A kind of graphene / boron nitride aerogel and preparation method thereof

By preparing graphene/boron nitride aerogel, the performance issues of battery module materials at high and low temperatures were solved, achieving heat insulation, heating, and buffering functions, improving battery safety and stability, and reducing production costs.

CN114597560BActive Publication Date: 2024-11-15XIAN BOXIN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210196120.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-28
Publication Date
2024-11-15
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

Existing battery module materials are prone to pulverization under high temperature and vibration conditions, which cannot effectively insulate heat and mitigate battery thermal runaway. Furthermore, the battery capacity decays severely in low temperature environments, requiring additional heating systems, which are costly.

Method used

Boron nitride aerogel was prepared by pyrolyzing melamine diborate aerogel using graphene/boron nitride aerogel, and graphene was grown on it using chemical vapor deposition to form a composite nanoribbon structure, achieving thermal insulation, Joule heating capability, and elasticity.

Benefits of technology

Graphene/boron nitride aerogel possesses excellent thermal insulation properties, Joule heating capability, and flexibility, which can effectively prevent battery thermal runaway, improve battery capacity degradation in low-temperature environments, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003524930660000011
    Figure HDA0003524930660000011
  • Figure HDA0003524930660000012
    Figure HDA0003524930660000012
  • Figure HDA0003524930660000021
    Figure HDA0003524930660000021
Patent Text Reader

Abstract

The invention provides a graphene / boron nitride aerogel and a preparation method thereof, comprising the following steps: subjecting melamine diborate aerogel to pyrolysis treatment to obtain boron nitride aerogel; using the boron nitride aerogel as a matrix, and depositing graphene on the matrix by chemical vapor deposition to obtain the graphene / boron nitride aerogel; when the graphene / boron nitride aerogel is used as a battery module material, it has the characteristics of heat insulation, Joule heating, elasticity and the like, and compared with traditional battery module aerogel materials, it can greatly reduce the production cost of the battery while improving the safety and stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a graphene / boron nitride aerogel and a preparation method thereof. Background Art

[0002] With the rapid development of new energy vehicles, the safety and stability of their internal power batteries have been closely watched. Thermal runaway and low-temperature battery capacity attenuation are the main factors affecting battery safety and stability. At present, the main measure to solve the problem of battery explosion caused by battery thermal runaway is to use some battery module materials with good thermal insulation effect, such as insulation board fireproof felt (such as glass fiber, ceramic fiber wool, etc.) as battery module materials, and use its good thermal insulation effect to achieve the purpose of suppressing battery thermal runaway. However, it has the problem that the surface fibers are easy to break and powder, causing floating fibers or powder pollution, and are not suitable for long-term use under high temperature, compression and vibration conditions.

[0003] In addition, the ambient temperature is an important factor affecting battery stability. When the battery is in a low temperature environment (<0℃), the battery capacity is very likely to decay (the decay is one-third of the room temperature), which seriously affects the range of new energy vehicles. At present, the solution to the low temperature capacity decay of batteries is mainly to start with battery research and development to improve the low temperature cycle stability of batteries. Although this measure can improve the problem of low temperature capacity decay of batteries, it increases the cost of battery production.

[0004] If an aerogel is prepared as a car battery module material, it will have functions such as heat insulation, Joule heating, and elasticity. It can not only improve the battery thermal runaway problem, but also provide heating function when the battery is in a low temperature environment, improving the battery's low-temperature capacity attenuation problem. Its elasticity can buffer the expansion and contraction forces generated by the battery during the charging and discharging process.

[0005] At present, the materials used in battery modules are mainly SiO2-based aerogels. Due to their brittleness, surface powder shedding and other problems, they need to be doped with fibers (such as glass fibers, ceramic fibers and carbon fibers) to enhance the strength and elasticity of the materials. However, SiO2-based aerogels only improve the problem of battery thermal runaway, and cannot achieve the battery heating function in low-temperature environments. An additional heating system is required to heat and insulate the entire battery module in low-temperature conditions.

[0006] Although carbon-based aerogels (such as graphene and carbon nanotubes) have excellent Joule heating properties, they are brittle and fragile during their application and cannot effectively alleviate the mechanical shrinkage and expansion problems caused by battery charging and discharging. Based on this, it is expected that a multifunctional aerogel module material with thermal insulation, Joule heating, elasticity and other properties can be achieved by combining carbon-based aerogels and ceramic-based aerogels. However, no related aerogels have been reported or patented. Summary of the invention

[0007] The object of the present invention is to provide a graphene / boron nitride aerogel and a preparation method thereof, which solves the above-mentioned deficiencies existing in the prior art.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] The present invention provides a method for preparing a graphene / boron nitride aerogel, comprising the following steps:

[0010] The melamine diborate aerogel is subjected to pyrolysis treatment to obtain a boron nitride aerogel;

[0011] Boron nitride aerogel is used as a substrate, and graphene is deposited on the substrate by chemical vapor deposition to obtain graphene / boron nitride aerogel.

[0012] Preferably, the method for preparing melamine diborate aerogel comprises the following steps:

[0013] Dissolving melamine and boric acid in a co-solvent and stirring sufficiently to obtain a melamine diborate solution, wherein the molar ratio of melamine to boric acid is 1:5 to 5:1;

[0014] The co-solvent includes water and methanol, ethanol, isopropanol, n-butanol or tert-butanol, wherein the volume ratio of water to methanol, ethanol, isopropanol, n-butanol or tert-butanol is 7:5 to 9:11;

[0015] The melamine diborate solution is freeze-dried to obtain the melamine diborate aerogel.

[0016] Preferably, the freeze-drying process is:

[0017] The vacuum freeze-drying treatment time is 12 to 48 hours.

[0018] Preferably, the specific process of pyrolyzing melamine diborate aerogel to obtain boron nitride aerogel is:

[0019] The pyrolysis is carried out in a high temperature atmosphere, the pyrolysis temperature is 500 to 2000°C, and the pyrolysis time is 0.5 to 12 hours.

[0020] Preferably, the high temperature atmosphere is one of ammonia, argon, and nitrogen, or a mixture of any two of them.

[0021] Preferably, graphene is deposited on the substrate by chemical vapor deposition, and the specific process is:

[0022] A carbon source with a high O / C ratio is used as the carbon source, and the graphene content in the graphene / boron nitride aerogel is 10-35% of the total amount of the graphene / boron nitride aerogel.

[0023] A graphene / boron nitride aerogel is prepared by the preparation method.

[0024] Preferably, the graphene / boron nitride aerogel is a composite nanoribbon structure.

[0025] Preferably, the length of the composite nanobelt structure is 1 μm to 900 μm, and the width is 50 nm to 15 μm.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention prepares boron nitride aerogel by pyrolyzing melamine diborate aerogel, and then in situ grows graphene on the boron nitride aerogel matrix by means of a chemical vapor deposition process, and then in situ grows graphene on the boron nitride by a chemical vapor deposition method, so that the graphene is uniformly grafted from the inside to the outside of the boron nitride aerogel, and a multifunctional aerogel with heat insulation, elasticity, and Joule heating properties is obtained; at the same time, the graphene grows seamlessly on the boron nitride matrix to form a three-dimensional conductive path with a high aspect ratio, so that the graphene / boron nitride aerogel has excellent flexibility.

[0028] Furthermore, compared with the traditional chemical vapor deposition process using methane as the carbon source, the graphene grown by the present invention using a high O / C ratio carbon source (methanol) produces almost no impurities such as amorphous carbon and low-temperature pyrolysis carbon, that is, the pyrolysis of a high O / C ratio carbon source (methanol) is a special process for preparing high-purity graphene in a simple and stable manner. The obtained graphene / boron nitride aerogel has multifunctional properties such as elasticity, heat insulation, and Joule heating. Specifically:

[0029] (1) Boron nitride aerogel is used as the matrix, which makes the material have excellent thermal insulation performance. The high O / C ratio carbon source (methanol) pyrolysis growth graphene process enhances the phonon / electron scattering during heat transfer, hinders the effective conduction of heat, and significantly improves the thermal insulation performance of the material. When it is applied to battery module materials, it can effectively isolate the heat transfer between batteries and improve the explosion problem caused by thermal runaway of batteries.

[0030] (2) The introduction of high-quality graphene enhances the thermal insulation of the boron nitride aerogel matrix and gives the material excellent Joule heating properties. When the battery is in a low-temperature environment (<0°C), applying a 1.5-6V voltage across the aerogel can achieve the battery heating function, ensuring the temperature environment for battery operation and improving the battery capacity attenuation problem caused by low temperature.

[0031] (3) The excellent elasticity enables graphene / boron nitride aerogel to effectively alleviate the shrinkage and expansion forces generated during battery charging and discharging when used as a battery module material.

[0032] (4) When used as a battery module material, the present invention has the characteristics of heat insulation, Joule heating, elasticity, etc. Compared with traditional battery module aerogel materials, it can greatly reduce the production cost of the battery while improving the safety and stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is an optical photograph of the graphene / boron nitride aerogel prepared in Example 1 of the present invention;

[0034] Figure 2 is a SEM photograph of the graphene / boron nitride aerogel prepared in Example 1 of the present invention;

[0035] Figure 3 is a TEM photo of the graphene / boron nitride aerogel prepared in Example 1 of the present invention;

[0036] Figure 4 The mechanical properties of the graphene / boron nitride aerogel prepared in Example 1 of the present invention;

[0037] Figure 5 The thermal insulation performance of the graphene / boron nitride aerogel prepared in embodiment 1 of the present invention;

[0038] Figure 6 This is the Joule heating performance of the graphene / boron nitride aerogel prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below in conjunction with embodiments.

[0040] The present invention proposes a multifunctional integrated graphene / boron nitride aerogel with heat insulation, elasticity and Joule heating and a preparation method thereof. Specifically, using boron nitride aerogel as a matrix, by means of chemical vapor deposition (CVD), graphene is uniformly grafted from the inside to the outside of the boron nitride aerogel to obtain a multifunctional aerogel with heat insulation, elasticity and Joule heating properties.

[0041] Graphene / boron nitride aerogel has a three-dimensional continuous conductive network, which is composed of three-dimensional graphene and boron nitride. Graphene grows seamlessly on the boron nitride matrix to form a three-dimensional conductive path with a high aspect ratio. Due to the use of a three-dimensional flexible boron nitride skeleton, graphene / boron nitride aerogel has excellent flexibility.

[0042] The main elements of the graphene / boron nitride aerogel are carbon, boron, nitrogen and oxygen.

[0043] The internal microstructure of the graphene / boron nitride aerogel is a composite nanobelt structure composed of graphene and boron nitride.

[0044] The length of the composite nanobelt composed of graphene and boron nitride in the graphene / boron nitride aerogel is 1 μm to 900 μm.

[0045] The width of the composite nanobelt composed of graphene and boron nitride in the graphene / boron nitride aerogel is 50nm-15μm.

[0046] The density of the graphene / boron nitride aerogel is 5-80 mg / mL.

[0047] The electrical conductivity of the graphene / boron nitride aerogel is 0.1-2.7 S / cm.

[0048] The graphene / boron nitride aerogel has Joule heating characteristics, that is, the graphene / boron nitride aerogel can achieve a heating function under voltage.

[0049] The graphene / boron nitride aerogel has a porosity of 1 to 97%.

[0050] Specifically, the present invention provides a method for preparing a graphene / boron nitride aerogel, comprising the following steps:

[0051] Step 1) preparing melamine diborate solution:

[0052] Melamine and boric acid are dissolved in a co-solvent to obtain a melamine diborate solution.

[0053] Step 2) freeze-drying the melamine diborate solution to obtain melamine diborate aerogel.

[0054] Step 3) pyrolyzing the melamine diborate aerogel in a high temperature atmosphere to obtain a boron nitride aerogel.

[0055] Step 4) A chemical vapor deposition process is used in the boron nitride aerogel to achieve uniform grafting of graphene from the inside to the outside on the boron nitride substrate to obtain graphene / boron nitride aerogel.

[0056] Specifically:

[0057] In step 1), the molar ratio of melamine to boric acid is 1:5 to 5:1.

[0058] The mixed volume ratio of water to methanol, ethanol, isopropanol, n-butanol or tert-butanol in the co-solvent is 7:5 to 9:11.

[0059] In step 2), a vacuum freeze-drying process is selected, and the vacuum freeze-drying treatment time is 12 to 48 hours.

[0060] In step 3), the pyrolysis temperature is 500-2000° C., and the high-temperature pyrolysis time is 0.5-12 h.

[0061] The atmosphere is ammonia, argon, nitrogen or a mixture of any two.

[0062] In step 4), chemical vapor deposition process:

[0063] A carbon source (methanol) with a high O / C ratio is used, and a chemical vapor deposition pump is used to control the residence time of the carbon source (methanol) gas inside the boron nitride aerogel. The rate of the chemical vapor deposition pump is 20-70%. The gas pressure in the chemical vapor deposition furnace is 5-20 kPa. The growth temperature of graphene is 850-1150° C., the growth time of graphene is 1-10 hours, and the graphene content in the graphene / boron nitride aerogel is 10-35% of the total amount of the graphene / boron nitride aerogel.

[0064] In summary, the multifunctional integrated graphene / boron nitride aerogel prepared by the present invention not only has excellent elasticity and thermal insulation properties, but also has Joule heating properties. After connecting to a voltage of 1.5-6V, it can maintain the normal working temperature environment of the battery and improve the problem of low-temperature capacity attenuation of the battery. While improving the safety and stability of the battery, it can greatly reduce the production cost of the battery. It is expected to be applied to battery module materials.

[0065] The technical solution of the present invention is further described in detail below through several embodiments in conjunction with the accompanying drawings.

[0066] Embodiment 1:

[0067] Weigh 0.4838g of melamine and 0.4762g of boric acid, and add them to 48mL of tert-butyl alcohol / distilled water co-solvent in sequence, wherein the ratio of tert-butyl alcohol to distilled water is 7:5, and the concentration of the mixed solution is 20mg / mL. A melamine diboric acid solution is obtained, which is transferred to a vacuum freeze dryer for 24h to obtain a melamine diboric acid aerogel.

[0068] The melamine diboric acid aerogel is transferred to a tubular furnace, heated to 1100°C in an ammonia / nitrogen environment for high-temperature heat treatment for 3 hours to obtain boron nitride aerogel.

[0069] The obtained boron nitride aerogel is placed in a chemical vapor deposition furnace, and the residence time of the carbon source gas in the boron nitride aerogel is controlled by using an adjustable rate chemical vapor deposition pump. The rate of the chemical vapor deposition pump is adjusted to 60% immediately after the sample is placed in the furnace cavity. The graphene growth temperature is 1050°C. After the temperature is raised to the target temperature, the chemical vapor deposition pump rate is adjusted to 20%, and the inlet valve is opened to adjust the pressure in the furnace to 5-20kPa. On this basis, graphene is grown for 2h. Graphene / boron nitride aerogel can be obtained; the graphene content in the graphene / boron nitride aerogel is 15% of the total amount of graphene / boron nitride aerogel.

[0070] 4. The test results show that the thermal conductivity can reach 0.045W / m·k, the electrical conductivity is 0.45S / cm, and the density is 25mg / cm3. Figure 1 It can be seen that graphene / boron nitride aerogel can be prepared in large quantities. Figure 2 , Figure 3 It can be seen that in the microstructure of the prepared graphene / boron nitride aerogel, graphene grows uniformly from the inside to the outside inside the boron nitride. Figure 4 It can be seen that graphene / boron nitride aerogel has excellent elasticity. Figure 5 It can be seen that graphene / boron nitride aerogel has excellent thermal insulation properties. Figure 6 It can be seen that graphene / boron nitride aerogel has Joule heating characteristics.

[0071] Embodiment 2:

[0072] Weigh 0.2419g of melamine and 0.2381g of boric acid, and add them to 48mL of tert-butyl alcohol / distilled water co-solvent in sequence, wherein the ratio of tert-butyl alcohol to distilled water is 7:5, and the concentration of the mixed solution is 10mg / mL. A melamine diboric acid solution is obtained, which is transferred to a vacuum freeze dryer for 24h to obtain a melamine diboric acid aerogel.

[0073] The melamine diboric acid aerogel is transferred to a tubular furnace, heated to 1100°C in an ammonia / nitrogen environment for high-temperature heat treatment for 3 hours to obtain boron nitride aerogel.

[0074] The obtained boron nitride aerogel is placed in a chemical vapor deposition furnace, and the residence time of the carbon source gas in the boron nitride aerogel is controlled by using an adjustable rate chemical vapor deposition pump. The rate of the chemical vapor deposition pump is adjusted to 60% immediately after the sample is placed in the furnace cavity. The graphene growth temperature is 1050°C. After the temperature is raised to the target temperature, the chemical vapor deposition pump rate is adjusted to 20%, and the air inlet valve is opened to adjust the pressure in the furnace to 5-20kPa. On this basis, graphene is grown for 2h. Graphene / boron nitride aerogel can be obtained, and the graphene content in the graphene / boron nitride aerogel is 20% of the total amount of graphene / boron nitride aerogel.

[0075] The test results show that the thermal conductivity is 0.035W / m·k, the electrical conductivity is 0.65S / cm, the density is 15mg / cm3, and the mechanical properties are stable.

[0076] Embodiment 3:

[0077] Weigh 0.4838g of melamine and 0.4762g of boric acid, and add them to 48mL of tert-butyl alcohol / distilled water co-solvent in sequence, wherein the ratio of tert-butyl alcohol to distilled water is 7:5, and the concentration of the mixed solution is 20mg / mL. A melamine diboric acid solution is obtained, which is transferred to a vacuum freeze dryer for 24h to obtain a melamine diboric acid aerogel.

[0078] The melamine diboric acid aerogel is transferred to a tubular furnace, heated to 1100°C in an ammonia / nitrogen environment for high-temperature heat treatment for 3 hours to obtain boron nitride aerogel.

[0079] The obtained boron nitride aerogel is placed in a chemical vapor deposition furnace, and the residence time of the carbon source gas in the boron nitride aerogel is controlled by using an adjustable rate chemical vapor deposition pump. The rate of the chemical vapor deposition pump is immediately adjusted to 60% after the sample is placed in the furnace cavity. The graphene growth temperature is 1050°C. After the temperature is raised to the target temperature, the chemical vapor deposition pump rate is adjusted to 20%, and the air inlet valve is opened to adjust the pressure in the furnace to 5-20kPa. On this basis, graphene is grown for 4 hours. Graphene / boron nitride aerogel can be obtained, and the graphene content in the graphene / boron nitride aerogel is 27% of the total amount of graphene / boron nitride aerogel.

[0080] The test results show that the thermal conductivity is 0.025W / m·k, the electrical conductivity is 0.84S / cm, the density is 30mg / cm3, and the mechanical properties are stable.

[0081] Embodiment 4:

[0082] Weigh 0.4838g of melamine and 0.4762g of boric acid, and add them to 48mL of tert-butyl alcohol / distilled water co-solvent in sequence, wherein the ratio of tert-butyl alcohol to distilled water is 7:5, and the concentration of the mixed solution is 20mg / mL. A melamine diboric acid solution is obtained, which is transferred to a vacuum freeze dryer for 24h to obtain a melamine diboric acid aerogel.

[0083] The melamine diboric acid aerogel is transferred to a tubular furnace, heated to 1100°C in an ammonia / nitrogen environment for high-temperature heat treatment for 3 hours to obtain boron nitride aerogel.

[0084] The obtained boron nitride aerogel is placed in a chemical vapor deposition furnace, and the residence time of the carbon source gas in the boron nitride aerogel is controlled by using an adjustable rate chemical vapor deposition pump. The rate of the chemical vapor deposition pump is adjusted to 60% immediately after the sample is placed in the furnace cavity. The graphene growth temperature is 1050°C. After the temperature is raised to the target temperature, the chemical vapor deposition pump rate is adjusted to 20%, and the air inlet valve is opened to adjust the pressure in the furnace to 5-20kPa. On this basis, graphene is grown for 6 hours. Graphene / boron nitride aerogel can be obtained, and the graphene content in the graphene / boron nitride aerogel is 35% of the total amount of graphene / boron nitride aerogel.

[0085] The test results show that the thermal conductivity is 0.025W / m·k, the electrical conductivity is 1.8S / cm, the density is 40mg / cm3, and the mechanical properties are stable.

Claims

1. A method for preparing graphene / boron nitride aerogel, characterized in that: The following steps are involved: The melamine diborate aerogel is subjected to pyrolysis treatment to obtain a boron nitride aerogel; Taking boron nitride aerogel as a substrate, graphene is deposited on the substrate by chemical vapor deposition to obtain graphene / boron nitride aerogel; Graphene is deposited on a substrate using chemical vapor deposition. The specific process is: Methanol is used as a carbon source, and the graphene content in the graphene / boron nitride aerogel is 10-35% of the total amount of the graphene / boron nitride aerogel; The graphene / boron nitride aerogel is a composite nanoribbon structure; The length of the composite nanobelt structure is 1 μm to 900 μm; The width is 50 nm~15μm.

2. The method for preparing a graphene / boron nitride aerogel according to claim 1, characterized in that: The preparation method of melamine diborate aerogel comprises the following steps: Dissolving melamine and boric acid in a co-solvent and stirring sufficiently to obtain a melamine diborate solution, wherein the molar ratio of melamine to boric acid is 1:5 to 5:1; The co-solvent includes water and methanol, ethanol, isopropanol, n-butanol or tert-butanol, wherein the volume ratio of water to methanol, ethanol, isopropanol, n-butanol or tert-butanol is 7:5 to 9:11; The melamine diborate solution is freeze-dried to obtain the melamine diborate aerogel.

3. The method for preparing a graphene / boron nitride aerogel according to claim 2, characterized in that: The process conditions for freeze drying are: The vacuum freeze-drying treatment time is 12 to 48 hours.

4. The method for preparing a graphene / boron nitride aerogel according to claim 1, characterized in that: The specific process of pyrolyzing melamine diborate aerogel to obtain boron nitride aerogel is as follows: The pyrolysis is carried out in a high temperature atmosphere, the pyrolysis temperature is 500~2000 ℃; the pyrolysis time is 0.5~12h.

5. The method for preparing a graphene / boron nitride aerogel according to claim 4, characterized in that: The high temperature atmosphere is ammonia, argon, nitrogen or a mixture of any two of them.

6. A graphene / boron nitride aerogel, characterized in that: The graphene / boron nitride aerogel is prepared by the preparation method according to any one of claims 1 to 5.