A method for writing nanostructures by manipulating the macroscopic movement trajectory of a substrate

By manipulating the macroscopic substrate movement trajectory design in the thermal evaporation or ion beam etching process, high-resolution micro-nanostructure preparation is achieved, which solves the problems of expensive equipment and mask resolution limitations in the existing technology, and achieves Efficient and flexible nanostructure preparation.

CN114524406BActive Publication Date: 2024-10-29ZHEJIANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111588983.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-23
Publication Date
2024-10-29
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

It is difficult to prepare high-resolution nanostructures with existing technology, and the photolithography process equipment is expensive and complex. Micro-nanostructures prepared by thermal evaporation are limited by the resolution of the mask, making it difficult to meet the industry's demand for fine structures.

Method used

By manipulating the macroscopic substrate movement trajectory design, micron-scale objects are used to support the mask during the thermal evaporation or ion beam etching process to control the macroscopic movement trajectory of the substrate, so that the material is formed on the substrate surface in line with the substrate movement trajectory. The same micro-nano structure enables the preparation of micro-nano structures.

Benefits of technology

It achieves high-resolution, low-cost, and easy-to-operate micro-nano structure preparation. It can prepare a variety of nanostructures of different shapes on any surface, significantly improving the resolution of micro-nano structures. It is suitable for metasurfaces, plasmons, and magnetism. Materials and semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003429134170000011
    Figure HDA0003429134170000011
  • Figure HDA0003429134170000021
    Figure HDA0003429134170000021
  • Figure HDA0003429134170000022
    Figure HDA0003429134170000022
Patent Text Reader

Abstract

The present invention discloses a method for designing and preparing micro-nano structures by manipulating the macroscopic movement trajectory of a substrate, comprising: using a micrometer-scale object to support a mask plate in the air on a substrate, and in the process of material growth such as evaporation or sputtering or ion beam etching or photolithography, by controlling the macroscopic movement trajectory of the substrate, the material or etching source forms a micro-nano structure with the same size as the macroscopic movement trajectory of the substrate on the surface of the substrate through the mask plate. The macroscopic movement trajectory of the substrate is not on a spherical surface with the evaporation source or sputtering source as the center of the sphere. The method of the present invention is simple to operate, flexible in design, and the size and shape of the prepared micro-nano structure are precisely controllable, and has great practical application potential in the fields of supersurfaces, plasmons, magnetic materials, semiconductor device manufacturing, etc. related to micro-nano structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of micro-nano processing technology, and specifically relates to preparing micro-nano structures of arbitrary shapes by controlling the macroscopic movement trajectory of a substrate covered by a mask in a thermal evaporation or ion beam etching process, thereby realizing the conversion of the macroscopic movement of the substrate into the nanoscale movement of the nanostructure. Background Art

[0002] When the structural size of materials is reduced to the nanometer range, they often show different properties and characteristics from macroscopic materials. Currently, the preparation of nanoscale materials and structures has become one of the hottest areas in micro-nano science and technology research. In recent decades, various micro-nano technologies have emerged and developed continuously, such as photolithography and electron beam exposure. For photolithography, the resolution of the prepared micro-nano pattern is proportional to the wavelength of the light beam, so the resolution of the prepared micro-nano structure is limited by the wavelength of the light beam, which has gradually failed to meet the increasingly demanding industrial demand for fine structures. In addition, expensive equipment and complex exposure systems have greatly increased the cost. According to de Broglie's matter wave theory, electrons are a wave with an extremely short wavelength, so the biggest advantage of electron beam exposure or etching compared to optical exposure technology is that it breaks through the limit of optical diffraction and can prepare nanostructures with higher resolution. However, the process is very time-consuming and difficult to apply to the preparation of large-area nanostructures. Therefore, it is urgent to develop a technology that is low-cost, easy to operate, and can prepare nanostructures with high structural resolution.

[0003] Thermal evaporation refers to a method in which a material such as metal is heated and vaporized in a vacuum chamber to form a vapor flow, and the gas molecules are deposited on the substrate or workpiece surface and condensed to form a solid film or coating. Compared with the photolithography process, the use of thermal evaporation to prepare micro-nano patterns has the characteristics of low price and easy operation. At present, the commonly used method for preparing micro-nano structures in the industrial and scientific research fields is to place the mask closely on the substrate and use thermal evaporation to prepare a micro-nano pattern with the same pattern as the mask. However, the micro-nano structure prepared by this method is limited by the resolution of the mask structure. Summary of the invention

[0004] The purpose of the present invention is to address the deficiencies of the prior art and provide a method for designing and preparing a micro-nano structure by manipulating the movement trajectory of a macroscopic substrate.

[0005] The technical solution adopted by the present invention is specifically as follows:

[0006] A method for designing and preparing micro-nano structures by manipulating the movement trajectory of a macroscopic substrate (micro-distance suspended net nano direct writing technology), comprising:

[0007] The mask is supported on the substrate in the air by a micrometer-scale object. During the evaporation or sputtering process, the macroscopic movement trajectory of the substrate (including the mask supported on the substrate in the air) is controlled so that the evaporated or sputtered material passes through the mask to form a micro-nano structure on the substrate surface that is the same as the macroscopic movement trajectory of the substrate but with a reduced size. The macroscopic movement trajectory of the substrate is not on a spherical surface with the evaporation source or sputtering source as the sphere center.

[0008] Alternatively, a micrometer-scale object is used to support the mask on the substrate, and during the ion beam etching or photolithography process, the macroscopic movement trajectory of the substrate is controlled so that the ion beam or light beam passes through the mask to etch a micro-nano structure on the substrate surface that is the same as the macroscopic movement trajectory of the substrate but with a reduced size. The macroscopic movement trajectory of the substrate is not on a spherical surface with the ion source as the sphere center.

[0009] This method uses micron-scale pillars (or balls, etc.) to suspend the mask and support it on a substrate (such as silicon or any other material). Through material growth techniques or etching techniques such as thermal evaporation or electron beam evaporation, the substrate can be moved at a macro scale to prepare a micro-nano structure on the substrate that is the same as the macroscopic movement trajectory. This technology is named micro-suspended mesh nano direct writing technology. The preparation method of the micro-suspended mesh micro-nano structure provided by the present invention only needs to design the macroscopic movement trajectory (usually at the centimeter scale) of the substrate based on the shape and size of the micro-nano structure to be prepared. The reduction factor of the obtained micro-nano structure relative to the macroscopic movement trajectory is equal to the distance from the mask to the source divided by the distance from the mask to the substrate, which can usually reach millions of times (i.e., 1 cm for a macroscopic movement, 1 nanometer for a microscopic structure). By performing multiple micro-suspended mesh nano direct writing processes, nanostructures of various compositions and shapes can be prepared on any smooth or rough surface of the substrate.

[0010] Furthermore, the micrometer-scale object is a micrometer ball or a nanometer column prepared by a processing technique such as photolithography.

[0011] Furthermore, the pattern of the mask is circular, strip-shaped and / or any other shape. The pattern can be one or more. By controlling the shape and number of the pattern of the mask, the number and distribution of the micro-nano structures formed on the substrate can be controlled.

[0012] Furthermore, the method of fixing the mask on the substrate via air using a micrometer-scale object is specifically as follows: fixing the micrometer-scale object on the substrate, and then transferring the mask to the substrate with the micrometer-scale object fixed thereon by a film transfer method.

[0013] Furthermore, the reduction factor of the micro-nano structure relative to the macroscopic moving track is equal to the ratio of the distance from the mask to the substrate to the distance from the evaporation source, sputtering source or ion source to the mask.

[0014] Furthermore, the method for controlling the macroscopic movement trajectory of the substrate is to intermittently move the substrate and / or to continuously move the substrate.

[0015] Specifically, in the process of thermal evaporation of materials, intermittently moving the substrate will obtain a micro-nano structure composed of a mask image (such as a circular hole grid) that is the same as the substrate movement trajectory, and continuously moving the substrate will obtain a continuous micro-nano structure.

[0016] Furthermore, micro-nano structures can be prepared on any smooth or concave-convex surface of materials.

[0017] Furthermore, by using ion beam etching with strong directionality, the etching of the substrate can be controlled at the nanometer scale by moving the substrate.

[0018] Compared with the existing technology, the beneficial effects of the present invention are embodied in:

[0019] The micro-suspended net nano-writing technology provided by the present invention only needs to design the macroscopic movement trajectory of the substrate based on the shape of the desired micro-nano structure to obtain a micro-nano structure of a specific shape, and the size of the micro-nano structure can be arbitrarily controlled by changing the distance from the mask to the substrate or the distance from the substrate to the source (evaporation source, sputtering source, ion source or light source, etc.). Theoretically, the characteristic size of the micro-nano structure can be arbitrarily reduced. The method described is simple to operate, flexible in design, and can significantly improve the resolution of the micro-nano structure. It has great potential in the fields of super-surfaces, plasmons, magnetic materials, semiconductor device manufacturing, etc. related to micro-nano structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram of the principle of preparing micro-nano structures by the method of the present invention. a. Schematic diagram of silver nano-grid suspended above a substrate; b. Schematic diagram of the formation of the nano-letter "W"; c. Schematic diagram of the macroscopic movement of the substrate and the microscopic movement of the corresponding nano-disk relative to the substrate; d. Schematic diagram of the formation of the nano-ring.

[0021] Figure 2 These are the preparation result diagrams in Example 1, wherein a is an electron microscope image of a tightly packed polystyrene (PS) sphere template with a diameter of 500 nm; b is an electron microscope image of a non-tightly packed PS sphere template; c is an electron microscope image of a silver nanomesh; d is an electron microscope image of a non-tightly packed PS sphere template covering a silver nanomesh; and e is a schematic diagram of the transfer of the silver nanomesh.

[0022] Figure 3 Electron microscope images of two nanodisks formed when the sample was translated on the sample stage by 4.5 cm (a), 5.5 cm (b), and 10 cm (c), respectively, during the thermal evaporation of silver in Example 1.

[0023] Figure 4 Schematic diagram of the macroscopic movement trajectory of the sample in Example 2 (a, wherein Ⅰ, the letter "W", Ⅱ, the letter "L", and Ⅲ, the letter "V") and scanning electron microscope images of the nano-letters "W" (b), "L" (c), and "V" (d).

[0024] Figure 5 (a) is a schematic diagram of rotating the sample four times in Example 3 and (b) is an electron microscope image of a cluster composed of four metal nanodisks of chromium, titanium, silver and gold, wherein the upper right corner of Figure b is an energy spectrum of the four metal nanodots.

[0025] Figure 6 The cross-sectional electron micrographs of the non-closely packed PS sphere templates with heights of 414 nm (a), 985 nm (b), and 1347 nm (c) in Example 4, electron micrographs of nanorings prepared using the above three templates (df), atomic force micrographs of nanorings prepared using the above three templates (gi), a schematic diagram of regulating the shape of the nanorings (j), and a plot of the experimental values ​​of the radius of the nanorings prepared using the above three templates and the straight line obtained from the theoretical formula (k).

[0026] Figure 7 Electron microscope images of the front (a) and cross-section (b) of the silicon nanotube in Application Example 1. DETAILED DESCRIPTION

[0027] The present invention provides a method for realizing nanostructure writing by manipulating the macroscopic movement trajectory of a substrate, comprising: using a micrometer-scale object to support a mask plate in the air on a substrate, and during a vapor deposition or sputtering process, by controlling the macroscopic movement trajectory of the substrate, allowing the vaporized or sputtered material to pass through the mask plate to form a micro-nanostructure on the substrate surface that is the same as the macroscopic movement trajectory of the substrate and has a reduced size.

[0028] Or use a micron-scale object to support the mask on the substrate. During the ion beam etching or photolithography process, by controlling the macroscopic movement trajectory of the substrate, the ion beam or light beam passes through the mask to etch a micro-nano structure on the substrate surface with the same size as the macroscopic movement trajectory of the substrate.

[0029] Figure 1 FIG. 1 is a schematic diagram showing the principle of the method of the present invention using evaporation as an example. Figure 1 As shown in the figure, the nano-grid as a mask is supported on the substrate by non-densely arranged micro-balls. During the thermal evaporation process, the nano-grid divides the metal vapor flow into millions of particle beams, as shown in the figure. Figure 1As shown in Figure a, as the substrate moves on the sample stage at a macro scale, the nanoparticle beam draws a nanoscale pattern on the surface of the substrate that is the same as the substrate's moving trajectory, realizing the conversion of the "large size" of the macroscopic moving trajectory to the "small size" of the nanopattern. For example, when the substrate moves along the outline of a macro letter, a corresponding nanoscale letter will be obtained on the surface of the substrate, as shown in the schematic diagram. Figure 1 b. As indicated Figure 1 As shown in c, according to the geometric relationship, the macroscopic moving distance AB of the substrate is H·tanθ1-H·tanθ2, and the corresponding moving distance of the nanodots is A′B′=h·tanθ1-h·tanθ2, where H and h represent the distance from the evaporation source to the nanomesh and the distance from the nanomesh to the substrate, respectively. Therefore, the reduction factor of the nanopattern relative to the macroscopic moving trajectory is equal to the distance from the nanomesh to the evaporation source divided by the distance from the nanomesh to the substrate. Theoretically, the size of the nanopattern can be arbitrarily reduced by reducing the distance from the nanomesh to the substrate. When the substrate rotates continuously during the thermal evaporation process, a nanoring structure will be formed on the surface of the substrate, as shown in the schematic diagram. Figure 1 d. The inner diameter and outer diameter of the ring can be controlled by controlling the spacing between the holes in the nanogrid and the distance from the nanogrid to the substrate. Therefore, the method of the present invention only needs to design the macroscopic motion trajectory of the substrate in advance according to the shape of the desired nanopattern, and the writing of nanostructures of arbitrary shapes on a microscopic scale can be achieved. By changing the material used for the evaporation source, the composition of the micro-nano pattern can be controlled.

[0030] It is foreseeable that the same effect will occur during ion beam etching or photolithography.

[0031] In addition, it should be pointed out that in order to change the angle between the moving substrate and the source (evaporation source, sputtering source, ion source or light source) and achieve trajectory reduction, the macroscopic movement trajectory of the substrate is not on a spherical surface with the source (evaporation source, sputtering source, ion source or light source) as the center.

[0032] In the following, in conjunction with the accompanying drawings, the present invention is further described by taking PS microspheres as micrometer-scale objects, fixing silver nano-grids as a mask on a substrate through air separation by thermal evaporation to manipulate the movement trajectory of a macroscopic substrate to design and prepare micro-nano structures as an example.

[0033] Example 1

[0034] 1. Preparation of nanogrids:

[0035] Cut the glass sheet into 1.5cm×1.5cm size, and ultrasonically clean it in anhydrous ethanol and deionized water for 10 minutes in turn. Then use oxygen plasma to hydrophilize the surface of the glass, and spin coat 10μL of PS microsphere emulsion with a mass fraction of 2.5wt% and a diameter of 500nm on the surface of the glass sheet. The speed of the spin coater is 2000rpm / min, and the spin coating time is 30s. After drying at room temperature, the glass sheet covered with PS microspheres is obliquely inserted into deionized water with a density of 700μL of sodium dodecyl sulfate (SDS) of 0.005g / mL. The PS balls assemble into a hexagonal, tightly packed single-layer array and float on the water surface. The hydrophilized glass sheet of 1.5cm×1.5cm is placed at a 45° angle to the water surface to pick up the PS balls floating on the water surface. After drying at room temperature, a tightly packed single-layer PS ball template with a diameter of 500nm is obtained, such as scanning electron microscopy. Figure 2 The densely packed PS sphere template was etched with oxygen plasma for 1 h to reduce the size of the PS spheres. The etching power was 85 W and the O2 flow rate was 50 sccm. The non-densely packed PS sphere template was obtained as shown in the scanning electron microscope. Figure 2 b. The non-closely arranged PS ball template was placed in a thermal evaporator, and 100 nm of silver was evaporated at a rate of 0.1 nm / s. It was then placed in a dichloromethane solution and ultrasonicated for 10 min to remove the PS balls, resulting in a silver nanogrid tightly attached to the glass sheet, as shown in scanning electron microscopy 2c. The spacing between the holes in the silver nanogrid was 500 nm.

[0036] 2. Preparation of non-densely arranged supported microspheres on substrate:

[0037] The same method as step 1 was used to obtain a PS sphere template with a diameter of 2 μm and a silicon wafer as the substrate. The template was etched by oxygen plasma for 90 min to obtain a PS sphere template with a non-dense arrangement. The height of the template was determined to be 985 nm by cross-sectional scanning.

[0038] 3. Transfer the nanogrid to the supporting microsphere template:

[0039] like Figure 2 As shown in Figure e, 2g of ammonium fluoride and 5mL of a 40wt% hydrofluoric acid solution are added to 50mL of deionized water to prepare a BOE buffer solution. The silver nanomesh obtained in step 1, which is tightly attached to the glass sheet, is placed in the above-mentioned BOE buffer solution and soaked for 3 minutes. After being taken out and naturally dried, it is inserted obliquely into deionized water. The silver nanomesh is separated from the glass sheet and floats on the water surface. The non-tightly arranged PS ball template obtained in step 2 is placed at 45° to the water surface to pick up the silver nanomesh floating on the water surface. After drying at room temperature, the non-tightly arranged PS balls prop up the silver nanomesh, making it suspended in the air above the silicon wafer, as shown in a scanning electron microscope. Figure 2 As shown in (d), the distance from the silver nanomesh to the silicon wafer is the height of the non-closely packed PS sphere template, i.e., 985 nm.

[0040] 4. Design the substrate's moving trajectory according to the desired nanostructure shape and perform thermal evaporation of the material:

[0041] Place the three samples prepared in step 3 on the sample stage of the thermal evaporator and evaporate 50nm of silver. After the evaporation is completed, move the three samples 4.5cm, 5.5cm and 10cm respectively and evaporate 50nm of silver again. As the samples move, the nanoparticle beam divided by the silver nanogrid deposits two nanodisks on the sample surface, as shown in the electron microscope. Figure 3 As shown in a-3c, the distances between the two nanodots in the above sample are 137.76nm, 166.62nm, and 288.76nm respectively. Figure 1 As shown in Figure c, according to the geometric relationship, the ratio of the distance moved by the nanodisk to the distance translated by the sample is equal to the distance from the evaporation source to the silver nanogrid divided by the distance from the nanogrid to the substrate. The distance from the silver nanogrid to the substrate is 985nm, and the distance from the evaporation source to the silver nanogrid is 33.5cm. In other words, every time the sample translates 1cm, the nanodisk moves 29.4nm. In theory, the distance between each two nanodots in the above three samples is 132.3nm, 161.7nm, and 294nm, respectively, which is consistent with the experimentally measured data. When the sample translates 4.5cm, the two nanodisks overlap; when the sample translates 5.5cm, the two nanodisks are just separated, and the gap between the nanodots is approximately 6nm; when the sample translates 10cm, the two nanodots are clearly separated. According to the theory, the relative position of the two nanodots can be precisely controlled by the above method.

[0042] Example 2

[0043] 1. Preparation of nanogrids:

[0044] The same method as step 1 in Example 1 was used to obtain a closely packed PS sphere template with a diameter of 1 μm, and the substrate was a glass sheet. The PS sphere template was isotropically etched by oxygen plasma for 2 h to reduce the size of the PS spheres, thereby obtaining a non-closely packed PS sphere template. The non-closely packed PS sphere template was placed in an evaporator, and 100 nm of silver was evaporated, with the evaporation rate maintained at 0.1 nm / s. It was then placed in a dichloromethane solution and ultrasonicated for 10 min to remove the PS spheres, thereby obtaining a silver nanomesh tightly attached to the glass sheet, with the spacing between the holes in the nanomesh being 1 μm.

[0045] 2. Preparation of non-densely arranged supported microspheres on substrate:

[0046] A 10wt% PS sphere emulsion with a diameter of 5μm and anhydrous ethanol were ultrasonically treated for 10 minutes in a ratio of 1:1 to prepare a mixed solution of PS sphere emulsion and anhydrous ethanol. A culture dish and a glass sheet of 2.5cm×2.5cm were treated with oxygen plasma for hydrophilicity, and the glass sheet was placed in the culture dish with the hydrophilic side facing up. The needle of the infusion tube was glued to the side of the culture dish, and the needle was slowly injected into the culture dish with deionized water. When the liquid level in the culture dish was flush with the glass sheet, 400μL of the mixed solution of PS sphere emulsion and anhydrous ethanol was slowly dripped on the surface of the glass sheet with a pipette. When the deionized water filled the culture dish, 700μL of SDS solution with a density of 0.005g / mL was added, and at this time, 5μm PS spheres were assembled into a hexagonal tightly arranged monolayer array floating on the water surface. The PS spheres floating on the water surface were picked up from a hydrophilic silicon wafer of 1.5 cm × 1.5 cm at a 45° angle to obtain a densely packed PS sphere template with a diameter of 5 μm. The template was etched with oxygen plasma for 3 hours to obtain a non-densely packed PS sphere template, and the height of the template was determined to be 1347 nm by cross-sectional scanning.

[0047] 3. Transfer the nanogrid to the supporting microsphere template:

[0048] The same method as step 3 in Example 1 was used to transfer the nanonet with a pore spacing of 1 μm to the surface of the non-closely arranged PS sphere template obtained in step 2, wherein the distance from the nanonet to the silicon wafer was 1347 nm.

[0049] 4. Design the substrate's moving trajectory according to the desired nanostructure shape and perform thermal evaporation of the material:

[0050] Move the sample obtained in step 3 to five points 1, 2, 3, 4, and 5 along the outline of the letter "W" on a macro scale on the sample stage of the thermal evaporator, as shown in the figure. Figure 4 As shown in Figure Ⅰ, 50 nm of silver was evaporated at each position to form five points of the letter "W" on the surface of the silicon wafer, as shown in the scanning electron microscope. Figure 4 b. The distance from the nanogrid to the silicon wafer is 1347nm, and the distance from the nanogrid to the evaporation source is 33.5cm, which means that for every 1cm the sample moves, the corresponding nanodot should move 40.09nm. The distance from point 1 to point 3 on the sample stage is 10cm. The theoretical distance between nanodots 1 and 3 is 400.09nm, which is quite consistent with the experimentally measured 403nm. Similarly, the sample is moved to points 1, 2, and 3 along the outline of the macroscopic letter "L" on the sample stage of the thermal evaporator, as shown in the diagram. Figure 4As shown in II of a, 50nm of silver was evaporated at each position to form the corresponding nanoscale letter "L" on the surface of the silicon wafer, as shown by scanning electron microscope Figure 4 c. Similarly, move the sample on the sample stage of the thermal evaporator along the outline of the letter "V" on the macro scale to points 1, 2, and 3 in sequence, as shown in the diagram. Figure 4 50 nm of silver was evaporated at each position to form a corresponding nanoscale letter "V" on the surface of the silicon wafer, as shown in the scanning electron microscope. Figure 4 Therefore, in the method of the present invention, it is only necessary to design the macroscopic moving track of the sample during the thermal evaporation process according to the shape of the desired micro-nano pattern, so as to realize arbitrary writing on the nanoscale.

[0051] Example 3

[0052] 1. Preparation of nanogrids:

[0053] The same method as step 1 in Example 2 was used to obtain a silver nanogrid closely attached to the glass sheet, wherein the spacing between the holes in the nanogrid was 1 μm.

[0054] 2. Preparation of non-densely arranged supported microspheres on substrate:

[0055] The same method as step 2 in Example 2 was used to obtain a non-densely arranged PS sphere template with a diameter of 5 μm. The substrate was a silicon wafer and the height of the template was 1347 nm.

[0056] 3. Transfer the nanogrid to the supporting microsphere template:

[0057] The silver nanogrid with a pore spacing of 1 μm was transferred to the surface of the non-closely arranged PS ball template obtained in step 2 by the same method as step 3 in Example 1, wherein the distance from the silver nanogrid to the silicon wafer was 1347 nm.

[0058] 4. Design the substrate's moving trajectory according to the desired nanostructure shape and perform thermal evaporation of the material:

[0059] Place the sample obtained in step 3 on the sample stage of the thermal evaporator at the same position and rotate it 4 times with a rotation angle of 90°. Then evaporate 50nm of Cr, Ti, Ag, and Au in sequence, as shown in the figure. Figure 5 a. The nanoparticle beams divided by the silver nanogrid form clusters of the above four metal nanodisks on the surface of the silicon wafer, as shown in the scanning electron microscope image and energy spectrum. Figure 5 b. Therefore, by replacing the evaporation source, this method can flexibly regulate the material composition of the micro-nano structure.

[0060] Example 4

[0061] 1. A silver nanogrid closely attached to the surface of a glass sheet was obtained by the same method as step 1 in Example 1, wherein the spacing between holes in the silver nanogrid was 500 nm.

[0062] 2. Use the same method as step 1 in Example 1 to obtain a closely packed PS sphere template with a diameter of 1 μm and a closely packed PS sphere template with a diameter of 2 μm. Use the same method as step 1 in Example 2 to obtain a closely packed PS sphere template with a diameter of 5 μm. Use oxygen plasma to isotropically etch the PS sphere template with a diameter of 1 μm and the PS sphere template with a diameter of 2 μm for 90 minutes, and treat the PS sphere template with a diameter of 5 μm for 3 hours, and obtain a series of non-closely packed PS sphere templates with heights of 414 nm, 985 nm, and 1347 nm, respectively. Figure 6 a-6c are cross-sectional electron microscope images of the above templates.

[0063] 3. Using the same method as step 3 in Example 1, transfer the silver nanogrid with a pore spacing of 500 nm to the surface of a series of non-closely arranged PS ball templates obtained in step 2.

[0064] 4. Fix the PS ball template with different heights of the suspended silver nano-grid on top obtained in step 3 on the sample stage of the thermal evaporator, evaporate 50nm of silver, and rotate the sample stage continuously during the thermal evaporation process. During the sample rotation process, the nanoparticle beams divided by the silver nano-grid draw nano-ring structures on the surface of the silicon wafer. Figure 6 d-6f are electron microscope images of the nanorings in the above three samples, Figure 6 g-6i are the atomic force microscopy images of the nanorings in the above three samples. As the height of the PS sphere template increases from 414nm to 1347nm, the radius of the ring gradually increases until the adjacent rings overlap when the height reaches 1347nm. Figure 6 As shown in Figure 1, d and r are the wall thickness and radius of the ring, respectively, which are important parameters for us to control the shape of the ring. The width d of the ring is approximately equal to the diameter of the particle beam, and the diameter of the particle beam is determined by the diameter D of the holes in the silver nanomesh, so the thickness of the ring can be controlled by controlling the size of the holes in the nanomesh. According to the geometric similarity relationship, the radius of the ring Where R and H represent the horizontal distance and vertical distance from the evaporation source to the silver nano-grid, respectively. In this embodiment, R and H in the thermal evaporator are equal to 6.5 cm and 33.5 cm, respectively. After conversion, r = 0.194h. Therefore, the radius of the ring can be controlled by controlling the distance between the silver nano-grid and the substrate. Figure 6As shown in k, the radius of the nanoring obtained from the above three samples is compared with the straight line drawn according to this formula, and the two are in good agreement. Therefore, by controlling the diameter of the holes in the silver nanomesh and the distance from the silver nanomesh to the substrate, the method of the present invention can design the shape of the nanoring as needed.

[0065] Application Example 1

[0066] The nano-rings obtained from the silicon wafer obtained in Example 4 after removing the PS balls are used as a mask to further anisotropically etch the silicon substrate to obtain a silicon nanotube structure, such as Figure 7 7a and 7b are electron microscope images of the front and cross-section of the prepared silicon nanotubes, respectively. The etching gas is 25sccm SF6 and 25sccm C4F8, the pressure of the reaction chamber is 20mTorr, the ICP power and RF power are 100W and 30W respectively, and the reaction time is 150s. By controlling the shape of the ring and changing the etching time, the height and inner and outer diameters of the silicon nanotubes can be adjusted.

[0067] Finally, it should be pointed out that the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for designing and preparing a micro-nanostructure by manipulating the movement trajectory of a macroscopic substrate, characterized in that: include: A micrometer-scale object is used to support the mask on the substrate in the air. During the evaporation or sputtering process, the macroscopic movement trajectory of the substrate is controlled so that the evaporated or sputtered material passes through the mask to form a micro-nano structure on the substrate surface with the same macroscopic movement trajectory as the substrate and reduced in size. The macroscopic movement trajectory of the substrate is not on a spherical surface with the evaporation source or the sputtering source as the sphere center; Or a micrometer-scale object is used to support the mask on the substrate. During the ion beam etching or photolithography process, the macroscopic movement trajectory of the substrate is controlled so that the ion beam or light beam passes through the mask to etch a micro-nano structure on the substrate surface that is the same as the macroscopic movement trajectory of the substrate but with a reduced size; the macroscopic movement trajectory of the substrate is not on a spherical surface with the ion source or light source as the center of the sphere.

2. The method according to claim 1, characterized in that: The micrometer-scale object is a micrometer ball or a nanometer column prepared by a photolithography process.

3. The method according to claim 1, characterized in that: The pattern of the mask is circular, strip-shaped and / or any other shape.

4. The method according to claim 1, characterized in that: The method of using a micrometer-scale object to support a mask on a substrate in the air is specifically as follows: fixing the micrometer-scale object on the substrate, and then transferring the mask to the substrate with the micrometer-scale object fixed thereon by a film transfer method.

5. The method according to claim 1, characterized in that: The reduction factor of the micro-nano structure relative to the macroscopic moving track is equal to the ratio of the distance from the mask to the substrate to the distance from the evaporation source, sputtering source or ion source to the mask.

6. The method according to claim 1, characterized in that: The method for controlling the macroscopic movement trajectory of the substrate is to move the substrate intermittently and / or to move the substrate continuously.

7. The method according to claim 1, characterized in that: The surface of the substrate is smooth and / or concave-convex.

Citation Information

Patent Citations

  • Preparation method of noble metal nano-particle array

    CN102747320A

  • High-precision shadow-mask-deposition system and method therefor

    CN109642309A