Sealing method and metal plate body

By using friction stir welding technology with acute angles and vacuum injection method on the pipe side walls of the temperature uniform plate, the problem of sealing large-thickness temperature uniform plates in the prior art is solved, and a smaller invalid width is achieved and better sealing method.

CN114535777BActive Publication Date: 2024-11-12FEICHENG TECH (FOSHAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210298916.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-25
Publication Date
2024-11-12
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

The existing friction stir welding temperature uniform plate sealing method has the problem that the sealing width is wide and it is difficult to seal the large thickness temperature uniform plate.

Method used

Using the design of the angle α between the two ends of the pipe and the direction of the stirring head as an acute angle, friction stir welding is performed along the side wall of the opened pipe to ensure that the welding point is continuously sealed, and the working medium is vacuumed through the filling pipe before welding. Improve sealing effect.

Benefits of technology

It realizes a smaller ineffective width seal for large-thick temperature uniform plates, improves the sealing effect, and is suitable for superconducting plates and other metal welding processes that need to avoid atmospheric contact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114535777B_ABST
    Figure CN114535777B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of metal processing technology, and discloses a sealing method, wherein the processing object of the method is a plate body made of metal material with a cavity inside, and the method is specifically as follows: Step 1: a pipe with one end extending to the cavity and at least one end extending to the atmosphere is opened on any side of the outer frame of the plate body; Step 2: a stir friction welding method is used to weld along the end face of the side wall where the pipe is opened to close the pipe; the angle α between the connecting line of the two ends of the pipe and the traveling direction of the stirring head for welding is an acute angle; the lower end of the stirring head has a preset distance from the inner cavity and is lower than the height of one end of the pipe connected to the atmosphere. The sealing method has no requirements for the thickness of the frame of the temperature equalizing plate, can produce a smaller invalid width, and is particularly suitable for large-thickness temperature equalizing plates. At the same time, the present invention also discloses a plate body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal processing, and more specifically, relates to a sealing method and a metal plate body. Background Art

[0002] Application No. CN201911408682.9 discloses a method for sealing a temperature-maintaining plate using stir friction welding. Since the welding depth of stir welding usually does not exceed 1 / 3 of the weld width, this sealing method has the problem of a wide sealing width and difficulty in sealing a temperature-maintaining plate with a large thickness. Summary of the invention

[0003] The main purpose of the present invention is to provide a sealing method, which has no requirements on the thickness of the frame of the temperature equalizing plate, can produce a smaller invalid width, and is particularly suitable for temperature equalizing plates with large thickness.

[0004] The invention is not only applicable to the manufacture of superconducting plates, but also applicable to any metal welding process that needs to avoid contact with the atmosphere.

[0005] Meanwhile, the invention also discloses a plate body.

[0006] According to a first aspect of the present invention, a sealing method is provided, wherein the processing object of the method is a metal plate having a cavity inside, and the method is specifically as follows:

[0007] Step 1: Open a pipe on any side of the outer frame of the plate body, with one end extending to the cavity and at least one end extending to the atmosphere;

[0008] Step 2: Use a friction stir welding method to weld along the end surface of the side wall of the pipeline to close the pipeline;

[0009] The angle α between the connecting line of the two ends of the pipeline and the moving direction of the stirring head for welding is an acute angle; the lower end of the stirring head has a preset distance from the inner cavity and is lower than the height of the end of the pipeline connected to the atmosphere.

[0010] The metal plate described in this embodiment is not limited to aluminum or aluminum alloy, but is actually also applicable to metal materials such as copper and iron.

[0011] The friction stir welding process of the present invention is a commonly used friction stir welding process and equipment in the art, and this embodiment does not impose too many restrictions on the process.

[0012] The angle α in the present invention refers to: the angle between the extension direction of the line to the atmosphere and the moving direction of the stirring head; the angle α can be selected to be 1°-60°, preferably 3° to 45°.

[0013] In the present invention, the board body is divided into a front side, a rear side, a left frame, a right frame, an upper frame, and a lower frame (for a non-square board body, it can be divided into a front side, a rear side, and a side frame), and the end face of the side wall refers to the side of the frame of the board body (which can be any of the left frame, the right frame, the upper frame, the lower frame, and the side frame) that is not connected to the front side and the rear side.

[0014] In the above sealing method, the plate body is a rectangular, square, circular, elliptical or irregularly shaped plate body.

[0015] In the above sealing method, the material of the plate body is aluminum alloy or pure aluminum.

[0016] In the above-mentioned sealing method, the plate body is a plate body having at least one corner;

[0017] The pipe is a T-shaped pipe; the pipe has two ends extending to the atmosphere; one end is located on one side of the angle, and the other end is located on the other side of the angle;

[0018] The stirring head is welded along one side of the corner and the end of the pipe on this side that is connected to the atmosphere is sealed with metal melt in advance.

[0019] Of course, the T-shaped pipe is not limited to the above-mentioned plate body, and is applicable to circular, elliptical or irregularly shaped plates.

[0020] In addition, the pipeline can also be a straight pipeline, which is applicable to the plate bodies of any specifications mentioned above.

[0021] In the above sealing method, after step 1 and before step 2, the method further includes:

[0022] Step 10: Connect a hard filling pipe to the end of the pipe, evacuate the inside of the cavity through the filling pipe, then inject the working medium into the cavity, and finally close the filling pipe;

[0023] After step 2, remove the filling pipe.

[0024] In the above-mentioned sealing method, the distance between the lower end of the stirring head and the surface of the outer frame of the plate body is 0.3-0.8 times the thickness of the outer frame of the plate body.

[0025] In the above-mentioned sealing method, the angle α between the connecting line of the two ends of the pipe and the moving direction of the stirring head for welding is 3° to 45°.

[0026] At the same time, the present invention also discloses a metal plate body, wherein the metal plate body is a plate body having a cavity inside, and is processed by any of the above methods;

[0027] The pipeline in the plate body is partially closed by friction stir welding.

[0028] One of the above technical solutions of the present invention has at least one of the following advantages or beneficial effects:

[0029] CN201911408682.9 shows a welding method in which the pipeline and the stirring head are perpendicular to each other in their traveling directions. Due to the ratio between the welding width and the welding depth, the resulting problem is that for thicker plates, the frame width increases. At the same time, this welding method has only one sealing point, and the sealing effect is questionable.

[0030] This case adopts a design in which the angle α between the connecting line at both ends of the pipeline and the moving direction of the stirring head for welding is an acute angle. When the stirring head moves, it contacts part of the pipeline, and welding is performed from the end face of the outer frame of the plate body. There is no limit to the width of the outer frame of the plate body, and the welding point will continuously seal a section of the pipeline, with a good sealing effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The present invention is further described below in conjunction with the accompanying drawings and embodiments;

[0032] Figure 1 is a structural diagram after processing in step 1 of embodiment 1 of the present invention;

[0033] Figure 2 1 is a schematic diagram of welding in step 2 of embodiment 1 of the present invention (the filling pipeline is omitted);

[0034] Figure 3 It is a welding schematic diagram of step 2 of embodiment 2 of the present invention (the filling pipeline is omitted). DETAILED DESCRIPTION

[0035] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements having the same or similar functions from beginning to end. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0036] The following disclosure provides many different embodiments or examples for implementing different solutions of the present invention.

[0037] Example 1

[0038] Reference Figure 1 and 2As shown, a sealing method is shown, wherein the processing object of the method is a plate body made of pure aluminum with a cavity inside, and the plate body is rectangular. However, in fact, this embodiment can be used for plates of any shape. The plate body of this embodiment includes: a front side surface 1, a rear side surface, and an outer frame 2. The side of the outer frame 2 that is not connected to the front side surface 1 and the rear side surface is an end surface 3 of the outer frame 2. The outer frame 2 of this embodiment is a rectangular outer frame.

[0039] The method is specifically as follows:

[0040] Step 1: A pipe 4 is opened on any side of the outer frame 2 of the plate body, one end of the pipe extending to the cavity, at least one end of the pipe extending to the end surface of the outer frame 2 and connected to the atmosphere;

[0041] The pipeline 4 is a straight pipeline 4, and the angle between the extension direction of the pipeline 4 to the atmosphere and the extension direction of the end surface of the side wall where the pipeline 4 is located is about 10°;

[0042] The cavity may be a cavity with capillary grooves on the inner wall, or may be a smooth cavity;

[0043] The cavity of this embodiment is filled with a medium that can change phase at the working temperature. In order to improve the thermal conductivity, non-condensable gases such as oxygen and nitrogen should be avoided in the medium. Therefore, during the filling and sealing processes, strict attention should be paid to isolation from the atmosphere. Based on this background, a sealing solution for this case is proposed.

[0044] Step 10: Connect a hard filling pipe 5 to the end of the pipe 4 by welding, evacuate the inside of the cavity through the filling pipe 5, then inject the working medium into the cavity, and finally close the filling pipe 5;

[0045] The filling pipe 5 can be closed by clamping it flat, or by adding a valve to the filling pipe 5, and closing the valve means closing the filling pipe 5.

[0046] Step 2: Using a friction stir welding method, welding is performed along the end surface of the side wall of the pipeline 4 to close the pipeline 4;

[0047] The size of the molten pool formed by the specifications of the stirring head 6 is larger than the diameter of the pipe 4;

[0048] The moving direction of the stirring head 6 is: firstly extending through the pipe 4 to the position of one end of the cavity, and then continuing to move forward.

[0049] The lower end of the stirring head 6 has a preset distance from the inner cavity and is lower than the height of the end of the pipeline 4 connected to the atmosphere.

[0050] The preset distance can be calculated according to the following provisions: the distance between the lower end of the stirring head 6 and the surface of the outer frame 2 of the plate body is 0.3 times the thickness of the outer frame 2 of the plate body.

[0051] Step 20: Cut and remove the filling pipe 5.

[0052] Example 2

[0053] refer to Figure 3 , which is substantially the same as Embodiment 1, except that: the pipe 4 is a T-shaped pipe 4; the pipe 4 has two ends extending to the atmosphere; one end is located on one side of the corner, and the other end is located on the other side of the corner;

[0054] The stirring head 6 is welded along one side of the corner and the end of the pipe 4 on this side that is connected to the atmosphere is sealed with the metal melt 7 in advance.

[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A sealing method, wherein the processing object of the method is a metal plate with a cavity inside, characterized in that: The method is specifically as follows: Step 1: Open a pipe on any side of the outer frame of the plate body, with one end extending to the cavity and at least one end extending to the atmosphere; Step 2: Use a friction stir welding method to weld along the end surface of the side wall of the pipeline to close the pipeline; The angle α between the connecting line of the two ends of the pipeline and the traveling direction of the stirring head for welding is an acute angle; the lower end of the stirring head is at a preset distance from the inner cavity and is lower than the height of the end of the pipeline connected to the atmosphere; The angle α between the connecting line of the two ends of the pipeline and the moving direction of the stirring head for welding is 3° to 45°.

2. The sealing method according to claim 1, characterized in that: The plate body is a rectangular, square, circular, elliptical or irregularly shaped plate body.

3. The sealing method according to claim 1, characterized in that: The plate body is made of aluminum alloy or pure aluminum.

4. The sealing method according to claim 1, characterized in that: The plate body is a plate body having at least one corner; The pipe is a T-shaped pipe; the pipe has two ends extending to the atmosphere; one end is located on one side of the angle, and the other end is located on the other side of the angle; The stirring head is welded along one side of the corner and the end of the pipe on this side that is connected to the atmosphere is sealed with metal melt in advance.

5. The sealing method according to claim 1, characterized in that: After step 1 and before step 2, the following steps are also included: Step 10: Connect a hard filling pipe to the end of the pipe, evacuate the cavity through the filling pipe, then inject the working medium into the cavity, and finally close the filling pipe; After step 2, remove the filling pipe.

6. The sealing method according to any one of claims 1 to 5, characterized in that: The distance between the lower end of the stirring head and the surface of the outer frame of the plate body is 0.3-0.8 times the thickness of the outer frame of the plate body.

7. A metal plate, characterized in that: The metal plate body is a plate body having a cavity inside, and is processed by any method as claimed in claims 1-6; The pipeline in the plate body is partially closed by friction stir welding.