A composite film and its preparation method and application

By growing the hydrotalcite layer in situ on the ion conductive film of the zinc-based liquid flow battery and forming a composite film, the problems of zinc dendrites growth and battery short circuit are solved, and efficient zinc-based battery performance improvement and long life are achieved.

CN114614039BActive Publication Date: 2024-11-19DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202011443489.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-08
Publication Date
2024-11-19
Estimated Expiration
2040-12-08

AI Technical Summary

Technical Problem

Uneven deposition of zinc in zinc-based flow batteries leads to dendrite growth, punctures the separator, causing battery short circuits and performance attenuation, affecting the cycle life of the battery.

Method used

The hydrotalcite layer is grown in situ on the ion conductive film, forming a composite film as a separator, preventing the growth and puncture of zinc dendrites, and preparing a 3D hydrotalcite buffer layer by hydrothermal reaction method, providing physical barriers and positive charge regulation.

Benefits of technology

Effectively prevent zinc dendrites from puncture, extend battery life, improve Coulomb efficiency and energy density, and significantly improve the capacity and stability of zinc-based batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114614039B_ABST
    Figure CN114614039B_ABST
Patent Text Reader

Abstract

The present application discloses a composite membrane and its preparation method and application, wherein the composite membrane comprises an ion-conducting membrane and a buffer layer; the buffer layer is in-situ grown on the surface of the ion-conducting membrane; the buffer layer comprises hydrotalcite. In the composite membrane of the present application, the buffer layer provides a physical barrier for the ion-conducting membrane, which can effectively prevent zinc dendrites from piercing the diaphragm, and effectively alleviate the problem of zinc dendrites causing battery short circuit and reduced battery life during battery cycling; at the same time, the surface capacity of the battery is improved, so that ultra-high capacity and long-life zinc-based batteries can be realized. The present application uses an improved urea method to in-situ grow a 3D hydrotalcite layer on the surface of a porous ion-conducting membrane, which is low-cost, and the resulting composite membrane has good stability and excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a composite film and a preparation method and application thereof, belonging to the technical field of alkaline zinc-based secondary batteries. Background Art

[0002] As energy shortages and environmental problems become increasingly severe, the demand for renewable energy such as solar and wind energy is becoming increasingly urgent. However, these renewable energy sources are unstable and discontinuous, which seriously hinders their widespread application. Energy storage devices, especially the widely used electrochemical energy storage technology, can effectively solve these problems: improve the stability and efficiency of the power grid of portable electronic devices, and in smart grid regulation. Among the many electrochemical energy storage technologies, flow batteries have good application prospects in the field of energy storage due to their perfect combination of high safety, high efficiency and high flexibility.

[0003] As a typical representative of hybrid flow batteries, zinc-based flow batteries (ZFBS) have the advantages of high energy density and low cost, and are very suitable for the application of fixed energy storage systems. The zinc negative electrode has the characteristics of low intrinsic electrode potential, fast kinetics, good cyclability, and abundant reserves. However, the uneven deposition of zinc leads to the growth of zinc dendrites at the negative electrode. The dendrites will pierce the diaphragm, causing the electrolyte to interpenetrate, resulting in a decrease in the coulombic efficiency of the battery, and at the same time causing the battery to short-circuit, resulting in rapid attenuation of battery performance; in addition, the abnormal growth of zinc leads to zinc shedding, which not only reduces the coulombic efficiency of the battery, but also causes the electrolyte circulation channel to be blocked, affecting the uniformity of the flow field distribution, thereby shortening the cycle life of the battery. Summary of the invention

[0004] According to one aspect of the present application, a composite membrane and a preparation method and application thereof are provided. The composite membrane is used as a flow battery diaphragm by in-situ growing a hydrotalcite layer on an ion-conducting membrane, thereby inhibiting the growth of zinc dendrites and preventing zinc dendrites from piercing the diaphragm, thereby solving the problem of zinc dendrites and zinc accumulation in alkaline zinc-based batteries.

[0005] The composite membrane comprises an ion conducting membrane and a buffer layer;

[0006] The buffer layer is grown in situ on the surface of the ion-conducting membrane;

[0007] The buffer layer includes hydrotalcite.

[0008] Optionally, the buffer layer has a three-dimensional network structure.

[0009] Optionally, the buffer layer has a porosity of 70-90% and a specific surface area of ​​60-100m 2 / g.

[0010] Optionally, the buffer layer has a thickness of 1-5 μm.

[0011] Optionally, the composite membrane has a thickness of 100-120 μm, a pore size of 0.5-40 nm, and a porosity of 60-90%.

[0012] Optionally, the ion-conducting membrane contains at least one of anion exchange groups such as sulfonic acid groups and nitrate groups;

[0013] Preferably, the ion conducting membrane is a porous ion conducting membrane;

[0014] More preferably, the porous ion conductive membrane is selected from any one of a PES / SPEEK porous membrane and a SPEEK porous membrane.

[0015] According to another aspect of the present application, a method for preparing the above-mentioned composite film is provided, the method comprising at least the following steps:

[0016] Step 1, reacting the polymer substrate film with a mixture containing a metal salt to obtain a reaction solution I;

[0017] Step 2: adding urea to the reaction solution I and subjecting it to a hydrothermal reaction to obtain the composite membrane.

[0018] Optionally, in step 1, the metal salt includes a divalent metal salt and a trivalent metal salt;

[0019] The cation in the divalent metal salt is Mg 2+ 、Ni 2+ 、Co 2+ 、Zn 2+ , Cu 2+ At least one of;

[0020] The cation in the trivalent metal salt is Al 3+ Cr 3+ , Fe 3+ Sc 3+ At least one of;

[0021] The anion in the metal salt is selected from NO3 - 、CO3 2- , Cl - OH - 、SO4 2- PO4 3- At least one of .

[0022] Preferably, the divalent metal salt is Mg(NO3)2, and the trivalent metal salt is Al(NO3)3.

[0023] In the mixture, the molar ratio of divalent metal cations to trivalent metal cations is 1-4:1;

[0024] Preferably, the molar ratio of divalent metal cations to trivalent metal cations is 2:1-3:1.

[0025] Specifically, in the molar ratio of the divalent metal cation to the trivalent metal cation, the ratio of the divalent metal cation can be independently selected from 1, 1.5, 2, 2.5, 3, 3.5, 4, or any value between the above two points.

[0026] Optionally, in step 1, the mixture further comprises a solvent;

[0027] The solvent includes water;

[0028] Preferably, the concentration of the metal salt in the mixture is 0.5-1 mol / L.

[0029] Specifically, in the mixture, the concentration of the metal salt can be independently selected from 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, or any value between the above two points.

[0030] Optionally, in step 2, the molar ratio of urea to metal salt is 1-2:30, calculated based on the molar ratio of cations in the metal salt.

[0031] Specifically, the lower limit of the molar ratio of urea to metal salt can be independently selected from 1:30, 1:26, 1:24, 1:22, 1:20; the upper limit of the molar ratio of urea to metal salt can be independently selected from 1:19, 1:18, 1:17, 1:16, 2:30.

[0032] Optionally, in step 2, the conditions of the hydrothermal reaction are:

[0033] The hydrothermal reaction temperature is 80-120°C, and the hydrothermal reaction time is 12-72h.

[0034] Preferably, the hydrothermal reaction temperature is 90-100° C., and the hydrothermal reaction time is 24-36 h.

[0035] Specifically, the lower limit of the hydrothermal reaction temperature can be independently selected from 80°C, 85°C, 90°C, 85°C, and 100°C; the upper limit of the hydrothermal reaction temperature can be independently selected from 105°C, 110°C, 115°C, 117°C, and 120°C.

[0036] Specifically, the lower limit of the hydrothermal reaction time can be independently selected from 12h, 18h, 24h, 30h, 36h; the lower limit of the hydrothermal reaction time can be independently selected from 42h, 48h, 54h, 60h, 72h.

[0037] In one embodiment of the present application, the method comprises:

[0038] a) immersing the porous ion conductive membrane in a mixed solution of a divalent metal salt and a trivalent metal salt for a certain period of time;

[0039] b) adding urea to the mixed solution to obtain a hydrotalcite precursor solution;

[0040] c) subjecting the hydrotalcite precursor solution to a hydrothermal reaction to obtain a 3D hydrotalcite buffer layer composite film.

[0041] 3D hydrotalcite layers can be grown on the surface of porous ion-conducting membranes by a hydrothermal method.

[0042] In one implementation mode of the present application, step b) is:

[0043] The urea powder is slowly added to the mixed aqueous solution in which the porous ion conductive membrane is soaked under stirring conditions, and stirred for 2-3 hours.

[0044] According to another aspect of the present application, there is provided an application of any of the above-mentioned composite membranes or composite membranes prepared by any of the methods in a liquid flow battery, characterized in that the composite membrane is used as a liquid flow battery diaphragm.

[0045] The flow battery is an alkaline-based flow battery;

[0046] Preferably, the alkaline-based flow battery is selected from any one of an alkaline-based zinc-iron flow battery, a zinc-nickel flow battery, a zinc-manganese flow battery, and a zinc-silver flow battery.

[0047] The beneficial effects of this application include:

[0048] 1. In the composite membrane of the present application, the buffer layer provides a physical barrier for the ion-conducting membrane, which can effectively prevent zinc dendrites from piercing the diaphragm, and effectively alleviate the problem of zinc dendrites causing battery short circuit and reduced battery life during battery cycling; at the same time, the surface capacity of the battery is increased, so that ultra-high capacity and long-life zinc-based batteries can be realized;

[0049] 2. The positive charge characteristics of the buffer layer surface in this application, the buffer layer is Zn(OH)4 2- During the deposition process, it plays a role in regulating the Zn(OH)4 on the electrode-diaphragm surface 2- The distribution effect makes Zn(OH)4 2- The actual speed of deposition on the electrode surface is reduced, that is, the actual current on the electrode surface is reduced, thereby inhibiting the growth of zinc dendrites; achieving the first application of regulating zinc dendrites through positive charges on the diaphragm surface;

[0050] 3. The present application utilizes the high hydroxide ion transport properties and interlayer selectivity of hydrotalcite to achieve the ion conductivity and active material selectivity of the composite membrane. Compared with the traditional polyethersulfone porous membrane, the composite membrane of the present application exhibits higher ion selectivity and higher ion conductivity in the alkaline electrolyte system;

[0051] 4. This application utilizes an improved urea method to in-situ grow a 3D hydrotalcite layer on the surface of a porous ion-conducting membrane, which is low-cost and the resulting composite membrane has good stability and excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 The first morphological characterization diagram of the composite membrane provided in Example 1, wherein a is a SEM diagram of the surface morphology of the composite membrane, and b and c are both enlarged diagrams of a;

[0053] Figure 2 is a second morphological characterization diagram of the composite membrane in Example 1, wherein a is a cross-sectional morphology SEM diagram of the in-situ grown composite membrane of hydrotalcite, and b is an enlarged diagram of a;

[0054] Figure 3 This is a characterization diagram of the surface hydrotalcite crystal structure of the composite film in Example 1;

[0055] Figure 4 a is an alkaline zinc-iron flow battery assembled with LDH-G1 and Base1 provided in Example 1 and Comparative Example 1 at 80 mA cm -2 Battery performance diagram;

[0056] Figure 4 b is the capacity decay curve of the alkaline zinc-iron flow battery assembled by LDH-G1 and Base1 provided in Example 1 and Comparative Example 1;

[0057] Figure 5 The zinc deposition morphology, zinc dendrite morphology and carbon felt morphology of the alkaline zinc-iron flow battery assembled with the membrane materials provided in Example 1 and Comparative Example 1 at the end of charging are shown respectively, wherein a is the zinc deposition morphology of the alkaline zinc-iron flow battery assembled with the LDH-G1 provided in Example 1 at the end of charging; b is the zinc dendrite morphology of the alkaline zinc-iron flow battery assembled with the Base1 provided in Comparative Example 1 at the end of charging; c is the carbon felt morphology of the alkaline zinc-iron flow battery assembled with the LDH-G1 provided in Example 1 at the end of discharging; d is the carbon felt morphology of the alkaline zinc-iron flow battery assembled with the Base1 provided in Comparative Example 1 at the end of discharging;

[0058] Figure 6 a is an alkaline zinc-iron flow battery assembled with LDH-G2 provided in Example 2 at 80 mA cm -2 Battery performance diagram;

[0059] Figure 6 b is the cycle performance of the zinc symmetric battery assembled with LDH-G2 provided in Example 2;

[0060] Figure 7a is an alkaline zinc-iron flow battery assembled with LDH-G3 provided in Example 3 at 80 mA cm -2 Battery performance diagram;

[0061] Figure 7 b is the cycling performance of the zinc symmetric battery assembled with LDH-G3 provided in Example 3. DETAILED DESCRIPTION

[0062] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0063] Unless otherwise specified, the raw materials in the examples of this application were purchased from commercial sources.

[0064] In the embodiments of the present application,

[0065] The porosity, surface area and pore size of the composite membrane were tested using a physical adsorption instrument BET instrument (model ASAP-2010).

[0066] The crystal structure of hydrotalcite was characterized by X-ray diffractometer (XRD, Rigaku D / Max2500PC).

[0067] The buffer layer was characterized using a scanning electron microscope (SEM) instrument (model JSM-7800F).

[0068] The zeta potential of the composite membrane surface was tested using a nanoparticle size analyzer (model Zetasizer Nano).

[0069] The battery performance was tested using an Arbin charge and discharge tester.

[0070] Example 1.

[0071] Polyethersulfone PES and sulfonated polyetheretherketone SPEEK were dissolved in DMAC solvent at a mass ratio of 9:1 to obtain a blended solution with a solid content of 35wt%, stirred evenly and allowed to stand, then poured onto a clean, flat glass plate. Under 20% humidity conditions, a 200μm scraper was used to scrape out a smooth diaphragm, immersed in water, and the solvent was dissolved. After removing the solvent, a PES / SPEEK porous base membrane (porous ion conductive membrane) was obtained, which was soaked in water for later use.

[0072] The PES / SPEEK porous substrate membrane obtained above was immersed in 75 mL of a mixed salt solution of 0.6 mol / L Mg(NO3)2 and 0.3 mol / L Al(NO3)3 for 15 h to ensure that SO 3-After fully interacting with the metal ions in the salt solution, urea was slowly added under stirring (the concentration of urea in the total system was 0.05 mol / L) and stirred for 3 hours; then it was transferred to a stainless steel reactor with a Teflon lining and subjected to a hydrothermal reaction at 90°C for 36 hours. The membrane layer was taken out and the surface was rinsed with ultrapure water to obtain a 3D array (i.e., a three-dimensional network structure) ( Figure 1 ), porosity 90%, specific surface area 80m 2 / g, 3D hydrotalcite buffer layer composite film with zeta potential of 30mV (denoted as LDH-G1). The thickness of the hydrotalcite buffer layer is 2μm ( Figure 2 ), the total thickness of the composite membrane is 120μm, the pore size of the composite membrane is 0.5-40nm (the hydrotalcite buffer layer is a nano-scale microporous structure, and the base membrane pore size is in the mesoporous range), and the porosity of the composite membrane is 70%. The X-ray diffraction results (XRD) show that the XRD characteristic peak (LDH-G1) corresponds to the characteristic peak of hydrotalcite ( Figure 3 ), indicating that a layer of hydrotalcite inorganic layer grows uniformly on the membrane surface.

[0073] LDH-G1 was applied to alkaline zinc-iron flow batteries, with LDH-G1 as the separator, carbon felt as the positive and negative electrodes, and 0.8 mol / L Fe(CN)6 4- +3mol / L OH - Solution; negative electrode electrolyte is 0.4mol / L Zn(OH)4 2- +3.8mol / LOH - solution; the volume of positive and negative electrolytes is 40 mL each; the battery adopts constant current charge and discharge mode at 80 mA cm -2 The current density was 80 mA cm-1 and the charge was continued for 50 min. -2 Discharge to 0.1V under the current density condition. From the performance of the battery ( Figure 4 a) It can be seen that at 80 mA cm -2 At the current density, the initial coulombic efficiency (CE) of the LDH-G1 assembled battery is 98.5%, the voltage efficiency (VE) is 92%, and the energy efficiency (EE) can reach 90.6%. The high coulombic efficiency achieved by the corresponding battery is analyzed to be due to the introduction of highly selective layered hydrotalcite materials on the surface, which effectively blocks the cross-linking of active substances, thereby improving the selectivity of the composite membrane. At the same time, the 3D array structure of hydrotalcite is conducive to the transmission of carrier hydroxide ions, thereby ensuring the high voltage efficiency of the diaphragm. The alkaline zinc-iron liquid flow battery assembled with LDH-G1 has a high current density of 80mA cm -2 It can still show high cycle stability at low current density and can complete 700 charge and discharge cycles without obvious performance degradation ( Figure 4 b). At the same time, the morphology of zinc deposition after cycling was characterized ( Figure 5 ), and found that the negative electrode zinc deposition is a uniform and dense zinc morphology ( Figure 5 a), verifying the anti-Zn dendrite effect of the 3D buffer layer.

[0074] LDH-G1 was applied to zinc symmetric batteries, with LDH-G1 as the separator and 0.4 mol / L Zn(OH)4 in both positive and negative electrolytes. 2- +4mol / L NaOH, volume 40mL each; the battery adopts constant current charge and discharge mode at 80mA cm -2 The current density was 80 mA cm-1 for 20 min. -2 At the current density, the initial coulombic efficiency (CE) of the battery assembled by LDH-G1 was 99%, and it was stably cycled for 700 cycles. The carbon felt at the end of discharge was analyzed and no obvious zinc accumulation was found ( Figure 5 c), indicating that the battery assembled with this membrane can realize a reversible zinc deposition process.

[0075] Example 2

[0076] Prepare a PES / SPEEK porous base membrane (porous ion conductive membrane) and soak it in water for later use. The preparation method is basically the same as that in Example 1.

[0077] The PES / SPEEK porous substrate membrane obtained above was immersed in 75 mL of a mixed salt solution of 0.6 mol / L Mg(NO3)2 and 0.2 mol / L Al(NO3)3 for 15 h to ensure that SO3 - After fully interacting with the metal ions in the salt solution, urea was slowly added under stirring (the concentration of urea in the total system was 0.05 mol / L) and stirred for 3 hours; then it was transferred to a stainless steel reactor with a Teflon lining and subjected to a hydrothermal reaction at 90°C for 36 hours. The membrane layer was removed and the surface was rinsed with ultrapure water to obtain a 3D array with a porosity of 90% and a specific surface area of ​​80 m 2 / g, 3D hydrotalcite buffer layer composite membrane with zeta potential of 20mV (denoted as LDH-G2), hydrotalcite layer thickness of 2μm, total composite membrane thickness of 120μm, composite membrane pore size of 0.5-40nm, composite membrane porosity of 60%.

[0078] LDH-G2 was applied to an alkaline zinc-iron flow battery in the same manner as in Example 1, except that LDH-G2 was used instead of LDH-G1 as the separator. The obtained alkaline zinc-iron flow battery was subjected to a performance test under the same battery test conditions as in Example 1. Figure 6 a) It can be seen that at 80 mA cm -2Under the current density, the initial coulombic efficiency (CE) of the LDH-G1 assembled battery is 97.5%, the voltage efficiency (VE) is 91%, and the energy efficiency (EE) can reach 88.7%.

[0079] LDH-G2 was applied to zinc symmetric cells in the same manner as in Example 1, except that LDH-G2 was used instead of LDH-G1 as the separator. -2 At the current density, the initial coulombic efficiency (CE) of the LDH-G2 assembled battery is 98%, and the stable cycle is 100 cycles ( Figure 6 b), the cycle life is reduced compared with Example 1, which can be attributed to the reduction of positive charge on the surface of hydrotalcite, which reflects the effect of surface charge in inhibiting zinc dendrites.

[0080] Example 3

[0081] Prepare a PES / SPEEK porous base membrane (porous ion conductive membrane) and soak it in water for later use. The preparation method is basically the same as that in Example 1.

[0082] The PES / SPEEK porous substrate membrane obtained above was immersed in 75 mL of a mixed salt solution of 0.6 mol / L Mg(NO3)2 and 0.6 mol / L Al(NO3)3 for 15 h to ensure that SO3 - After fully interacting with the metal ions in the salt solution, urea was slowly added under stirring (the concentration of urea in the total system was 0.05 mol / L) and stirred for 3 hours; then it was transferred to a stainless steel reactor with a Teflon lining and subjected to a hydrothermal reaction at 90°C for 36 hours. The membrane layer was removed and the surface was rinsed with ultrapure water to obtain a 3D array with a porosity of 90% and a specific surface area of ​​80 m 2 / g, zeta potential 10mV 3D hydrotalcite buffer layer composite membrane (denoted as LDH-G3). The hydrotalcite layer thickness is 2μm, the total thickness of the composite membrane is 120μm, the pore size of the composite membrane is 0.5-40nm, and the porosity of the composite membrane is 60%.

[0083] LDH-G3 was applied to an alkaline zinc-iron flow battery in the same manner as in Example 1, except that LDH-G3 was used instead of LDH-G1 as the separator. The obtained alkaline zinc-iron flow battery was subjected to a performance test under the same battery test conditions as in Example 1. Figure 7 a) It can be seen that at 80 mA cm -2 Under the current density, the initial coulombic efficiency (CE) of the LDH-G1 assembled battery is 96.5%, the voltage efficiency (VE) is 90%, and the energy efficiency (EE) can reach 86.8%.

[0084] LDH-G3 was applied to zinc symmetric cells in the same manner as in Example 1, except that LDH-G3 was used instead of LDH-G1 as the separator. -2 At the current density, the initial coulombic efficiency (CE) of the LDH-G3 assembled battery was 97%, and the stable cycle was 80 cycles ( Figure 7 b), the cycle life is reduced compared with Examples 1 and 2, which can be attributed to the reduction of positive charge on the surface of hydrotalcite, which causes the attenuation of battery performance. This shows the effect of surface charge in inhibiting zinc dendrites.

[0085] Comparative Example 1

[0086] Dissolve polyethersulfone PES and sulfonated polyetheretherketone SPEEK in DMAC solvent at a mass ratio of 9:1 to obtain a blended solution with a solid content of 35wt%, stir evenly and let stand, then pour on a clean and flat glass plate, scrape out a flat membrane with a 200μm scraper under 20% humidity, immerse in water, wait for the solvent to dissolve, remove the solvent to obtain a polyethersulfone porous ion conductive membrane, soak in water for standby use. Directly dry at room temperature for 10min to obtain a polyethersulfone porous ion conductive membrane (denoted as Base1) without hydrotalcite, with a pore size of 1 to 40nm and a porosity of 50%.

[0087] It is applied to alkaline zinc-iron flow batteries, with Base as the diaphragm, carbon felt as the positive and negative electrodes, and 0.8 mol / L Fe(CN)6 4- +3mol / L OH - Solution; negative electrode electrolyte is 0.4mol / L Zn(OH)4 2- +3.8mol / L OH - solution; the volume of positive and negative electrolytes is 40 mL each; the battery adopts constant current charge and discharge mode at 80 mA cm -2 The current density was 80 mA cm-1 and the charge was continued for 50 min. -2 Discharge to 0.1V under the current density condition. From the performance of the battery ( Figure 4 a) It can be seen that the battery assembled by Base is 80mA cm -2 At a current density of 1.5 Å, its CE is only 92%. As the cycle progresses, it shows obvious capacity decay ( Figure 4 b), this is because during the battery cycle, the unevenness of zinc deposition leads to battery capacity decay. Compared with the battery assembled in Examples 1, 2, and 3, the performance is relatively low, and the zinc deposition morphology after cycling is dendritic ( Figure 5 b), which poses a great threat to the separator and affects the battery life. The battery assembled with this membrane can only be cycled 30 times, proving the structural and performance advantages of the 3D hydrotalcite buffer layer.

[0088] Base1 was used in zinc symmetric batteries, with Base1 as the separator and 0.4 mol / L Zn(OH)4 in both positive and negative electrolytes. 2- +4mol / L NaOH, volume 40mL each; the battery adopts constant current charge and discharge mode at 80mA cm -2 The current density was 80 mA cm-1 for 20 min. -2 At the current density, the initial coulombic efficiency (CE) of the battery assembled by Base1 is 94%. After only 20 cycles, the efficiency is significantly reduced, which is mainly caused by the irreversible zinc deposition process. Analysis of the carbon felt at the end of discharge shows obvious zinc accumulation ( Figure 5 d), indicating that the battery assembled with this membrane can realize a reversible zinc deposition process.

[0089] Comparative Example 2

[0090] Prepare a PES / SPEEK porous base membrane (porous ion conductive membrane) and soak it in water for later use. The preparation method is basically the same as that in Example 1.

[0091] The PES / SPEEK porous substrate membrane obtained above was immersed in 75 mL of a mixed salt solution of 0.6 mol / L Mg(NO3)2 and 0.6 mol / L Zn(NO3)2 for 15 h to ensure that SO3 - After fully interacting with the metal ions in the salt solution, urea was slowly added under stirring (the concentration of urea in the total system was 0.05 mol / L) and stirred for 3 hours; then it was transferred to a stainless steel reactor with a Teflon lining and subjected to a hydrothermal reaction at 90°C for 36 hours. The membrane layer was removed and the surface was rinsed with ultrapure water to obtain a 3D array with a porosity of 90% and a specific surface area of ​​80 m 2 / g, zeta potential 0mV 3D hydrotalcite buffer layer composite membrane (denoted as LDH-G0). The hydrotalcite layer thickness is 1μm, the total thickness of the composite membrane is 116μm, the pore size of the composite membrane is 0.5-40nm, and the porosity of the composite membrane is 60%.

[0092] LDH-G0 was applied to an alkaline zinc-iron flow battery in the same manner as in Example 1, except that LDH-G0 was used instead of LDH-G1 as the separator. The obtained alkaline zinc-iron flow battery was subjected to a performance test under the same battery test conditions as in Example 1. It can be seen from the battery performance that at 80 mA cm -2 At the current density of 80 mA cm, the initial coulombic efficiency (CE) of the battery assembled with LDH-G0 was 95%, the voltage efficiency (VE) was 90%, and the energy efficiency (EE) was 85.5%. -2Only 50 charge-discharge cycles can be achieved at the current density. Compared with Comparative Example 1, the 3D network structure provides a better zinc deposition buffer, so that its cycle life is higher than that without the 3D buffer layer. However, compared with Examples 1, 2, and 3, LDH-G0 has no charge, and the cycle life of the battery is significantly reduced. This is mainly due to the Zn(OH)4 2- The uneven distribution of Zn leads to the formation of zinc dendrites, which reduces the battery cycle life.

[0093] Comparative Example 3

[0094] Prepare a PES / SPEEK porous base membrane (porous ion conductive membrane) and soak it in water for later use. The preparation method is basically the same as that in Example 1.

[0095] The PES / SPEEK porous substrate membrane obtained above was immersed in 75 mL of a precursor solution of 0.8 mol / L 2-methylimidazole and 0.1 mol / L zinc nitrate and stirred for 3 h. It was then transferred to a stainless steel reactor with a Teflon lining and subjected to a hydrothermal reaction at 90 °C for 8 h. The membrane layer was then taken out and the surface was rinsed with ultrapure water to obtain a 3D array with a porosity of 80% and a specific surface area of ​​70 m 2 / g, 3D ZIF buffer layer composite membrane with zeta potential of 0 mV (denoted as ZIF-M), ZIF layer thickness of 1 μm, total composite membrane thickness of 117 μm, composite membrane pore size of 0.5-40 nm, composite membrane porosity of 50%.

[0096] The membrane was assembled into an alkaline zinc-iron flow battery, which -2 Under this condition, the battery coulombic efficiency (CE) is 96%, the voltage efficiency (VE) is only 88%, and the cycle life is only 30 cycles. The 3D ZIF layer is conducive to the transmission of ions, which brings about an improvement in the voltage efficiency (VE). However, the ZIF material itself has poor alkali resistance and non-charged surface characteristics, and the cycle life is poor, but it is improved compared with comparative example 1, which proves the effect of the 3D buffer layer. However, compared with Examples 1, 2, and 3, the battery performance has not been significantly improved.

[0097] Comparative Example 4

[0098] Prepare a PES / SPEEK porous base membrane (porous ion conductive membrane) and soak it in water for later use. The preparation method is basically the same as that in Example 1.

[0099] 0.04g of boron nitride nanosheets (BNNSs) particles were uniformly dispersed in 2g of 1wt% perfluorosulfonic acid (Nafion) isopropanol solution and then uniformly dispersed in ultrasound for 4 hours to obtain a BNNSs uniform dispersion, with a mass ratio of BNNSs (g) to 1wt% Nafion binder (g) of 0.02:1. 0.1ml of the prepared dispersion was drawn with a syringe and uniformly sprayed on the surface of the polyethersulfone PES / SPEEK porous base membrane to obtain a BNNSs-modified 2D porous ion conductive membrane (BNNSs-M), with a zeta potential of 0mV, a BNNSs layer thickness of 2μm, and a composite membrane thickness of 118μm; the BNNSs layer is a two-dimensional layered nanomaterial, which is 2D distributed on the membrane surface and constructs a 2D structure on the membrane surface.

[0100] The membrane was assembled into an alkaline zinc-iron flow battery, which -2 Under the conditions, the battery coulombic efficiency (CE) is 94%, the voltage efficiency (VE) is only 80%, and the cycle life is only 30 cycles. The reason for this is that the non-in situ grown 2D surface brings poor ion transport, that is, low voltage efficiency. Compared with the 3D structures of Examples 1, 2, and 3, the battery performance of the 2D BNNSs-M membrane surface is poor.

[0101] Comparative Example 5

[0102] Prepare a PES / SPEEK porous base membrane (porous ion conductive membrane) and soak it in water for later use. The preparation method is basically the same as that in Example 1.

[0103] Weigh 0.04g of montmorillonite particles and disperse them uniformly in 2g of 1wt% Nafion solution, and then disperse them uniformly in ultrasound for 4 hours to obtain a uniform dispersion of montmorillonite, and the mass ratio of montmorillonite (g) to 1wt% Nafion binder (g) is 0.02:1. Use a syringe to draw 0.1ml of the prepared dispersion and spray it uniformly on the surface of the polyethersulfone PES / SPEEK porous base membrane to obtain a montmorillonite-modified 2D porous ion conductive membrane (MT-M), with a zeta potential of -20mV, a montmorillonite layer thickness of 2μm, and a composite membrane thickness of 118μm; the montmorillonite layer is a two-dimensional layered nanomaterial, which is 2D distributed on the membrane surface, so that the membrane surface is negatively charged.

[0104] The membrane was assembled into an alkaline zinc-iron flow battery, which -2 Under the condition of CE 95%, VE is only 78%, and the cycle life is only 50 cycles. The low voltage efficiency corresponds to the poor ion transport of the 2D structure. However, due to the negative charge on the surface, which is consistent with the charge of the base film, Zn(OH)4 can be repelled. 2- , but cannot regulate Zn(OH)4 2-Therefore, there is no obvious improvement effect on battery performance. This indirectly reflects the advantages of the 3D structure and surface positive charge in the embodiment.

[0105] Comparative Example 6

[0106] Prepare a PES / SPEEK porous base membrane (porous ion conductive membrane) and soak it in water for later use. The preparation method is basically the same as that in Example 1.

[0107] The PES / SPEEK porous substrate membrane obtained above was immersed in 75 mL of a mixed salt solution of 0.6 mol / L Mg(SO4)2 and 0.3 mol / L Zn(SO4)2 for 15 h to ensure that SO3 - After fully interacting with the metal ions in the salt solution, urea was slowly added under stirring (the concentration of urea in the total system was 0.05 mol / L) and stirred for 3 hours; then it was transferred to a stainless steel reactor with a Teflon lining and subjected to a hydrothermal reaction at 90°C for 36 hours. The membrane layer was taken out and the surface was rinsed with ultrapure water to obtain a hydrotalcite buffer layer composite membrane (denoted as LDH-GS). Due to the weak SO4 2- The resulting composite membrane hydrotalcite failed to grow completely due to interaction, and there were large area defects. The pore size of the composite membrane was 1-40nm, and the porosity was 50%.

[0108] LDH-GS was applied to an alkaline zinc-iron flow battery in the same manner as in Example 1, except that LDH-GS was used instead of LDH-G1 as the separator. The obtained alkaline zinc-iron flow battery was subjected to a performance test under the same battery test conditions as in Example 1. -2 At the current density, the initial coulombic efficiency (CE) of the LDH-GS assembled battery was 95%, the voltage efficiency (VE) was 90%, and the energy efficiency (EE) was 85.5%. Due to the uneven distribution of hydrotalcite on the membrane surface, the battery performance was poor and decayed rapidly.

[0109] The application of the 3D hydrotalcite buffer layer composite membrane provided in the present application in alkaline-based flow batteries, compared with the traditional polyethersulfone porous membrane, the 3D non-conductive buffer layer of the 3D hydrotalcite buffer layer composite membrane provides a physical barrier and the positive charge characteristics of the hydrotalcite surface inhibit zinc dendrites, thereby obtaining a high-stability dendrite-free zinc-based flow battery. It has similar effects in other alkaline-based flow batteries such as alkaline zinc-nickel flow batteries, zinc-manganese flow batteries, and zinc-silver flow batteries.

[0110] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a composite membrane for alkaline zinc-based flow battery, It is characterized in that At least the following steps are included: Step 1, reacting the polymer substrate film with a mixture containing a metal salt to obtain a reaction solution I; Step 2, adding urea to the reaction solution I, and subjecting the reaction solution to a hydrothermal reaction to obtain the composite membrane; The composite membrane comprises an ion conducting membrane and a buffer layer; The buffer layer is in-situ grown on the surface of the ion conducting membrane; The buffer layer includes hydrotalcite; The buffer layer has a three-dimensional network structure; The surface of the buffer layer has a positive charge; The metal salt is a mixture of a divalent metal salt and a trivalent metal salt.

2. The preparation method according to claim 1, It is characterized in that The porosity of the buffer layer is 70-90%, and the specific surface area is 60-100 m 2 / g.

3. The preparation method according to claim 1, It is characterized in that The thickness of the buffer layer is 1-5 μm.

4. The preparation method according to claim 1, It is characterized in that The zeta potential of the buffer layer surface is 10-30 mV.

5. The preparation method according to claim 1, It is characterized in that The ion conducting membrane contains at least one of a sulfonic acid group and a nitrate group.

6. The preparation method according to claim 1, It is characterized in that In step 1, The cation in the divalent metal salt is Mg 2+ 、Ni 2+ 、Co 2+ 、Zn 2+ , Cu 2+ At least one of; The cation in the trivalent metal salt is Al 3+ Cr 3+ , Fe 3+ Sc 3+ At least one of; The anion in the metal salt is selected from NO 3 - , CO 3 2- , Cl - OH - 、SO 4 2- ,PO 4 3- At least one of .

7. The preparation method according to claim 1, It is characterized in that In the mixture, the molar ratio of divalent metal cations to trivalent metal cations is 1-4:

1.

8. The preparation method according to claim 7, It is characterized in that The molar ratio of divalent metal cations to trivalent metal cations is 2:1-3:

1.

9. The preparation method according to claim 1, It is characterized in that In step 1, the mixture further comprises a solvent; The solvent includes water.

10. The preparation method according to claim 1, It is characterized in that In the mixture, the concentration of the metal salt is 0.5-1 mol / L.

11. The preparation method according to claim 1, It is characterized in that In step 1, the reaction time is at least 12 h.

12. The preparation method according to claim 1, It is characterized in that In step 2, the molar ratio of urea to metal salt is 1-2:30 based on the molar ratio of cations in the metal salt.

13. The preparation method according to claim 1, It is characterized in that In step 2, the conditions of the hydrothermal reaction are: The hydrothermal reaction temperature is 80-120°C, and the hydrothermal reaction time is 12-72 h.

14. The preparation method according to claim 1, It is characterized in that The alkaline zinc-based flow battery is selected from any one of an alkaline zinc-iron flow battery, a zinc-nickel flow battery, a zinc-manganese flow battery, and a zinc-silver flow battery.

Citation Information

Patent Citations

  • Method for synthesizing hydrotalcite composite membrane in situ

    CN106861454A

  • Gas-barrier and ionic-conduction bifunctional thin-film material and preparation method thereof

    CN107666003A

  • One-step hydrothermal preparation method for magnesium-aluminum hydrotalcite film on magnesium alloy surface

    CN107740086A

  • Application of porous ion conduction membrane with negative charges in alkaline zinc-based battery

    CN110165308A