Electrolyte and lithium ion battery containing same
By using electrolyte containing butylsulfonolide, vinyl carbonate and fluorovinylcarbonate in lithium-ion batteries, the problem of battery capacity decay at low temperatures of lithium iron phosphate batteries is solved, and high conductivity and low temperatures are achieved Improvement of capacity retention.
Patent Information
- Application Number
- CN202210301400.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-03-24
AI Technical Summary
Lithium iron phosphate batteries exhibit problems such as battery capacity attenuation and mileage shrinkage in low temperature environments, mainly due to the decrease in conductivity of the electrolyte and the increase in the impedance of the SEI film, resulting in an increase in the diffusion resistance of the lithium ion.
Using an electrolyte, including organic solvents, lithium salts and additives, specifically butylsulfonolide, vinyl carbonate and fluorovinyl carbonate, these components increase the charge transfer rate of lithium ions to form a lower impedance SEI film enhances conductivity and reduces the melting point of the solvent through the strong electron-absorbing effect of halogen atoms of fluorovinyl carbonate.
The high ion conductivity and low-temperature capacity retention rate of lithium-ion batteries at low temperatures are achieved, with conductivity reaching 10.1S/m and the low-temperature capacity retention rate reaching 85.01% at -20℃/1C, which significantly improves the low-temperature performance of the battery.
Smart Images

Figure CN114597496B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion batteries, and in particular to an electrolyte and a lithium ion battery containing the electrolyte. Background Art
[0002] Lithium iron phosphate positive electrode materials have excellent structural stability during the charging and discharging process and have been widely used in pure electric vehicles and hybrid vehicles. However, lithium iron phosphate power batteries currently experience significant performance degradation, battery capacity attenuation, and reduced driving range in low temperature environments. Therefore, the low-temperature performance of lithium iron phosphate batteries urgently needs to be improved.
[0003] At low temperatures, the deterioration of lithium-ion low-temperature performance is mainly manifested in the attenuation of rate discharge capacity to 50-70% of normal temperature and a significant decrease in the voltage platform. There are three main reasons for the deterioration of lithium-ion battery performance at low temperatures. At low temperatures, the electrolyte ion conductivity decreases, the viscosity increases, the impedance of the SEI film passivation layer at the solid-liquid interface increases, and it becomes difficult for lithium ions to pass through the SEI film, resulting in an increase in the diffusion resistance of lithium ions in the graphite electrode. The development of high and low temperature electrolytes has become an effective way to solve the electrochemical performance problems of lithium iron phosphate power batteries at high and low temperatures.
[0004] The current commercial lithium battery electrolyte system mainly uses ethylene carbonate (EC) as the main solvent, accounting for more than 30%, because EC can form a solid-liquid interface SEI film with good physical and chemical properties when the battery is aged, allowing only lithium ions to be inserted and removed during charging and discharging, and preventing further decomposition of the electrolyte solvent and peeling of the graphite layer. However, EC has a high melting point, and its solubility decreases at low temperatures, increasing its viscosity, and the electrolyte is prone to crystallization, resulting in increased lithium ion diffusion impedance. The macroscopic manifestation is that the wettability of the pole piece becomes poor, and the diaphragm dries up and black spots appear, which greatly deteriorates the battery rate discharge performance and cycle performance.
[0005] At present, there are two main methods for low-temperature electrolytes: (1) Optimizing the composition of each component solvent, lowering the eutectic point, improving the electrolyte conductivity, and increasing the electrolyte viscosity. (2) Improving the SEI film quality by adding low-temperature additives, improving the SEI film lithium ion conductivity, and preventing the accumulation of charge on the graphite surface at low temperatures, which leads to enhanced polarization and lithium ion precipitation on the graphite surface.
[0006] CN 110556582 A discloses a lithium iron phosphate battery, an electrolyte and a preparation method of a lithium iron phosphate battery, which includes additives of vinylene carbonate, propane sultone, ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate, and can improve the low temperature performance of the battery, improve the discharge efficiency of the battery in a low temperature environment and extend the service life of the lithium iron phosphate battery. However, the impedance of the SEI film of the battery is high, resulting in graphite polarization of the battery at low temperatures, and the impedance of the battery becomes high.
[0007] CN 102496740A discloses a non-aqueous electrolyte capable of improving the low-temperature performance of a lithium iron phosphate battery and a preparation method thereof. A high conductivity and low viscosity solvent are mixed to ensure that the battery maintains a certain viscosity while improving the conductivity, thereby improving the low-temperature performance of lithium iron phosphate and improving the capacity and low-temperature conductivity. The additive used is a pyridine dione derivative or phthalic anhydride for SEI film formation. However, the SEI film thickness of the battery is large, and there is also the problem of high battery impedance.
[0008] Therefore, how to prepare a low-temperature electrolyte with excellent low-temperature performance on a large scale and in a simple and cost-effective manner is an important research direction in this field. Summary of the invention
[0009] In view of the problems existing in the prior art, the present invention provides a large-scale, low-cost and simplified preparation method of a low-temperature electrolyte with excellent low-temperature performance and a lithium-ion battery containing the same.
[0010] To achieve this object, the present invention adopts the following technical solutions:
[0011] One of the purposes of the present invention is to provide an electrolyte, which comprises an organic solvent, a lithium salt and an additive, wherein the additive comprises butyl sultone, vinylene carbonate and fluoroethylene carbonate.
[0012] In the present invention, butyl sultone is added to the electrolyte to increase the charge transfer rate of lithium ions, form a sulfur-containing SEI film with lower impedance and thinner, and greatly reduce the polarization of graphite at low temperatures; vinylene carbonate is added to make the SEI film formed on the interface more stable and increase the conductivity of the electrolyte solution at low temperatures; by introducing fluoroethylene carbonate, the strong electron-withdrawing effect of the halogen atoms in the fluoroethylene carbonate is utilized to increase the reduction potential of the solvent, reduce the consumption of Li in the SEI film, improve the first effect, increase the hydrogen bonds in the molecule, and reduce the melting point of the solvent. The electrolyte prepared by the present invention has excellent low-temperature performance, and its preparation method is simple and easy to achieve large-scale production.
[0013] As a preferred technical solution of the present invention, the volume fraction of the butyl sultone in the electrolyte is 0.5-1.5%, calculated by volume fraction, wherein the volume fraction can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4% or 1.5%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 0.8-1.2%.
[0014] As a preferred technical solution of the present invention, the volume fraction of the vinylene carbonate in the electrolyte is 1.5-2.5%, calculated by volume fraction, wherein the volume fraction can be 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4% or 2.5%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 1.8-2.2%.
[0015] As a preferred technical solution of the present invention, the volume fraction of the fluoroethylene carbonate in the electrolyte is 1.5-2.5%, calculated by volume fraction, wherein the volume fraction can be 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4% or 2.5%, etc., preferably 1.8-2.2%.
[0016] As a preferred technical solution of the present invention, the organic solvent includes ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate.
[0017] As a preferred technical solution of the present invention, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:(1-2):(1-5), and the mass ratio includes 1:1:1, 1:1:2, 1:1:3, 1:1:4, 1:1:5, 1:2:1, 1:2:2, 1:2:3, 1:2:4, 1:2:5, 2:3:5 or 2:4:5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is any one of 1:1:1, 2:3:5 or 2:4:5.
[0019] As a preferred technical solution of the present invention, the lithium salt includes any one of LiPF6, LiBF4, LiBOB, LiClO4 or LiAsF6, or a combination of at least two of them, wherein typical but non-limiting examples of the combination include: a combination of LiPF6 and LiBF4, a combination of LiBF4 and LiBOB, a combination of LiBOB and LiClO4, or a combination of LiClO4 and LiAsF6, etc.
[0020] Preferably, the lithium salt comprises LiPF6.
[0021] Preferably, the concentration of the lithium salt in the electrolyte is 1.0 to 1.2 mol / L, wherein the concentration may be 1.0 mol / L, 1.02 mol / L, 1.04 mol / L, 1.06 mol / L, 1.08 mol / L, 1.1 mol / L, 1.12 mol / L, 1.14 mol / L, 1.16 mol / L, 1.18 mol / L or 1.2 mol / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] A second object of the present invention is to provide a lithium ion battery, wherein the lithium ion battery comprises the electrolyte as described in the first object.
[0023] The lithium-ion battery further comprises a positive electrode, a negative electrode and a separator.
[0024] As a preferred technical solution of the present invention, the active material of the positive electrode includes lithium iron phosphate.
[0025] As a preferred technical solution of the present invention, the active material of the negative electrode includes artificial graphite and / or natural graphite.
[0026] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The battery prepared by the present invention has high ionic conductivity and low-temperature capacity retention rate, wherein the ionic conductivity can reach 10.1S / m; the low-temperature capacity retention rate can reach 85.01% at -20℃ / 1C BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a low-temperature discharge curve diagram of the electrolyte with different contents of butyl sultone in Example 1, Example 8 and Example 9 of the present invention.
[0030] Figure 2 It is a low temperature discharge curve diagram of electrolytes with different contents of vinylene carbonate in Comparative Examples 4, 6 and 7 of the present invention.
[0031] Figure 3 It is a low temperature discharge curve diagram of the electrolyte with different contents of fluoroethylene carbonate in Comparative Examples 5, 8 and 9 of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0033] Example 1
[0034] This embodiment provides a lithium ion electrolyte:
[0035] In this embodiment, the electrolyte includes 1.1 mol / L LiPF6, 1% of butyl sultone, 2% of vinylene carbonate, and 2% of fluoroethylene carbonate. The solvent is selected from vinyl carbonate, dimethyl carbonate, and ethyl methyl carbonate in a mass ratio of 2:3:5.
[0036] Example 2
[0037] This embodiment provides a lithium ion electrolyte:
[0038] In this embodiment, the electrolyte includes 1.0 mol / L LiPF6, 0.8% of butyl sultone by volume of the electrolyte, 2.2% of vinylene carbonate by volume of the electrolyte, and 2.2% of fluoroethylene carbonate by volume of the electrolyte. The solvent is selected from vinyl carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 2:3:5.
[0039] Example 3
[0040] In this embodiment, the electrolyte includes 1.2 mol / L LiPF6, 1.2% of butyl sultone by volume of the electrolyte, 1.8% of vinylene carbonate by volume of the electrolyte, and 1.8% of fluoroethylene carbonate by volume of the electrolyte. The solvent is selected from vinyl carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 2:3:5.
[0041] Example 4
[0042] In this embodiment, the electrolyte includes 1.1 mol / L LiPF6, 0.5% of butyl sultone by volume of the electrolyte, 2.5% of vinylene carbonate by volume of the electrolyte, and 2.5% of fluoroethylene carbonate by volume of the electrolyte. The solvent is selected from vinyl carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 2:3:5.
[0043] Example 5
[0044] In this embodiment, the electrolyte includes 1.1 mol / L LiPF6, 1.5% of butyl sultone, 1.5% of vinylene carbonate, and 1.5% of fluoroethylene carbonate. The solvent is selected from vinyl carbonate, dimethyl carbonate, and ethyl methyl carbonate in a mass ratio of 2:3:5.
[0045] Example 6
[0046] In this embodiment, except that the solvent is replaced by ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 2:3:5 with ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 1:1:1, other conditions are the same as those in Example 1.
[0047] Example 7
[0048] In this embodiment, except that the solvent is replaced by ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 2:3:5 with ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 2:4:5, other conditions are the same as those in Example 1.
[0049] Example 8
[0050] In this embodiment, except that 2% of the volume fraction of the electrolyte liquid is replaced by 1% of the volume fraction of the electrolyte liquid, other conditions are the same as those of Embodiment 1.
[0051] Example 9
[0052] In this embodiment, except that 2% of the volume fraction of the electrolyte liquid is replaced by 3% of the volume fraction of the electrolyte liquid, other conditions are the same as those of Embodiment 1.
[0053] Comparative Example 1
[0054] In this comparative example, except that butyl sultone was replaced by 1,3-propane sultone, other conditions were the same as those in Example 1.
[0055] Comparative Example 2
[0056] In this comparative example, except that butyl sultone was replaced by ethyl sultone, other conditions were the same as those in Example 1.
[0057] Comparative Example 3
[0058] Except that butyl sultone was not added, other conditions in this comparative example were the same as those in Example 1.
[0059] Comparative Example 4
[0060] Except that vinylene carbonate and fluoroethylene carbonate are not added, other conditions in this comparative example are the same as those in Example 1.
[0061] Comparative Example 5
[0062] Except that fluoroethylene carbonate was not added, other conditions in this comparative example were the same as those in Example 1.
[0063] Comparative Example 6
[0064] In this comparative example, except that 1% of butyl sultone by volume of the electrolyte liquid is replaced by 2% of butyl sultone by volume of the electrolyte liquid, other conditions are the same as those of comparative example 4.
[0065] Comparative Example 7
[0066] In this comparative example, except that 1% of butyl sultone by volume of the electrolyte liquid is replaced by 3% of butyl sultone by volume of the electrolyte liquid, other conditions are the same as those of comparative example 4.
[0067] Comparative Example 8
[0068] In this comparative example, except that 2% of the volume fraction of the electrolytic liquid of vinylene carbonate is replaced by 1% of the volume fraction of the electrolytic liquid of vinylene carbonate, other conditions are the same as those of comparative example 5.
[0069] Comparative Example 9
[0070] In this comparative example, except that 2% of the volume fraction of the electrolytic liquid is replaced by 3% of the volume fraction of the electrolytic liquid, other conditions are the same as those of comparative example 5.
[0071] The conductivity and viscosity of the electrolytes in Examples 1-9 and Comparative Examples 1-9 were tested.
[0072] The electrolytes in Examples 1-9 and Comparative Examples 1-9 were assembled into lithium-ion batteries. The battery model was DW505070. The positive electrode active material of the battery was lithium iron phosphate, and the negative electrode active material was natural graphite. The battery was tested for capacity retention at -20°C / 1C. The low-temperature discharge curves of the electrolytes with different contents of butyl sultone in Examples 1, 8 and 9 were as follows: Figure 1 As shown; Comparative Example 4, Comparative Example 6 and Comparative Example 7, the low temperature discharge curves of different contents of vinylene carbonate electrolyte are shown Figure 2 As shown; Comparative Example 5, Comparative Example 8 and Comparative Example 9 in different contents of fluoroethylene carbonate electrolyte low temperature discharge curve as shown Figure 3 The test results are shown in Table 1.
[0073] Table 1
[0074]
[0075]
[0076] It can be seen from the above results that the conductivity and viscosity are mainly determined by the solvent composition. From Example 1 and Examples 6-7, it can be seen that the conductivity and viscosity of the solvent composition of 2:3:5 are optimal, which is the main factor affecting the low-temperature performance of the electrolyte; through Examples 1 and Examples 8-9, it can be obtained that by optimizing the proportion of film-forming additives, the low-temperature performance of the electrolyte can be effectively regulated, and the low-temperature electrolyte ratio of 1% butyl sultone, 2% of vinyl carbonate accounting for 2% of the volume fraction of the electrolyte liquid, and 2% of fluoroethylene carbonate accounting for 2% of the volume fraction of the electrolyte liquid is optimal.
[0077] According to Comparative Examples 1 and 2, after butyl sultone is replaced by 1,3-propane sultone and ethyl sultone, the capacity retention rate of the battery decreases compared with Example 1; according to Comparative Example 3, butyl sultone is not added, and the capacity retention rate of the battery decreases; through the low-temperature discharge curves of the electrolytes with different contents of butyl sultone in Examples 1, 8 and 9, through Comparative Examples 4, 6 and 7 ( Figure 2 ),
[0078] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A low-temperature electrolyte, characterized in that: The electrolyte includes an organic solvent, a lithium salt and an additive, wherein the additive includes butyl sultone, vinylene carbonate and fluoroethylene carbonate; The organic solvent is ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a mass ratio of 2:3:5; In terms of volume fraction, the volume fraction of the butyl sultone in the electrolyte is 0.6 to 1.5%; In terms of volume fraction, the volume fraction of the vinylene carbonate in the electrolyte is 1.5-2.5%; Calculated by volume fraction, the volume fraction of the fluoroethylene carbonate in the electrolyte is 1.5-2.5%.
2. The electrolyte according to claim 1, characterized in that Calculated by volume fraction, the volume fraction of the butyl sultone in the electrolyte is 0.8-1.2%.
3. The electrolyte according to claim 1, characterized in that Calculated by volume fraction, the volume fraction of the vinylene carbonate in the electrolyte is 1.8-2.2%.
4. The electrolyte according to claim 1, characterized in that Calculated by volume fraction, the volume fraction of the fluoroethylene carbonate in the electrolyte is 1.8-2.2%.
5. The electrolyte according to claim 1, characterized in that The lithium salt includes any one of LiPF6, LiBF4, LiBOB, LiClO4 or LiAsF6, or a combination of at least two thereof.
6. The electrolyte according to claim 5, characterized in that The lithium salt is LiPF6.
7. The electrolyte according to claim 1, characterized in that The concentration of the lithium salt in the electrolyte is 1.0 to 1.2 mol / L.
8. A lithium ion battery, characterized in that: The lithium-ion battery comprises the electrolyte according to any one of claims 1 to 7; The lithium-ion battery further comprises a positive electrode, a negative electrode and a separator.
9. The lithium-ion battery according to claim 8, characterized in that: The active material of the positive electrode includes lithium iron phosphate.
10. The lithium ion battery according to claim 8, characterized in that The active material of the negative electrode includes artificial graphite and / or natural graphite.