[0085] As the primary amine to the tertiary amine, from the viewpoint of the surface property of the synovial fluid, the carbon number is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more. From the same viewpoint, the carbon number is preferably 20 or less, more preferably 18 or less, and further preferably 16 or less (excluding amino-modified polysiloxane compounds). Specific examples of the primary amine to the tertiary amine include ethylamine, diethylamine, triethylamine, propylamine, dipropylamine, butylamine, dibutylamine, hexylamine, dihexylamine, octylamine, dioctylamine, trioctylamine, dodecylamine, didodecylamine, stearylamine, distearylamine, monoethanolamine, diethanolamine, triethanolamine, aniline, benzylamine, and amino-modified polysiloxane compounds. Examples of the quaternary ammonium compound include tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetraethylammonium chloride, tetrapropylammonium hydroxide (TPAH), tetrabutylammonium hydroxide (TBAH), tetrabutylammonium chloride, lauryltrimethylammonium chloride, dilauryldimethylammonium chloride, stearyltrimethylammonium chloride, distearyldimethylammonium chloride, cetyltrimethylammonium chloride, and alkylbenzyldimethylammonium chloride. Among them, from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the fluid, propylamine, dipropylamine, butylamine, dibutylamine, hexylamine, dihexylamine, octylamine, dioctylamine, trioctylamine, dodecylamine, didodecylamine, distearylamine, amino-modified silicone compounds, tetraethylammonium hydroxide (TEAH), tetrabutylammonium hydroxide (TBAH), tetrapropylammonium hydroxide (TPAH), and aniline are preferred; propylamine, dodecylamine, amino-modified silicone compounds, tetrabutylammonium hydroxide (TBAH), and aniline are more preferred; and amino-modified silicone compounds are further preferred.
[0086] Among these compounds, hydrophobically modified cellulose fibers obtained by using amino-modified polysiloxane compounds are particularly useful as raw materials for membranes, especially synovial surface membranes. Therefore, in one embodiment of the present invention, a hydrophobically modified cellulose fiber is provided in which an anionic group of an anionic modified cellulose fiber is bonded with an amino-modified polysiloxane compound. When the hydrophobically modified cellulose fiber is made into a synovial surface membrane, the effect of excellent synovial surface properties and the ability to inhibit oil from moving toward a flowing object can be exerted.
[0087] (Amino-modified polysiloxane compound)
[0088] As the amino-modified polysiloxane compound, a preferred example is an amino-modified polysiloxane having a kinematic viscosity at 25° C. of 10 to 20,000 mm 2 / s, an amino-modified polysiloxane compound having an amino equivalent of 400 to 8,000 g / mol.
[0089] The kinematic viscosity at 25°C can be determined using an Ostwald viscometer, and is more preferably 200 to 10,000 mm2 from the viewpoint of the surface properties of the synovial fluid and the suppression of the migration of the oil into the fluid. 2 / s, more preferably 500 to 5,000 mm 2 / s.
[0090] In addition, from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the fluid, the amino equivalent is preferably 400 to 8,000 g / mol, more preferably 600 to 5,000 g / mol, and further preferably 800 to 3,000 g / mol. In addition, the amino equivalent is the molecular weight corresponding to one nitrogen atom, and can be obtained by amino equivalent (g / mol) = mass average molecular weight / number of nitrogen atoms per molecule. Here, the mass average molecular weight is a value obtained by gel permeation chromatography using polystyrene as a standard substance, and the number of nitrogen atoms can be obtained by elemental analysis.
[0091] Specific examples of the amino-modified polysiloxane compound include compounds represented by the general formula (a1).
[0092] [Chemical formula 1]
[0093]
[0094] [Where R 1a R represents a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxyl group, an alkoxy group having 1 to 3 carbon atoms, or a hydrogen atom, and is preferably a methyl group or a hydroxyl group from the viewpoint of the surface properties of the synovial fluid and the inhibition of the migration of oil into the fluid. 2a is a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxyl group or a hydrogen atom, and preferably a methyl group or a hydroxyl group from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the fluid. B represents a side chain having at least one amino group, and R 3a represents an alkyl group having 1 to 3 carbon atoms or a hydrogen atom. x and y represent the average degree of polymerization, respectively, and are selected so that the kinematic viscosity and amino equivalent of the compound at 25° C. are within the above ranges. 1a , R 2a , R 3a They may be the same or different. In addition, multiple R 2a Can be the same or different]
[0095] In the compound of the general formula (a1), from the viewpoint of the synovial surface property and the inhibition of the migration of oil to the fluid, x is preferably a number of 10 to 10,000, more preferably a number of 20 to 5,000, and further preferably a number of 30 to 3,000. y is preferably a number of 1 to 1,000, more preferably a number of 1 to 500, and further preferably a number of 1 to 200. The mass average molecular weight of the compound of the general formula (a1) is preferably 2,000 to 1,000,000, more preferably 5,000 to 100,000, and further preferably 8,000 to 50,000.
[0096] In the general formula (a1), examples of the side chain B having an amino group include the following groups.
[0097] -C3H6-NH2
[0098] -C3H6-NH-C2H4-NH2
[0099] -C3H6-NH-[C2H4-NH] e -C2H4-NH2
[0100] -C3H6-NH(CH3)
[0101] -C3H6-NH-C2H4-NH(CH3)
[0102] -C3H6-NH-[C2H4-NH] f -C2H4-NH(CH3)
[0103] -C3H6-N(CH3)2
[0104] -C3H6-N(CH3)-C2H4-N(CH3)2
[0105] -C3H6-N(CH3)-[C2H4-N(CH3)] g -C2H4-N(CH3)2
[0106] -C3H6-NH-cyclo-C5H 11
[0107] (Here, e, f, and g are numbers from 1 to 30 respectively)
[0108] The amino-modified polysiloxane compound used in the present invention can be produced, for example, by using a basic catalyst such as sodium hydroxide and heating to 80 to 110° C. to allow the hydrolyzate obtained by hydrolyzing the organoalkoxysilane represented by the general formula (a2) with excess water to react with dimethylcyclopolysiloxane, and when the reaction mixture reaches a desired viscosity, using an acid to neutralize the basic catalyst (see Japanese Patent Application Laid-Open No. 53-98499).
[0109] H2N(CH2)2NH(CH2)3Si(CH3)(OCH3)2 (a2)
[0110] In addition, as the amino-modified polysiloxane compound, from the viewpoint of the surface properties of the synovial fluid and the inhibition of the migration of oil to the fluid, it is preferably selected from one or more of a monoamino-modified polysiloxane having one amino group in one side chain B and a diamino-modified polysiloxane having two amino groups in one side chain B, and more preferably selected from one or more of a compound in which the side chain B having an amino group is represented by -C3H6-NH2 (hereinafter referred to as component (a1-1)) and a compound in which the side chain B having an amino group is represented by -C3H6-NH-C2H4-NH2 (hereinafter referred to as component (a1-2)).
[0111] As the amino-modified polysiloxane compound in the present invention, TSF4703 (kinematic viscosity: 1000, amino equivalent: 1600), TSF4708 (kinematic viscosity: 1000, amino equivalent: 2800) manufactured by Momentive Performance Materials, SF8457C (kinematic viscosity: 1200, amino equivalent: 1800), SF8417 (kinematic viscosity: 1200, amino equivalent: 1700), BY16-209 (kinematic viscosity: 500, amino equivalent: 1800), BY16-892 (kinematic viscosity: 1500, amino equivalent: 2000), BY16-898 (kinematic viscosity: 2000, amino equivalent: 2900), FZ-3760 (kinematic viscosity: 1200, amino equivalent: 1800), BY16-899 (kinematic viscosity: 1500, amino equivalent: 2000), BY16-900 (kinematic viscosity: 2000, amino equivalent: 2900), FZ-3770 (kinematic viscosity: 1200, amino equivalent: 1800), BY16-10 ...1 (kinematic viscosity: 1200, amino equivalent: 1800), BY16-1002 (kinematic viscosity: 1500, amino equivalent: 2000), BY16-1003 (kinematic viscosity: 1500, amino equivalent: 2000), BY16-1004 (kinematic viscosity: 1500, amino equivalent: 2900), FZ-3761 (kine Kinematic viscosity: 220, amino equivalent: 1600), KF8002 (kinematic viscosity: 1100, amino equivalent: 1700), KF867 (kinematic viscosity: 1300, amino equivalent: 1700), KF-864 (kinematic viscosity: 1700, amino equivalent: 3800), BY16-213 (kinematic viscosity: 55, amino equivalent: 2700), BY16-853U (kinematic viscosity: 14, amino equivalent: 450) manufactured by Shin-Etsu Chemical Co., Ltd. In "()", the kinematic viscosity indicates the measured value at 25°C (unit: mm 2 / s), and the unit of amino equivalent is g / mol.
[0112] As the component (a1-1), BY16-213 (kinematic viscosity: 55, amino equivalent: 2700) and BY16-853U (kinematic viscosity: 14, amino equivalent: 450) are more preferred.
[0113] As the component (a1-2), SF8417 (kinematic viscosity: 1200, amino equivalent: 1700), BY16-209 (kinematic viscosity: 500, amino equivalent: 1800), and FZ-3760 (kinematic viscosity: 220, amino equivalent: 1600) are more preferred.
[0114] The average bonding amount of the modifying group in the hydrophobically modified cellulose fiber (A) is preferably 0.01 mmol / g or more, more preferably 0.05 mmol / g or more, further preferably 0.1 mmol / g or more, further preferably 0.3 mmol / g or more, further preferably 0.5 mmol / g or more, relative to the unit mass of the cellulose fiber, from the viewpoint of the synovial surface property and the inhibition of the movement of oil to the flowing object. In addition, from the viewpoint of reactivity, it is preferably 3 mmol / g or less, more preferably 2.5 mmol / g or less, further preferably 2 mmol / g or less, further preferably 1.8 mmol / g or less, further preferably 1.5 mmol / g or less. Here, when any two or more modifying groups are introduced into the cellulose fiber as modifying groups at the same time, the average bonding amount of the modifying groups is preferably such that the total amount of the modified groups introduced is within the above range.
[0115] The introduction rate of the modifying groups in the hydrophobically modified cellulose fibers (A) is preferably 10% or more, more preferably 30% or more, further preferably 50% or more, further preferably 60% or more, further preferably 70% or more, for each modifying group, from the viewpoint of the synovial surface property and the inhibition of the migration of oil to the fluid, and preferably 99% or less, more preferably 97% or less, further preferably 95% or less, further preferably 90% or less from the viewpoint of reactivity. Here, when two or more modifying groups are introduced simultaneously as modifying groups into the cellulose fibers, it is preferred that the upper limit of the total introduction rate does not exceed 100% and is within the above range.
[0116] Furthermore, the above-mentioned modifying group may further have a substituent. For example, in the case of a hydrocarbon group, the total carbon number of the modifying group including the substituent is preferably within the above range. As the substituent, for example, alkoxy groups having 1 to 6 carbon atoms such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, sec-butoxy, tert-butoxy, pentyloxy, isopentyloxy, and hexyloxy groups can be listed; alkoxy-carbonyl groups having 1 to 6 carbon atoms such as methoxycarbonyl, ethoxycarbonyl, propoxycarbonyl, isopropoxycarbonyl, butoxycarbonyl, isobutoxycarbonyl, sec-butoxycarbonyl, tert-butoxycarbonyl, pentyloxycarbonyl, and isopentyloxycarbonyl groups; halogen atoms such as fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms; acyl groups having 1 to 6 carbon atoms such as acetyl and propionyl groups; aralkyl groups; aralkyloxy groups; alkylamino groups having 1 to 6 carbon atoms; and dialkylamino groups having 1 to 6 carbon atoms in the alkyl group. Furthermore, the above-mentioned hydrocarbon group itself can be bonded as a substituent.
[0117] In this specification, the average bonding amount and introduction rate of the modifying group in the hydrophobically modified cellulose fiber (A) can be adjusted by the addition amount or type of the compound used to introduce the modifying group, the reaction temperature, the reaction time, the solvent, etc. The so-called average bonding amount (mmol / g) and introduction rate (%) of the modifying group refer to the amount and ratio of the modifying group introduced on the anionic group on the surface of the hydrophobically modified cellulose fiber (A). The anionic group content of the hydrophobically modified cellulose fiber (A) can be measured and calculated by a known method (such as titration, IR measurement, etc.). The average bonding amount and introduction rate of the modifying group in the hydrophobically modified cellulose fiber (A) are calculated, for example, by the method described in the examples.
[0118] [Method for producing hydrophobically modified cellulose fibers (A)]
[0119] The hydrophobically modified cellulose fiber (A) used in the present invention can be produced by a known method, and is not particularly limited as long as a modifying group can be introduced into the anionic modified cellulose fiber. The anionic modified cellulose fiber mentioned here may be an oxidized cellulose fiber from which an aldehyde group has been removed, and can be produced by referring to a known method, for example, the method described in Japanese Patent Application Laid-Open No. 2011-140632, and then performing the additional oxidation treatment or reduction treatment.
[0120] As a specific production method, the following two methods can be mentioned depending on the method of introducing the modifying group into the oxidized cellulose fiber. That is, there can be mentioned a method in which the modifying group is bonded to the oxidized cellulose fiber via an ionic bond (method A) and a method in which the modifying group is bonded to the oxidized cellulose fiber via a covalent bond (method B). In addition, regarding the covalent bond, the case of an amide bond is disclosed below.
[0121] [Method A]
[0122] Step (1): oxidizing natural cellulose fibers in the presence of an N-oxyl radical compound to obtain oxidized cellulose fibers
[0123] Step (2A): Mixing the oxidized cellulose fibers obtained in step (1) with a compound for introducing a modifying group
[0124] [Method B]
[0125] Step (1): oxidizing natural cellulose fibers in the presence of an N-oxyl radical compound to obtain oxidized cellulose fibers
[0126] Step (2B): subjecting the oxidized cellulose fibers obtained in step (1) to an amidation reaction with a compound for introducing a modifying group
[0127] Regarding the method for introducing the modifying group, for example, in the case of form A, it can be carried out with reference to the method described in Japanese Patent Publication No. 2015-143336, and in the case of form B, it can be carried out with reference to the method described in Japanese Patent Publication No. 2015-143337. In addition, in the present invention, the following methods can be adopted: a method in which the following micronization step is performed after step (1), and after preparing microfine cellulose fibers, step (2A or 2B) is performed (first manufacturing form); and a method in which step (2A or 2B) is performed in sequence after step (1), and then a micronization step is performed to obtain microfine cellulose fibers (second manufacturing form). In addition, the micronized cellulose fibers are sometimes particularly referred to as "microfine cellulose fibers".
[0128] Hereinafter, a method for producing fine cellulose fibers will be described based on the first production form of aspect A.
[0129] [Process (1)]
[0130] Step (1) oxidizes natural cellulose fibers in the presence of an N-oxyl radical compound to obtain oxidized cellulose fibers. Specifically, the natural cellulose fibers are subjected to an oxidation treatment step described in Japanese Patent Application Laid-Open No. 2015-143336 or Japanese Patent Application Laid-Open No. 2015-143337 (for example, oxidation treatment using 2,2,6,6-tetramethylpiperidin-1-oxyl radical (TEMPO)) and a purification step (if necessary) to obtain oxidized cellulose fibers having a carboxyl content of preferably 0.1 mmol / g or more. By using TEMPO as a catalyst to oxidize the cellulose fibers, the hydroxymethyl group (-CH2OH) at the C6 position of the cellulose structural unit is selectively converted into a carboxyl group. This method is particularly advantageous in that it has excellent selectivity for the hydroxyl group at the C6 position that is the oxidation target on the surface of the raw cellulose fiber, and the reaction conditions are also stable.
[0131] (Micro-refining process)
[0132] Next, after the purification step (which may be performed as necessary), the oxidized cellulose fibers obtained in step (1) are subjected to a micronizing step to obtain fine oxidized cellulose fibers. In the micronizing step, the oxidized cellulose fibers subjected to the purification step are preferably dispersed in a solvent to be subjected to micronizing treatment.
[0133] Regarding the solvent used as the dispersion medium, in addition to water, examples include: alcohols having 1 to 6 carbon atoms, preferably 1 to 3 carbon atoms, such as methanol, ethanol, and propanol; ketones having 3 to 6 carbon atoms, such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; linear or branched saturated or unsaturated hydrocarbons having 1 to 6 carbon atoms; aromatic hydrocarbons such as benzene and toluene; halogenated hydrocarbons such as dichloromethane and chloroform; lower alkyl ethers having 2 to 5 carbon atoms; polar solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and diesters of succinic acid and triethylene glycol monomethyl ether, and the like. These may be used alone or in combination of two or more. From the viewpoint of operability in the micronization treatment, polar solvents such as water, alcohols having 1 to 6 carbon atoms, ketones having 3 to 6 carbon atoms, lower alkyl ethers having 2 to 5 carbon atoms, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and methyl triethylene glycol succinate are preferred. From the viewpoint of reducing environmental load, water is more preferred. The amount of the solvent used is not particularly limited as long as it is an effective amount for dispersing the oxidized cellulose fibers. It is preferably used in an amount of 1 to 500 times by mass, more preferably 2 to 200 times by mass, relative to the oxidized cellulose fibers.
[0134] As the device used in the micronization treatment, it is preferable to use a known disperser. For example, a dissociator, a beater, a low-pressure homogenizer, a high-pressure homogenizer, a grinder, a shearing mill, a ball mill, a jet mill, a short-shaft extruder, a double-shaft extruder, a pressurized kneading machine, a Banbury mixer, a small mixing extruder (Laboplastomill), an ultrasonic mixer, a household juicer mixer, etc. can be used. In addition, the solid content of the reactant fiber in the micronization treatment is preferably 50% by mass or less.
[0135] In this manner, cellulose fibers can be obtained in which the hydroxyl group at the C6 position of the cellulose fiber structural unit is selectively oxidized to a carboxyl group via an aldehyde group.
[0136] [Step (2A)]
[0137] In the first production form, step (2A) is to mix the oxidized cellulose fibers obtained through the above steps with a compound for introducing a modifying group to obtain hydrophobically modified cellulose fibers (A). Specifically, the oxidized cellulose fibers and the compound for introducing a modifying group are mixed in a solvent, and can be produced, for example, according to the method described in Japanese Patent Application Laid-Open No. 2015-143336.
[0138] Examples of the compound for introducing a modifying group used in step (2A) include the above-mentioned compounds.
[0139] The amount of the compound to be used can be determined according to the desired bonding amount of the modifying group in the hydrophobically modified cellulose fiber (A). From the viewpoint of reactivity, the amount of the amino group is preferably 0.01 mol or more, more preferably 0.1 mol or more, based on 1 mol of the carboxyl group contained in the oxidized cellulose fiber. From the viewpoint of product purity, the amount of the amino group is preferably 50 mol or less, more preferably 20 mol or less, and further preferably 10 mol or less. The compound in the amount contained in the above range may be used for the reaction at once or in divided portions. When the compound is a monoamine, the amino group is equivalent to an amine.
[0140] As a solvent, it is preferred to select a solvent that can dissolve the compound used, for example, methanol, ethanol, isopropyl alcohol (IPA), N, N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), N, N-dimethylacetamide, tetrahydrofuran (THF), succinic acid and triethylene glycol monomethyl ether diester, acetone, methyl ethyl ketone (MEK), acetonitrile, dichloromethane, chloroform, toluene, acetic acid, water, etc., one of which can be used alone or two or more can be used in combination. Among these polar solvents, succinic acid and triethylene glycol monomethyl ether diester, ethanol, DMF, water are preferred.
[0141] The temperature during mixing is preferably 0° C. or higher, more preferably 5° C. or higher, and further preferably 10° C. or higher from the viewpoint of the reactivity of the compound. In addition, from the viewpoint of product quality such as coloring, it is preferably 50° C. or lower, more preferably 40° C. or lower, and further preferably 30° C. or lower. The mixing time can be appropriately set according to the types of the compound and solvent used, but from the viewpoint of the reactivity of the compound, it is preferably 0.01 hours or higher, more preferably 0.1 hours or higher, and further preferably 1 hour or higher, and from the viewpoint of productivity, it is preferably 48 hours or lower, and further preferably 24 hours or lower.
[0142] After the hydrophobically modified cellulose fibers (A) are produced, post-treatment may be appropriately performed to remove unreacted compounds, etc. Examples of the post-treatment method include filtration, centrifugal separation, and dialysis.
[0143] In addition, regarding the manufacturing method of form B, since step (1) is carried out in the same manner as in form A, step (2B) in the first manufacturing form is described below. In addition, for example, it can be manufactured by the method described in Japanese Patent Application Laid-Open No. 2013-151661.
[0144] [Step (2B)]
[0145] In the first production embodiment, in step (2B), the oxidized cellulose fibers obtained through the above step are subjected to an amidation reaction with a compound for introducing a modifying group, thereby obtaining cellulose fibers. The above mixing method has no particular problem as long as the mixing degree allows the raw materials to react. Specifically, the above raw materials are mixed in the presence of a condensing agent to cause a condensation reaction between the carboxyl group contained in the oxidized cellulose fibers and the amino group of the compound for introducing a modifying group to form an amide bond.
[0146] Examples of the compound for introducing a modifying group used in step (2B) include those described above.
[0147] In step (2B), oxidized cellulose fibers and a compound for introducing a modifying group are amidated in the presence of a condensing agent.
[0148] The amount of the compound for introducing a modifying group is preferably used in an amount such that the number of amino groups is preferably 0.1 mol or more, more preferably 0.5 mol or more, based on 1 mol of carboxyl groups contained in the oxidized cellulose fiber from the viewpoint of reactivity, and preferably used in an amount such that the number of amino groups is preferably 50 mol or less, more preferably 20 mol or less, and further preferably 10 mol or less from the viewpoint of product purity. The compound in an amount within the above range may be used in the reaction at once or in divided portions.
[0149] The condensing agent is not particularly limited, and examples thereof include the condensing agents described in Synthetic Chemistry Series Peptide Synthesis (Maruzen Co., Ltd.) P116, or the condensing agents described in Tetrahedron, 57, 1551 (2001), and the like. For example, 4-(4,6-dimethoxy-1,3,5-triazine-2-yl)-4-methylmorpholinium chloride (hereinafter sometimes referred to as "DMT-MM") and the like can be mentioned.
[0150] In the amidation reaction, the solvent used in the micronization step can be used, and it is preferred to select a solvent that can dissolve the compound used.
[0151] The reaction time and reaction temperature in the amidation reaction can be appropriately selected according to the type of compound and solvent used, and from the viewpoint of reaction rate, it is preferably 1 to 24 hours, and more preferably 10 to 20 hours. In addition, regarding the reaction temperature, from the viewpoint of reactivity, it is preferably 0° C. or more, more preferably 5° C. or more, and further preferably 10° C. or more. In addition, from the viewpoint of product quality such as coloring, it is preferably 200° C. or less, more preferably 80° C. or less, and further preferably 30° C. or less.
[0152] After the above reaction, post-treatment may be appropriately performed to remove unreacted compounds, condensing agents, etc. Examples of the post-treatment method include filtration, centrifugal separation, and dialysis.
[0153] Furthermore, regardless of method A or method B, in the second manufacturing form, the above-mentioned steps are carried out in the order of step (1), step (2A) or step (2B), and miniaturization step, and other than that, it can be carried out by the same method as the first manufacturing form.
[0154] In addition, it may be a hydrophobically modified cellulose fiber obtained by combining the aspects A and B, that is, a hydrophobically modified cellulose fiber having a modifying group linked via an ionic bond and a modifying group linked via an amide bond. In this case, either step (2A) or step (2B) may be performed first.
[0155] In this way, hydrophobically modified cellulose fibers in which the modifying groups are linked to the cellulose fibers via ionic bonds and / or covalent bonds can be obtained.
[0156] <Hydrophobic modified cellulose fiber (B) (etherified cellulose fiber)>
[0157] The hydrophobically modified cellulose fiber (B) (also referred to as etherified cellulose fiber) of the present invention is characterized in that a modifying group is bonded to the surface of the cellulose fiber via an ether bond, and preferably has a cellulose I-type crystal structure. In this specification, "bonded via an ether bond" means a state in which the modifying group reacts with the hydroxyl group on the surface of the cellulose fiber to form an ether bond.
[0158] The modifying group in the etherified cellulose fiber is preferably a hydrocarbon group which may have a substituent. Here, among the hydrocarbon groups which may have a substituent, examples of the hydrocarbon group include: a saturated or unsaturated straight-chain or branched aliphatic hydrocarbon group, an aromatic hydrocarbon group such as a phenyl group, or an alicyclic hydrocarbon group such as a cyclohexyl group. In addition, among the hydrocarbon groups which may have a substituent in the present invention, examples of the substituent include: a halogen atom, an oxyalkylene group such as an oxyethylene group, and a hydroxyl group.
[0159] As a preferred embodiment of such etherified cellulose fibers (referred to as "embodiment 1"), for example, the following can be cited: cellulose fibers are bonded to one or more substituents selected from the substituents represented by the following general formula (1) and the substituents represented by the following general formula (2) via ether bonds, and have a cellulose I type crystal structure.
[0160] -CH2-CH(R0)-R1 (1)
[0161] -CH2-CH(R0)-CH2-(OA) n -O-R1 (2)
[0162] [In the formulae, R0 in the general formula (1) and the general formula (2) represents a hydrogen atom or a hydroxyl group, R1 each independently represents a linear or branched alkyl group having 3 or more and 30 or less carbon atoms, n in the general formula (2) represents a number from 0 to 50 or less, and A represents a linear or branched divalent saturated hydrocarbon group having 1 or more and 6 or less carbon atoms]
[0163] As a specific example of embodiment 1, for example, etherified cellulose fibers represented by the following general formula (4) can be exemplified.
[0164] [Chemical formula 2]
[0165]
[0166] [In the formula, R is the same or different and represents hydrogen or a substituent selected from the substituent represented by the above general formula (1) and the substituent represented by the above general formula (2), and m is preferably an integer of 20 to 3000, except when all R are simultaneously hydrogen]
[0167] The etherified cellulose fiber represented by the general formula (4) has a repeating structure of cellulose units into which the above-mentioned substituents are introduced. m in the general formula (4) as the number of repetitions of the repeating structure is preferably an integer of 20 to 3000 from the viewpoint of synovial surface properties.
[0168] (Hydrocarbon group which may have a substituent)
[0169] The etherified cellulose fiber of embodiment 1 is introduced with one or more substituents selected from the substituents represented by the above general formula (1) and the following general formula (2) either alone or in any combination. When the introduced substituents are from any of the above substituent groups, the same substituent or a combination of two or more substituents from each substituent group may be introduced.
[0170] From the viewpoint of the synovial fluid surface properties, R0 in the general formula (1) and the general formula (2) is preferably a hydroxyl group.
[0171] From the viewpoint of the surface properties of the synovial fluid, the carbon number of R1 in the general formula (1) is preferably 25 or less. Specific examples include propyl, butyl, pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, undecyl, dodecyl, hexadecyl, octadecyl, isooctadecyl, eicosyl, triacontyl and the like.
[0172] The carbon number of R1 in the general formula (2) is preferably 4 or more from the viewpoint of synovial surface properties, and preferably 27 or less from the viewpoint of improving synovial surface properties, availability and reactivity. Specific examples thereof include the same as those of R1 in the general formula (1).
[0173] A in the general formula (2) forms an oxyalkylene group with the adjacent oxygen atom. The carbon number of A is preferably 2 or more from the viewpoints of synovial surface properties, availability and cost, and preferably 4 or less from the same viewpoints. Specifically, methylene, ethylene, propylene, butylene, pentylene, hexylene and the like can be exemplified.
[0174] In the general formula (2), n represents the number of added moles of alkylene oxide. n is preferably 3 or more from the viewpoints of synovial surface properties, availability and cost, and is preferably 40 or less from the same viewpoints.
[0175] The combination of A and n in the general formula (2) is preferably a combination in which A is a linear or branched divalent saturated hydrocarbon group having 2 to 3 carbon atoms and n is 0 to 20 from the viewpoint of synovial surface properties.
[0176] Specific examples of the substituent represented by the general formula (1) include pentyl, hexyl, octyl, 2-ethylhexyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, isooctyl, eicosyl, propyl hydroxyethyl, butyl hydroxyethyl, pentyl hydroxyethyl, hexyl hydroxyethyl, heptyl hydroxyethyl, octyl hydroxyethyl, 2-ethylhexyl hydroxyethyl, nonyl hydroxyethyl, decyl hydroxyethyl, undecyl hydroxyethyl, dodecyl hydroxyethyl, hexadecyl hydroxyethyl, octadecyl hydroxyethyl, isooctyl hydroxyethyl, eicosyl hydroxyethyl, triacontyl hydroxyethyl and the like.
[0177] Specific examples of the substituent represented by the general formula (2) include 3-butoxy-2-hydroxy-propyl, 3-hexyloxy-2-hydroxy-propyl, 3-hexyloxy-2-hydroxy-propyl, 3-octyloxy-2-hydroxy-propyl, 3-octyloxy-2-hydroxy-propyl, 6-ethyl-3-hexyloxy-2-hydroxy-propyl, 6-ethyl-3-hexyloxy-2-hydroxy-propyl, 3-dec ... The present invention also includes 3-hydroxy-2-hydroxy-propyl, 3-decyloxy-2-hydroxy-propyl, 3-undecyloxy-2-hydroxy-propyl, 3-dodecyloxy-2-hydroxy-propyl, 3-dodecyloxy-2-hydroxy-propyl, 3-hexadecyloxy-2-hydroxy-propyl, 3-hexadecyloxy-2-hydroxy-propyl, 3-octadecyloxy-2-hydroxy-propyl, and the like. The number of moles of alkylene oxide added may be 0 or more and 50 or less, and examples thereof include substituents having alkylene oxides such as ethylene oxide and the like, wherein the number of moles of alkylene oxide added is 10, 12, 13, or 20.
[0178] (Introduction rate)
[0179] In the etherified cellulose fiber, the introduction rate of the modifying group relative to 1 mol of the anhydroglucose unit of cellulose depends on the type of the modifying group and cannot be generalized. From the viewpoint of synovial surface properties, it is preferably 0.0001 mol or more, and from the viewpoint of having a cellulose I-type crystal structure and synovial surface properties, it is preferably 1.5 mol or less. Here, when both the substituent represented by the general formula (1) and the substituent represented by the general formula (2) are introduced as modifying groups at the same time, the total introduction molar rate is indicated. Furthermore, in this specification, the introduction rate of the modifying group in the etherified cellulose fiber can be measured according to the method described in the following Examples.
[0180] (Average fiber diameter)
[0181] The average fiber diameter of the etherified cellulose fibers in the present invention is not particularly limited regardless of the type of the substituent, and examples thereof include an embodiment in which the average fiber diameter is on the order of micrometers and an embodiment in which the average fiber diameter is on the order of nanometers.
[0182] The etherified cellulose fibers in the micron order are preferably 5 μm or more from the viewpoints of synovial surface properties, operability, availability, and cost. In addition, the upper limit is not particularly set, but from the viewpoints of synovial surface properties and operability, it is preferably 100 μm or less. In this specification, the average fiber diameter of the micron-order cellulose fibers can be measured by the same method as the average fiber diameter of the raw material cellulose fibers.
[0183] The nano-scale etherified cellulose fibers are preferably 1 nm or larger in terms of synovial surface properties, operability, availability, and cost, and preferably 500 nm or smaller in terms of synovial surface properties and operability. In this specification, the average fiber diameter of nano-scale cellulose fibers can be measured by the same method as the average fiber diameter of anion-modified cellulose fibers.
[0184] [Method for producing etherified cellulose fibers]
[0185] As described above, the etherified cellulose fiber of the present invention has a modifying group, preferably the above-mentioned hydrocarbon group which may have a substituent, bonded to the surface of the cellulose fiber via an ether bond, and the introduction of the modifying group can be carried out by a known method and is not particularly limited. A specific example of the method for producing the etherified cellulose fiber of embodiment 1 is described below.
[0186] As a specific example of the method for producing the etherified cellulose fibers of the embodiment 1, there is mentioned an embodiment in which the cellulose fibers as the above-mentioned raw material are reacted with a specific compound in the presence of an alkali.
[0187] In addition, from the viewpoint of reducing the number of manufacturing steps, cellulose fibers that have been previously micronized can be used as raw materials. In this case, the average fiber diameter is preferably 1 nm or more from the viewpoint of availability and cost. In addition, the upper limit is not particularly set, but from the viewpoint of operability, it is preferably 500 nm or less.
[0188] (Alkali)
[0189] In the present production method, an alkali is mixed with the above-mentioned raw material cellulose fibers.
[0190] The base is not particularly limited, but is preferably one or more selected from alkali metal hydroxides, alkaline earth metal hydroxides, primary to tertiary amines, quaternary ammonium salts, imidazole and its derivatives, pyridine and its derivatives, and alkoxides from the viewpoint of promoting the etherification reaction.
[0191] Examples of the alkali metal hydroxide and alkaline earth metal hydroxide include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, and barium hydroxide.
[0192] The primary to tertiary amines refer to primary amines, secondary amines and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine, and triethylamine.
[0193] Examples of the quaternary ammonium salt include tetrabutylammonium hydroxide, tetrabutylammonium chloride, tetrabutylammonium fluoride, tetrabutylammonium bromide, tetraethylammonium hydroxide, tetraethylammonium chloride, tetraethylammonium fluoride, tetraethylammonium bromide, tetramethylammonium hydroxide, tetramethylammonium chloride, tetramethylammonium fluoride, and tetramethylammonium bromide.
[0194] Examples of imidazole and derivatives thereof include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.
[0195] Examples of pyridine and derivatives thereof include N,N-dimethyl-4-aminopyridine and picoline.
[0196] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium tert-butoxide.
[0197] The amount of the base is preferably 0.01 equivalent or more relative to the anhydroglucose unit of the raw material cellulose fiber from the viewpoint of promoting the etherification reaction, and is preferably 10 equivalents or less from the viewpoint of production cost.
[0198] Furthermore, the mixing of the above-mentioned raw material cellulose fiber and the alkali may be carried out in the presence of a solvent. The solvent is not particularly limited, and examples thereof include water, isopropyl alcohol, tert-butyl alcohol, dimethylformamide, toluene, methyl isobutyl ketone, acetonitrile, dimethyl sulfoxide, dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, hexane, 1,4-dioxane, and mixtures thereof.
[0199] The temperature and time for mixing the raw material cellulose fibers and the alkali are not particularly limited as long as they can be mixed uniformly.
[0200] Next, a compound for introducing a modifying group, preferably a compound for introducing a hydrocarbon group which may have a substituent, is added to the mixture of the raw cellulose fiber and the alkali obtained above, and the raw cellulose fiber is reacted with the compound. As the compound, there is no particular limitation as long as one or more substituents preferably selected from the substituents represented by the general formula (1) and the substituents represented by the general formula (2) can be bonded to the cellulose fiber via an ether bond when reacting with the raw cellulose fiber. In the present invention, from the perspective of reactivity and non-halogen compounds, it is preferred to use a compound having a cyclic structural group which is reactive, and more preferably a compound having an epoxy group. The following illustrates each compound.
[0201] As compounds that can bond the substituent represented by the general formula (1) to the cellulose fiber via an ether bond, for example, an oxyalkylene compound represented by the following general formula (1A) and an alkyl halide represented by the general formula (1B) are preferred. The compound can be prepared by a known technique or a commercially available product. The total carbon number of the compound is preferably 3 or more from the viewpoint of the synovial surface property, and is preferably 32 or less from the viewpoint of the synovial surface property.
[0202] [Chemical formula 3]
[0203]
[0204] [In the formula, R1 represents a linear or branched alkyl group having 3 or more and 30 or less carbon atoms]
[0205] X-(CH2)2-R1 (1B)
[0206] [In the formula, R1 represents a linear or branched alkyl group having 3 or more and 30 or less carbon atoms, and X is a halogen atom selected from fluorine, chlorine, bromine, and iodine]
[0207] The carbon number of R1 in the general formula (1A) and (1B) is preferably 4 or more from the viewpoint of synovial surface properties, and preferably 25 or less from the viewpoint of synovial surface properties. Specifically, the substituents described in the R1 term in the general formula (1) are mentioned.
[0208] Specific examples of the compound represented by the general formula (1A) include 1,2-epoxyhexane, 1,2-epoxydecane, and 1,2-epoxyoctadecane.
[0209] Specific examples of the compound represented by the general formula (1B) include 1-chloropentane, 1-chlorohexane, 1-chlorooctane, 1-chlorodecane, 1-chlorododecane, 1-chlorohexadecane, 1-chlorooctadecane, 1-bromopentane, 1-bromohexane, 1-bromooctane, 1-bromodecane, 1-bromodedodecane, 1-bromohexadecane, 1-bromooctadecane, 1-iodopentane, 1-iodohexane, 1-iodooctane, 1-iododecane, 1-iodododecane, 1-iodohexadecane, and 1-iodooctadecane.
[0210] As a compound that can bond the substituent represented by the general formula (2) to the cellulose fiber via an ether bond, for example, a glycidyl ether compound represented by the following general formula (2A) is preferred. The compound can be prepared by a known technique or a commercially available product. The total carbon number of the compound is preferably 5 or more from the viewpoint of synovial surface properties, and preferably 100 or less from the viewpoint of synovial surface properties.
[0211] [Chemical formula 4]
[0212]
[0213] [In the formula, R1 represents a linear or branched alkyl group having 3 to 30 carbon atoms, A represents a linear or branched divalent saturated hydrocarbon group having 1 to 6 carbon atoms, and n represents a number of 0 to 50.]
[0214] The carbon number of R1 in the general formula (2A) is preferably 4 or more from the viewpoint of synovial surface properties, and preferably 27 or less. Specifically, the substituents described in the R1 term in the general formula (2) are mentioned.
[0215] A in the general formula (2A) forms an oxyalkylene group with the adjacent oxygen atom. The carbon number of A is preferably 2 or more from the viewpoint of availability and cost, and preferably 4 or less from the same viewpoint. Specifically, the substituents described in the A item in the general formula (2) can be exemplified, among which ethylene and propylene are preferred, and ethylene is more preferred.
[0216] n in the general formula (2A) represents the number of added moles of alkylene oxide. n is preferably 3 or more from the viewpoint of availability and cost, and is preferably 40 or less from the viewpoint of the same.
[0217] Specific examples of the compound represented by the general formula (2A) include butyl glycidyl ether, 2-ethylhexyl glycidyl ether, dodecyl glycidyl ether, stearyl glycidyl ether, isostearyl glycidyl ether, and polyoxyalkylene alkyl ether.
[0218] The amount of the compound used to introduce the modifying group can be determined according to the desired introduction rate of the modifying group in the obtained etherified cellulose fibers, and is preferably 0.01 equivalents or more from the viewpoint of reactivity, and preferably 10 equivalents or less from the viewpoint of manufacturing cost, relative to the anhydroglucose unit of the raw material cellulose fibers.
[0219] (Etherification reaction)
[0220] The etherification reaction of the above compound and the raw material cellulose fiber can be carried out by mixing the two in the presence of a solvent. The solvent is not particularly limited, and the above-mentioned exemplary solvents that can be used in the presence of a base can be used.
[0221] The amount of the solvent used depends on the type of raw material cellulose fibers or the compound used to introduce the modifying group and cannot be generalized, but is preferably 30 parts by mass or more from the viewpoint of reactivity and preferably 10,000 parts by mass or less from the viewpoint of productivity, relative to 100 parts by mass of the raw material cellulose fibers.
[0222] The mixing conditions are not particularly limited as long as the raw material cellulose fibers or the compound for introducing the modifying group can be uniformly mixed to allow the reaction to proceed sufficiently, and continuous mixing treatment may or may not be performed. When a relatively large reaction vessel such as one exceeding 1 L is used, appropriate stirring may be performed from the viewpoint of controlling the reaction temperature.
[0223] The reaction temperature depends on the type of raw material cellulose fiber or the compound for introducing the modifying group and the target introduction rate, and cannot be generalized. From the viewpoint of improving reactivity, it is preferably 40°C or higher, and from the viewpoint of suppressing thermal decomposition, it is preferably 120°C or lower.
[0224] The reaction time depends on the type of raw material cellulose fiber or the compound for introducing the modifying group and the target introduction rate, and cannot be generalized, but is preferably 0.5 hours or longer from the viewpoint of reactivity and preferably 60 hours or shorter from the viewpoint of productivity.
[0225] After the reaction, post-treatment may be appropriately performed to remove unreacted compounds, bases, etc. If necessary, drying (vacuum drying, etc.) may be further performed.
[0226] In this way, etherified cellulose fibers were obtained.
[0227] Regardless of the above-mentioned hydrophobically modified cellulose fibers (A) or (B), the obtained hydrophobically modified cellulose fibers can be used in the state of a dispersion after the above-mentioned post-treatment, or can be used in the state of a dry powdered hydrophobically modified cellulose fibers obtained by removing the solvent from the dispersion by drying treatment, etc. Here, the so-called "powdered state" means a powdered state in which the hydrophobically modified cellulose fibers are aggregated, and does not mean cellulose particles.
[0228] Examples of the powdered hydrophobic modified cellulose fibers include: a dried product obtained by directly drying the above-mentioned dispersion of cellulose fibers; a product obtained by mechanically treating the dried product to form a powder; a product obtained by powdering the above-mentioned dispersion of cellulose fibers by a known spray drying method; a product obtained by powdering the above-mentioned dispersion of cellulose fibers by a known freeze drying method, etc. The above-mentioned spray drying method is a method of spraying the above-mentioned dispersion of cellulose fibers in the air to dry it.
[0229] The average fiber diameter of the obtained fine cellulose fibers is preferably 0.1 nm or more, more preferably 0.5 nm or more, further preferably 1 nm or more, further preferably 2 nm or more, further more preferably 3 nm or more, from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the flowing object. In addition, from the same viewpoint, it is preferably 100 nm or less, more preferably 50 nm or less, further preferably 20 nm or less, further preferably 10 nm or less, further preferably 6 nm or less, further more preferably 5 nm or less.
[0230] The length (average fiber length) of the obtained fine cellulose fibers is preferably 150 nm or more, more preferably 200 nm or more, from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the fluid. From the same viewpoint, it is preferably 1000 nm or less, more preferably 750 nm or less, further preferably 500 nm or less, further preferably 400 nm or less.
[0231] In the present invention, the average fiber diameter and average fiber length of the cellulose fibers are not limited to the above ranges, and for example, micron-order cellulose fibers may be used.
[0232] In addition, the average aspect ratio (fiber length / fiber diameter) of the obtained fine cellulose fibers is preferably 1 or more, more preferably 10 or more, further preferably 20 or more, further preferably 40 or more, further preferably 50 or more, from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the flowing object, and preferably 150 or less, more preferably 140 or less, further preferably 130 or less, further preferably 100 or less, further preferably 95 or less, further preferably 90 or less from the same viewpoint. In addition, when the average aspect ratio is within the above range, from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the flowing object, the standard deviation of the aspect ratio is preferably 60 or less, more preferably 50 or less, further preferably 45 or less, and the lower limit is not particularly set, and from the viewpoint of economic efficiency, it is preferably 4 or more. The fine cellulose fibers with the above low aspect ratio are not only excellent in heat resistance, but also excellent in dispersibility in the resin composition, and a resin composition with high mechanical strength and not prone to brittle failure can be obtained.
[0233] <Oil with SP value of 10 or less>
[0234] In the present invention, an oil having an SP value of 10 or less as defined above is used as the lubricating oil constituting the film.
[0235] The SP value in this specification refers to the solubility parameter (unit: (cal / cm 3 ) 1 / 2 ), for example, in the references “SP value foundation, application and calculation method” (Information Research Institute, 2005), Polymer handbook Third edition (A Wiley-Interscience publication, 1989), etc.
[0236] The mass average molecular weight of the oil having an SP value of 10 or less is not particularly limited, but is preferably 100 or more, and is preferably 100,000 or less, more preferably 50,000 or less, and further preferably 20,000 or less.
[0237] The amount of the oil having an SP value of 10 or less in the film of the present invention is not particularly limited, and from the viewpoint of the mobility of the oil and the durability of the film, preferably 50% by mass or more, more preferably 55% by mass or more, and then preferably 60% by mass or more. In addition, from the same viewpoint, preferably 98% by mass or less, more preferably 97% by mass or less, and then preferably 96% by mass or less. When there are two or more situations in which the oil having an SP value of 10 or less exists, the amount of the oil having an SP value of 10 or less is the total amount of each oil.
[0238] The mass ratio of the cellulose fiber in the hydrophobically modified cellulose fiber in the film of the present invention to the oil having an SP value of 10 or less (cellulose fiber: oil having an SP value of 10 or less) is not particularly limited, but is preferably 1:1 or more, more preferably 1:2 or more, and further preferably 1:3 or more from the viewpoint of exerting the following synovial surface properties. In addition, from the viewpoint of the durability of the film, it is preferably 1:100 or less, more preferably 1:50 or less, and further preferably 1:20 or less. Furthermore, the amount of the cellulose fiber in the hydrophobically modified cellulose fiber can be obtained as a converted amount according to the method described in the following Examples.
[0239] Examples of the oil having an SP value of 10 or less used in the present invention include oleic acid (SP value: 9.2), D-limonene (SP value: 9.4), PEG400 (SP value: 9.4), dimethyl succinate (SP value: 9.9), neopentyl glycol dicaprate (SP value: 8.9), hexyl laurate (SP value: 8.6), isopropyl laurate (SP value 8.5), isopropyl myristate (SP value 8.5), isopropyl palmitate (SP value 8.5), isopropyl oleate (SP value: 8.6), hexadecane (SP value: 8.0), olive oil (SP value: 9.3), jojoba oil (SP value: 8.6), squalane (SP value: 7.9), liquid paraffin (SP value: 7.9), Fluorinert FC-40 (manufactured by 3M, SP value: 6.1), Fluorinert FC-43 (manufactured by 3M Co., Ltd., SP value: 6.1), Fluorinert FC-72 (manufactured by 3M Co., Ltd., SP value: 6.1), Fluorinert FC-770 (manufactured by 3M Co., Ltd., SP value: 6.1), KF96-1cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96-10cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96-50cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96-100cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96-1000cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), etc. Among them, the SP value of the oil is preferably 9.5 or less, more preferably 9.0 or less, and further preferably 8.5 or less from the viewpoint of the surface property of the synovial fluid and the suppression of the migration of the oil to the fluid.
[0240] <Polymer compounds>
[0241] From the viewpoint of suppressing the migration of oil having an SP value of 10 or less into the fluid and improving the durability of the membrane, the membrane of the present invention preferably contains a polymer compound in addition to the above-mentioned components.
[0242] The polymer compound constituting the membrane of the present invention is one or more polymer compounds selected from the following (X) and (Y). From the viewpoint of suppressing the migration of oil having an SP value of 10 or less into the fluid and the durability of the membrane, the polymer compound (X) is preferred.
[0243] (X) a polycondensation polymer having an ester group, an amide group, a carbamate group, an imine group, an ether group or a carbonate group
[0244] (Y) a methacrylic or acrylic polymer having an ester group or an amide group in a side chain
[0245] From the viewpoint of the mobility of the oil with an SP value of less than 10 and the durability of the film, the above-mentioned polymer compound preferably contains a polymer component with a molecular weight of more than 100,000. Regarding the amount of such a polymer component in the polymer compound, from the same viewpoint, preferably more than 1% by mass, more preferably more than 5% by mass, and further preferably more than 10% by mass, and further preferably more than 15% by mass, from the same viewpoint, preferably less than 50% by mass, more preferably less than 45% by mass, and further preferably less than 40% by mass, and further preferably less than 35% by mass. The mass average molecular weight of the polymer compound or the amount of the polymer component with a molecular weight of more than 100,000 in the polymer compound can be measured according to the method described in the following examples.
[0246] The mass average molecular weight of the polymer compound is preferably 1,000 or more from the viewpoint of oil mobility and film durability at an SP value of 10 or less, and is preferably 500,000 or less from the same viewpoint.
[0247] Examples of the polycondensation polymer (X) having an ester group include condensates of dicarboxylic acids such as adipic acid, sebacic acid, dodecanedioic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, and alkenylsuccinic acid, and diols such as ethylene glycol, propylene glycol, and butanediol.
[0248] Examples of the polycondensation polymer (X) having an amide group include condensates of diamines such as dicarboxylic acids such as adipic acid, sebacic acid, dodecanedioic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, and alkenylsuccinic acid, and aliphatic diamines such as ethylenediamine, hexamethylenediamine, and propylenediamine.
[0249] Examples of the polycondensation polymer (X) having a urethane group include condensates of diisocyanates such as tolylene diisocyanate, diphenyl isocyanate, xylylene diisocyanate, and hexamethylene diisocyanate, and diols such as ethylene glycol, propylene glycol, and butanediol.
[0250] Examples of the polycondensation polymer (X) having an imino group include condensates of hydrocarbon imines such as ethyleneimine, propyleneimine, butyleneimine, dimethylethyleneimine, pentyleneimine, and hexyleneimine, and melamine-formamide condensates.
[0251] Examples of the polycondensation polymer (X) having an ether group include condensates of alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide, condensates of epichlorohydrin and bisphenol A, and condensates of formaldehyde.
[0252] Examples of the polycondensation polymer (X) having a carbonate group include condensates of polyols such as 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane and 1,1-bis(4-hydroxyphenyl)cyclohexane with phosgene.
[0253] From the viewpoint of the mobility of oil having an SP value of 10 or less and the durability of the film, the polycondensation polymer (X) preferably further contains a trifunctional or higher-functional monomer as a structural unit.
[0254] Examples of trifunctional or higher monomers include trifunctional or higher amines such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, di(methylethylene)triamine, dibutylenetriamine, tributylenetetramine, and pentamethylenehexamine; trifunctional or higher alcohols such as trimethylol, trimethylolpropane, glycerol, pentaerythritol, and di(trimethylol)propane; trimellitic acid, benzophenonetetracarboxylic acid, trimellitic anhydride, pyromellitic acid, pyrophenyl Trifunctional or higher carboxylic acids such as tetracarboxylic anhydride, benzophenonetetracarboxylic anhydride, trimesic acid, ethylene glycol bis(anhydrotrimellitate), and glycerol tri(anhydrotrimellitate) are preferred. From the viewpoint of the mobility of oils having an SP value of 10 or less and the durability of the film, trifunctional or higher amines such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, di(methylethylene)triamine, dibutylenetriamine, tributylenetetramine, and pentamethylenehexamine are preferred.
[0255] The polycondensation polymer (X) is considered to form crosslinking points by further including a trifunctional or higher-functional monomer as a structural unit, and the formation of crosslinking points improves the mobility of oils having an SP value of 10 or less and the durability of the membrane.
[0256] The content of trifunctional or higher monomers in the polycondensation polymer (X) is preferably 0.2 mol% or more, more preferably 0.5 mol% or more, and further preferably 2.5 mol% or more, from the viewpoint of the mobility of oils with an SP value of 10 or less and the durability of the film. From the viewpoint of the mobility of oils with an SP value of 10 or less, it is preferably 25 mol% or less, more preferably 20 mol% or less, and further preferably 15 mol% or less.
[0257] The polycondensation polymer (X) is preferably a polymer compound selected from one or more of the following (a) and (b) from the viewpoint of the mobility of oil with an SP value of less than 10 and the durability of the membrane, and is more preferably a polyamide compound of (a) from the viewpoint of suppressing the migration of oil with an SP value of less than 10 to the fluid and the durability of the membrane.
[0258] (a) Polyamide compounds
[0259] (b) Polyalkyleneimine compounds
[0260] (a) Polyamide compounds
[0261] As a polyamide compound, as long as it is a polymer compound without a cellulose structure and having an amide bond (-CONH-), a polyamide compound with any chemical structure can be used. The polyamide compound can be, for example, a nylon mainly containing an aliphatic skeleton, or an aromatic polyamide mainly having an aromatic skeleton. Furthermore, it can also be a person having a skeleton structure other than the two. On the other hand, as a structure preferably used, there can be listed: a polyamide containing a diamine and a carboxylic acid selected from one or more of a monocarboxylic acid, a dicarboxylic acid and a polymerized fatty acid.
[0262] The mass average molecular weight of the polyamide compound is preferably 5,000 or more, more preferably 10,000 or more, further preferably 20,000 or more, further preferably 30,000 or more, from the viewpoint of the mobility of oil with an SP value of 10 or less and the durability of the film. From the same viewpoint, it is preferably 500,000 or less, more preferably 250,000 or less, further preferably 100,000 or less, further preferably 50,000 or less.
[0263] Polyamide compounds are generally obtained by ring-opening polymerization of cyclic lactams, self-condensation of amino acids or their derivatives, polycondensation of carboxylic acids and amine compounds, etc. The polyamide compound obtained by the polycondensation of carboxylic acids and amine compounds can be obtained, for example, by condensation (polycondensation) of carboxylic acids and amine compounds.
[0264] As the carboxylic acid which is one of the raw materials for the polycondensation reaction, monocarboxylic acids, dicarboxylic acids and polymerized fatty acids can be preferably used.
[0265] Examples of the monocarboxylic acid include acetic acid, propionic acid, butyric acid, valeric acid, lauric acid, palmitic acid, stearic acid, eicosanoic acid, and behenic acid, which function as polymerization terminators in the reaction of producing the polyamide compound. In addition, examples of the unsaturated aliphatic monocarboxylic acid include oleic acid, linoleic acid, linolenic acid, eicosenoic acid, erucic acid, and mixed fatty acids obtained from natural oils and fats (tall oil fatty acid, rice bran fatty acid, soybean oil fatty acid, tallow fatty acid, etc.), and the like, which may be used alone or in combination of two or more.
[0266] From the viewpoint of the mobility of oil having an SP value of 10 or less and the durability of the film, the monocarboxylic acid used in the present invention is preferably a monocarboxylic acid having 8 to 24 carbon atoms, more preferably a monocarboxylic acid having 10 to 22 carbon atoms, and still more preferably a monocarboxylic acid having 12 to 18 carbon atoms.
[0267] Examples of the dicarboxylic acid include adipic acid, sebacic acid, dodecanedioic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, and alkenylsuccinic acid. As the alkenylsuccinic acid, it is preferred that the alkenyl group has 4 to 20 carbon atoms.
[0268] The so-called polymerized fatty acid is a polymer obtained by polymerizing a monobasic fatty acid having an unsaturated bond, or a polymer obtained by polymerizing an esterified product of a monobasic fatty acid having an unsaturated bond. Examples of the polymerized fatty acid include structures obtained by a dehydration condensation reaction of a dimer acid derived from vegetable oils and fats.
[0269] As the monobasic fatty acid having an unsaturated bond, an unsaturated fatty acid having 1 to 3 unsaturated bonds and a total carbon number of 8 to 24 is generally used. Examples of these unsaturated fatty acids include oleic acid, linolenic acid, linolenic acid, natural drying oil fatty acids, and natural semi-drying oil fatty acids. In addition, as esters of monobasic fatty acids having unsaturated bonds, esters of the above-mentioned monobasic fatty acids having unsaturated bonds and aliphatic alcohols, preferably aliphatic alcohols having 1 to 3 carbon atoms, can be listed. The above-mentioned polymerized fatty acid, which is a polymer obtained by polymerizing a monobasic fatty acid having an unsaturated bond or a polymer obtained by polymerizing an esterified product of a monobasic fatty acid having an unsaturated bond, preferably has a dimer as the main component. For example, a polymer of an unsaturated fatty acid having 18 carbon atoms can be obtained as a commercial product, and its composition is as follows: 0 to 10% by mass of a monobasic acid (monomer) having 18 carbon atoms, 60 to 99% by mass of a dibasic acid (dimer) having 36 carbon atoms, and 30% or less of an acid having a tribasic acid or more (trimer or more) having 54 carbon atoms.
[0270] Furthermore, as the carboxylic acid component, in addition to the monocarboxylic acid, dicarboxylic acid and polymerized fatty acid, other carboxylic acids may be added within a range that does not impair the physical properties of the film.
[0271] Among these carboxylic acids, a combination of a monocarboxylic acid and a polymerized fatty acid is particularly preferably used. Furthermore, the carboxylic acid may be an ester with an alcohol having 1 to 3 carbon atoms.
[0272] In addition, as for the amine compound which is another raw material of the polycondensation reaction, polyamines, aminocarboxylic acids, amino alcohols, etc. can be listed. As polyamines, aliphatic diamines such as ethylenediamine, hexamethylenediamine, and propylenediamine can be listed, polyalkylene polyamines such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, di(methylethylene)triamine, dibutylenetriamine, tributylenetetramine, and pentamethylenehexamine can be listed, aromatic diamines such as (o-, p-, or m-)phenylenediamine and diphenylmethanediamine can be listed, and alicyclic diamines such as piperazine and isophoronediamine can be listed. As aminocarboxylic acids, methylglycine, trimethylglycine, 6-aminocaproic acid, δ-aminooctanoic acid, ε-caprolactam can be listed. As amino alcohols, ethanolamine, propanolamine, etc. can be listed.
[0273] Furthermore, as the amine compound, a monoamine that functions as a polymerization terminator in a reaction for producing a polyamide compound can be used.
[0274] Each compound used as these raw materials can be used alone or in combination of two or more.
[0275] In addition, from the viewpoint of the mobility of oil with an SP value of 10 or less and the durability of the film, as the amine compound, an amine component containing a polyamine can be preferably used, and as the above-mentioned amine compound, an amine component containing a diamine and one or more selected from triamine, tetraamine, pentamine and hexatetraamine (referred to as "amine component"), or an amine component containing two or more diamines (referred to as "amine component 2") can be more preferably used. From the viewpoint of the sliding speed, the amine compound is more preferably amine component 1. As for the mass ratio of each component in amine component 1 when used in combination, from the viewpoint of the mobility of oil with an SP value of 10 or less and the durability of the film, [diamine: one or more selected from triamine, tetraamine, pentamine and hexaamine] is preferably 99.5:0.5 to 50:50, more preferably 99:1 to 60:40, and further preferably 95:5 to 70:30. As the mass ratio of each component in the amine component 2 when used together, [one diamine: another diamine] is preferably 99.5:0.5 to 50:50, more preferably 99:1 to 60:40, and further preferably 95:5 to 64:36 from the viewpoint of the mobility of oil with an SP value of 10 or less and the durability of the film. As one diamine, for example, ethylenediamine and the like are mentioned, and as the other diamine, for example, meta-xylylenediamine and the like are mentioned.
[0276] (b) Polyalkyleneimine compounds
[0277] The polyalkyleneimine compound refers to a polymer compound having a repeating unit of an alkylene group and an amino group in the main chain and having a repeating unit of the structure of the following formula (A) and / or formula (B).
[0278] [Chemical formula 5]
[0279]
[0280] In the above formula (A) and formula (B), Q represents an alkylene group. Here, examples of the alkylene group represented by Q include ethylene, propylene, butylene, etc. The alkylene group may be only one type or may be two or more types. Among them, the alkylene group is preferably ethylene. That is, the polyalkylene imine is preferably polyethylene imine.
[0281] The mass average molecular weight of the polyalkyleneimine compound is preferably 1000 or more, more preferably 2000 or more, further preferably 5000 or more, further preferably 10,000 or more, from the viewpoint of the mobility of oil with an SP value of 10 or less and the durability of the film. From the same viewpoint, it is preferably 200,000 or less, more preferably 100,000 or less, further preferably 50,000 or less, further preferably 20,000 or less.
[0282] Examples of the polymer (Y), i.e., a methacrylic or acrylic polymer having an ester group or an amide group in a side chain, include poly(meth)acrylic acid alkyl esters such as polymethyl (meth)acrylate, polyethyl (meth)acrylate, and polybutyl (meth)acrylate; and poly(meth)acrylamides such as poly(meth)acrylamide, poly-N-methyl (meth)acrylamide, poly-N,N-dimethyl (meth)acrylamide, and poly-N-phenyl (meth)acrylamide.
[0283] When the film of the present invention contains a macromolecular compound, the amount of the macromolecular compound in the film is not particularly limited. From the perspective of the mobility of the oil below the SP value of 10 and the durability of the film, preferably 4% by mass or more, more preferably 8% by mass or more, and then preferably 12% by mass or more, and from the perspective of the same viewpoint, preferably 30% by mass or less, more preferably 25% by mass or less, and then preferably 20% by mass or less. When the macromolecular compound is more than two kinds, the amount of the macromolecular compound is the total amount of each macromolecular compound.
[0284] The film of the present invention may also contain any component that does not impair the effect of the present invention. The content of these arbitrary components in the film is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and further preferably 0.5% by mass or more, and further preferably 20% by mass or less, more preferably 15% by mass or less, and further preferably 10% by mass or less. When there are two or more arbitrary components, the amount of the arbitrary component is the total amount of each arbitrary component.
[0285] [Method for forming a film on a molded body]
[0286] The method for forming a film on a formed body of the present invention comprises:
[0287] Step 1 of preparing a dispersion containing hydrophobically modified cellulose fibers and an oil having an SP value of 10 or less; and Step 2 of applying the dispersion prepared in step 1 to a molded body.
[0288] <Process 1>
[0289] The dispersion containing the hydrophobically modified cellulose fibers and the oil having an SP value of 10 or less can be prepared by mixing these components with a solvent.
[0290] Examples of the solvent include isopropyl alcohol, ethanol, and methyl ethyl ketone.
[0291] As mixing conditions of these components, for example, 15 to 35° C. and, further, 10 to 60 minutes are preferred as mixing time.
[0292] <Process 2>
[0293] The dispersion obtained in step 1 is applied to a molded body having a solid surface such as glass or resin. Examples of the coating method include a coating method using an applicator, a rod coater, a spin coater, etc. The thickness of the coating film on the molded body is preferably 10 μm or more, more preferably 20 μm or more, and further preferably 30 μm, from the viewpoint of sliding speed and durability, and is preferably 2000 μm or less, more preferably 1500 μm or less, and further preferably 1200 μm or less from the viewpoint of coating properties.
[0294] Next, the coating is dried to obtain a film. The drying conditions may be under reduced pressure or normal pressure, and the temperature range is preferably 15 to 75° C. The drying time is preferably 1 to 24 hours.
[0295] In this way, a film, preferably a synovial surface film, is formed to obtain a shaped body having a film.
[0296] [molded body]
[0297] The molded body having a film can be produced in the above manner, and the molded body having a film is included in the present invention.
[0298] By applying the film of the present invention, preferably the synovial surface film, to a solid surface as described above, the solid surface can be modified into a synovial surface. Therefore, the present invention includes the above-mentioned film for modifying a solid surface into a synovial surface. The film of the present invention not only has a high effect of preventing the adhesion of oily components, but also can maintain this effect for a long time, and therefore can be preferably used for various purposes, such as packaging materials for daily necessities, cosmetics, home appliances, etc., packaging containers such as bubble wrap or trays, lunch box lids, food containers, industrial pallets for transporting or protecting industrial parts, etc.
[0299] [Dispersion for membranes]
[0300] As one embodiment of the present invention, a film dispersion is provided, which comprises hydrophobically modified cellulose fibers having a modifying group bonded to one or more groups selected from anionic groups and hydroxyl groups of the cellulose fibers, and an oil having an SP value of 10 or less. The film dispersion can be provided in the form of a coating liquid for forming a film, preferably a synovial surface film. The film dispersion may also contain the solvent or other components listed in the above-mentioned [Method for forming a film on a molded body] as needed.
[0301] About the content of the hydrophobic modified cellulose fiber in the dispersion for film, from the viewpoint of suppressing the movement of the oil below SP value 10 and durability, preferably 0.2 mass % or more, more preferably 0.3 mass % or more, and then preferably 0.4 mass % or more. In addition, from the same viewpoint, preferably 15 mass % or less, more preferably 10 mass % or less, and then preferably 5 mass % or less.
[0302] The content of the oil having an SP value of 10 or less in the dispersion for film is preferably 4.0% by mass or more, more preferably 5.0% by mass or more, and further preferably 6.0% by mass or more from the viewpoint of the migration inhibition and durability of the oil. In addition, from the same viewpoint, it is preferably 40% by mass or less, more preferably 20% by mass or less, and further preferably 15% by mass or less.
[0303] The content of the solvent in the film dispersion is preferably 80.0% by mass or more, more preferably 85.0% by mass or more, and further preferably 88.0% by mass or more, from the viewpoint of fully dispersing the hydrophobic modified cellulose fibers, etc. In addition, from the viewpoint of shortening the film-forming time, it is preferably 92.8% by mass or less, more preferably 91.7% by mass or less, and further preferably 90.6% by mass or less.
[0304] When the film dispersion contains a polymer compound, the content of the polymer compound in the film dispersion is preferably 0.8% by mass or more, more preferably 1.0% by mass or more, and further preferably 1.2% by mass or more from the viewpoint of suppressing the migration and durability of oil having an SP value of less than 10. In addition, from the same viewpoint, it is preferably 3.0% by mass or less, more preferably 2.5% by mass or less, and further preferably 2.0% by mass or less.
[0305] The above-mentioned dispersion may also contain any component that does not impair the effect of the present invention. The content of these optional components in the dispersion is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and further preferably 0.5% by mass or more, and further preferably 20% by mass or less, more preferably 15% by mass or less, and further preferably 10% by mass or less. When there are two or more optional components, the amount of the optional components is the total amount of each optional component.
[0306] With regard to the above-mentioned embodiments, the present invention further discloses the following film, a molded body having the film, a method for forming a film on a molded body, and a dispersion for a film.
[0307] <1> A film comprising:
[0308] Hydrophobically modified cellulose fibers in which a modifying group is bonded to one or more groups selected from anionic groups and hydroxyl groups of the cellulose fibers, and an oil having an SP value of 10 or less.
[0309] <2> The film as described in <1>, wherein the preferred surface hardness of the film is 0.1 (N / mm) in terms of Martens hardness (HM) when measured using a microhardness tester. 2 )above.
[0310] <3> The film as described in <1> or <2>, wherein the arithmetic mean roughness of the film is preferably 0.3 μm or more, more preferably 0.5 μm or more, and further preferably 0.8 μm or more, and is preferably 40 μm or less, more preferably 35 μm or less, and further preferably 30 μm or less.
[0311] <4> The film as described in any one of <1> to <3>, wherein the thickness of the film is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more, and is preferably 2000 μm or less, more preferably 1200 μm or less, further preferably 500 μm or less, and further preferably 100 μm or less.
[0312] <5> The film according to any one of <1> to <4>, wherein the film has a sliding angle of preferably 80° or less, more preferably 50° or less, and still more preferably 40° or less.
[0313] <6> A membrane as described in any one of <1> to <5>, wherein the sliding speed of the membrane is preferably 1.5 cm / minute or more, more preferably 2.0 cm / minute or more, and further preferably 2.5 cm / minute or more, and further, the sliding speed during the fifth measurement is preferably 1.5 cm / minute or more, more preferably 2.0 cm / minute or more, and further preferably 2.5 cm / minute or more.
[0314] <7> The film according to any one of <1> to <6>, wherein the lubricant oil transfer rate of the film is preferably 10.0% or less, more preferably 7.5% or less, further preferably 5.0% or less, and further preferably 0%.
[0315] <8> A membrane as described in any one of <1> to <7>, wherein the hydrophobic modified cellulose fiber is a cellulose fiber having a modifying group bonded to one or more groups selected from anionic groups and hydroxyl groups of the cellulose fiber, preferably a cellulose fiber having a modifying group bonded to anionic groups of the cellulose fiber, and more preferably a cellulose fiber having a carboxyl group as the anionic group and a modifying group bonded to the carboxyl group of the cellulose fiber.
[0316] <9> The film according to any one of <1> to <8>, wherein the degree of crystallinity of the hydrophobically modified cellulose fiber is preferably 10% or more and preferably 90% or less.
[0317] <10> The film according to any one of <1> to <9>, wherein the preferred ranges of the average fiber diameter and average fiber length of the hydrophobically modified cellulose fibers are the same as the preferred ranges of the average fiber diameter and average fiber length of the fine cellulose fibers.
[0318] <11> A film as described in any one of <1> to <10>, wherein the amount of hydrophobic modified cellulose fibers in the film is preferably 1 mass % or more, more preferably 3 mass % or more, and further preferably 4 mass % or more, and is preferably 40 mass % or less, more preferably 35 mass % or less, and further preferably 30 mass % or less.
[0319] <12> The membrane as described in any one of <1> to <11>, wherein the hydrophobically modified cellulose fiber is preferably hydrophobically modified cellulose fiber (A) or hydrophobically modified cellulose fiber (B), more preferably hydrophobically modified cellulose fiber (A), and further preferably oxidized cellulose fiber bonded with a modifying group.
[0320] <13> A membrane as described in any one of <1> to <12>, wherein the average bonding amount of the modifying groups in the hydrophobically modified cellulose fibers (A) is preferably 0.01 mmol / g or more, more preferably 0.05 mmol / g or more, further preferably 0.1 mmol / g or more, further preferably 0.3 mmol / g or more, further preferably 0.5 mmol / g or more, and preferably 3 mmol / g or less, more preferably 2.5 mmol / g or less, further preferably 2 mmol / g or less, further preferably 1.8 mmol / g or less, further preferably 1.5 mmol / g or less.
[0321] <14> A membrane as described in any one of <1> to <13>, wherein the introduction rate of the modifying group in the hydrophobically modified cellulose fiber (A) is preferably 10% or more, more preferably 30% or more, further preferably 50% or more, further preferably 60% or more, further preferably 70% or more, and preferably 99% or less, more preferably 97% or less, further preferably 95% or less, further preferably 90% or less.
[0322] <15> A membrane as described in any one of <1> to <14>, wherein the anionic groups contained in the anionic modified cellulose fibers are preferably carboxyl groups, sulfonic acid groups and phosphoric acid groups, more preferably carboxyl groups, and further, the relative ions of the anionic groups in the anionic modified cellulose fibers are preferably sodium ions, potassium ions, calcium ions, aluminum ions and protons.
[0323] <16> A membrane as described in any one of <1> to <15>, wherein the anionic group content in the anionic modified cellulose fiber is preferably 0.1 mmol / g or more, more preferably 0.4 mmol / g or more, further preferably 0.6 mmol / g or more, further preferably 0.8 mmol / g or more, and is preferably 3 mmol / g or less, more preferably 2 mmol / g or less, further preferably 1.8 mmol / g or less.
[0324] <17> The membrane according to any one of <1> to <16>, wherein the preferred ranges of the average fiber diameter and average fiber length of the anionically modified cellulose fibers are the same as the preferred ranges of the average fiber diameter and average fiber length of the fine cellulose fibers.
[0325] <18> A membrane as described in any one of <1> to <17>, wherein the modifying group in the hydrophobically modified cellulose fiber (A) is preferably a hydrocarbon group, more preferably a hydrocarbon group such as a chain saturated hydrocarbon group, a chain unsaturated hydrocarbon group, a cyclic saturated hydrocarbon group, and an aromatic hydrocarbon group, and further preferably the carbon number of the hydrocarbon group is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more, and further preferably 30 or less, more preferably 24 or less, and further preferably 18 or less.
[0326] <19> A film as described in any one of <1> to <18>, wherein the number of carbon atoms in a modifying group of the chain saturated hydrocarbon group is preferably 1 or more, more preferably 2 or more, further preferably 3 or more, further preferably 6 or more, further preferably 8 or more, and further preferably 30 or less, more preferably 24 or less, further preferably 18 or less, further preferably 16 or less.
[0327] <20> A film as described in any one of <1> to <19>, wherein the chain saturated hydrocarbon group is preferably methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, isobutyl, pentyl, tert-pentyl, isopentyl, hexyl, isohexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, dodecyl, tridecyl, tetradecyl, octadecyl, docosyl, and octacosyl, and more preferably propyl, isopropyl, butyl, sec-butyl, tert-butyl, isobutyl, pentyl, tert-pentyl, isopentyl, hexyl, isohexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, dodecyl, tridecyl, tetradecyl, octadecyl, docosyl, and octacosyl.
[0328] <21> The film as described in any one of <1> to <20>, wherein the carbon number of the chain unsaturated hydrocarbon group is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more, and is preferably 30 or less, more preferably 18 or less, further preferably 12 or less, and further preferably 8 or less.
[0329] <22> A film as described in any one of <1> to <21>, wherein the chain unsaturated hydrocarbon group is preferably vinyl, propenyl, butenyl, isobutenyl, isoprene, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, dodecenyl, tridecenyl, tetradecenyl, and octadecenyl, and more preferably vinyl, propenyl, butenyl, isobutenyl, isoprene, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, and dodecenyl.
[0330] <23> The film as described in any one of <1> to <22>, wherein the carbon number of the cyclic saturated hydrocarbon group is preferably 3 or more, more preferably 4 or more, and further preferably 5 or more, and is preferably 20 or less, more preferably 16 or less, further preferably 12 or less, and further preferably 8 or less.
[0331] <24> A film as described in any one of <1> to <23>, wherein the cyclic saturated hydrocarbon group is preferably cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, cyclododecyl, cyclotridecyl, cyclotetradecyl, and cyclooctadecyl, and more preferably cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, and cyclododecyl.
[0332] <25> A film as described in any one of <1> to <24>, wherein the aromatic hydrocarbon group is preferably selected from an aryl group and an aralkyl group, the total carbon number of the above-mentioned aryl group is preferably 6 or more, and is preferably 24 or less, more preferably 20 or less, further preferably 14 or less, further preferably 12 or less, further preferably 10 or less, and the total carbon number of the above-mentioned aralkyl group is preferably 7 or more, more preferably 8 or more, and is preferably 24 or less, more preferably 20 or less, further preferably 14 or less, further preferably 13 or less, further preferably 11 or less.
[0333] <26> A film as described in any one of <1> to <25>, wherein the aromatic group is preferably phenyl, naphthyl, anthracenyl, phenanthrenyl, biphenyl, triphenyl, terphenyl, and groups formed by further substitution of these groups with substituents, more preferably phenyl, biphenyl, and terphenyl, and the aralkyl group is preferably benzyl, phenethyl, phenylpropyl, phenylpentyl, phenylhexyl, phenylheptyl, phenyloctyl, and groups formed by further substitution of aromatic groups of these groups with substituents, more preferably benzyl, phenethyl, phenylpropyl, phenylpentyl, phenylhexyl, and phenylheptyl.
[0334] <27> A film as described in any one of <1> to <26>, wherein the carbon number of the primary to tertiary amine is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more, and is preferably 20 or less, more preferably 18 or less, and further preferably 16 or less (excluding amino-modified polysiloxane compounds).
[0335] <28> A film as described in any one of <1> to <27>, wherein the primary to tertiary amines are preferably ethylamine, diethylamine, triethylamine, propylamine, dipropylamine, butylamine, dibutylamine, hexylamine, dihexylamine, octylamine, dioctylamine, trioctylamine, dodecylamine, didodecylamine, stearylamine, distearylamine, monoethanolamine, diethanolamine, triethanolamine, aniline, and benzylamine, as well as amino-modified polysiloxane compounds, and the quaternary ammonium compounds are preferably tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetraethylammonium chloride, tetrapropylammonium hydroxide (TPAH), tetrabutylammonium hydroxide (TBAH), tetrabutylammonium chloride, and lauryltrimethylammonium chloride. , dilauryldimethylammonium chloride, stearyltrimethylammonium chloride, distearyldimethylammonium chloride, cetyltrimethylammonium chloride, alkylbenzyldimethylammonium chloride, more preferably propylamine, dipropylamine, butylamine, dibutylamine, hexylamine, dihexylamine, octylamine, dioctylamine, trioctylamine, dodecylamine, didodecylamine, distearylamine, amino-modified polysiloxane compounds, tetraethylammonium hydroxide (TEAH), tetrabutylammonium hydroxide (TBAH), tetrapropylammonium hydroxide (TPAH), aniline, and further preferably propylamine, dodecylamine, amino-modified polysiloxane compounds, tetrabutylammonium hydroxide (TBAH), aniline, and further preferably amino-modified polysiloxane compounds.
[0336] <29> The film according to any one of <1> to <28>, wherein the amino-modified polysiloxane compound preferably has a kinematic viscosity at 25° C. of 10 to 20,000 mm 2 / s, more preferably 200 to 10,000 mm 2 / s, more preferably 500 to 5,000 mm 2 / s.
[0337] <30> The film according to any one of <1> to <29>, wherein the amino equivalent of the amino-modified polysiloxane compound is preferably 400 to 8,000 g / mol, more preferably 400 to 8,000 g / mol, further preferably 600 to 5,000 g / mol, further preferably 800 to 3,000 g / mol.
[0338] <31> The film according to any one of <1> to <30>, wherein the amino-modified polysiloxane compound is preferably a compound represented by the general formula (a1).
[0339] [Chemical formula 6]
[0340]
[0341] [Where R 1aR represents a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxyl group, an alkoxy group having 1 to 3 carbon atoms, or a hydrogen atom, and is preferably a methyl group or a hydroxyl group from the viewpoint of the surface properties of the synovial fluid and the inhibition of the migration of oil into the fluid. 2a is a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxyl group or a hydrogen atom, and preferably a methyl group or a hydroxyl group from the viewpoint of the surface property of the synovial fluid and the inhibition of the migration of oil to the fluid. B represents a side chain having at least one amino group, and R 3a represents an alkyl group having 1 to 3 carbon atoms or a hydrogen atom. x and y represent the average degree of polymerization, respectively, and are selected so that the kinematic viscosity and amino equivalent of the compound at 25° C. are within the above ranges. 1a , R 2a , R 3a They may be the same or different. In addition, multiple R 2a Can be the same or different]
[0342] <32> A membrane as described in any one of <1> to <31>, wherein in the compound of general formula (a1), from the viewpoint of synovial surface properties and inhibition of oil migration to the flowing object, x is preferably a number of 10 to 10,000, more preferably a number of 20 to 5,000, and further preferably a number of 30 to 3,000; y is preferably a number of 1 to 1,000, more preferably a number of 1 to 500, and further preferably a number of 1 to 200; and the mass average molecular weight of the compound of general formula (a1) is preferably 2,000 to 1,000,000, more preferably 5,000 to 100,000, and further preferably 8,000 to 50,000.
[0343] <33> The film according to any one of <1> to <32>, wherein the side chain B having an amino group in the general formula (a1) is preferably the following.
[0344] -C3H6-NH2
[0345] -C3H6-NH-C2H4-NH2
[0346] -C3H6-NH-[C2H4-NH] e -C2H4-NH2
[0347] -C3H6-NH(CH3)
[0348] -C3H6-NH-C2H4-NH(CH3)
[0349] -C3H6-NH-[C2H4-NH] f -C2H4-NH(CH3)
[0350] -C3H6-N(CH3)2
[0351] -C3H6-N(CH3)-C2H4-N(CH3)2
[0352] -C3H6-N(CH3)-[C2H4-N(CH3)] g -C2H4-N(CH3)2
[0353] -C3H6-NH-cyclo-C5H 11
[0354] (Here, e, f, and g are numbers from 1 to 30 respectively)
[0355] <34> The film as described in any one of <1> to <33>, wherein as specific examples of amino-modified polysiloxane compounds, preferred are TSF4703 and TSF4708 manufactured by Momentive Performance Materials, SF8457C, SF8417, BY16-209, BY16-892, BY16-898, and FZ-3760 manufactured by DowCorning Toray Silicone Co., Ltd., and KF8002, KF867, KF-864, BY16-213, and BY16-853U manufactured by Shin-Etsu Chemical Co., Ltd.
[0356] <35> A membrane as described in any one of <1> to <34>, wherein the modifying group in the hydrophobic modified cellulose fiber (B) is preferably a hydrocarbon group which may have a substituent, and among the hydrocarbon groups which may have a substituent, the preferred hydrocarbon group is a saturated or unsaturated straight chain or branched aliphatic hydrocarbon group, an aromatic hydrocarbon group such as phenyl, or an alicyclic hydrocarbon group such as cyclohexyl, and the preferred substituents among the hydrocarbon groups which may have a substituent are halogen atoms, oxyalkylene groups such as oxyethylene, and hydroxyl groups, etc.
[0357] <36> A membrane as described in any one of <1> to <35>, wherein a preferred embodiment of the hydrophobically modified cellulose fiber (B) is as follows: the cellulose fiber is bonded to one or more substituents selected from the substituents represented by the following general formula (1) and general formula (2) via ether bonds, and has a cellulose I type crystalline structure.
[0358] -CH2-CH(R0)-R1 (1)
[0359] -CH2-CH(R0)-CH2-(OA) n -O-R1 (2)
[0360] [wherein, R0 represents a hydrogen atom or a hydroxyl group, R1 each independently represents a linear or branched alkyl group having 3 to 30 carbon atoms, n represents a number from 0 to 50, and A represents a linear or branched divalent saturated hydrocarbon group having 1 to 6 carbon atoms]
[0361] <37> The film according to any one of <1> to <36>, wherein a more preferred embodiment of the hydrophobically modified cellulose fiber (B) is an etherified cellulose fiber represented by the following general formula (4).
[0362] [Chemical formula 7]
[0363]
[0364] [wherein, R are the same or different and represent hydrogen or a substituent selected from the substituent represented by the above general formula (1) and the substituent represented by the above general formula (2), and m is preferably an integer of 20 to 3000, except when all R are simultaneously hydrogen]
[0365] <38> The film according to any one of <1> to <37>, wherein the introduction rate of the modifying group of the hydrophobically modified cellulose fiber (B) is preferably 0.0001 mol or more and preferably 1.5 mol or less.
[0366] <39> A membrane as described in any one of <1> to <38>, wherein the average fiber diameter of the fine cellulose fibers is preferably greater than 0.1 nm, more preferably greater than 0.5 nm, further preferably greater than 1 nm, further preferably greater than 2 nm, further preferably greater than 3 nm, and is preferably less than 100 nm, more preferably less than 50 nm, further preferably less than 20 nm, further preferably less than 10 nm, further preferably less than 6 nm, further preferably less than 5 nm.
[0367] <40> The film as described in any one of <1> to <39>, wherein the length of the fine cellulose fibers (average fiber length) is preferably 150 nm or more, more preferably 200 nm or more, and is preferably 1000 nm or less, more preferably 750 nm or less, further preferably 500 nm or less, and further preferably 400 nm or less.
[0368] <41> The film according to any one of <1> to <40>, wherein the mass average molecular weight of the oil having an SP value of 10 or less is preferably 100 or more, and preferably 100,000 or less, more preferably 50,000 or less, and still more preferably 20,000 or less.
[0369] <42> The film as described in any one of <1> to <41>, wherein the amount of oil having an SP value of less than 10 is preferably 50 mass% or more, more preferably 55 mass% or more, and further preferably 60 mass% or more, and is preferably 98 mass% or less, more preferably 97 mass% or less, and further preferably 96 mass% or less.
[0370] <43> A membrane as described in any one of <1> to <42>, wherein the mass ratio of cellulose fibers in the hydrophobically modified cellulose fibers to oil with an SP value of less than 10 (cellulose fibers: oil with an SP value of less than 10) is preferably 1:1 or more, more preferably 1:2 or more, and even more preferably 1:3 or more, and is preferably 1:100 or less, more preferably 1:50 or less, and even more preferably 1:20 or less.
[0371] <44> The film as described in any one of <1> to <43>, wherein the oil having an SP value of 10 or less is preferably oleic acid, D-limonene, PEG400, dimethyl succinate, neopentyl glycol dicaprate, hexyl laurate, isopropyl laurate, isopropyl myristate, isopropyl palmitate, isopropyl oleate, hexadecane, olive oil, jojoba oil, squalane, liquid paraffin, Fluorinert FC-40, Fluorinert FC-43, Fluorinert FC-72, Fluorinert FC-770, KF96-1cs, KF-96-10cs, KF-96-50cs, KF-96-100cs and KF-96-1000cs, and the SP value of the oil is preferably 9.5 or less, more preferably 9.0 or less, and even more preferably 8.5 or less.
[0372] <45> The film according to any one of <1> to <44>, further comprising a polymer compound, wherein the polymer compound is one or more polymer compounds selected from the following (X) and (Y).
[0373] (X) a polycondensation polymer having an ester group, an amide group, a carbamate group, an imine group, an ether group or a carbonate group
[0374] (Y) a methacrylic or acrylic polymer having an ester group or an amide group in a side chain
[0375] <46> The film according to any one of <1> to <45>, wherein the mass average molecular weight of the polymer compound is preferably 1,000 or more and preferably 500,000 or less.
[0376] <47> A film as described in any one of <1> to <46>, wherein the amount of the polymer compound is preferably 4 mass% or more, more preferably 8 mass% or more, and further preferably 12 mass% or more, and is preferably 30 mass% or less, more preferably 25 mass% or less, and further preferably 20 mass% or less.
[0377] <48> A film as described in any one of <1> to <47>, wherein the content of any component is preferably 0.1 mass % or more, more preferably 0.2 mass % or more, and further preferably 0.5 mass % or more, and is preferably 20 mass % or less, more preferably 15 mass % or less, and further preferably 10 mass % or less.
[0378] <49> A molded article comprising the film according to any one of <1> to <48>.
[0379] <50> A method for forming a film on a formed body, comprising:
[0380] A process 1 for preparing a dispersion containing hydrophobically modified cellulose fibers and an oil having an SP value of less than 10; and a process 2 for applying the dispersion prepared in process 1 on a formed body; and the dispersion is preferably prepared by mixing the hydrophobically modified cellulose fibers, the oil having an SP value of less than 10, and a solvent.
[0381] <51> The method for forming a film on a formed body as described in <50>, wherein the solvent is preferably isopropyl alcohol, ethanol or methyl ethyl ketone.
[0382] <52> A method for forming a film on a formed body as described in <50> or <51>, wherein the thickness of the dispersion (coating film) on the formed body is preferably greater than 10 μm, more preferably greater than 20 μm, and further preferably 30 μm, and is preferably less than 2000 μm, more preferably less than 1500 μm, and further preferably less than 1200 μm.
[0383] <53> A membrane dispersion comprising hydrophobic modified cellulose fibers having a modifying group bonded to one or more groups selected from anionic groups and hydroxyl groups of the cellulose fibers, and an oil having an SP value of 10 or less, wherein the content of the hydrophobic modified cellulose fibers in the membrane dispersion is preferably 0.2% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.4% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less.
[0384] <54> The film dispersion as described in <53>, wherein the content of oil having an SP value of 10 or less is preferably 4.0 mass% or more, more preferably 5.0 mass% or more, and even more preferably 6.0 mass% or more, and is preferably 40 mass% or less, more preferably 20 mass% or less, and even more preferably 15 mass% or less.
[0385] <55> The film dispersion as described in <53> or <54>, wherein the content of the solvent is preferably 80.0 mass % or more, more preferably 85.0 mass % or more, and further preferably 88.0 mass % or more, and is preferably 92.8 mass % or less, more preferably 91.7 mass % or less, and further preferably 90.6 mass % or less.
[0386] <56> A film dispersion as described in any one of <53> to <55>, wherein the content of the polymer compound is preferably 0.8 mass % or more, more preferably 1.0 mass % or more, and further preferably 1.2 mass % or more, and is preferably 3.0 mass % or less, more preferably 2.5 mass % or less, and further preferably 2.0 mass % or less.
[0387] <57> A film dispersion as described in any one of <53> to <56>, wherein the content of any component is preferably 0.1 mass % or more, more preferably 0.2 mass % or more, and further preferably 0.5 mass % or more, and is preferably 20 mass % or less, more preferably 15 mass % or less, and further preferably 10 mass % or less.
[0388] [Example]
[0389] The present invention is specifically described below by way of examples. Note that the examples are merely examples of the present invention and do not have any limiting meaning. Unless otherwise specified, the parts in the examples represent parts by mass. Note that "normal pressure" means 101.3 kPa, and "room temperature" means 25°C.
[0390] [Average fiber diameter, average fiber length, and average aspect ratio of anionically modified cellulose fibers and hydrophobically modified cellulose fibers]
[0391] Water is added to the target cellulose fiber to prepare a dispersion with a content of 0.0001% by mass, and the dispersion is dripped onto mica, dried and used as an observation sample. An atomic force microscope (AFM, NanoscopeIII Tapping mode AFM, manufactured by Digital instrument, and the probe is Point Probe (NCH) manufactured by NANOSENSORS) is used to measure the fiber height of the target cellulose fiber in the observation sample. At this time, more than 100 cellulose fibers are selected from the microscope image that can clearly display the cellulose fibers, and the average fiber diameter is calculated based on their fiber height. The average fiber length is calculated based on the distance in the fiber direction. The average aspect ratio is calculated based on the average fiber length / average fiber diameter, and the standard deviation is also calculated. In general, the smallest unit of cellulose nanofibers prepared from higher plants is composed of 6×6 molecular chains stacked in a roughly square shape, so the height obtained by analyzing the AFM image can be regarded as the width of the fiber.
[0392] [Average fiber diameter and average fiber length of raw material cellulose fibers]
[0393] Ion exchange water was added to the cellulose fibers to be measured, and a dispersion having an ion exchange water content of 0.01% by mass was prepared. The dispersion was measured using a wet dispersion type image analysis particle size distribution meter (manufactured by Jasco International, trade name: IF-3200) under the following conditions: front lens: 2x, telecentric zoom lens: 1x, image resolution: 0.835 μm / pixel, syringe inner diameter: 6515 μm, spacer thickness: 500 μm, image recognition mode: ghosting, threshold: 8, analysis sample volume: 1 mL, sampling: 15%. More than 100 cellulose fibers were measured, and their average ISO fiber diameter was calculated as the average fiber diameter, and the average ISO fiber length was calculated as the average fiber length.
[0394] [Anionic Group Content of Anionic Group-Containing Cellulose Fibers and Hydrophobically Modified Cellulose Fibers (A)]
[0395] Take 0.5g of the cellulose fiber of the object of measurement with a dry mass and place it in a 100mL beaker, add ion exchange water or a mixed solvent of methanol / water = 2 / 1 to make the whole 55mL, add 5mL of 0.01M sodium chloride aqueous solution to prepare a dispersion, and stir the dispersion until the cellulose fiber of the object of measurement is fully dispersed. Add 0.1M hydrochloric acid to the dispersion to adjust the pH value to 2.5-3, use an automatic titrator (manufactured by East Asia DKK Company, trade name "AUT-710"), add 0.05M sodium hydroxide aqueous solution to the dispersion under the condition of waiting time of 60 seconds, measure the conductivity and pH value every 1 minute, and continue to measure until the pH value reaches about 11 to obtain a conductivity curve. According to the conductivity curve, the sodium hydroxide titration amount is calculated, and the anionic group content of the cellulose fiber of the object of measurement is calculated according to the following formula.
[0396] Anionic group content (mmol / g) = sodium hydroxide titration × sodium hydroxide aqueous solution concentration (0.05M) / mass of cellulose fiber to be measured (0.5g)
[0397] [Aldehyde content of oxidized cellulose fibers and hydrophobically modified cellulose fibers]
[0398] 100.0 g of the target cellulose fiber (solid content 1.0 mass %), acetic acid buffer (pH 4.8), 0.33 g of 2-methyl-2-butene, and 0.45 g of sodium chlorite were added to a beaker and stirred at room temperature for 16 hours to perform oxidation treatment of aldehyde groups. After the reaction was completed, the mixture was filtered and the obtained filter cake was washed with ion exchange water to obtain the target cellulose fiber with aldehyde groups oxidized. The reaction solution was freeze-dried and the carboxyl content of the obtained dry product was measured by the above-mentioned anionic group content determination method to calculate the carboxyl content of the target cellulose fiber with oxidation treatment. Then, the aldehyde content of the oxidized cellulose fiber or the hydrophobically modified cellulose fiber was calculated according to Formula 1.
[0399] Aldehyde content (mmol / g) = (carboxyl content of oxidized cellulose fiber or hydrophobically modified cellulose fiber after oxidation treatment) - (carboxyl content of oxidized cellulose fiber or hydrophobically modified cellulose fiber) Formula 1
[0400] [Solid content in dispersion]
[0401] The measurement was performed using a halogen moisture meter MOC-120H (manufactured by Shimadzu Corporation) at a constant temperature of 150° C., and 1 g of the sample was measured every 30 seconds, and the value when the mass reduction became 0.1% or less was defined as the solid content.
[0402] [Average Bonding Amount and Introduction Rate (Ionic Bond) of Modifying Groups in Hydrophobically Modified Cellulose Fibers (A)]
[0403] The bonding amount of the modifying group is determined by the following IR measurement method, and the average bonding amount and introduction rate are calculated according to the following formula. Regarding IR measurement, specifically, an infrared absorption spectrometer (IR) (manufactured by Thermo Fisher Scientific, trade name: Nicolet 6700) is used to measure the dried hydrophobic modified cellulose fiber (A) by the ATR method, and the average bonding amount and introduction rate of the modifying group are calculated according to the following formula. The following represents the case where the anionic group is a carboxyl group. The following "1720cm -1 The "peak intensity" is the peak intensity derived from the carbonyl group. In the case of anionic groups other than the carboxyl group, the average bonding amount and introduction rate of the modifying group can be calculated by appropriately changing the value of the peak intensity.
[0404] Average bonding amount of the modifying group (mmol / g) = [carboxyl content of the cellulose fiber before the modification group is introduced (mmol / g)] × [(1720 cm -1 Peak intensity of hydrophobically modified cellulose fiber (A) at 1720 cm -1The peak intensity of the cellulose fiber before the introduction of the modified group is 1720 cm -1 The peak intensity of
[0405] 1720cm -1 Peak intensity: Peak intensity of carbonyl group from carboxylic acid
[0406] Introduction rate of modifying group (%) = {average bonding amount of modifying group (mmol / g) / carboxyl group content in cellulose fiber before modification group introduction (mmol / g)} × 100
[0407] [Average Bonding Amount and Introduction Rate (Amide Bond) of Modifying Groups in Hydrophobically Modified Cellulose Fibers (A)]
[0408] The average bonding amount of the modifying group is calculated according to the following formula. The following shows the case where the anionic group is a carboxyl group. Furthermore, in the case of an anionic group other than a carboxyl group, the average bonding amount and introduction rate of the modifying group can be calculated by replacing the carboxyl group with the anionic group.
[0409] Average bonding amount of modifying groups (mmol / g) = carboxyl content in cellulose fibers before the introduction of modifying groups (mmol / g) - carboxyl content in cellulose fibers after the introduction of modifying groups (mmol / g)
[0410] Introduction rate of modifying group (%) = {average bonding amount of modifying group (mmol / g) / carboxyl group content in cellulose fiber before modification group introduction (mmol / g)} × 100
[0411] [Introduction rate of the modifying group in the hydrophobically modified cellulose fiber (B)]
[0412] The content (mass%) of the modified group contained in the obtained etherified cellulose fiber is calculated according to the Zeisel method known in the industry as a method for analyzing the average number of added moles of alkoxy groups of cellulose ethers, as described in Analytical Chemistry, Vol. 51, No. 13, 2172 (1979), "The 15th Revised Edition of the Japanese Pharmacopoeia ("Analysis Method for Hydroxypropyl Cellulose")", etc. The following discloses the process.
[0413] (i) Add 0.1 g of n-octadecane to a 200 mL volumetric flask and make up to the mark with hexane to prepare an internal standard solution.
[0414] (ii) 100 mg of purified and dried etherified cellulose fibers and 100 mg of adipic acid were accurately weighed and placed in a 10 mL vial, 2 mL of hydroiodic acid was added, and the vial was sealed.
[0415] (iii) The mixture in the vial was heated using a heating block at 160° C. for 1 hour while being stirred using a stirrer chip.
[0416] (iv) After heating, 3 mL of the internal standard solution and 3 mL of diethyl ether were injected into the vial in sequence and stirred at room temperature for 1 minute.
[0417] (v) The upper layer (diethyl ether layer) of the two-phase separated mixture in the vial was analyzed using a gas chromatograph ("GC2010 Plus" manufactured by Shimadzu Corporation). The analysis conditions are as follows.
[0418] Column: DB-5 manufactured by Agilent Technology (12 m, 0.2 mm x 0.33 μm)
[0419] Column temperature: 100℃→10℃ / min→280℃(maintain for 10min)
[0420] Injector temperature: 300°C, detector temperature: 300°C, injection volume: 1 μL
[0421] The content (mass %) of the modifying group in the etherified cellulose fibers was calculated from the detected amount of the compound used for introducing the modifying group.
[0422] From the obtained content of the modifying group, the molar substitution degree (MS) (the molar amount of the modifying group per 1 mol of the anhydroglucose unit) was calculated using the following formula (1).
[0423] (Equation 1)
[0424] MS=(W1 / Mw) / ((100-W1) / 162.14)
[0425] W1: Content of modification groups in etherified cellulose fibers (mass %)
[0426] Mw: Molecular weight of the compound used to introduce the modifying group (g / mol)
[0427] [Confirmation of the crystalline structure in hydrophobically modified cellulose fibers]
[0428] The crystal structure of the hydrophobically modified cellulose fiber was confirmed by measuring it under the following conditions using an X-ray diffractometer ("RigakuRINT 2500VC X-RAY Diffractometer" manufactured by RIGAKU Corporation).
[0429] The measurement conditions were as follows: X-ray source: Cu / Kα-radiation, tube voltage: 40 kV, tube current: 120 mA, measurement range: diffraction angle 2θ = 5 to 45°, X-ray scanning speed: 10° / min. The sample for measurement was a 320 mm 2 The pellets having a thickness of 1 mm were compressed to prepare the cellulose. The crystallinity of the cellulose type I crystal structure was calculated from the obtained X-ray diffraction intensity according to the following formula (A).
[0430] Cellulose I type crystallinity (%) = [(I22.6-I18.5) / I22.6] × 100 (A)
[0431] [where I22.6 represents the diffraction intensity of the lattice plane (002 plane) (diffraction angle 2θ=22.6°) in X-ray diffraction, and I18.5 represents the diffraction intensity of the amorphous part (diffraction angle 2θ=18.5°)]
[0432] On the other hand, when the crystallinity obtained according to the above formula (A) is 35% or less, from the viewpoint of improving the calculation accuracy, it is preferred to calculate according to the following formula (B) based on the description of P199-200 of "Wood Science Experiment Manual" (edited by the Japan Wood Society).
[0433] Therefore, when the crystallinity obtained by the above formula (A) is 35% or less, the value calculated by the following formula (B) may be adopted as the crystallinity.
[0434] Cellulose I type crystallinity (%) = [Ac / (Ac+Aa)] × 100 (B)
[0435] [wherein Ac represents the sum of the peak areas of the lattice planes (002 plane) (diffraction angle 2θ=22.6°), (011 plane) (diffraction angle 2θ=15.1°) and (0-11 plane) (diffraction angle 2θ=16.2°) in X-ray diffraction, and Aa represents the peak area of the amorphous part (diffraction angle 2θ=18.5°). Each peak area is obtained by fitting the obtained X-ray diffraction pattern using a Gaussian function]
[0436] [Measurement of arithmetic mean roughness of film]
[0437] The arithmetic mean roughness of the film was measured as follows. A laser microscope (manufactured by KEYENCE, trade name: "VK-9710") was used to measure the arithmetic mean roughness of the film under the following measurement conditions. The measurement conditions were set as follows: objective lens: 10 times, light intensity: 3%, brightness: 1548, Z spacing: 0.5 μm. The arithmetic mean roughness of the film was measured at 5 points using built-in image processing software, and the average value was used.
[0438] [Cellulose fibers in hydrophobically modified cellulose fibers (converted amount)]
[0439] The cellulose fibers (converted amount) in the hydrophobically modified cellulose fibers are measured by the following method.
[0440] (1) When the added "compound for introducing a modifying group" is one type
[0441] The cellulose fiber amount (converted amount) was calculated according to the following formula A.
[0442] <Formula A>
[0443] Cellulose fiber amount (converted amount) (g) = mass of hydrophobically modified cellulose fiber (g) / [1 + molecular weight of the compound for introducing the modifying group (g / mol) × bonding amount of the modifying group (mmol / g) × 0.001]
[0444] (2) When there are two or more types of "compounds for introducing a modifying group" added
[0445] The amount of cellulose fibers (converted amount) was calculated in consideration of the molar ratio of each compound (that is, the molar ratio when the total molar amount of the added compounds is taken as 1).
[0446] Furthermore, when the bonding method between the cellulose fiber and the modifying group is ionic bonding, the "molecular weight of the compound for introducing the modifying group" in the above formula A means "the molecular weight of the entire compound for introducing the modifying group". On the other hand, when the bonding method between the cellulose fiber and the compound for introducing the modifying group is amide bonding, the "molecular weight of the compound for introducing the modifying group" in the above formula A means "the molecular weight of the entire compound for introducing the modifying group - 18".
[0447] [Preparation of cellulose fiber dispersion]
[0448] Preparation Example 1 (Dispersion of oxidized cellulose fibers obtained by reacting natural cellulose fibers with an N-oxyl radical compound)
[0449] As natural cellulose fiber, bleached kraft pulp of coniferous trees (manufactured by Fletcher Challenge Canada, trade name "Machenzie", CSF650ml) was used. As TEMPO, a commercial product (manufactured by ALDRICH, Free radical, 98% by mass) was used. As sodium hypochlorite, a commercial product (manufactured by Wako Pure Chemical Industries, Ltd.) was used. As sodium bromide, a commercial product (manufactured by Wako Pure Chemical Industries, Ltd.) was used.
[0450] First, 100 g of bleached kraft pulp fiber of a conifer is fully stirred in 9900 g of ion exchange water, and then 1.25 g of TEMPO, 12.5 g of sodium bromide, and 28.4 g of sodium hypochlorite are added to the mass of 100 g of the pulp in sequence. Using a pH STAT, 0.5 M sodium hydroxide is added dropwise to maintain the pH value at 10.5. After the reaction is carried out for 120 minutes (20° C.), the addition of sodium hydroxide is stopped to obtain oxidized pulp. The obtained oxidized pulp is fully washed with ion exchange water and then dehydrated. Thereafter, a high-pressure homogenizer (manufactured by SUGINO MACHINE, StarburstLab HJP-2 5005) is used to perform two micronization treatments on 3.9 g of oxidized pulp and 296.1 g of ion exchange water at 245 MPa to obtain an oxidized cellulose fiber dispersion (solid content 1.3% by mass). The oxidized cellulose fibers had an average fiber diameter of 3.3 nm and a carboxyl group content of 1.62 mmol / g.
[0451] Preparation Example 2 (Dispersion of Oxidized Cellulose Fibers with Aldehyde Groups Reducing Treatment)
[0452] 3846.15 g (solid content 1.3% by mass) of the oxidized cellulose fiber dispersion obtained in Preparation Example 1 was placed in a beaker, 1M sodium hydroxide aqueous solution was added thereto to adjust the pH to about 10, and then 2.63 g of sodium borohydride (manufactured by Wako Pure Chemical Industries, Ltd., purity 95% by mass) was added, and the mixture was reacted at room temperature for 3 hours to perform aldehyde reduction treatment. After the reaction was completed, 405 g of 1M hydrochloric acid aqueous solution and 4286 g of ion exchange water were added to prepare a 0.7% by mass aqueous solution, and the mixture was reacted at room temperature for 1 hour to perform protonation. After the reaction was completed, the mixture was filtered, and the obtained filter cake was washed with ion exchange water to remove hydrochloric acid and salt. Finally, the solvent was replaced with isopropanol to obtain an oxidized cellulose fiber dispersion treated with aldehyde groups. The obtained oxidized cellulose fiber dispersion treated with aldehyde groups (solid content 2.0% by mass) had an average fiber diameter of 3.3 nm and a carboxyl group content of 1.62 mmol / g.
[0453] [Preparation of hydrophobically modified cellulose fibers]
[0454] Production Example 1
[0455] In a beaker equipped with a magnetic stirrer and a stirring bar, 300 g (solid content: 2.0% by mass) of the oxidized cellulose fiber dispersion obtained in Preparation Example 2 was added. Then, an amino-modified polysiloxane ("BY16-209" manufactured by Dow Corning Toray Co., Ltd., abbreviated as "polysiloxane 1") was added in an amount corresponding to 0.5 mol of amino groups per 1 mol of carboxyl groups in the oxidized cellulose fibers, and 100 g of isopropyl alcohol was added, and the mixture was reacted at room temperature (25° C.) for 14 hours. After the reaction, the mixture was filtered, and the obtained filter cake was washed with isopropyl alcohol, stirred for 2 minutes with an ultrasonic homogenizer (manufactured by Nippon Seiki Co., Ltd., US-300E), and finely treated with a high-pressure homogenizer (manufactured by SUGINO MACHINE Co., Ltd., StarburstLab HJP-2 5005) at 100 MPa for 1 pass and 150 MPa for 9 passes, thereby obtaining hydrophobically modified cellulose fibers in which amino-modified polysiloxane was linked to oxidized cellulose fibers via ionic bonds. The introduction rate of the modifying group was 40% of the carboxyl group of the oxidized cellulose fibers. The average fiber diameter of the hydrophobically modified cellulose fibers was 3.3 nm, and the average fiber length was 578 nm.
[0456] Production Examples 2 to 7
[0457] Hydrophobically modified cellulose fibers were obtained by the same method as in Production Example 1 except that the compound for introducing a modifying group and the amount added were changed as shown in Table 1. The detailed description of the compound for introducing a modifying group in Table 1 is as follows.
[0458] Polysiloxane 2: SF8417 manufactured by Dow Corning Toray Co., Ltd.
[0459] Polysiloxane 3: manufactured by Dow Corning Toray Co., Ltd., FZ-3760
[0460] Dodecylamine: Made by Wako Pure Chemical Industries, Ltd.
[0461] Oleylamine: Made by Wako Pure Chemical Industries, Ltd.
[0462] Production Example 8
[0463] 300 g (solid content 1.2% by mass) of the dispersion of the hydrophobically modified cellulose fibers obtained in Preparation Example 1 was added to a beaker equipped with a magnetic stirrer and a stirrer. Then, dodecylamine (manufactured by Wako Pure Chemical Industries) was added in an amount equivalent to 0.5 mol of amino groups relative to 1 mol of carboxyl groups of the hydrophobically modified cellulose, and 100 g of isopropanol was added, and the mixture was reacted at room temperature (25° C.) for 14 hours. After the reaction was completed, hydrophobically modified cellulose fibers to which amino-modified polysiloxane and dodecylamine were linked via ionic bonds were obtained in the same manner as in Preparation Example 1.
[0464] [Table 1]
[0465] Table 1
[0466]
[0467] The addition amount in Table 1 indicates the amount (mol) of the amino group relative to 1 mol of the carboxyl group.
[0468] [Preparation of synovial surface film]
[0469] Example 1
[0470] Using the hydrophobically modified cellulose fibers obtained in Preparation Example 1, a dispersion for a film was prepared as follows to prepare a synovial surface film. The hydrophobically modified cellulose fibers, squalane and a solvent (isopropyl alcohol) were mixed so that the mass ratio of the hydrophobically modified cellulose fibers to squalane (lubricating oil) was 1:20, and the solvent accounted for 90% by mass of the entire dispersion. The mixture was stirred in a spiral tube at room temperature for 30 minutes. Thereafter, the mixture was deaerated at 2200 rpm for 2 minutes using an automatic revolution stirrer ("Degassing Rentaro" manufactured by Thinky Co., Ltd.) to obtain a dispersion for a coating film. The obtained coating film sample was applied to a glass substrate (Micro Slide Glass S2112 manufactured by MATSUNAMI Co., Ltd.) using an applicator (manufactured by Tester Industry Co., Ltd.) to a thickness of 100 μm, and dried at 50°C under vacuum for 12 hours to volatilize the isopropyl alcohol, thereby obtaining a synovial surface film having a film thickness of 10 μm.
[0471] Embodiments 2 to 15
[0472] A synovial surface film was obtained by the same method as in Example 1 except that the type of hydrophobically modified cellulose fiber, the type of oil (lubricant) having an SP value of 10 or less, the mass ratio of cellulose fiber to lubricant, and the film thickness were changed as shown in Tables 3 and 4.
[0473] [Preparation of surface film coated with lubricating oil]
[0474] Comparative Example 1
[0475] A lubricating oil film having a film thickness of 10 μm was obtained by the same method as in Example 1 except that squalane (lubricating oil) and isopropyl alcohol were prepared in a ratio of 10:90.
[0476] [Preparation of a surface film coated with lubricating oil on a concave-convex structure]
[0477] Comparative Example 2
[0478] A drainage sheet having a concavo-convex structure ("Toyal Ultra Lotus (registered trademark)" manufactured by Toyo Alumi) was attached to a glass substrate ("Micro Slide Glass S2112" manufactured by MATSUNAMI) using a transparent tape. 2 0.064 g of squalane was applied as a lubricating oil to prepare a lubricating oil-coated surface film having a film thickness of 10 μm. The results are shown in Table 3.
[0479] [Production of surface film using oil with an SP value exceeding 10]
[0480] Comparative Example 3
[0481] The same operation as in Example 8 was carried out except that glycerol (SP value: 16.5) was used instead of squalane as the lubricating oil to prepare a surface film having a film thickness of 1000 μm.
[0482] [Performance test of membrane]
[0483] The following experiments were carried out at room temperature. The details of the fluid A used in the experiments are as follows.
[0484] Quartamin E-80K (manufactured by Kao Corporation): 3% by mass
[0485] Propylene glycol (manufactured by Wako Pure Chemical Industries, Ltd.): 1 mass%
[0486] Ion exchange water: the remainder
[0487] Test Example 1 (Sliding Speed Measurement Test)
[0488] 50 mg of the fluid A was placed on the film produced in the example or comparative example, the film was tilted 90 degrees together with the glass substrate, and the average sliding distance of the fluid A per minute was measured.
[0489] Test Example 2 (Lubricating Oil Mobility Measurement Test)
[0490] On the membrane prepared in the embodiment or comparative example, a fluid A in an amount 100 times the mass of the lubricating oil in the membrane was applied, and the membrane was left to stand at room temperature in a petri dish. After 72 hours, the sample of the fluid A was collected to evaluate the mobility of the lubricating oil from the membrane to the fluid A. The mobility is expressed as the mobility of the lubricating oil, which is evaluated based on the amount (mass %) of the lubricating oil that moves to the sampled fluid A (sample) when the mass of the lubricating oil originally contained in the membrane is set to 100. Squalane, isopropyl palmitate, jojoba oil, oleic acid and glycerin in the sample were measured by GC, and silicone oil was measured by NMR under the following conditions.
[0491] <GC method>
[0492] In the following measurement method, the mobility was measured based on the peak area derived from each lubricating oil detected at the time shown in Table 2.
[0493] [Table 2]
[0494] Table 2
[0495]
[0496] Device: Agilent 6850 Series II
[0497] Column: DB-5 (Agilent), 12m×200μm×0.33μm
[0498] Method: Keep at 100℃ for 3 minutes → Raise the temperature from 100℃ to 320℃ at 10℃ / min → Keep at 320℃ for 15 minutes
[0499] Detector: 330℃ (FID), H2: 30mL / min, Air: 400mL / min, He: 30mL / min
[0500] Carrier gas: He
[0501] Injection volume: 1μL
[0502] Sample: solution diluted 100 times with isopropanol after sampling
[0503] <NMR method>
[0504] The mobility of the silicone oil was determined from the ratio of the peak intensity at 0 ppm derived from the silicone oil to the peak intensity at 7.3 ppm derived from 1,4-dibromobenzene as an internal standard.
[0505] Device: Agilent-NMR-vnmr400
[0506] Sample: 1% deuterated chloroform solution (containing 0.06 wt% 1,4-dibromobenzene as internal standard)
[0507] Total times: 16 times
[0508] Test Example 3 (Sliding Angle Measurement Test)
[0509] At room temperature 20°C, 2 μL of dodecane droplets (20°C) were added to the film, and after standing for 10 seconds, the surface was tilted at a speed of 1° / s, and the angle at which the droplets began to flow was measured. As a representative example, the sliding angle of the slippery surface film of Example 1 was 7°. In addition, the sliding angles of the surface films of Comparative Examples 1 and 2 could not be measured.
[0510] The results are shown in Tables 3 and 4 below.
[0511] [Table 3]
[0512]
[0513] [Table 4]
[0514]
[0515] In Tables 3 and 4, the film roughness refers to the arithmetic mean roughness of the film on the surface of the synovial fluid.
[0516] The detailed description of the lubricating oil used above is as follows.
[0517] Squalane (manufactured by Wako Pure Chemical Industries, Ltd., SP value: 7.9)
[0518] Polysiloxane 100cs (manufactured by Shin-Etsu Silicones Co., Ltd., trade name: KF96-100cs, SP value: 7.3)
[0519] Isopropyl palmitate (manufactured by Wako Pure Chemical Industries, Ltd., SP value: 8.5)
[0520] Jojoba oil (manufactured by Wako Pure Chemical Industries, Ltd., SP value: 8.6)
[0521] Oleic acid (manufactured by Wako Pure Chemical Industries, Ltd., SP value: 9.2)
[0522] Glycerin (manufactured by Wako Pure Chemical Industries, Ltd., SP value: 16.5)
[0523] According to the above table, the following can be known.
[0524] It can be seen that the surface films of Examples are all excellent surface films with high sliding speed and low lubricant oil migration rate.
[0525] On the other hand, it is understood that Comparative Example 1 itself cannot produce a slippery surface, and of course cannot measure the sliding speed and the like.
[0526] It is found that the surface film of Comparative Example 2, that is, the surface film containing oil having an SP value of 10 or less in the conventional film having a concavo-convex structure, has a sliding speed as good as that of the examples, but has a lubricating oil migration rate much higher than that of the examples.
[0527] It is found that the surface film of Comparative Example 3, that is, the film produced using glycerin as an oil having an SP value exceeding 10, has a sliding speed of 0 cm / min, that is, the effect of suppressing the adhesion of flowing matter is poor.
[0528] [Film production]
[0529] Examples 21 to 26, Reference Example 1
[0530] In Examples 21, 22, 24 to 26 and Reference Example 1, the hydrophobically modified cellulose fibers obtained in Preparation Example 1 were used, and in Example 23, the hydrophobically modified cellulose fibers obtained in Preparation Example 2 were used to prepare a dispersion for a film in the following manner to produce a film. That is, the hydrophobically modified cellulose fibers, the polymer compound, the lubricating oil (squalane) and the solvent (isopropyl alcohol) were mixed in a spiral tube in such a manner that the solvent became 90% by mass of the entire dispersion and in such a manner as to form the mass ratio shown in Table 6. Then, the contents of the spiral tube were stirred for 12 hours at a magnetic stirrer speed of 500 rpm and room temperature (25° C.). Thereafter, an automatic revolution stirrer (manufactured by Thinky, Degassing Rentaro) was used to stir at 2200 rpm for 2 minutes to deaerate, and a dispersion for a coating film was obtained. The obtained dispersion for coating film was applied to a glass substrate (Micro Slide Glass S2112, manufactured by MATSUNAMI) as a molded body using an applicator (manufactured by Tester Industry Co., Ltd.) to a thickness of 400 μm, and dried under vacuum at 50° C. for 12 hours to volatilize the isopropyl alcohol, thereby obtaining a film with a thickness of 40 μm.
[0531] Method for determining molecular weight of polymer compounds
[0532] The mass average molecular weight (Mw) was measured by gel permeation chromatography (GPC) using a Hitachi L-6000 high performance liquid chromatograph. The eluent flow pump used was a Hitachi L-6000, the detector used a Shodex RI SE-61 differential refractive index detector, and the column used was a column connected with two GMHHR-Hs. The sample was 20 μL with a concentration adjusted to 0.5 g / 100 mL by the eluent. The eluent used was a chloroform solution of Farmin DM20 (manufactured by Kao Corporation) with a concentration of 1 mmol / L. The column temperature was 40°C and the flow rate was 1.0 mL / min. Polystyrene (manufactured by Tosoh Corporation) was used as a standard polymer for preparing a calibration curve.
[0533] From the chart obtained by GPC measurement, the amount of the polymer component having a molecular weight of 100,000 or more in the polymer compound was calculated by the following formula.
[0534] Amount of components with molecular weight of 100,000 or more = (area with molecular weight of 100,000 or more) / (total area)
[0535] The lubricating oil (oil having an SP value of 10 or less) used above is described in detail below.
[0536] Squalane (manufactured by Wako Pure Chemical Industries, Ltd., SP value: 7.9)
[0537] The detailed description of the polymer compound used above is as follows.
[0538] Polyamides 1 to 3: Polyamides synthesized using raw materials at the ratios listed in Table 5
[0539] Polyalkyleneimine: EPOMIN P-1000 (manufactured by Nippon Catalyst Co., Ltd.)
[0540] Synthesis method of polyamide 1
[0541] 450 g of Haridimer 250K was placed in a 2 L separable flask, heated to 70°C, and then replaced with nitrogen. Then, 45 g of ethylenediamine and 5 g of diethylenetriamine were slowly added, and the temperature was raised until the internal temperature reached 145°C. After stirring at 145°C for 1 hour, the temperature was raised until the internal temperature reached 210°C, and stirred for 6 hours. Then, the internal temperature was kept at 210°C, and the pressure was reduced using a vacuum pump until the internal pressure reached 45 KPa, and stirred for 0.5 hours to produce polyamide 1.
[0542] Synthesis method of polyamide 2-3
[0543] Polyamides 2 and 3 were produced by the same method as that of Polyamide 1 using the raw materials shown in Table 5.
[0544] [Table 5]
[0545] Table 5
[0546]
[0547] In Table 5, the content of diethylenetriamine in polyamide 1 is 3.0 mol%. Furthermore, in Table 5, the amount of the polymer component means the ratio of the polymer component having a molecular weight of 100,000 or more in the polymer compound.
[0548] The composition of the raw materials used above is as follows.
[0549] Haridimer 250K (manufactured by Harima Chemicals Co., Ltd.): Cas No. 61788-89-4: 100% (C36 dimer acid)
[0550] Tsunodime 205 (manufactured by Tsuno Food Industry Co., Ltd.): A mixture of Cas No. 61788-89-4: 70% (C36 dimer acid), Cas No. 68937-90-6: 18% (trimeric linoleic acid), and Cas No. 68955-98-6: 12% (branched and linear unsaturated fatty acids of C16-18 and C18)
[0551] [Performance test of membrane]
[0552] Using the above-mentioned flow medium A, the following experiment was carried out.
[0553] Test Example A (Sliding Speed Measurement Test)
[0554] The test was carried out in the same manner as in the above-mentioned Test Example 1. This test was carried out five times. Table 6 shows the sliding speed at the first time and the sliding speed at the fifth time.
[0555] Test Example B (Lubricating Oil Mobility Test)
[0556] The test was carried out in the same manner as in the above-mentioned Test Example 2 to evaluate the mobility. The results are shown in Table 6.
[0557] Test Example C (Sliding Angle Measurement Test)
[0558] The test was carried out to measure the sliding angle in the same manner as in the above-mentioned Test Example 3. As a representative example, the sliding angle of the film of Example 21 was 7°.
[0559] Test Example D (Hardness Measurement Test)
[0560] The surface hardness (Martens hardness) of each film was measured using a hardness tester (manufactured by Shimadzu Scientific Instruments, DUH-211) under the following conditions.
[0561] Test force: 0.1mN
[0562] Load holding time: 5(s)
[0563] Unload holding time: 1(s)
[0564] [Table 6]
[0565]
[0566] In Table 6, the mass ratio refers to the ratio of "cellulose fiber of hydrophobically modified cellulose fiber: polymer compound: lubricating oil".
[0567] According to Table 6, the following can be known.
[0568] Compared with the film of Reference Example 1 which does not contain a polymer compound, the films of each example can be confirmed to have an increase in sliding speed, a decrease in the mobility of oils with an SP value of 10 or less, and an improvement in durability. Furthermore, it can be confirmed that the greater the amount of the specific polymer compound, the greater the value of the surface hardness of the film.
[0569] Industrial Applicability
[0570] Since the film of the present invention has a high slippery surface property, it can be used in the field of materials for packaging containers of cosmetics or foods.
Claims
1. A film comprising: Hydrophobically modified cellulose fibers having a modifying group bonded to anionic groups of the cellulose fibers, and oil having an SP value of 10 or less, The hydrophobically modified cellulose fiber is formed by bonding an amino-modified polysiloxane compound to an anionic group of the cellulose fiber. The SP value represents the solubility parameter calculated by the Fedors method, and the unit is (cal / cm 3 ) 1 / 2 .
2. The film according to claim 1, wherein The kinematic viscosity of the amino-modified polysiloxane compound at 25°C is 200 mm 2 / s~5000mm 2 / s.
3. The film according to claim 1, wherein The amino group equivalent of the amino-modified polysiloxane compound is 800 g / mol to 3000 g / mol.
4. The film according to claim 1, wherein The amount of the hydrophobically modified cellulose fibers in the film is 1% by mass or more and 40% by mass or less.
5. The film according to claim 1, wherein The mass average molecular weight of the oil having an SP value of 10 or less is 100 or more and 100,000 or less.
6. The film according to claim 1, wherein The amount of oil having an SP value of 10 or less is 50% by mass or more and 98% by mass or less.
7. The film according to claim 1, wherein The amount of oil having an SP value of 10 or less is 60% by mass or more and 97% by mass or less.
8. The film according to claim 1, wherein The SP value of the oil having an SP value of 10 or less is 7.3 or more and 9.5 or less.
9. The film according to claim 1, wherein The mass ratio of the cellulose fibers to the oil having an SP value of 10 or less in the hydrophobically modified cellulose fibers, that is, the cellulose fibers:the oil having an SP value of 10 or less, is 1:1 to 1:
100.
10. The film according to claim 1, wherein When measured with a microhardness tester, the surface hardness of the film was 0.1 N / mm in terms of Martens hardness, ie, HM. 2 above.
11. The film according to claim 1, wherein The arithmetic mean roughness of the film is 0.8 μm or more and 10.5 μm or less.
12. The film according to claim 1, wherein The thickness of the film is 5 μm or more and 1200 μm or less.
13. The film according to claim 1, wherein The introduction rate of the modification group is 20% or more and 90% or less.
14. The film according to any one of claims 1 to 13, wherein The anionic group is a carboxyl group.
15. The film according to any one of claims 1 to 13, wherein The bonding of the modifying group is ionic bonding.
16. The film according to any one of claims 1 to 13, wherein The oil having an SP value of 10 or less is selected from oleic acid, isopropyl palmitate, jojoba oil and squalane.
17. The film according to any one of claims 1 to 13, wherein The amino-modified polysiloxane compound is a compound represented by the general formula (a1): [Where R 1a represents a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxyl group, an alkoxy group having 1 to 3 carbon atoms, or a hydrogen atom, and R 2a is a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxyl group or a hydrogen atom, B represents a side chain having at least one amino group, and R 3a represents an alkyl group having 1 to 3 carbon atoms or a hydrogen atom, x and y represent the average degree of polymerization, and are selected so that the kinematic viscosity and amino equivalent of the compound at 25° C. are within the above ranges, and R 1a , R 2a , R 3a Each of the R 2a The same or different options are available. In the compound of the general formula (a1), x is a number from 10 to 10,000, and y is a number from 1 to 1,000.
18. The film according to claim 17, wherein The mass average molecular weight of the compound of general formula (a1) is 2,000 to 1,000,000.
19. The film according to claim 18, wherein In the general formula (a1), the side chain B having an amino group is any of the following groups, -C3H6-NH2 -C3H6-NH-C2H4-NH2 -C3H6-NH-[C2H4-NH] e -C2H4-NH2 -C3H6-NH(CH3) -C3H6-NH-C2H4-NH(CH3) -C3H6-NH-[C2H4-NH] f -C2H4-NH(CH3) -C3H6-N(CH3)2 -C3H6-N(CH3)-C2H4-N(CH3)2 -C3H6-N(CH3)-[C2H4-N(CH3)] g -C2H4-N(CH3)2 -C3H6-NH-cyclo-C5H 11 Here, e, f, and g are numbers ranging from 1 to 30, respectively.
20. The membrane according to claim 18 or 19, wherein The amino-modified polysiloxane compound is one or more selected from monoamino-modified polysiloxane having one amino group in one side chain B and diamino-modified polysiloxane having two amino groups in one side chain B.
21. The film according to any one of claims 1 to 13, wherein The amino-modified polysiloxane compound is selected from SF8417, BY16-209 and FZ-3760.
22. A formed body comprising the film according to any one of claims 1 to 21.
23. A method for forming a film on a formed body, comprising: Step 1 of preparing a dispersion containing hydrophobically modified cellulose fibers and an oil having an SP value of 10 or less; as well as Step 2 of applying the dispersion prepared in step 1 onto a molded body, The hydrophobically modified cellulose fiber is formed by bonding an amino-modified polysiloxane compound to an anionic group of the cellulose fiber. The SP value represents the solubility parameter calculated by the Fedors method, and the unit is (cal / cm 3 ) 1 / 2 .
24. The forming method according to claim 23, wherein: The dispersion comprises hydrophobically modified cellulose fibers, an oil having an SP value of 10 or less, and a solvent.
25. The forming method according to claim 23, wherein: The solvent is isopropanol, ethanol or methyl ethyl ketone.
26. A dispersion for a film, comprising: Hydrophobically modified cellulose fibers having a modifying group bonded to anionic groups of the cellulose fibers, and oil having an SP value of 10 or less, The hydrophobically modified cellulose fiber is formed by bonding an amino-modified polysiloxane compound to an anionic group of the cellulose fiber. The SP value represents the solubility parameter calculated by the Fedors method, and the unit is (cal / cm3 ) 1 / 2 .
27. The film dispersion according to claim 26, wherein The content of oil having an SP value of 10 or less is 4.0% by mass or more and 40% by mass or less.
28. The film dispersion according to claim 26, wherein The content of the hydrophobically modified cellulose fibers is 0.2% by mass or more and 15% by mass or less.
29. The dispersion for film according to any one of claims 26 to 28, wherein The oil having an SP value of 10 or less is selected from at least one of oleic acid, isopropyl palmitate, jojoba oil and squalane.
30. The dispersion for film according to any one of claims 26 to 28, wherein The SP value of the oil having an SP value of 10 or less is 7.3 or more and 9.5 or less.