Method for manufacturing electrode lead and pouch type secondary battery

Through the design of the two-stage electrode leads, the problem of poor gas emissions in the bag-type secondary battery is solved, and safety and stability are improved, heat generation is reduced and the connection stability of the electrode leads is improved.

CN114556686BActive Publication Date: 2024-11-08LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080071654.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-20
Filing Date
2020-08-27
Publication Date
2024-11-08
Estimated Expiration
2040-08-27

AI Technical Summary

Technical Problem

The existing bag-type secondary batteries lack an effective gas emission mechanism, which leads to an increase in internal pressure, which may lead to shell damage, early operation of protection circuits, electrode deformation and explosion.

Method used

A two-stage electrode lead is adopted, the first electrode lead is connected to the electrode joint, and the second electrode lead is protruded outside the battery case, and is combined with the battery case through an insulating part, and an electroplating film is not formed at the connecting part to reduce the resistance.

Benefits of technology

Effectively discharge gas generated in the battery case, ensure safety, reduce heat generation, and improve the connection stability of the electrode leads by reducing resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114556686B_ABST
    Figure CN114556686B_ABST
Patent Text Reader

Abstract

A method for manufacturing an electrode lead for solving the problem according to one embodiment of the present invention includes the following steps: manufacturing a first electrode lead and a second electrode lead respectively; and forming a connection portion by bonding the first electrode lead and the second electrode lead to each other. The step of manufacturing the first electrode lead includes the following steps: unwinding a first metal plate from a first metal reel; attaching a first tape to a first connection area to be formed as a connection portion on the first metal plate for shielding; performing electroplating and surface treatment on the first metal plate; and removing the first tape. The step of manufacturing the second electrode lead includes the following steps: unwinding a second metal plate from a second metal reel; attaching a second tape to a second connection area to be formed as a connection portion on the second metal plate for shielding; performing electroplating and surface treatment on the second metal plate; and removing the second tape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an electrode lead and a pouch-type secondary battery, and more particularly, to a method for manufacturing an electrode lead, wherein the electrode lead is formed in two sections to discharge gas generated in a battery case to the outside to ensure safety, and wherein the resistance between the two-section electrode lead is reduced to reduce the heat that will be generated, and the present invention relates to a pouch-type secondary battery including the electrode lead. Background Art

[0002] Generally speaking, secondary batteries include nickel-cadmium batteries, nickel-metal hydride batteries, lithium-ion batteries and lithium-ion polymer batteries. Such secondary batteries are applied to and used in small products (such as digital cameras, P-DVDs, MP3Ps, mobile phones, PDAs, portable game devices, power tools, electric bicycles, etc.) and large products that require high power (such as electric vehicles and hybrid vehicles, power storage devices for storing surplus power or renewable energy, and backup power storage devices).

[0003] In order to manufacture an electrode assembly, a cathode (hereinafter referred to as a positive electrode), a separator and an anode (hereinafter referred to as a negative electrode) are manufactured and stacked. Specifically, a positive electrode active material slurry is applied to a positive electrode current collector, and a negative electrode active material slurry is applied to a negative electrode current collector to manufacture a positive electrode and a negative electrode. In addition, when a separator is inserted and stacked between the manufactured positive electrode and the manufactured negative electrode, a unit cell is formed. The unit cells are stacked on each other to form an electrode assembly. In addition, when the electrode assembly is housed in a specific housing and an electrolyte is injected, a secondary battery is manufactured.

[0004] Such secondary batteries are classified into pouch-type secondary batteries and can-type secondary batteries according to the material of the battery case that accommodates the electrode assembly. In the pouch-type secondary battery, the electrode assembly is accommodated in a pouch made of a flexible polymer material having a variable shape. In addition, in the can-type secondary battery, the electrode assembly is accommodated in a case made of a metal or plastic material having a predetermined shape.

[0005] The pouch-type battery case is manufactured by stretching a flexible pouch film to form a cup-shaped portion. When the cup-shaped portion is formed, the electrode assembly is accommodated in the accommodation space of the cup-shaped portion, and then the battery case is folded to seal the sealing portion, thereby manufacturing a secondary battery.

[0006] In a secondary battery, gas in the secondary battery may be generated due to internal short circuit, overcharge, over discharge, etc. Here, the gas may increase the internal pressure of the secondary battery, thereby causing problems such as weakening of the bonding force between components, damage to the housing of the secondary battery, premature operation of the protection circuit, deformation of the electrode, internal short circuit, explosion, etc. Therefore, in the case of a can type secondary battery, a protective member such as a CID filter and a safety vent is provided so as to physically interrupt the electrical connection when the internal pressure of the housing increases. However, in the case of a pouch type secondary battery according to the prior art, a protective member is not adequately provided. Summary of the invention

[0007] Technical issues

[0008] The object of the present invention to solve the above problems is to provide a method for manufacturing an electrode lead, which is formed in two sections to discharge the gas generated in the battery case to the outside to ensure safety, and wherein the resistance between the two-section electrode lead is reduced to reduce the heat generated, and the present invention provides a pouch-type secondary battery including the electrode lead.

[0009] The objects of the present invention are not limited to the above objects, but those skilled in the art will clearly understand other objects described herein from the following description.

[0010] Technical Solution

[0011] In order to achieve the above purpose, a method for manufacturing an electrode lead according to one embodiment of the present invention includes: a step of manufacturing each of a first electrode lead and a second electrode lead; and a step of combining the first electrode lead to the second electrode lead to form a connecting portion, wherein the step of manufacturing the first electrode lead includes: a step of unwinding a first metal plate from a first metal reel; a step of attaching a first tape for shielding on a first connecting area of ​​the first metal plate to form the connecting portion; a step of electroplating and surface treating the first metal plate; and a step of removing the first tape, wherein the step of manufacturing the second electrode lead includes: a step of unwinding a second metal plate from a second metal reel; a step of attaching a second tape for shielding on a second connecting area of ​​the second metal plate to form the connecting portion; a step of electroplating and surface treating the second metal plate; and a step of removing the second tape.

[0012] In addition, one end of the first electrode lead may be connected to the electrode tab, and the first connection region may be formed on the other end of the first electrode lead.

[0013] In addition, the second connection region may be formed on one end of the second electrode lead.

[0014] In addition, the step of manufacturing the first electrode lead may further include the step of cutting the first metal plate at regular intervals after the step of removing the first tape; and the step of manufacturing the second electrode lead may further include the step of cutting the second metal plate at regular intervals after the step of removing the second tape.

[0015] In addition, the step of manufacturing the first electrode lead may further include the step of cutting the first metal plate at regular intervals before the step of attaching the first tape for shielding, and the step of manufacturing the second electrode lead may further include the step of cutting the second metal plate at regular intervals before the step of attaching the second tape for shielding.

[0016] Furthermore, when the steps of the electroplating and the surface treatment are performed, a first film may be formed on the outer surface of the first metal plate, and a second film may be formed on the outer surface of the second metal plate.

[0017] Furthermore, in the step of performing electroplating and surface treatment, the surface treatment may include at least one of chromate treatment, zirconium oxide treatment, or titanium treatment.

[0018] In order to achieve the above purpose, a pouch-type secondary battery according to one embodiment of the present invention includes: an electrode assembly, in which electrodes and separators are stacked, the electrodes including a positive electrode and a negative electrode; a battery case having a pouch shape, the battery case being configured to accommodate the electrode assembly; an electrode tab, the electrode tab being connected to the electrode to protrude from one side of the electrode assembly; a first electrode lead, one end of the first electrode lead being connected to the electrode tab; a second electrode lead, one end of the second electrode lead being connected to the other end of the first electrode lead, and the other end of the second electrode lead protruding to the outside of the battery case; and a connecting portion, the connecting portion being configured to combine the first electrode lead and the second electrode lead with each other, wherein, in the first electrode lead, a first film is formed on an outer surface of the first electrode lead, and the first film is not formed on a first connecting region for forming the connecting portion, and in the second electrode lead, a second film is formed on an outer surface of the second electrode lead, and the second film is not formed on a second connecting region for forming the connecting portion.

[0019] Furthermore, the first film or the second film may include at least one of a chromate film, a zirconium oxide film, or a titanium film.

[0020] In addition, the pouch-type secondary battery may further include an insulating portion surrounding a portion of each of the first electrode lead and the second electrode lead to combine the first electrode lead and the second electrode lead with the battery case.

[0021] In addition, a bonding force between each of the first electrode lead and the second electrode lead and the connection portion may be smaller than a bonding force between each of the first electrode lead and the second electrode lead and the insulation portion.

[0022] In addition, the insulating portion may surround a portion where the first electrode lead and the second electrode lead are connected to each other via the connecting portion.

[0023] Furthermore, the insulating portion may be made of at least one of a thermoplastic resin, a thermosetting resin, and a photocurable resin having electrical insulating properties.

[0024] Furthermore, the connection portion may include a conductive material and a conductive polymer.

[0025] In addition, the connection portion may have a thickness of 1 μm to 500 μm.

[0026] Details of other implementations are included in the detailed description and accompanying drawings.

[0027] Beneficial Effects

[0028] According to the embodiments of the present invention, there are at least the following effects.

[0029] The electrode lead can be provided in plurality to form a two-stage electrode lead. In this way, even if gas is generated in the battery case to increase the internal pressure, the gas can be discharged to the outside to ensure safety.

[0030] Furthermore, even if plating and surface treatment are performed on the first electrode lead and the second electrode lead, a film may not be formed on the first and second connection regions connected to each other via the connection portion to reduce resistance.

[0031] The effects of the present invention are not limited to the above description, and therefore, more various effects are involved in this specification. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is an assembly diagram of a secondary battery according to one embodiment of the present invention.

[0033] Figure 2 is a perspective view of a secondary battery according to one embodiment of the present invention.

[0034] Figure 3is a perspective view showing a state in which the volume of a pouch-type secondary battery according to one embodiment of the present invention is expanded.

[0035] Figure 4 The invention relates to a pouch-type secondary battery according to an embodiment of the present invention. Figure 2 A partial cross-sectional view taken along line A-A'.

[0036] Figure 5 The pouch-type secondary battery according to one embodiment of the present invention is expanded in volume. Figure 2 A partial cross-sectional view taken along line A-A'.

[0037] Figure 6 is a flowchart illustrating a method for manufacturing a first electrode lead and a second electrode lead according to one embodiment of the present invention.

[0038] Figure 7 is a schematic diagram showing a state in which an adhesive tape is attached to a metal plate unwound from a metal reel according to one embodiment of the present invention.

[0039] Figure 8 1 is a schematic diagram showing a state in which an adhesive tape is peeled off from a metal plate unwound from a metal reel according to one embodiment of the present invention.

[0040] Fig. 9 1 is a schematic diagram showing a state in which a first electrode lead and a second electrode lead are coupled to each other according to one embodiment of the present invention.

[0041] Fig.10 is a schematic diagram showing a state in which a first electrode lead and a second electrode lead are combined with each other to completely manufacture a two-stage electrode lead according to one embodiment of the present invention.

[0042] Fig.11 is a flowchart illustrating a method for manufacturing a first electrode lead and a second electrode lead according to another embodiment of the present invention. DETAILED DESCRIPTION

[0043] The advantages and features of the present invention and its implementation methods will be explained by the following embodiments described with reference to the accompanying drawings. However, the present invention can be embodied in different forms and should not be construed as being limited to the embodiments described herein. On the contrary, these embodiments are provided to make this disclosure thorough and complete and to fully convey the scope of the present invention to those skilled in the art. In addition, the present invention is limited only by the scope of the claims. Throughout the text, similar reference numerals refer to similar elements.

[0044] Unless the terms used in the present invention are defined differently, all terms used herein (including technical and scientific terms) have the same meanings as generally understood by those skilled in the art. In addition, unless clearly and obviously defined in this description, the terms defined in the commonly used dictionaries are not ideally or excessively interpreted as having a formal meaning.

[0045] In the following description, technical terms are only used to explain specific exemplary embodiments, but do not limit the present invention. In this specification, unless otherwise mentioned, terms in the singular may include plural forms. The meaning of "include" and / or "includes" does not exclude other components other than the mentioned components.

[0046] Hereinafter, preferred embodiments will be described in detail with reference to the accompanying drawings.

[0047] Figure 1 is an assembly diagram of a secondary battery 1 according to one embodiment of the present invention, and Figure 2 is a perspective view of a secondary battery 1 according to one embodiment of the present invention.

[0048] like Figure 1 As shown in , a pouch-type secondary battery 1 according to one embodiment of the present invention includes an electrode assembly 10 in which electrodes such as a positive electrode and a negative electrode and a separator are stacked, and a pouch-type battery case 13 in which the electrode assembly 10 is accommodated.

[0049] In order to manufacture the pouch-type secondary battery 1, first, a slurry in which an electrode active material, a binder, and a plasticizer are mixed with each other is applied to a positive electrode collector and a negative electrode collector to manufacture electrodes such as a positive electrode and a negative electrode. The electrodes are stacked on both sides of a separator to manufacture an electrode assembly 10 having a predetermined shape. Then, the electrode assembly 10 is inserted into a battery case 13, and the battery case 13 is sealed after an electrolyte is injected into the battery case 13.

[0050] In particular, the electrode assembly 10 may be a laminated structure including two types of electrodes such as a positive electrode and a negative electrode and a separator, the separator being arranged between the electrodes to insulate the electrodes from each other, or being arranged on the left or right side of one electrode. The laminated structure may have various shapes, without being limited by the shape. For example, a cathode and an anode each having a predetermined standard may be laminated with a separator therebetween, or the laminated structure may be wound in the form of a jelly roll. Each of the two types of electrodes (i.e., the positive electrode and the negative electrode) has a structure in which an active material slurry is applied to an electrode current collector having a metal foil or metal mesh shape. The slurry may be formed by stirring a granular active material, an auxiliary conductor, a binder, and a plasticizer with an added solvent. The solvent may be removed in subsequent processing.

[0051] like Figure 1As shown in , the electrode assembly 10 includes an electrode tap 11. The electrode tap 11 is respectively connected to the positive electrode and the negative electrode of the electrode assembly 10 to protrude to the outside of the electrode assembly 10, thereby providing a path for electrons to move between the inside and the outside of the electrode assembly 10. The electrode current collectors of the electrode assembly 10 are each composed of a portion coated with an electrode active material and a distal portion (i.e., a non-coated portion) that is not coated with an electrode active material. In addition, each electrode tap 11 can be formed by cutting the non-coated portion or connecting a separate conductive member to the non-coated portion by ultrasonic welding. As shown in FIG. Figure 1 As shown in FIG. 1 , the electrode tabs 11 may protrude from one side of the electrode assembly 10 in the same direction, but the present invention is not limited thereto. For example, the electrode tabs 11 may protrude in different directions from each other.

[0052] In the electrode assembly 10, the electrode lead 12 for supplying power to the outside of the secondary battery 1 is connected to the electrode tab 11 by spot welding. The electrode lead 12 according to one embodiment of the present invention is provided in plurality to form a two-stage electrode lead 12. In addition, in the two-stage electrode lead 12, the first electrode lead 123 (see Figure 4 ) is connected to the electrode connector 11 of the electrode assembly 10, and the second electrode lead 124 (see Figure 4 ) protrudes to the outside of the battery case 13. A detailed description about the two-segment electrode lead 12 will be described later.

[0053] A portion of the electrode lead 12 is surrounded by the insulating portion 14. The insulating portion 14 may be arranged to be confined within the sealing portion 134, where the upper shell 131 and the lower shell 132 of the battery case 13 are thermally melted so that the electrode lead 12 is combined with the battery case 13. In addition, the power generated from the electrode assembly 10 can be prevented from flowing to the battery case 13 via the electrode lead 12, and the sealing of the battery case 13 can be maintained. Therefore, the insulating portion 14 may be made of a non-conductor having non-conductivity, which does not have conductivity. In general, although an insulating tape that is easily attached to the electrode lead 12 and has a relatively thin thickness is mainly used as the insulating portion 14, the present invention is not limited thereto. For example, various components can be used as the insulating portion 14, as long as these components can insulate the electrode lead 12.

[0054] The electrode lead 12 includes: a positive electrode lead 121, one end of which is connected to the positive electrode terminal 111 so as to extend in the direction in which the positive electrode terminal 111 protrudes; and a negative electrode lead 122, one end of which is connected to the negative electrode terminal 112 so as to extend in the direction in which the negative electrode terminal 112 protrudes. Figure 1As shown in , all the other ends of the positive electrode lead 121 and the negative electrode lead 122 protrude to the outside of the battery case 13. Therefore, the power generated in the electrode assembly 10 can be supplied to the outside. In addition, since the positive electrode tab 111 and the negative electrode tab 112 are formed to protrude in different directions, respectively, the positive electrode lead 121 and the negative electrode lead 122 can extend in different directions, respectively.

[0055] The positive electrode lead 121 and the negative electrode lead 122 may be made of different materials from each other. That is, the positive electrode lead 121 may be made of the same material as the positive electrode current collector (i.e., aluminum (Al) material), and the negative electrode lead 122 may be made of the same material as the negative electrode current collector (i.e., copper (Cu) material or copper material coated with nickel (Ni)). In addition, the portion of the electrode lead 12 protruding to the outside of the battery case 13 may be set as a terminal portion and electrically connected to an external terminal.

[0056] The battery case 13 is a bag made of a flexible material, in which the electrode assembly 10 is accommodated. Hereinafter, the case where the battery case 13 is a bag will be described. When a flexible bag-shaped film 135 is drawn using a punch or the like, a portion of the bag film 135 is stretched to form a cup-shaped portion 133 including a bag-shaped accommodation space 1331, thereby manufacturing the battery case 13. The battery case 13 accommodates the electrode assembly 10 so that a portion of the electrode lead 12 (i.e., the terminal portion) is exposed and then sealed. Figure 1 As shown in , the battery case 13 includes an upper case 131 and a lower case 132. A receiving space 1331 may be provided in the lower case 132, in which a cup-shaped portion 133 is formed to receive the electrode assembly 10, and the upper case 131 may cover the upper side of the receiving space 1331 so that the electrode assembly 10 is not separated to the outside of the battery case 13. In addition, the sealing portion 134 is sealed to seal the receiving space 1331. Here, the cup-shaped portion 133 having the receiving portion 1331 may be formed in the upper case 131 to receive the electrode assembly 10 in the upper portion. As shown in FIG. Figure 1 As shown in FIG. 1 , one side of the upper housing 131 and one side of the lower housing 132 may be connected to each other. However, the present invention is not limited thereto. For example, the upper housing 131 and the lower housing 132 may be separately manufactured to be separated from each other.

[0057] When the electrode lead 12 is connected to the electrode connector 11 of the electrode assembly 10 and an insulating portion 14 is provided on a portion of the electrode lead 12, the electrode assembly 10 can be accommodated in a accommodating space 1331 provided in the cup-shaped portion 133 of the lower shell 132, and the upper shell 131 can cover the accommodating space from the upper side. In addition, an electrolyte is injected, and a sealing portion 134 extending outward from the edges of the upper shell 131 and the lower shell 132 is sealed. The electrolyte can move lithium ions generated by the electrochemical reaction of the electrodes during charging and discharging of the secondary battery 1. The electrolyte may include a non-aqueous organic electrolyte that is a mixture of a lithium salt and a high-purity organic solvent or a polymer using a polymer electrolyte. As Figure 2 As shown in , the pouch type secondary battery 1 may be manufactured by the above method.

[0058] Figure 3 1 is a perspective view showing a state in which the volume of the pouch-type secondary battery 1 is expanded according to one embodiment of the present invention.

[0059] In general, the pouch-type secondary battery 1 may abnormally generate a large amount of gas due to heat caused by internal short circuit, overcharge, overdischarge, etc., external impact on the electrode assembly 10, and electrolyte decomposition and thermal runaway caused by heat. In addition, when the secondary battery is stored at high temperature, the electrochemical reaction between the electrolyte and the electrode active material is rapidly promoted by the high temperature, thereby generating gas.

[0060] In order to manufacture the pouch-type battery case 13, a flexible pouch film 135 is drawn using a punch or the like, and the cup-shaped portion 133 is recessed in the lower case 132. Drawing is performed by inserting the pouch film 135 into a press and applying pressure to the pouch film 135 via a punch to stretch the pouch film 135. As described above, the pouch film 135 is stretched to form the cup-shaped portion 133, thereby manufacturing the battery case 13. The pouch film 135 is formed by laminating a surface protective layer made of nylon resin or polyethylene terephthalate (PET), a gas barrier layer mainly made of an aluminum film (Al foil), and a sealant layer mainly made of a polymer such as polypropylene (PP) or polyethylene (PE).

[0061] However, if gas is generated in the battery case 13, since all layers have flexibility in the battery case 13, as shown in FIG. Figure 3 As shown in , the internal pressure of the secondary battery 1 increases due to the generated gas, thereby expanding the volume of the secondary battery 1. In addition, there are problems such as weakening of the bonding force between components, damage to the housing of the secondary battery 1, premature operation of the protection circuit, deformation of electrodes, internal short circuit, explosion, etc.

[0062] Figure 4 The invention relates to a pouch-type secondary battery according to an embodiment of the present invention. Figure 2 A partial cross-sectional view taken along line A-A'.

[0063] When gas is generated in the battery case 13 , the internal pressure of the secondary battery 1 increases, resulting in weakened bonding between components, damage to the case of the secondary battery 1 , premature operation of the protection circuit, deformation of electrodes, internal short circuit, explosion, etc.

[0064] In order to solve the above problems, in a pouch-type secondary battery 1 according to one embodiment of the present invention, as Figure 4 As shown in , the electrode lead 12 is provided in two sections. That is, the electrode lead 12 includes: a first electrode lead 123 connected to the electrode tap 11 of the electrode assembly 10; and a second electrode lead 124 protruding to the outside of the battery case 13. In addition, one surface of the other end of the first electrode lead 1230 and one surface of one end of the second electrode lead 1240 can be combined with each other by means of a connecting portion 15, thereby being connected to each other.

[0065] When the battery case 13 is normal, the first electrode lead 123 and the second electrode lead 124 must be stably connected to each other. When the secondary battery 13 expands, the first electrode lead 123 and the second electrode lead 124 must be easily detached from each other. Therefore, it is preferred that the first electrode lead 123 and the second electrode lead 124 are arranged on different planes so that the upper surface and the lower surface thereof are connected to each other, rather than the first electrode lead 123 and the second electrode lead 124 being arranged on the same plane so that the side surfaces thereof are connected to each other.

[0066] Preferably, the connection portion 15 for coupling the first electrode lead 123 and the second electrode lead 124 to each other has an extremely thin thickness of 1 μm to 500 μm. Therefore, even if a step portion is formed between the first electrode lead 123 and the second electrode lead 124, the size of the step portion is not too large.

[0067] As described above, a portion of the electrode lead 12 is surrounded by the insulating portion 14. Moreover, the electrode lead is combined with the battery case via the insulating portion 14. In the process of sealing the upper shell 131 and the lower shell 132, a relatively high pressure may be applied to the portion in contact with the electrode lead 12, thereby damaging the sealant layer of the battery case 13. Since the sealant layer is directly in contact with the electrode assembly 10 as described above, the sealant layer can have insulating properties. However, if the sealant layer is damaged, electricity may flow to the battery case 13 via the electrode lead 12. In particular, since the gas barrier layer of the battery case 13 is made of a metal such as aluminum, if the sealant layer is partially damaged to expose the gas barrier layer, electricity may easily flow due to contact with the electrode lead 12.

[0068] Therefore, the insulating part 14 can be made of a non-conductor with non-conductivity, which is non-conductive. In addition, the insulating part 14 has high mechanical strength and heat resistance. Therefore, the insulating part 14 may include, for example, a polyolefin-based resin, such as polypropylene (PP) or polyethylene (PE). In particular, polypropylene (PP) has excellent mechanical properties such as tensile strength, rigidity, surface hardness, wear resistance, heat resistance, and chemical properties such as corrosion resistance, and is therefore mainly used to manufacture the insulating part 14. In addition, acid-treated polypropylene can be provided to improve the bonding force of the insulating part 14. For example, acid-treated polypropylene and ordinary polypropylene can be mixed with each other, and polypropylene can be further mixed or only acid-treated polypropylene can be provided. Here, the acid-treated polypropylene can be maleic anhydride polypropylene (MAH PP).

[0069] Therefore, when the upper shell 131 and the lower shell 132 are thermally fused, the insulating portion 14 can maintain the shape, thereby preventing the electrode lead 12 and the gas barrier layer from contacting each other even if a part of the sealant layer is damaged. Therefore, the power generated from the electrode assembly 10 can be prevented from flowing to the battery case 13 via the electrode lead 12. In addition, the insulating portion 14 has a high bonding force. Therefore, the insulating portion 14 can be arranged to be confined in a sealing portion, where the upper shell 131 and the lower shell 132 are thermally melted, so that the electrode lead 12 is combined with the battery case 13. In general, the insulating portion 14 can be made of at least one of a thermoplastic resin, a thermosetting resin, and a photocurable resin having electrical insulation properties as a polymer resin. In general, although an insulating tape that is easily attached to the electrode lead 12 and has a relatively thin thickness is mainly used as the insulating portion 14, the present invention is not limited thereto. For example, various components can be used as the insulating portion 14 as long as these components can insulate the electrode lead 12.

[0070] like Figure 4 As shown in , the insulating portion 14 may surround all of the first electrode lead 123, the connecting portion 15, and the second electrode lead 124. If the first electrode lead 123 or the connecting portion 15 is not surrounded by the insulating portion 14, even if the battery case 13 expands, a repulsive force may not be applied to the first electrode lead 123 and the second electrode lead 124. The repulsive force will be described in detail below.

[0071] Figure 5 The pouch-type secondary battery according to one embodiment of the present invention is expanded in volume. Figure 2 A partial cross-sectional view taken along line A-A'.

[0072] As described above, when the internal pressure of the pouch type secondary battery 13 increases, the volume of the pouch type secondary battery 1 expands. Figure 5As shown in , the outer wall of the battery housing 13 moves outward. Here, the upper wall and the lower wall of the outer wall of the battery housing 13 may have a large area and are not sealed, resulting in higher flexibility. Therefore, the upper wall of the battery housing 13 may move upward, and the lower wall of the battery housing 13 may move downward. The outer wall of the battery housing 13 may move outward to apply a repulsive force to the first electrode lead 123 and the second electrode lead 124 connected by means of the insulating portion 14. Therefore, as the internal pressure of the battery housing 13 gradually increases, the moving force of the outer wall of the battery housing 13 may increase more, and the repulsive force applied to the first electrode lead 123 and the second electrode lead 124 increases more.

[0073] When the binding force between the first electrode lead 123 and the second electrode lead 124 is greater than the repulsive force, as shown in FIG. Fig. 9 As shown in , the first electrode lead 123 and the second electrode lead 124 can be detached from each other. Therefore, the electrical connection can be physically interrupted so that electricity can no longer flow. Here, detachment may mean that the adsorption or attachment parts are separated from each other. However, the bonding force between the first electrode lead 123 and the second electrode lead 124 and the connecting part 15 may be less than the bonding force between the first electrode lead 123 and the second electrode lead 124 and the insulating part 14. Therefore, when a repulsive force is applied to the first electrode lead 123 and the second electrode lead 124, the bonding force between the first electrode lead 123 and the second electrode lead 124 and the insulating part 14 can be maintained to maintain the sealing of the battery case 13, but the first electrode lead 123 and the second electrode lead 124 can be detached from each other.

[0074] When manufacturing the electrode lead 12, in order to make the insulating portion 14 easily bonded to the electrode lead 12 later, electroplating and surface treatment are performed on the metal plate to form a film on the outer surface. However, if the electroplating and surface treatment are performed before the first electrode lead 123 and the second electrode lead 124 are bonded to each other, the resistance in the bonded surface may increase because the films formed on the outer surface are bonded to each other after the first electrode lead 123 and the second electrode lead 124 are bonded to each other. On the contrary, if the electroplating and surface treatment are performed after the first electrode lead 123 and the second electrode lead 124 are bonded, the connecting portion 15 connecting the first electrode lead 123 and the second electrode lead 124 may be damaged.

[0075] Figure 6 is a flowchart illustrating a method for manufacturing the first electrode lead 123 and the second electrode lead 124 according to one embodiment of the present invention.

[0076] According to one embodiment of the present invention, even if plating and surface treatment are performed on the first electrode lead 123 and the second electrode lead 124, a film may not be formed on each of the first connection region 1231 and the second connection region 1241 connected to each other via the connection portion 15 to reduce resistance.

[0077] To this end, the method for manufacturing the electrode lead 12 according to one embodiment of the present invention includes: the step of manufacturing each of the first electrode lead 123 and the second electrode lead 124; and the step of combining the first electrode lead 123 and the second electrode lead 124 to form a connection portion. The step of manufacturing the first electrode lead 123 includes: the step of unwinding the first metal plate 211 from the first metal reel 21; the step of attaching the first tape 21 to the first connection area 1231 of the first metal plate 211 where the connection portion is to be formed for masking; the step of electroplating and surface treatment on the first metal plate 211; and the step of removing the first tape 31, while the step of manufacturing the second electrode lead 124 includes: the step of unwinding the second metal plate 221 from the second metal reel 22; the step of attaching the second tape 32 to the second connection area 1241 of the second metal plate 221 where the connection portion is to be formed for masking; the step of electroplating and surface treatment on the second metal plate 211; and the step of removing the second tape 32.

[0078] In addition, according to one embodiment of the present invention, the pouch-type secondary battery 1 including the electrode lead 12 manufactured by the above method includes: an electrode assembly 10, in which electrodes (including a positive electrode and a negative electrode) and a separator are stacked; a battery case having a pouch shape, which is configured to accommodate the electrode assembly 10; an electrode tap 11, which is connected to the electrode so as to protrude from one side of the electrode assembly 10; a first electrode lead 123, one end of which is connected to the electrode tap 11; a second electrode lead 124, one end of which is connected to the other end of the first electrode lead 123, and the other end protrudes to the outside of the battery case; and a connecting portion, which is configured to combine the first electrode lead 123 and the second electrode lead 124 with each other. In the first electrode lead 123, a first film 1232 is formed on its outer surface, and the first film 1232 is not formed on the first connection area 1231 for forming a connection portion, and in the second electrode lead 124, a second film 1242 is formed on its outer surface, and the second film 1242 is not formed on the second connection area 1241 for forming a connection portion.

[0079] In the following, reference will be made to Figures 7 to 10 describe Figure 6 Each step is shown in the flow chart.

[0080] Figure 72 is a schematic diagram showing a state in which adhesive tapes 31 and 32 are attached to metal plates 211 and 221 unwound from metal reels 21 and 22 , respectively, according to one embodiment of the present invention.

[0081] In order to manufacture the two-stage electrode lead 12, first, the first electrode lead 123 and the second electrode lead 124 are separately manufactured. In addition, the first electrode lead 123 and the second electrode lead 124 are combined with each other to form a connection portion.

[0082] In order to manufacture the first electrode lead 123, first, the first metal plate 211 is unwound from the first metal reel 21 (S601). The first metal reel 21 is a reel wound with the first metal plate 211, and the first metal plate is unwound from the first metal reel 21 at a constant speed. Also, the first metal plate 211 serves as a raw material of the first electrode lead 123.

[0083] When the first metal plate 211 is unwound, the first adhesive tape 31 is attached to the first connection region 1231 to perform shielding (S602). As described above, one end of the first electrode lead 123 is connected to the electrode tap 11, and the other end is connected to one end of the second electrode lead 124. Therefore, the first connection region 1231 is formed on the other end of the first electrode lead 123 so as to be connected to the second electrode lead 124 later. In addition, as Figure 7 As shown in FIG. 2 , in the first metal plate 211, it is preferred that the first connection region 1231 is formed to stretch in the longitudinal direction along one edge of the first metal plate 211. Therefore, one piece of the first adhesive tape 31 can be attached to the first connection region 1231 at a time, without attaching the first adhesive tape 31 multiple times by cutting the first adhesive tape 31 into several pieces.

[0084] When the masking treatment of the first tape 31 is completed, surface treatments such as electroplating, oxidation and film treatment are performed on the first metal plate 211 (S603). If the electrode lead 12 serves as the positive lead 121 (as described above), the metal plates 211 and 221 can be made of the same aluminum (Al) material as the positive current collector. In addition, if the electrode lead 12 serves as the negative lead 122, the metal plates 211 and 221 can be made of the same copper (Cu) material as the negative current collector. Electroplating treatment is performed on the metal plates 211 and 221 with a metal such as nickel (Ni). The electroplating treatment is not limited to electroplating or electroless plating, and can be performed in various ways.

[0085] When the electroplating treatment is completed, surface treatment is performed to prevent oxidation of the metal plates 211 and 221 and to improve the bonding force with the insulating portion 14. The surface treatment can be a chromate treatment using chromium. Chromate treatment is a chemical film treatment in which an insoluble chromate (chromate) film containing a chromium component is thinly formed on the metal surface. To this end, the metal plates 211 and 221 are immersed in an aqueous solution containing chromium ions. As a result, the chromium ions undergo an oxidation reaction and insoluble chromium oxide is produced on the outer surface of each of the metal plates 211 and 221, thereby forming a chromate film. Here, there is no restriction on chromium ions, and various types of ions, such as hexavalent or trivalent ions, can be used. In addition, various non-restrictive materials such as chromic anhydride, chromium nitrate, chromium sulfate, chromium acetate and chromium chloride can be used as an aqueous solution containing chromium ions.

[0086] The surface treatment may be a non-chromate treatment using a material other than chromium. Here, the material other than chromium may be, for example, zirconium. If a zirconium oxide treatment using zirconium is performed, the metal plates 211 and 221 are immersed in an aqueous solution containing zirconium ions. As a result, the zirconium ions undergo an oxidation reaction, and zirconium oxide is generated on one surface 1521 of the metal plates 211 and 221, thereby forming a zirconium oxide film. The non-chromate treatment is not limited thereto, and may include a titanium treatment using titanium. That is, the surface treatment of the metal plates 211 and 221 may not be limited, but may be implemented in various ways.

[0087] Figure 8 1 is a schematic diagram showing a state in which adhesive tapes 31 and 32 are peeled off metal plates 211 and 221 unwound from metal reels 21 and 22 according to one embodiment of the present invention.

[0088] After the surface treatment of the first metal plate 211 is completed, Figure 8 As shown in , the masked first tape 31 is peeled off and removed (S604). As described above, when the surface treatment of the first metal plate 211 is completed, the first film 1232 is formed on the outer surface of the first metal plate 211, but the first film 1232 is not formed on the outer surface only in the first connection area 1231 masked by the first tape 31. Here, while performing the surface treatment, the first tape 31 should not be corroded or deformed. Therefore, it is preferred that the first tape is made of a material excellent in corrosion resistance and wear resistance.

[0089] Thereafter, the first metal plate 211 is cut at regular intervals (S605). As a result, the first electrode lead 123 may be completely manufactured.

[0090] To manufacture the second electrode lead 124, the same procedure as the method of manufacturing the first electrode lead 123 is performed. Hereinafter, contents repeated with the above contents will be omitted, but this is for convenience of description and is not intended to limit the scope of rights.

[0091] In particular, first, the second metal plate 221 is unwound from the second metal reel 22 (S601). In addition, when the second metal plate 221 is unwound, the second tape 32 is attached to the second connection area 1241 for shielding (S602). As described above, one end of the second electrode lead 124 is connected to the outer end of the first electrode lead 123, and the other end protrudes to the outside of the battery case. Therefore, the second connection area 1241 is formed at one end of the second electrode lead 124 so as to be connected to the first electrode lead 123 later. In addition, as Figure 7 As shown in , in the second metal plate 221 , it is preferred that the second connection region 1241 is formed to extend in the longitudinal direction along one edge of the second metal plate 221 .

[0092] When the masking process of the second adhesive tape 32 is completed, the second metal plate 221 (S603) is subjected to surface treatment such as electroplating, oxidation and film treatment. Figure 8 As shown in , the masked second tape 32 is peeled off and removed (S604). As described above, after the surface treatment of the second metal plate 221 is completed, the second film 1242 is formed on the outer surface of the second metal plate 221, but the second film 1242 is not formed on the outer surface only in the second connection area 1241 masked with the second tape 32. Here, while performing the surface treatment, the second tape 32 should not be corroded or deformed. Therefore, it is preferred that the second tape is made of a material excellent in corrosion resistance and wear resistance.

[0093] Thereafter, the second metal plate 221 is cut at regular intervals (S605). Thus, the second electrode lead 124 may be completely manufactured.

[0094] It is preferred that each of the first electrode lead 123 and the second electrode lead 124 has a rectangular shape. In addition, in order to be able to easily combine with each other later, it is preferred that the first electrode lead 123 and the second electrode lead 124 have the same width. Therefore, the predetermined interval for cutting the first metal plate 211 and the predetermined interval for cutting the second metal plate 221 can be the same.

[0095] When cutting the metal plates 211 and 221 , a punching device may be used, or a laser may be used. That is, in order to manufacture the first electrode lead 123 and the second electrode lead 124 , the metal plates 211 and 221 may be cut in various ways without limitation.

[0096] Fig. 9 is a schematic diagram showing a state in which a first electrode lead 123 and a second electrode lead 124 are coupled to each other according to an embodiment of the present invention, and Fig.101 is a schematic diagram showing a state in which the first electrode lead 123 and the second electrode lead 124 are combined with each other to completely manufacture the two-stage electrode lead 12 according to one embodiment of the present invention.

[0097] like Fig. 9 As shown in FIG. 1 , an adhesive 151 is applied to at least one of a first connection region 1231 at one end of a first electrode lead 123 or a second connection region 1241 at the other end of a second electrode lead 124. In addition, the first connection region 1231 and the second connection region 1241 are bonded to each other to form a lead stack.

[0098] The binder 151 includes a material having conductivity. Therefore, the power generated from the electrode assembly 10 can be easily discharged to the outside. To this end, the binder 151 is preferably formed by mixing a conductive material and a polymer.

[0099] The conductive material may include at least one of natural or artificial graphite; carbon black such as acetylene black, Krebs black, channel black, furnace black, lamp black, and summer black; conductive fiber such as carbon fiber or metal fiber; metal powder such as carbon fluoride, aluminum, nickel, gold, silver, and copper powder; powder having a core / shell structure in which different kinds of metals are coated on one metal; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive materials such as polyphenyl derivatives, in particular, may most preferably include silver. Preferably, the content of the conductive material contained in the adhesive 151 is 70wt% to 80wt%.

[0100] The polymer may include at least one of acrylic resin, epoxy resin, ethylene propylene diene monomer (EPDM) resin, chlorinated polyethylene (CPE) resin, silicone, polyurethane, urea resin, melamine resin, phenol resin, unsaturated ester resin, polypropylene (PP), polyethylene (PE), polyimide or polyamide, and may most preferably include epoxy resin or acrylic resin. Preferably, the content of the polymer contained in the adhesive 151 is 20wt% to 30wt%.

[0101] After applying the adhesive 151, when heat is applied to the lead stack, the adhesive 151 dries and cures to form the connection portion 15, and thus, the connection portion 15 includes a conductive material and a conductive polymer. Fig.10 As shown in , the two-section electrode lead 12 in which the first electrode lead 123 and the second electrode lead 124 are connected to each other can be completely manufactured.

[0102] Fig.11 is a flowchart illustrating a method for manufacturing the first electrode lead 123 and the second electrode lead 124 according to another embodiment of the present invention.

[0103] According to one embodiment of the present invention, in order to manufacture the first electrode lead 123 or the second electrode lead 124, after peeling and removing the first tape 31 and the second tape 32, the step of cutting the first metal plate 211 or the second metal plate 221 is performed. As a result, since the metal plates 211 and 221 are not cut into several pieces but are continuously formed as a whole, it is not necessary to cut the tapes 31 and 32 into several pieces and attach the tapes 31 and 32 multiple times, and therefore, one tape 31 or 32 can be attached to the first connection area 1231 and the second connection area 1241 at one time.

[0104] According to another embodiment of the present invention, in order to manufacture the first electrode lead 123 or the second electrode lead 124, before attaching the first tape 31 or the second tape 32 for shielding, a step of cutting the first metal plate 211 or the second metal plate 221 is performed. That is, when the first metal plate 211 or the second metal plate 221 is unwound from the first metal reel 21 or the second metal reel 22, the first metal plate 211 or the second metal plate 221 is cut into several pieces. In particular, first, the metal plates 211 and 221 are unwound from the metal reels 21 and 22, respectively (S1101). When the metal plates 211 and 221 are unwound, the metal plates 211 and 221 are cut at regular intervals (S1102). Thereafter, the first tape 31 or the second tape 32 is attached to the first connection area 1231 or the second connection area 1241 for shielding (S1103). After the masking process of the tapes 31 and 32 is completed, the metal plates 211 and 221 are subjected to surface treatments such as electroplating, oxidation, and film treatment (S1104). After the surface treatment of the metal plates 211 and 221 is completed, the masked tapes 31 and 32 are peeled off and removed (S1105). Thus, the first electrode lead 123 or the second electrode lead 124 can be completely manufactured.

[0105] When the above method is performed, since the first tape 31 or the second tape 32 is cut into several pieces, the size of the first tape 31 or the second tape 32 is reduced. Therefore, the first tape 31 or the second tape 32 can be accurately attached to the first connection area 1231 or the second connection area 1241 at a desired position. In addition, since the masking process is performed even after the metal plates 211 and 221 have been cut, the process order can be flexibly changed.

[0106] Those skilled in the art to which the present invention relates will appreciate that the present invention may be implemented in other specific forms without changing the technical ideas or essential features. Therefore, the embodiments disclosed above should be considered illustrative rather than restrictive. Therefore, the scope of the present invention is defined by the appended claims rather than the preceding description and the exemplary embodiments described therein. Various modifications made within the equivalent meanings of the claims of the present invention and within the claims should be considered to be within the scope of the present invention.

[0107] CROSS-REFERENCE TO RELATED APPLICATIONS

[0108] This application claims the benefit of Korean Patent Application No. 10-2019-0149920, filed on November 20, 2019, which is hereby incorporated by reference in its entirety.

Claims

1. A method for manufacturing an electrode lead used in a pouch-type secondary battery, the method comprising: a step of manufacturing each of a first electrode lead and a second electrode lead; as well as a step of bonding the first electrode lead to the second electrode lead to form a connection portion, The steps of manufacturing the first electrode lead include: the step of unwinding a first metal sheet from a first metal reel; a step of attaching a first adhesive tape to a first connection region of the first metal plate where the connection portion is to be formed for masking; The step of electroplating and surface treating the first metal plate; and a step of removing the first adhesive tape, The step of manufacturing the second electrode lead includes: the step of unwinding a second metal sheet from a second metal reel; a step of attaching a second adhesive tape on a second connection region of the second metal plate where the connection portion is to be formed for masking; a step of electroplating and surface treating the second metal plate; and The step of removing the second tape, wherein the step of manufacturing the first electrode lead further comprises the step of cutting the first metal plate at regular intervals after the step of removing the first tape; and The step of manufacturing the second electrode lead further includes the step of cutting the second metal plate at regular intervals after the step of removing the second tape.

2. The method according to claim 1, wherein: One end of the first electrode lead is connected to the electrode connector, and The first connection region is formed on the other end of the first electrode lead.

3. The method according to claim 2, wherein: The second connection region is formed on one end of the second electrode lead.

4. The method according to claim 1, wherein: When performing the plating and surface treatment steps, forming a first film on an outer surface of the first metal plate, and A second film is formed on the outer surface of the second metal plate.

5. The method according to claim 1, wherein: In the step of performing electroplating and surface treatment, the surface treatment includes at least one of chromate treatment, zirconium oxide treatment and titanium treatment.

6. A pouch-type secondary battery comprising an electrode lead manufactured by the method according to claim 1, the pouch-type secondary battery comprising: An electrode assembly, in which electrodes and a separator are stacked, wherein the electrodes include a positive electrode and a negative electrode; a battery case having a pouch shape, the battery case being configured to accommodate the electrode assembly; an electrode connector connected to the electrode to protrude from one side of the electrode assembly; a first electrode lead, one end of which is connected to the electrode connector; a second electrode lead, one end of which is connected to the other end of the first electrode lead and the other end of which protrudes outside the battery case; as well as a connecting portion configured to connect the first electrode lead and the second electrode lead to each other, wherein, in the first electrode lead, a first film is formed on an outer surface of the first electrode lead, and the first film is not formed on a first connection region where the connection portion is formed, and In the second electrode lead, a second film is formed on an outer surface of the second electrode lead, and the second film is not formed on a second connection region where the connection portion is formed.

7. The pouch type secondary battery according to claim 6, wherein: The first film or the second film includes at least one of a chromate film, a zirconium oxide film, and a titanium film. 8 . The pouch type secondary battery of claim 6 , further comprising an insulating portion surrounding a portion of each of the first electrode lead and the second electrode lead to combine the first electrode lead and the second electrode lead with the battery case.

9. The pouch type secondary battery according to claim 8, wherein: A bonding force between each of the first electrode lead and the second electrode lead and the connection portion is smaller than a bonding force between each of the first electrode lead and the second electrode lead and the insulation portion.

10. The pouch type secondary battery according to claim 8, wherein The insulating portion surrounds a portion where the first electrode lead and the second electrode lead are connected to each other via the connecting portion.

11. The pouch type secondary battery according to claim 8, wherein The insulating portion is made of at least one of a thermoplastic resin, a thermosetting resin, and a photocurable resin having electrical insulating properties.

12. The pouch type secondary battery according to claim 6, wherein: The connection portion includes a conductive material and a conductive polymer.

13. The pouch type secondary battery according to claim 6, wherein: The connecting portion has a thickness of 1 μm to 500 μm.