Carbon nanotube / carbon fiber paper composite electrode material and preparation method thereof and all-vanadium liquid flow battery
By bonding and carbonizing carbon nanotubes and carbon fiber paper at low temperature, the problems of complex modification and poor binding force of existing carbon fiber paper electrode materials are solved, and high hydrophilicity, low resistivity and strong binding force are achieved. Carbon nanotube/carbon fiber paper composite electrode material, suitable for large-scale production and application.
Patent Information
- Application Number
- CN202011366869.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-11-27
AI Technical Summary
The existing carbon fiber paper electrode materials have complex modification methods, poor binding force, unsuitable for large-scale production, and insufficient electrical performance.
The carbon nanotubes are bonded to carbon fiber paper with binder, and the carbon nanotubes are subjected to low-temperature carbonization under the protection of inert gas to form a carbon nanotube/carbon fiber paper composite electrode material.
The preparation process is simplified, the hydrophilicity, specific surface area and resistivity of the material are improved, and the bonding force and electrical properties of the electrode are enhanced, making it suitable for large-scale production.
Smart Images

Figure CN114566655B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of carbon fiber paper electrode materials, and in particular to a carbon nanotube / carbon nanofiber paper composite electrode material and a preparation method thereof, and an all-vanadium liquid flow battery. Background Art
[0002] Electrodes are key components of all-vanadium flow batteries. Electrodes should have appropriate porosity, high surface activity, low resistivity, high strength and long service life. Carbon fiber paper is the main electrode material for flow batteries, but carbon fiber paper has poor hydrophilicity and must be surface treated before it can be used as an electrode.
[0003] The existing modification methods of carbon fiber paper for flow batteries mainly involve introducing functional groups, metals or metal compounds, carbon nanotubes, etc. on the surface of carbon fiber paper through acid treatment or heat treatment. These modification methods can improve the performance of carbon fiber paper electrodes to a certain extent, but their operation methods are complicated, and the binding force between the introduced substances and the carbon fiber surface is poor, which is not suitable for large-scale application and production.
[0004] CN108091888A uses air oxidation to modify the electrode surface and increase oxygen-containing groups, but the mechanical properties of the electrode decrease after air oxidation. CN103887524A uses acid corrosion to increase oxygen-containing functional groups on the electrode surface, but due to the introduction of strong acid, it is not suitable for large-scale production. CN104332638A introduces metal elements to modify the surface of carbon fiber electrodes, but the metal elements have poor binding force with the electrode surface and are not suitable for long-term use.
[0005] The modification method of the carbon fiber paper electrode of the flow battery also includes the method of preparing carbon nanotube and carbon fiber composite electrode by vapor deposition and melt spinning, but this modification method is difficult to be applied on a large scale due to the complex processing process and high cost. CN102522568A introduces carbon nanotube modified carbon fiber electrode by electrostatic spinning, but the electrostatic spinning method has low production capacity and is not suitable for large-scale production.
[0006] Therefore, there is an urgent need to provide a carbon nanotube / carbon nanofiber paper composite electrode material with a simple preparation method, high specific surface area, low resistivity, high reaction activity and good hydrophilicity. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of the prior art that the preparation process of carbon nanotube / carbon nanofiber paper composite electrode materials is complex, the electrical properties are poor, the binding force between the introduced material and the surface of the carbon fiber paper is small, and it is not suitable for large-scale production. A preparation method of carbon nanotube / carbon nanofiber paper composite electrode materials is provided. The method has the advantages of a simple preparation method, and the prepared carbon nanotube / carbon nanofiber paper composite electrode material has good hydrophilicity, high specific surface area, large binding force, low resistivity and high reaction activity.
[0008] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing a carbon nanotube / carbon fiber paper composite electrode material, wherein the method comprises: firstly bonding the carbon nanotubes and carbon fiber paper with a binder to obtain a binder, and then subjecting the obtained binder to a low-temperature carbonization treatment to obtain a carbon nanotube / carbon fiber paper composite electrode material; wherein the low-temperature carbonization treatment is carried out under the protection of an inert gas, and the treatment temperature is 400-800°C.
[0009] The second aspect of the present invention provides a carbon nanotube / carbon fiber paper composite electrode material prepared by the method described in the first aspect of the present invention.
[0010] The third aspect of the present invention provides an all-vanadium liquid flow battery, the battery comprising the carbon nanotube / carbon fiber paper composite electrode material described in the second aspect of the present invention.
[0011] Through the above technical solution, the beneficial technical effects of the present invention are as follows:
[0012] 1) The method for preparing the carbon nanotube / carbon fiber paper composite electrode material provided by the present invention directly combines the carbon nanotubes and the carbon fiber paper together by means of a binder bonding and a low-temperature carbonization treatment, which is simple to operate and easy to promote on a large scale commercially;
[0013] 2) The carbon nanotube / carbon fiber paper composite electrode material provided by the present invention has a contact angle with water of substantially 0°, good hydrophilicity, and a high specific surface area, and has a surface area of 20-350 m 2 / g, the resistivity is between 10-600μΩ·m, and the conductivity is good;
[0014] 3) The reaction activity and power density of the liquid flow battery electrode prepared by using the carbon nanotube / carbon fiber paper composite electrode material provided by the present invention are high. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 is a power density diagram of a flow battery assembled from the carbon nanotube / carbon fiber paper composite material prepared in Example 2 and Comparative Example 1;
[0016] Figure 2is a scanning electron microscope image of the carbon nanotube / carbon fiber paper composite material prepared in Example 3;
[0017] Figure 3 is an X-ray photoelectron spectrum of the carbon nanotube / carbon fiber paper composite material prepared in Example 3;
[0018] Figure 4 Graphs showing contact angles of carbon nanotube / carbon fiber paper composite materials prepared in Example 3 and Comparative Example 1 with water;
[0019] Figure 5 This is a scanning electron microscope image of the carbon nanotube / carbon fiber paper composite material prepared in Example 3 assembled into a liquid flow battery after 100 cycles. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] The first aspect of the present invention provides a method for preparing a carbon nanotube / carbon fiber paper composite electrode material, the method comprising: firstly bonding carbon nanotubes and carbon fiber paper with a binder to obtain a binder, and then subjecting the obtained binder to a low-temperature carbonization treatment to obtain a carbon nanotube / carbon fiber paper composite electrode material; wherein the low-temperature carbonization treatment is carried out under the protection of an inert gas at a treatment temperature of 400-800°C.
[0022] At present, the modification of carbon fiber paper is generally carried out by introducing a modifier on the surface of the carbon fiber paper through acid treatment, heat treatment, vapor deposition and melt spinning, rather than by using a binder for bonding. This is because the introduced binder generally reduces the conductivity of the electrode itself, and the low bonding strength of the binder will also cause the modifier to fall off, affecting the modification effect. The inventors of the present invention have found through research that a method of bonding with an adhesive and subjecting the bonded material to low-temperature carbonization treatment can solve the above problems, thereby simplifying the preparation method of the carbon nanotube / carbon fiber paper composite electrode material and preparing a carbon nanotube / carbon fiber paper composite electrode material with good hydrophilicity, high specific surface area, low resistivity and strong bonding force.
[0023] In a preferred embodiment, the carbon nanotubes are multi-walled carbon nanotubes (MWCNTs).
[0024] The present invention does not specifically limit the multi-walled carbon nanotubes and carbon fiber paper, and the multi-walled carbon nanotubes and carbon fiber paper commonly used in the art can be applied to the present invention.
[0025] In a preferred embodiment, the binder is a water-soluble binder selected from polyvinyl alcohol and / or polyethylene oxide, preferably polyethylene oxide.
[0026] In a preferred embodiment, the weight average molecular weight of the polyethylene oxide is 200 g / mol-1,000,000 g / mol, preferably 20,000 g / mol-1,000,000 g / mol; the residual carbon rate of the polyethylene oxide is 1 wt%-10 wt%, preferably 5 wt%-10 wt%.
[0027] In a preferred embodiment, the weight average molecular weight of the polyvinyl alcohol is 20000 g / mol-150000 g / mol, preferably 60000 g / mol-100000 g / mol; the residual carbon rate of the polyvinyl alcohol is 1wt%-10wt%, preferably 5wt%-10wt%.
[0028] In the present invention, the test method for the residual carbon rate of polyethylene oxide or polyvinyl alcohol is to put polyethylene oxide or polyvinyl alcohol into a tubular furnace into which nitrogen is passed, and heat it to 400°C for 1 hour, 500°C for 2 hours, 600°C for 3 hours and 800°C for 4 hours at a heating rate of 5°C / min, and then weigh it, and compare the mass after treatment with the mass before placement to obtain the residual carbon rate.
[0029] In the present invention, the inventors have found through research that when polyethylene oxide is used as a binder, the prepared carbon nanotube / carbon fiber paper composite electrode material not only has good bonding strength, but also has low resistivity and good conductivity. The higher the residual carbon rate of polyethylene oxide, the better the electrical and mechanical properties of the prepared carbon nanotube / carbon fiber paper composite material.
[0030] In a preferred embodiment, the bonding process includes:
[0031] (1) firstly impregnating the carbon fiber paper in a binder dispersion to obtain an impregnation material I, and then performing a first drying treatment on the obtained impregnation material I to obtain an intermediate material;
[0032] (2) The intermediate material is first impregnated in a carbon nanotube dispersion for a second time to obtain an impregnated product II, and then the obtained impregnated product II is dried for a second time to obtain the bonded product.
[0033] In step (1):
[0034] In a preferred embodiment, the binder dispersion is a mixture of a binder and a solvent I. The solvent I is water, preferably deionized water; and the content of the binder in the binder dispersion is 1-10 wt %, preferably 1-5 wt %.
[0035] Among them, the present invention uses a water-soluble polymer binder. Dispersing the binder with water helps to improve the dispersibility of the binder in water, so that the subsequent carbon nanotubes are more evenly distributed on the carbon fiber paper.
[0036] In a preferred embodiment, the conditions for the first immersion include: the first immersion temperature is 20-40°C, preferably 25-35°C; the first immersion time is 5-20s, preferably 5-10s.
[0037] Among them, the present invention does not specifically limit the amount of binder dispersion used, as long as the carbon fiber paper can be immersed. Preferably, for 5×5cm carbon fiber paper, the amount of binder dispersion used can be 50-100mL. In the present invention, the immersion time of carbon fiber paper is related to the amount of binder retained on the surface of carbon fiber paper. When the carbon fiber paper is completely immersed in the binder dispersion, generally immersed for about 10s, the binder is basically completely bonded to the surface of the carbon fiber paper. If the time is extended, the amount of binder retained on the surface of the carbon fiber paper will not continue to increase. Therefore, the immersion time in the present invention is preferably 5-10s.
[0038] In a preferred embodiment, the conditions for the first drying include: a first drying temperature of 80-120° C., preferably 90-110° C.; and a first drying time of 1-4 h, preferably 1-2 h.
[0039] In step (2):
[0040] In a preferred embodiment, the carbon nanotube dispersion is a mixture of carbon nanotubes and solvent II, wherein the solvent II is water, preferably deionized water; in the carbon nanotube dispersion, the content of carbon nanotubes is 1-20wt%, preferably 3-15wt%.
[0041] In a preferred embodiment, in order to improve the dispersibility of carbon nanotubes in solvent II, a surfactant is added to the carbon nanotube dispersion, and the surfactant is selected from SDS (sodium dodecyl sulfate) and TB (hexadecyl trimethyl ammonium bromide), preferably SDS. In the carbon nanotube dispersion, the content of the surfactant is 0.1-1wt%, preferably 0.2-0.4wt%.
[0042] In a preferred embodiment, the conditions for the second immersion include: the second immersion temperature is 20-40°C, preferably 25-35°C; the second immersion time is 5-20s, preferably 5-10s.
[0043] In a preferred embodiment, the conditions for the second drying include: a second drying temperature of 80-120° C., preferably 90-110° C.; and a second drying time of 1-4 h, preferably 1-2 h.
[0044] Among them, the conditions of the second impregnation and the conditions of the first impregnation may be the same or different, preferably the same. The conditions of the second drying and the conditions of the first drying may be the same or different, preferably the same. Moreover, the present invention does not impose any special limitation on the amount of carbon nanotube dispersion, as long as the intermediate material can be immersed. Preferably, for a 5×5cm intermediate material, the amount of carbon nanotube dispersion may be 50-100mL. In the present invention, the binder is solidified on the surface of the carbon fiber paper after drying. Since the second impregnation time is relatively short, the binder will not be lost due to dissolution.
[0045] In a preferred embodiment, the inert gas is selected from at least one of nitrogen, argon and helium, preferably nitrogen.
[0046] In a preferred embodiment, the carbonization treatment conditions include: the carbonization treatment temperature is 400-800° C., preferably 400-600° C.; the carbonization treatment time is 1-5 h, preferably 1-3 h.
[0047] Among them, the inert gas described in the present invention refers to a gas that does not react chemically with the binder, carbon nanotubes and carbon fiber paper under carbonization conditions. In order to make the carbon fiber paper meet the requirements of battery conductivity, it is generally necessary to graphitize the carbon fiber paper in an inert gas atmosphere at a high temperature of 2600-2800°C when modifying the carbon fiber paper. The purpose is to make the carbon fiber crystal orientation more orderly to improve the conductivity of the carbon fiber paper. Or it is calcined in an oxygen-containing atmosphere. The purpose is to form defects (carboxyl and hydroxyl groups) on the smooth surface of the carbon fiber that can serve as active sites for battery reactions, so as to improve the reaction efficiency of the battery. However, in the present invention, the binder is carbonized for the purpose of carbonizing the binder. During the carbonization process, since the carbonization temperature is 400-800°C, the carbon fibers and carbon nanotubes themselves will not change.
[0048] The reason why the present invention performs low-temperature carbonization treatment on the binder is that the binder used in the present invention contains hydrogen and oxygen elements in addition to carbon elements, and is not conductive itself, but is an insulating resin. If the binder is not subjected to low-temperature carbonization treatment, the binder in the prepared carbon nanotube / carbon fiber paper composite electrode material will significantly increase the resistance of the material, sharply reduce the conductivity, and deteriorate the conductivity. At the same time, the presence of the binder in the prepared carbon nanotube / carbon fiber paper composite electrode material will also reduce the hydrophilicity of the material, making it more hydrophobic.
[0049] In the present invention, the inventor has found through research that by subjecting the binder to low-temperature carbonization treatment under the protection of inert gas, the binder can be carbonized while ensuring that the carbon fiber and the carbon nanotube do not change, that is, other elements in the binder except the carbon element are removed, so that only the carbon element remains in the binder after the low-temperature carbonization treatment. Among them, in the carbon nanotube / carbon fiber paper composite electrode material obtained after the low-temperature carbonization treatment, the carbon element remaining after the carbonization of the binder generally firmly bonds the carbon nanotube and the carbon fiber paper together like a solder, so that the carbon nanotube, the carbon fiber paper and the carbon remaining after the carbonization of the binder are integrated into one, so that the bonding force between the carbon nanotube and the carbon fiber paper is increased, the mechanical properties are improved, and it can be used for a long time without the problem of carbon nanotube falling off. Moreover, since there is only carbon element in the carbon nanotube / carbon fiber paper composite electrode material, the resistivity of the material is low, and the conductivity can be significantly improved. In addition, since carbon nanotubes are combined on the surface of the carbon fiber, the specific surface area of the composite electrode material will also increase accordingly. The greater the specific surface area is, the more carbon nanotubes are incorporated, and the better the electrical properties of the prepared composite electrode material are.
[0050] The second aspect of the present invention provides a carbon nanotube / carbon fiber paper composite electrode material prepared by the method described in the first aspect of the present invention.
[0051] In a preferred embodiment, the specific surface area of the carbon nanotube / carbon fiber paper composite electrode material is 20-350 m 2 / g, preferably 50-330m 2 / g, more preferably 150-325m 2 / g.
[0052] In a preferred embodiment, the resistivity of the carbon nanotube / carbon fiber paper composite electrode material is 10-1100 μΩ·m, preferably 40-500 μΩ·m, and more preferably 40-440 μΩ·m.
[0053] In a preferred embodiment, the porosity of the carbon nanotube / carbon fiber paper composite electrode material is 70-95%, preferably 90-95%, and more preferably 92-93%.
[0054] In a preferred embodiment, the contact angle between the carbon nanotube / carbon fiber paper composite electrode material and water is substantially 0°, preferably 0°.
[0055] The third aspect of the present invention provides an all-vanadium liquid flow battery, the battery comprising the carbon nanotube / carbon fiber paper composite electrode material described in the second aspect of the present invention.
[0056] In the present invention, carbon nanotubes and carbon fiber paper are directly combined together by a binder and a low-temperature carbonization treatment method. This method is not only simple to operate and suitable for large-scale production, but also the prepared carbon nanotube / carbon fiber paper composite electrode material has a large specific surface area, good hydrophilicity, low resistivity, and high reaction activity. It can effectively improve the surface reaction activity of the liquid flow battery electrode and reduce the internal resistance of the liquid flow battery, thereby effectively improving the power density of the liquid flow battery, which is conducive to promoting the further application of the liquid flow battery in the field of large-scale energy storage.
[0057] The present invention will be described in detail below through examples.
[0058] Example 1
[0059] The carbon fiber paper of 5×5 cm was impregnated in 50 mL of an aqueous solution containing 1 wt% of polyethylene oxide (molecular weight of 200,000 and residual carbon content of 8%) at a temperature of 30° C. for 10 s to obtain an impregnated material I; the impregnated material I was dried in an oven at 100° C. for 1 h to obtain an intermediate material;
[0060] The dried intermediate material was immersed in 50 mL of an aqueous solution containing 3 wt% multi-walled carbon nanotubes (MWCNT) and 0.2 wt% surfactant SDS at a temperature of 30° C. for 10 s to obtain an impregnated product II; the impregnated product II was dried in an oven at 100° C. for 1 h to obtain a bonded product;
[0061] The dried binder was placed in a carbonization furnace for carbonization (nitrogen atmosphere) at a carbonization temperature of 400° C. and maintained for 1 hour to obtain a carbon nanotube / carbon fiber paper composite electrode material.
[0062] Example 2
[0063] The carbon fiber paper of 5×5 cm was impregnated in 50 mL of an aqueous solution containing 3 wt % polyethylene oxide (molecular weight of 200,000 and residual carbon content of 6%) at a temperature of 30° C. for 10 s to obtain an impregnated material I; the impregnated material I was dried in an oven at 100° C. for 1 h to obtain an intermediate material;
[0064] The dried intermediate material was immersed in 50 mL of an aqueous solution containing 5 wt% multi-walled carbon nanotubes (MWCNT) and 0.3 wt% surfactant SDS at a temperature of 30° C. for 10 seconds to obtain an impregnated product II; the impregnated product II was dried in an oven at 100° C. for 1 hour to obtain a bonded product;
[0065] The dried binder was placed in a carbonization furnace for carbonization (nitrogen atmosphere) at a temperature of 500° C. and maintained for 2 h to obtain a carbon nanotube / carbon fiber paper composite electrode material.
[0066] Example 3
[0067] 5×5 cm carbon fiber paper was impregnated in 100 mL of a 5 wt % aqueous solution of polyethylene oxide (molecular weight of 20,000, residual carbon rate of 5.5%), the impregnation temperature was 30° C., the impregnation time was 10 s, and an impregnation material I was obtained; the impregnation material I was dried in an oven at 100° C. for 1 h to obtain an intermediate material;
[0068] The dried intermediate material was immersed in 100 mL of an aqueous solution containing 15 wt% multi-walled carbon nanotubes (MWCNT) and 0.4 wt% surfactant SDS at a temperature of 30° C. for 10 s to obtain an impregnated product II; the impregnated product II was dried in an oven at 100° C. for 1 h to obtain a bonded product;
[0069] The dried binder was placed in a carbonization furnace for carbonization (nitrogen atmosphere) at a temperature of 600° C. for 3 h to obtain a carbon nanotube / carbon fiber paper composite electrode material.
[0070] Example 4
[0071] Similar to Example 1, except that polyvinyl alcohol (molecular weight of 100,000, residual carbon content of 10 wt%) is used to replace polyethylene oxide, and TB is used to replace SDS to obtain a carbon nanotube / carbon fiber paper composite electrode material.
[0072] Example 5
[0073] Similar to Example 1, except that no surfactant was added.
[0074] Comparative Example 1
[0075] The carbon fiber paper of 5×5 cm was impregnated in 50 mL of an aqueous solution containing 3 wt % polyethylene oxide (molecular weight of 200,000 and residual carbon content of 6%) at a temperature of 30° C. for 10 s to obtain an impregnated material I; the impregnated material I was dried in an oven at 100° C. for 1 h to obtain an intermediate material;
[0076] The dried intermediate material was immersed in 50 mL of an aqueous solution containing 5 wt% multi-walled carbon nanotubes (MWCNT) and 0.3 wt% surfactant SDS at a temperature of 30° C. for 10 seconds to obtain an impregnated product II; the impregnated product II was dried in an oven at 100° C. for 1 hour to obtain a bonded product;
[0077] The dried binder was placed in a carbonization furnace for carbonization (nitrogen atmosphere) at a temperature of 300° C. and maintained for 2 h to obtain a carbon nanotube / carbon fiber paper composite electrode material.
[0078] Comparative Example 2
[0079] The carbon fiber paper of 5×5 cm was impregnated in 50 mL of an aqueous solution containing 30 wt % polyethylene oxide (molecular weight of 200,000 and residual carbon content of 6%) for 30 seconds to obtain an impregnation material I; the impregnation material I was dried in an oven at 100° C. for 1 hour to obtain an intermediate material;
[0080] The dried intermediate material is immersed in an aqueous solution containing 5 wt% multi-walled carbon nanotubes (MWCNT) and 0.3 wt% surfactant SDS at a temperature of 30° C. for 10 seconds to obtain an impregnated product II; the impregnated product II is dried in an oven at 100° C. for 1 hour to obtain a bonded product;
[0081] The dried binder was placed in a carbonization furnace for carbonization (nitrogen atmosphere) at a temperature of 500° C. and maintained for 2 h to obtain a carbon nanotube / carbon fiber paper composite electrode material.
[0082] Test Example 1
[0083] The specific surface area, porosity and resistivity of the carbon nanotube / carbon fiber paper composite electrode materials prepared in Examples 1-5 and Comparative Examples 1-2 were tested, wherein the specific surface area and porosity were tested using a high pressure mercury injection porosimeter, and the resistivity was measured using a four-probe method of a resistivity instrument. The test results are shown in Table 1:
[0084] Table 1
[0085]
[0086] Test Example 2
[0087] The carbon nanotube / carbon fiber paper composite materials prepared in Example 2 and Comparative Example 1 were assembled into a liquid flow battery, wherein the liquid flow battery included a bipolar plate, a diaphragm of Nafion 117, and an electrolyte of VOSO4. The power density of the liquid flow battery was tested under the following test conditions: the prepared CP / MWCNT composite electrode was cut into a 2 cm × 2 cm square sheet, five sheets were stacked together as one side electrode, a 2 cm × 2 cm Nafion-115 perfluorosulfonic acid membrane was cut as a battery diaphragm, 25 ml of a 1 mol VOSO4 + 5 mol H2SO4 solution was used as the positive and negative electrolytes, and the electrolyte bottle was connected to a flow control pump (flow rate 90 ml min -1 ), the battery is at 100mA cm 2 The charge and discharge tests were carried out at a current density of .
[0088] The results are as follows Figure 1 As shown:
[0089] from Figure 1 It can be seen that the power density of the battery assembled with Example 2 as the electrode is high, indicating that the electrode in Example 2 provides more reactive sites due to the modification of multi-walled carbon nanotubes, and the power density of the battery is improved. However, the battery assembled with Comparative Example 1 is found to have a low power density, indicating that the 300°C low-temperature carbonization treatment cannot completely carbonize the binder, the resistance of the electrode increases, the reaction activity decreases, and the power density of the battery is low.
[0090] Test Example 3
[0091] The carbon nanotube / carbon fiber paper composite material prepared in Example 3 was characterized by scanning electron microscopy. Figure 2 As shown:
[0092] from Figure 2 It can be seen that a large number of flocculent multi-walled carbon nanotubes are attached to the surface of the carbon fiber paper. The multi-walled carbon nanotubes are entangled with each other and are closely connected to the rough grooves on the surface of the carbon fiber paper. The multi-walled carbon nanotubes form a network structure on the surface of the carbon fiber paper, which helps to improve the conductivity of the electrode. Moreover, since there are many oxygen-containing functional groups on the surface of the multi-walled carbon nanotubes, it helps to improve the performance of the electrode (electrochemical reversibility and reaction activity). In addition, there are many pore structures on the carbon fiber, so the specific surface area and porosity of the composite electrode material are relatively large, which is consistent with the test results of the specific surface area.
[0093] Test Example 4
[0094] The characteristic peak curve of the carbonized binder in the carbon nanotube / carbon fiber paper composite material prepared in Example 3 was tested by X-ray photoelectron spectroscopy according to the method of ASTM E995-2004. The result is shown in 3: Figure 3 Only the characteristic peak of C appears in the graphite, which proves that after carbonization, only carbon element remains in the binder of the carbon nanotube / carbon fiber paper composite material, so the carbon nanotube / carbon fiber paper composite material has low resistivity and good conductivity.
[0095] Test Example 5
[0096] Figure 4 Compared with Comparative Example 1 ( Figure 4 a) and Example 3 ( Figure 4 b) The contact angle between the composite electrode and water. As can be seen from the figure, the contact angle between the comparative example 1 and water is 146 0 It is hydrophobic, and the contact angle of Example 3 with water is 0 0 , showing good hydrophilicity. In actual electrochemical reactions, the electrolyte can reach the fiber electrode surface at a faster rate, accelerating the electrochemical reaction rate of the battery.
[0097] Test Example 6
[0098] The carbon nanotube / carbon fiber paper composite material prepared in Example 3 was assembled into a flow battery according to the method of Test Example 2. Nafion-115 perfluorosulfonic acid membrane was used as the battery separator. 25 ml of 1 mol VOSO4+5 mol H2SO4 solution was used as the positive and negative electrolytes. The electrolyte bottle was connected to a flow control pump (flow rate 90 ml / min). The battery was operated at 200 mA cm 2 The charge and discharge test was carried out at a current density of 100 cycles and observed using a scanning electron microscope. Figure 5 It can be seen that after 100 cycles, the multi-walled carbon nanotubes are still tightly adhered to the surface of the carbon fiber. At the same time, no black multi-walled carbon nanotubes remain in the electrolyte, indicating that the carbon nanotubes have a strong bond with the carbon fiber and have not fallen off.
[0099] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a carbon nanotube / carbon fiber paper composite electrode material, It is characterized in that The method comprises: firstly bonding carbon nanotubes and carbon fiber paper by a binder to obtain a bond, and then subjecting the obtained bond to low-temperature carbonization treatment to obtain a carbon nanotube / carbon fiber paper composite electrode material; wherein the low-temperature carbonization treatment is carried out under the protection of an inert gas, the low-temperature carbonization treatment temperature is 500-600°C, and the low-temperature carbonization treatment time is 2-3h; Wherein, the bonding process includes: (1) Firstly, the carbon fiber paper is impregnated in a binder dispersion to obtain an impregnation material I, and then the impregnation material I is dried to obtain an intermediate material; the binder is polyethylene oxide, the weight average molecular weight of the polyethylene oxide is 20000 g / mol-200000 g / mol, the residual carbon rate is 1wt%-10wt%, and the content of the binder in the binder dispersion is 3-5wt%; (2) firstly, the intermediate material is impregnated for a second time in a carbon nanotube dispersion to obtain an impregnated product II, and then the obtained impregnated product II is dried for a second time to obtain the bonded product; in the carbon nanotube dispersion, the content of carbon nanotubes is 5-15wt%; Wherein, a surfactant is added into the carbon nanotube dispersion, and the surfactant is sodium dodecyl sulfate. In the carbon nanotube dispersion, the content of the surfactant is 0.3-0.4wt%.
2. The preparation method according to claim 1, in, The binder dispersion is a mixture of a binder and a solvent I; wherein the solvent I is water.
3. The preparation method according to claim 1, in, The conditions of the first dipping include: the first dipping temperature is 20-40° C., and the first dipping time is 5-20 seconds; And / or, the conditions for the first drying include: a first drying temperature of 80-120° C., and a first drying time of 1-4 hours.
4. The preparation method according to claim 3, in, The conditions of the first dipping include: the first dipping temperature is 25-35° C., and the first dipping time is 5-10 seconds; And / or, the conditions for the first drying include: a first drying temperature of 90-110° C., and a first drying time of 1-2 h.
5. The preparation method according to claim 3 or 4, in, The conditions of the second dipping include: the second dipping temperature is 20-40° C., and the second dipping time is 5-20 seconds; And / or, the conditions for the second drying include: the second drying temperature is 80-120° C., and the second drying time is 1-4 hours.
6. The preparation method according to claim 5, in, The conditions of the second dipping include: the second dipping temperature is 25-35° C., and the second dipping time is 5-10 seconds; And / or, the conditions for the second drying include: the second drying temperature is 90-110° C., and the second drying time is 1-2 hours.
7. The preparation method according to claim 1, in, The inert gas is selected from at least one of nitrogen, argon and helium.
8. A carbon nanotube / carbon fiber paper composite electrode material prepared by the method according to any one of claims 1 to 7.
9. The composite electrode material according to claim 8, in, The specific surface area of the carbon nanotube / carbon fiber paper composite electrode material is 178-321 m 2 / g; And / or, the resistivity of the carbon nanotube / carbon fiber paper composite electrode material is 43-273 μΩ·m; And / or, the porosity of the carbon nanotube / carbon fiber paper composite electrode material is 92-93%.
10. An all-vanadium liquid flow battery, It is characterized in that The battery comprises the carbon nanotube / carbon fiber paper composite electrode material according to claim 8 or 9.