CNFs / ZnO composite wave absorbing material based on bacterial cellulose and preparation method thereof

By compounding bacterial cellulose with ZnO, an efficient CNFs/ZnO composite microwave absorbing material is prepared, which solves the problems of performance degradation at high temperatures and complicated preparation processes of existing technologies, and achieves efficient microwave absorption and environmentally friendly industrial production.

CN114614271BActive Publication Date: 2024-10-18SOUTH CHINA UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210193409.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-28
Publication Date
2024-10-18
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

The performance of existing microwave absorbing materials decreases under high temperature conditions, and the preparation process of carbon-based materials is complex and not environmentally friendly, making it difficult to meet the requirements of high-performance microwave absorbing materials for military and civilian needs.

Method used

Bacterial cellulose is used as the carbon source, acidified CNFs are obtained through pyrolysis and acid treatment, and compounded with ZnO. CNFs/ZnO composite absorbing materials are prepared through hydrothermal method to achieve industrial production.

Benefits of technology

The material exhibits greater dielectric loss and efficient microwave absorption performance at high temperatures, and the preparation process is environmentally friendly and low-cost, in line with the concept of green synthesis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114614271B_ABST
    Figure CN114614271B_ABST
Patent Text Reader

Abstract

The invention discloses a CNFs / ZnO composite absorbing material based on bacterial cellulose and a preparation method thereof, comprising the following steps: (1) purifying bacterial cellulose and freeze-drying to obtain pure bacterial cellulose; (2) placing the pure bacterial cellulose in a tube furnace for pyrolysis reaction under an inert atmosphere, and then treating with acid to obtain acidified CNFs; (3) weighing the acidified CNFs and Zn(CH3COO)2·2H2O and dissolving them in diethylene glycol, and mechanically stirring the mixture to obtain a mixed solution; (4) placing the mixed solution in a reactor under a sealed condition for heating reaction; (5) centrifuging, washing, and drying the product obtained after the reaction. The invention adopts biological material bacterial fiber as a carbon source, and utilizes a hydrothermal method to prepare a CNFs / ZnO composite material, which uses green and environmentally friendly materials, has a simple preparation process, does not require complex synthesis equipment, has low cost, and is suitable for industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wave absorbing materials, and in particular to a CNFs / ZnO composite wave absorbing material based on bacterial cellulose and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of microwave communication technology, electromagnetic radiation pollution in the environment has become a problem that cannot be ignored. It not only interferes with the normal operation of electronic equipment, but also causes harm to human health. At the same time, the rapid development of modern electronic countermeasure technology has also made various weapons in future wars, such as missiles, aircraft, tanks, ships, etc., face huge threats. Therefore, the key to continuously improving the battlefield survival, penetration and deep strike capabilities of weapons is to apply micro-absorption materials to stealth technology, so as to solve some difficult problems in the military. Stealth material technology is to use various high-tech means in a specific remote sensing detection environment to effectively suppress the target's radar, infrared, laser, electromagnetic signals and other characteristic signals, and ultimately make weapons difficult to be discovered, identified and attacked within a certain range. Therefore, the importance of research on microwave absorbing materials is self-evident. On the one hand, good microwave absorbing materials can improve the advancement of military weapons, and on the other hand, they can improve the level of communication technology and bring great convenience to people's lives. Therefore, there is a great demand for microwave absorbing materials in military and civilian applications, and the requirements are getting higher and higher.

[0003] Carbon-based materials are currently the most widely used microwave absorbing materials due to their light weight, good conductivity and low cost, such as carbon microspheres, graphene, carbon nanotubes, carbon fibers, etc. Unfortunately, the dielectric loss of pure carbon is large, which can easily cause impedance mismatch and lead to poor microwave absorption. Therefore, carbon materials are usually combined with magnetic materials to achieve high-performance microwave absorption. However, magnetic materials are prone to lose their magnetism at high temperatures and cannot be used in high temperature conditions.

[0004] Dielectric loss absorbing materials have developed rapidly in the field of microwave absorption due to their advantages such as high temperature resistance, low density and high strength. For example, in the metal semiconductor oxide / carbon-based nanomaterial composite system, ZnO has poor conductivity, which can effectively adjust the dielectric constant of carbon-based materials. After loading ultra-light materials, additional interface interactions can be generated, and the presence of oxygen vacancies will cause interface polarization and defect dipoles, so that the material exhibits greater dielectric loss and efficient microwave absorption, while also reducing the density of the absorber. There are also some studies on C / ZnO composite absorbing materials, but the choice of carbon materials is mostly graphene, carbon nanotubes, micron-sized fibers, etc., and the carbon source materials are not environmentally friendly, the preparation process is complex, and the preparation cost is high (Lu MM, Cao WQ, Shi HL, et al. Multi-wall carbon nanotubes decorated with ZnO nanocrystals: mild solution-process synthesis and highly efficient microwave absorption properties at elevated temperature [J]. Journal of Materials Chemistry A, 2014, 2 (27): 10540-10547.). As a renewable and environmentally friendly material, bacterial cellulose is an extracellular polysaccharide synthesized by microorganisms. It has better properties than plant fibers, such as high purity, high crystallinity, good biocompatibility, and biodegradability. It has been widely used in food, papermaking, acoustic equipment, especially in the field of biomedical materials, but has been less studied in the field of microwave absorption. Bacterial cellulose is a natural nanofiber material (20-100nm in diameter and several microns in length). These nano-sized microfibers form a three-dimensional network structure, which is a highly porous structure. After carbonization treatment at a certain temperature, a highly oriented, network-like nanocarbonized fiber is obtained. Therefore, using bacterial cellulose as a carbon source can better solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to provide a CNFs / ZnO composite absorbing material based on bacterial cellulose and a preparation method thereof. The material preparation method is simple, the raw materials are environmentally friendly, the cost is low, and industrial large-scale production can be achieved.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a CNFs / ZnO composite wave absorbing material based on bacterial cellulose comprises the following steps:

[0008] Step 1, purifying bacterial cellulose and freeze-drying it to obtain pure bacterial cellulose;

[0009] Step 2, under an inert atmosphere, placing the pure bacterial cellulose obtained in step 1 in a tubular furnace for pyrolysis reaction, and then treating it with acid for a certain period of time to obtain acidified CNFs;

[0010] Step 3, weighing a certain amount of the acidified CNFs and Zn(CH3COO)2·2H2O obtained in step 2, dissolving them in diethylene glycol, and mechanically stirring the mixture to obtain a mixed solution;

[0011] Step 4, placing the mixed solution obtained in step 3 in a reaction vessel under sealed conditions for heating reaction;

[0012] Step 5, centrifuging, washing and drying the product obtained after the reaction in step 4 to obtain the CNFs / ZnO composite absorbing material based on bacterial cellulose.

[0013] Furthermore, in step 1, the reagents for the purification treatment are distilled water and NaOH solution.

[0014] Furthermore, in step 1, the freeze-drying temperature is -35°C to -50°C, and the freeze-drying time is 72 to 96 hours.

[0015] Furthermore, in step 2, the acid for the acid treatment is nitric acid or sulfuric acid, and the treatment time is 6 to 24 hours. Furthermore, in step 2, the temperature of the pyrolysis reaction is 800 to 1000°C, the heating rate is 2 to 5°C / min, and the pyrolysis time is 2 to 6 hours.

[0016] Furthermore, in step 3, the concentration of Zn(CH3COO)2·2H2O in diethylene glycol is 0.2-0.3M.

[0017] Furthermore, in step 4, the heating reaction temperature is 120-180° C. and the time is 4-9 hours.

[0018] Furthermore, in step 5, the washing is performed alternately using anhydrous ethanol and distilled water.

[0019] Furthermore, in step 5, the drying condition is under vacuum condition, the drying temperature is 60-80° C., and the drying time is 12-24 hours.

[0020] The present invention also provides a CNFs / ZnO composite wave absorbing material based on bacterial cellulose prepared by the above preparation method.

[0021] Compared with the prior art, the beneficial effects of the present invention are:

[0022] (1) In the CNFs / ZnO composite absorber based on bacterial cellulose described in the present invention, ZnO can effectively adjust the dielectric constant of the carbon-based material, and the loaded carbon material can also produce additional interface interactions. The presence of oxygen vacancies can cause interface polarization and defect dipoles, thereby making the material exhibit greater dielectric loss and efficient microwave absorption, while also reducing the density of the absorber.

[0023] (2) The present invention uses biomaterial bacterial fiber as a carbon source and utilizes a hydrothermal method to prepare CNFs / ZnO composite absorbing materials. The raw materials involved are environmentally friendly and green; and the preparation method involved is simple, low-cost, and conforms to the preparation concept of green synthesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 XRD patterns of pure CNFs material and CNFs / ZnO composite absorbers based on bacterial cellulose prepared in Examples 1, 2 and 3;

[0025] Figure 2 This is the SEM image of pure CNFs material;

[0026] Figure 3 This is a SEM image of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 1;

[0027] Figure 4 This is a SEM image of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 2;

[0028] Figure 5 This is a SEM image of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 3;

[0029] Figure 6 This is the relationship curve between the electromagnetic wave reflection coefficient and frequency of pure CNFs material at different thicknesses;

[0030] Figure 7 The relationship between the electromagnetic wave reflection coefficient and the frequency of the CNFs / ZnO composite absorbing material based on bacterial cellulose prepared in Example 1 at different thicknesses is shown in FIG.

[0031] Figure 8 The relationship between the electromagnetic wave reflection coefficient and the frequency of the CNFs / ZnO composite absorbing material based on bacterial cellulose prepared in Example 2 at different thicknesses;

[0032] Fig. 9 The relationship between the electromagnetic wave reflection coefficient and the frequency of the CNFs / ZnO composite absorbing material based on bacterial cellulose prepared in Example 3 at different thicknesses;

[0033] Fig.10 The relationship between the electromagnetic wave reflection coefficient and the frequency of the CNFs / ZnO composite absorbing material based on bacterial cellulose prepared in Example 4 at different thicknesses;

[0034] Fig.11 This is a curve diagram showing the relationship between the electromagnetic wave reflection coefficient and frequency of the CNFs / ZnO composite absorbing material based on bacterial cellulose prepared in Example 5 at different thicknesses. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but the content of the present invention is not limited to the following embodiments.

[0036] Example 1

[0037] A method for preparing a CNFs / ZnO composite wave absorbing material based on bacterial cellulose comprises the following steps:

[0038] Step 1, soaking the bacterial cellulose in distilled water for 48 hours until it is neutral, then placing it in a 2 mol / L NaOH solution at 80° C. for 3 hours, and then soaking it in distilled water until it is neutral, and then purifying it and freeze-drying it with liquid nitrogen for 72 hours to obtain pure bacterial cellulose;

[0039] Step 2, under a nitrogen atmosphere, the pure bacterial cellulose obtained in step 1 was placed in a tube furnace for pyrolysis at 800°C for 6 hours at a heating rate of 5°C / min, and then treated with 3 mol / L HNO3 for 6 hours to obtain acidified CNFs;

[0040] Step 3, weigh 0.02 g of the acidified CNFs obtained in step 2 and 0.6585 g of Zn(CH3COO)2·2H2O, dissolve them in 15 mL of diethylene glycol, and mechanically stir the mixture for 30 min to obtain a mixed solution;

[0041] Step 4, under sealed conditions, placing the mixed solution obtained in step 3 in a reaction vessel for heating reaction, wherein the heating temperature is 120° C. and the heating time is 4 hours;

[0042] Step 5, centrifuging, washing and drying the product obtained after the reaction in step 4 to obtain a CNFs / ZnO composite absorbing material based on bacterial cellulose, the drying temperature is 60° C., and the drying time is 12 h.

[0043] Example 2

[0044] A method for preparing a CNFs / ZnO composite wave absorbing material based on bacterial cellulose comprises the following steps:

[0045] Step 1, soaking the bacterial cellulose in distilled water for 48 hours until it is neutral, then placing it in a 2 mol / L NaOH solution at 80° C. for 3 hours, and then soaking it in distilled water until it is neutral, and then purifying it and freeze-drying it with liquid nitrogen for 72 hours to obtain pure bacterial cellulose;

[0046] Step 2, under a nitrogen atmosphere, the pure bacterial cellulose obtained in step 1 was placed in a tube furnace for pyrolysis at 800°C for 6 hours with a heating rate of 5°C / min, and then treated with 3 mol / L HNO3 for 12 hours to obtain acidified CNFs;

[0047] Step 3, weigh 0.02 g of the acidified CNFs obtained in step 2 and 0.8323 g of Zn(CH3COO)2·2H2O, dissolve them in 15 mL of diethylene glycol, and mechanically stir the mixture for 30 min to obtain a mixed solution;

[0048] Step 4, under sealed conditions, placing the mixed solution obtained in step 3 in a reaction vessel for heating reaction, wherein the heating temperature is 150° C. and the heating time is 7 hours;

[0049] Step 5, centrifuging, washing and drying the product obtained after the reaction in step 4 to obtain a CNFs / ZnO composite absorbing material based on bacterial cellulose, the drying temperature is 60° C., and the drying time is 12 h.

[0050] Example 3

[0051] A method for preparing a CNFs / ZnO composite wave absorbing material based on bacterial cellulose comprises the following steps:

[0052] Step 1, soaking the bacterial cellulose in distilled water for 48 hours until it is neutral, then placing it in a 2 mol / L NaOH solution at 80° C. for 3 hours, and then soaking it in distilled water until it is neutral, and then purifying it and freeze-drying it with liquid nitrogen for 72 hours to obtain pure bacterial cellulose;

[0053] Step 2, under a nitrogen atmosphere, the pure bacterial cellulose obtained in step 1 was placed in a tube furnace for pyrolysis at 800°C for 6 hours with a heating rate of 5°C / min, and then treated with 3 mol / L HNO3 for 24 hours to obtain acidified CNFs;

[0054] Step 3, weigh 0.02 g of the acidified CNFs obtained in step 2 and 0.9878 g of Zn(CH3COO)2·2H2O, dissolve them in 15 mL of diethylene glycol, and mechanically stir the mixture for 30 min to obtain a mixed solution;

[0055] Step 4, under sealed conditions, placing the mixed solution obtained in step 3 in a reaction vessel for heating reaction, wherein the heating temperature is 180° C. and the heating time is 9 hours;

[0056] Step 5, centrifuging, washing and drying the product obtained after the reaction in step 4 to obtain a CNFs / ZnO composite absorbing material based on bacterial cellulose, the drying temperature is 60° C., and the drying time is 12 h.

[0057] Example 4

[0058] A method for preparing a CNFs / ZnO composite wave absorbing material based on bacterial cellulose comprises the following steps:

[0059] Step 1, soaking the bacterial cellulose in distilled water for 48 hours until it is neutral, then placing it in a 2 mol / L NaOH solution at 80° C. for 3 hours, and then soaking it in distilled water until it is neutral, and then purifying it and freeze-drying it with liquid nitrogen for 84 hours to obtain pure bacterial cellulose;

[0060] Step 2, under a nitrogen atmosphere, the pure bacterial cellulose obtained in step 1 was placed in a tube furnace for pyrolysis at 900°C for 4 hours with a heating rate of 5°C / min, and then treated with 3 mol / L HNO3 for 6 hours to obtain acidified CNFs;

[0061] Step 3, weigh 0.02 g of the acidified CNFs obtained in step 2 and 0.8232 g of Zn(CH3COO)2·2H2O, dissolve them in 15 mL of diethylene glycol, and mechanically stir the mixture for 30 min to obtain a mixed solution;

[0062] Step 4, under sealed conditions, placing the mixed solution obtained in step 3 in a reaction vessel for heating reaction, wherein the heating temperature is 150° C. and the heating time is 7 hours;

[0063] Step 5, centrifuging, washing and drying the product obtained after the reaction in step 4 to obtain the CNFs / ZnO composite absorbing material based on bacterial cellulose, the drying temperature is 70° C., and the drying time is 18 h.

[0064] Example 5

[0065] A method for preparing a CNFs / ZnO composite wave absorbing material based on bacterial cellulose comprises the following steps:

[0066] Step 1, soaking the bacterial cellulose in distilled water for 48 hours until it is neutral, then placing it in a 2 mol / L NaOH solution at 80° C. for 3 hours, and then soaking it in distilled water until it is neutral, and then freeze-drying it with liquid nitrogen for 96 hours to obtain pure bacterial cellulose;

[0067] Step 2, under a nitrogen atmosphere, the pure bacterial cellulose obtained in step 1 was placed in a tube furnace for pyrolysis at 800°C for 6 hours at a heating rate of 5°C / min, and then treated with 3 mol / L HNO3 for 6 hours to obtain acidified CNFs;

[0068] Step 3, weigh 0.02 g of the acidified CNFs obtained in step 2 and 0.8323 g of Zn(CH3COO)2·2H2O, dissolve them in 15 mL of diethylene glycol, and mechanically stir the mixture for 30 min to obtain a mixed solution;

[0069] Step 4, under sealed conditions, placing the mixed solution obtained in step 3 in a reaction vessel for heating reaction, wherein the heating temperature is 150° C. and the heating time is 7 hours;

[0070] Step 5, centrifuging, washing and drying the product obtained after the reaction in step 4 to obtain the CNFs / ZnO composite absorbing material based on bacterial cellulose, the drying temperature is 80° C., and the drying time is 24 hours.

[0071] Figure 1 Figure 3 is the XRD diagram of pure CNFs material and CNFs / ZnO composite absorber based on bacterial cellulose prepared in Examples 1, 2 and 3. It can be seen from the figure that pure CNFs has a broad peak near 23°, indicating that the CNFs is amorphous carbon. When CNFs are composited with ZnO, although the broad peak of CNFs is not obvious in comparison, the (100), (002), (101), (102), (110), (103), (200), (112) and (201) diffraction crystal planes of ZnO appear in Examples 1, 2 and 3, indicating that the prepared product is a CNFs / ZnO composite.

[0072] Figure 2 This is the SEM image of pure CNFs material. It can be seen from the figure that pure CNFs present the morphology of nanofibers with a three-dimensional porous network.

[0073] Figure 3 This is a SEM image of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 1. It can be seen from the image that the CNFs / ZnO composite material presents a three-dimensional porous network of nanofibers with ZnO nanoparticles attached to them, and the ZnO particles are agglomerated.

[0074] Figure 4 This is a SEM image of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 2. It can be seen from the figure that the CNFs / ZnO composite material presents a three-dimensional porous network of nanofibers with ZnO nanoparticles attached to them, and the ZnO particles are relatively evenly distributed on the CNFs.

[0075] Figure 5 This is the SEM image of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 3. It can be seen from the figure that the CNFs / ZnO composite material presents a three-dimensional porous network of nanofibers with ZnO nanoparticles attached to them. The ZnO particles are evenly distributed without obvious agglomeration.

[0076] Figure 6 This is a curve diagram of the relationship between the electromagnetic wave reflection coefficient and frequency of pure CNFs material at different thicknesses. It can be seen from the figure that the reflection loss of CNFs at different thicknesses does not reach -10dB.

[0077] Figure 7 This is a curve diagram of the relationship between the electromagnetic wave reflection coefficient and frequency of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 1 at different thicknesses. It can be seen from the figure that the reflection loss of the CNFs / ZnO composite material at a thickness of 2.3 mm is the lowest, which is -17.34 dB.

[0078] Figure 8 The relationship between the electromagnetic wave reflection coefficient and the frequency of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 2 at different thicknesses is shown in the figure. Figure 6 The wave absorption performance of pure CNFs materials has been significantly improved. The reflection loss of CNFs / ZnO composite materials at a thickness of 2.8 mm is the lowest, at -57.5 dB, which is much higher than that of pure CNFs materials.

[0079] Fig. 9 This is a curve diagram of the relationship between the electromagnetic wave reflection coefficient and frequency at different thicknesses of the CNFs / ZnO composite absorbing material based on bacterial cellulose prepared in Example 3. It can be seen from the figure that the reflection loss of the CNFs / ZnO composite material at a thickness of 3.1 mm is the lowest, which is -32.49 dB, much higher than that of pure CNFs material.

[0080] Fig. 9 This is a curve diagram of the relationship between the electromagnetic wave reflection coefficient and frequency at different thicknesses of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 4. It can be seen from the figure that the reflection loss of the CNFs / ZnO composite material at a thickness of 2.3 mm is the lowest, which is -19.79 dB.

[0081] Fig.11This is a curve diagram of the relationship between the electromagnetic wave reflection coefficient and frequency of the CNFs / ZnO composite absorber based on bacterial cellulose prepared in Example 5 at different thicknesses. It can be seen from the figure that the reflection loss of the CNFs / ZnO composite material at a thickness of 2.3 mm is the lowest, which is -16.05 dB.

[0082] According to the above analysis, the absorbing performance of the CNFs / ZnO composite absorbing materials based on bacterial cellulose prepared in Examples 1, 2, 3, 4, and 5 is significantly better than that of the existing pure CNFs materials, indicating that the preparation method of the present invention can make the material exhibit greater dielectric loss and efficient microwave absorption, and has broad application prospects in the field of absorbing material technology.

[0083] The above only describes the preferred embodiments of the present invention. The present invention is not limited to the above embodiments. The above embodiments and the description are only for explaining the principle of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a CNFs / ZnO composite absorbing material based on bacterial cellulose, characterized in that: The steps include: Step 1, purifying bacterial cellulose and freeze-drying it to obtain pure bacterial cellulose; Step 2, under an inert atmosphere, placing the pure bacterial cellulose obtained in step 1 in a tube furnace for pyrolysis reaction, and then treating with acid to obtain acidified CNFs; Step 3, weighing the acidified CNFs and Zn(CH3COO)2·2H2O obtained in step 2, dissolving them in diethylene glycol, and mechanically stirring the mixture to obtain a mixed solution; Step 4, placing the mixed solution obtained in step 3 in a reaction vessel under sealed conditions for heating reaction; Step 5, centrifuging, washing and drying the product obtained after the reaction in step 4 to obtain the CNFs / ZnO composite absorbing material based on bacterial cellulose.

2. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 1, the reagents for the purification treatment are distilled water and NaOH solution.

3. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 1, the freeze-drying temperature is -35°C to -50°C, and the freeze-drying time is 72 to 96 hours.

4. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 2, the acid used in the acid treatment is nitric acid or sulfuric acid, and the treatment time is 6 to 24 hours.

5. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 2, the temperature of the pyrolysis reaction is 800-1000° C., the heating rate is 2-5° C. / min, and the pyrolysis time is 2-6 hours.

6. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 3, the concentration of Zn(CH3COO)2·2H2O in diethylene glycol is 0.2-0.3M.

7. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 4, the heating reaction temperature is 120-180° C. and the time is 4-9 hours.

8. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 5, the washing is performed alternately using anhydrous ethanol and distilled water.

9. The method for preparing the CNFs / ZnO composite absorbing material based on bacterial cellulose according to claim 1, characterized in that: In step 5, the drying condition is under vacuum condition, the drying temperature is 60-80° C., and the drying time is 12-24 hours.

10. A CNFs / ZnO composite absorbing material based on bacterial cellulose prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Carbonized bacterial cellulose / magnetic composite wave-absorbing material and preparation method thereof

    CN102093840A

  • Carbon nanometer fiber / ferrite composite absorbing material and preparation method thereof

    CN103834361A