A light guide plate and backlight module with infrared transmission and visible light reflection functions

By designing a light guide plate with infrared reflection visible light in the LCD backlight module, the problem of the inability to transmit infrared rays in the prior art is solved, the thickness thinning and anti-warping performance of the backlight module is achieved, and the screen brightness is improved. and fingerprint recognition signal acquisition capability.

CN114660696BActive Publication Date: 2024-12-03NINGBO EXCITON TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202011522772.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-22
Publication Date
2024-12-03
Estimated Expiration
2040-12-22

AI Technical Summary

Technical Problem

The existing LCD backlight module cannot pass through infrared rays, causing the fingerprint recognition device to lose its signal acquisition capability.

Method used

Design a light guide plate with infrared-transmitted light reflecting visible light. By laminating the light guide plate and the reflective film into one, using the alternating deposition technology of inorganic plating, the structure of high refractive index and low refractive index is formed to achieve visible light efficient reflection and infrared transmission.

Benefits of technology

It realizes the thickness reduction and anti-warping performance of the backlight module, improves the screen brightness and fingerprint recognition signal acquisition capabilities, and meets the needs of efficient use of the comprehensive screen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114660696B_ABST
    Figure CN114660696B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of LCD backlight sources, and also covers the field of LCD backlight source fingerprint recognition, and in particular to a light guide plate and a backlight module with the function of transmitting infrared rays and reflecting visible light. In order to solve the problem that the existing backlight module cannot transmit infrared rays, the present invention provides a light guide plate and a backlight module with the function of transmitting infrared rays and reflecting visible light. The light guide plate includes a substrate and a functional layer from top to bottom, and the functional layer is an inorganic coating. The inorganic coating is composed of a high-refractive-index inorganic substance A and a low-refractive-index inorganic substance B. The refractive index of the inorganic substance A is greater than the refractive index of the inorganic substance B. The inorganic coating A and the inorganic coating B are alternately deposited on the surface of the light guide plate, and the deposition order is ABABA...BAB, and the number of deposited layers is 4 to 58. The backlight module provided by the present invention can transmit infrared rays and reflect visible light, and has a thinner thickness and stronger anti-warping performance, and can be applied to fingerprint recognition devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of LCD backlight sources, and also covers the field of LCD backlight source fingerprint recognition, in particular to a light guide plate and a backlight module with the functions of transmitting infrared rays and reflecting visible light. Technical Background

[0002] With the rapid development of display technology, people's demand for display screens is also tending towards large-area screens (known as full-screen in the industry). The advent of the full-screen era has squeezed the space for currently used capacitive or ultrasonic fingerprint recognition devices, and the efficient use of the front screen is particularly important.

[0003] The under-screen optical fingerprint recognition device solves this problem well and addresses the position conflict between the full screen and the fingerprint recognition device.

[0004] TFT-LCD (thin film transistor-liquid crystal display) is a non-self-luminous display technology device that requires a backlight source (also called a backlight module) to drive the display image.

[0005] The LCD backlight module contains a reflective film, a light guide plate, a diffusion film and a brightness enhancement film. In particular, the linear light source of the LED light bar will be converted into a surface light source through the light guide plate, and at the same time, a part of the light will escape from the bottom of the light guide plate. The reflective film reflects this part of the light back to the backlight module with high efficiency and low loss, thereby reducing light loss and improving the brightness of the backlight module.

[0006] The reflective film reflects visible light (usually with a wavelength of 380nm-780nm) back to the backlight module, and at the same time, infrared light (usually with a wavelength greater than 780nm) is also reflected. The signal recognized and received by the fingerprint sensor comes from infrared light, so it cannot receive signals and loses the fingerprint recognition ability. Summary of the invention

[0007] In order to solve the problem that the existing backlight module cannot transmit infrared rays, the present invention provides a light guide plate and a backlight module with the function of transmitting infrared rays and reflecting visible light. The light guide plate with the function of transmitting infrared rays and reflecting visible light is a light guide plate and a reflective film in the backlight module that are combined into one, and the functional layer is directly attached to the surface of one side of the light guide plate. Compared with the traditional backlight module, the light guide plate with the function of transmitting infrared rays and reflecting visible light provided by the present invention can transmit infrared rays and reflect visible light, solving the problem that the existing backlight module transmits infrared rays while reflecting visible light. The light guide plate provided by the present invention is thinner and has stronger anti-warping performance.

[0008] The light guide plate having the function of transmitting infrared rays and reflecting visible light comprises a substrate and a functional layer in order from top to bottom.

[0009] The substrate is a light guide plate used in an LCD backlight source.

[0010] The material of the substrate is selected from polycarbonate (PC), polymethyl methacrylate (PMMA) or colorless transparent polyimide (CPI). The thickness of the substrate is 0.075mm-0.36mm.

[0011] The light guide plate is obtained by injection molding to obtain a corresponding shape and thickness.

[0012] The functional layer is an inorganic coating layer prepared by vacuum magnetron sputtering or vacuum evaporation.

[0013] The inorganic coating layer is composed of a high-refractive-index inorganic substance A and a low-refractive-index inorganic substance B, wherein the refractive index of the inorganic substance A is greater than the refractive index of the inorganic substance B.

[0014] The thickness of the inorganic coating layer A is 10-300 nm. Further, the thickness of the inorganic coating layer A is 190 nm.

[0015] The material of the inorganic coating A is selected from metal oxides. Further, the material of the inorganic coating A is selected from one or a combination of at least two of titanium oxide, niobium pentoxide, aluminum oxide, and zinc oxide. Further, the targets used to prepare the titanium oxide, niobium pentoxide, aluminum oxide, and zinc oxide coatings are titanium oxide target, niobium pentoxide target, aluminum oxide target, and zinc oxide target, respectively. Further, the material of the inorganic coating A is niobium pentoxide.

[0016] The thickness of the inorganic coating layer B is 10-300 nm. Further, the thickness of the inorganic coating layer B is 270 nm.

[0017] The material of the inorganic coating B is one or a combination of at least two of silicon oxide, magnesium fluoride and zinc sulfide. Further, the target materials used to prepare the silicon oxide, magnesium fluoride and zinc sulfide coatings are silicon target, magnesium fluoride target and zinc sulfide target respectively. Further, the material of the inorganic coating B is silicon oxide.

[0018] The inorganic coating layer A and the inorganic coating layer B are alternately deposited on the surface of the light guide plate in the order of ABABA...BAB, and the number of deposited layers is 4 to 58. Furthermore, the number of deposited layers is 48.

[0019] The present invention provides a light guide plate with infrared transmission and visible light reflection function, the light guide plate includes a substrate and a functional layer from top to bottom; the substrate is made of polycarbonate (PC), the thickness of the substrate is 0.36mm; the functional layer is an inorganic coating, the inorganic coating is composed of a high refractive index inorganic substance A and a low refractive index inorganic substance B; the thickness of the inorganic coating A is 190nm, the material of the inorganic coating A is niobium pentoxide; the thickness of the inorganic coating B is 270nm, the material of the inorganic coating B is silicon oxide; the inorganic coating A and the inorganic coating B are alternately deposited on the surface of the light guide plate, the deposition order is ABABA...BAB, and the number of deposited layers is 48. The above technical solution includes embodiment 7.

[0020] Light is an electromagnetic wave with wave properties, and interference is one of the basic characteristics of light wave properties. Only light waves emitted by two coherent light sources with the same frequency, the same vibration direction or the same vibration component, the same phase or a constant phase difference are coherent waves. The reflected light and transmitted light between the film layers are coherent light, which meets the interference conditions. In the same medium, the refractive index of light of different wavelengths is different. Light with a shorter wavelength (for example, the visible light band) has a larger refractive index, while light with a longer wavelength (for example, the infrared band) has a smaller refractive index. Due to the difference in wavelength, visible light and infrared light have different optical path differences when passing through media with different refractive indices, so the situations of constructive interference and destructive interference are also different, so the transmission and reflection situations of the two also show differences.

[0021] The present invention provides a method for preparing a light guide plate having the functions of transmitting infrared light and reflecting visible light, the method comprising the following steps:

[0022] (1) Purge the substrate surface with nitrogen for 3-5 minutes to remove larger particles of impurities;

[0023] (2) cleaning the substrate surface by argon plasma bombardment for 10-15 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0024] (3) depositing an inorganic coating layer A on the substrate by high vacuum medium frequency magnetron sputtering;

[0025] (4) depositing an inorganic coating layer B on the substrate by high vacuum medium frequency magnetron sputtering;

[0026] (5) The inorganic coating layer A and the inorganic coating layer B are deposited alternately in this way until the required number of layers is reached.

[0027] Coating A is a high refractive index material, which comes from metal oxides, such as aluminum oxide, titanium oxide, niobium oxide, etc. The adhesion of metal oxides to PMMA or PC is better, so the inorganic coating A is first deposited on the substrate.

[0028] Through the above steps, a light guide plate having the functions of transmitting infrared rays and reflecting visible light is obtained by sputtering and depositing in sequence. The light guide plate has the functions of efficiently reflecting visible light and transmitting infrared rays.

[0029] The present invention further provides a backlight module, comprising the light guide plate provided by the present invention which has the functions of transmitting infrared rays and reflecting visible light.

[0030] Furthermore, the backlight module does not include a separate reflective film.

[0031] Furthermore, the backlight module includes a light source, a light guide plate with the function of transmitting infrared rays and reflecting visible light, a diffusion film and a brightness enhancement film. The light guide plate converts the light emitted by the light source into a surface light source, and at the same time, efficiently reflects part of the escaped visible light back to the module, while the infrared rays are transmitted normally, the diffusion film is used to improve the uniformity of the light, and the brightness enhancement film is used to gather light to improve the brightness of the backlight module.

[0032] Compared with the prior art, the present invention achieves the following excellent effects:

[0033] (1) By combining the light guide plate with the reflective functional layer, a light guide plate with the functions of transmitting infrared light and reflecting visible light is obtained. Since there is no separate reflective film, the thickness of the backlight module is greatly reduced, which is more in line with the lightweight design and meets the market demand;

[0034] (2) Since there is no separate reflective film, the escaping light does not experience the air layer interface, the optical path becomes shorter, and the absorption of light is also weakened, thereby improving the utilization rate of light;

[0035] (3) Multi-layer coating will generate great internal stress, causing the single reflective film to be severely warped, affecting the assembly and use of the backlight. However, the present invention uses a multi-layer coating attached to the surface of the light guide plate. Due to the special material of the light guide plate, the light guide plate has strong resistance to internal stress. Therefore, the light guide plate with infrared transmission and visible light reflection is very flat and meets market requirements.

[0036] (4) A light guide plate that transmits infrared light and reflects visible light, with a reflectivity of more than 95% for visible light and a transmittance of more than 85% for infrared light, which is very beneficial for improving screen brightness and collecting signals for fingerprint recognition devices.

[0037] The light guide plate with the function of transmitting infrared rays and reflecting visible light provided by the present invention can transmit infrared rays and reflect visible light, which solves the problem that the existing backlight module transmits infrared rays while reflecting visible light, and can be applied to fingerprint recognition devices. Furthermore, the light guide plate provided by the present invention is thinner and has stronger anti-warping performance. The backlight module provided by the present invention can transmit infrared rays and reflect visible light, and is thinner and has stronger anti-warping performance, and can be applied to fingerprint recognition devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a schematic diagram of the cross-sectional structure of a light guide plate with the function of transmitting infrared rays and reflecting visible light provided by the present invention.

[0039] 10: Light guide plate

[0040] 20: Plating A

[0041] 30: Plating B DETAILED DESCRIPTION

[0042] The present invention will be described in detail below with reference to the accompanying drawings and embodiments.

[0043] like Figure 1 As shown, the present invention provides a light guide plate with the function of transmitting infrared rays and reflecting visible light, comprising a light guide plate 10, and a coating layer A20 and a coating layer B30 are alternately attached to one side of the light guide plate 10.

[0044] Example 1

[0045] Provided is a light guide plate having the function of transmitting infrared rays and reflecting visible light, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and the preparation method comprises the following steps:

[0046] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0047] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0048] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0049] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0050] (5) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for two co-deposition cycles (the total number of deposited layers is 4);

[0051] Example 2

[0052] Provided is a light guide plate having the function of transmitting infrared rays and reflecting visible light, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and the preparation method comprises the following steps:

[0053] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0054] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0055] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0056] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0057] (5) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for a total of 4 cycles (a total of 8 layers);

[0058] Example 3

[0059] Provided is a light guide plate having the function of transmitting infrared rays and reflecting visible light, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and the preparation method comprises the following steps:

[0060] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0061] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0062] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0063] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0064] (5) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for a total of 6 cycles (a total of 12 layers);

[0065] Example 4

[0066] Provided is a light guide plate having the function of transmitting infrared rays and reflecting visible light, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and the preparation method comprises the following steps:

[0067] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0068] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0069] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0070] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0071] (5) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for a total of 8 cycles (a total of 16 layers);

[0072] Example 5

[0073] Provided is a light guide plate having the function of transmitting infrared rays and reflecting visible light, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and the preparation method comprises the following steps:

[0074] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0075] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0076] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0077] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0078] (5) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for 12 cycles (a total of 24 layers);

[0079] Example 6

[0080] Provided is a light guide plate having the function of transmitting infrared rays and reflecting visible light, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and the preparation method comprises the following steps:

[0081] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0082] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0083] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0084] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0085] (5) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for a total of 16 cycles (a total of 32 layers);

[0086] Example 7

[0087] Provided is a light guide plate having the function of transmitting infrared rays and reflecting visible light, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and the preparation method comprises the following steps:

[0088] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0089] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0090] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0091] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0092] (5) Repeat steps (3) and (4) to alternately deposit the niobium pentoxide coating A and the silicon dioxide coating B for 24 cycles (48 layers in total).

[0093] Comparative Example 1

[0094] Provided is a light guide plate, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and a preparation method comprises the following steps:

[0095] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0096] (2) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0097] (3) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0098] (4) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for two co-deposition cycles (deposition of AB is one cycle);

[0099] The difference between the light guide plate provided in this comparative example and the technical solution provided in this application is that the substrate used in this comparative example is not cleaned by argon plasma bombardment, in order to demonstrate that argon plasma attack cleaning of the substrate is beneficial to improving adhesion.

[0100] Comparative Example 2

[0101] Provided is a light guide plate, wherein the substrate is made of polycarbonate (PC) with a thickness of 0.36 mm, and a preparation method comprises the following steps:

[0102] (1) Purge the substrate surface with nitrogen for 3 min to remove larger particles of impurities;

[0103] (2) The vacuum degree of the coating chamber is 0.1 mbar, the argon gas flow rate is 20 sccm, the negative bias power supply voltage is 700 V, and the surface of the substrate is cleaned by argon plasma bombardment for 10 minutes to remove surface oxides and increase the surface energy of the substrate, thereby improving the adhesion between the coating and the substrate;

[0104] (3) Depositing a niobium pentoxide coating A on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 120 sccm and an oxygen flow rate of 60 sccm, turning on a medium frequency sputtering power source loaded on a niobium pentoxide target, and controlling the power at 12 kW to deposit a niobium pentoxide coating A with a thickness of 190 nm;

[0105] (4) Depositing silicon dioxide B on the substrate by high vacuum medium frequency magnetron sputtering, with an argon flow rate of 100 sccm and an oxygen flow rate of 80 sccm, turning on the medium frequency sputtering power source loaded on the silicon target, and controlling the power at 17 kW to deposit a silicon dioxide coating B with a thickness of 270 nm;

[0106] (5) repeating steps (3) and (4) to alternately deposit the niobium pentoxide coating layer A and the silicon dioxide coating layer B for 30 cycles (a total of 60 layers);

[0107] The difference between the light guide plate provided in this comparative example and the technical solution provided in this application is that the total number of coating layers in this comparative example is increased to 60 layers, in order to reflect that the total number of coating layers has an upper limit.

[0108] The light guide plates prepared in the embodiments of the present invention and the comparative examples were tested for their main properties in the following manner:

[0109] 1. Reflectivity and transmittance test: According to the standard of NIST 2054, the reflectivity and transmittance of the wavelength of 380nm-1000nm are tested using Agilent Cary5000 UV-visible near-infrared spectrophotometer. The average value of the reflectivity of the wavelength of 380nm-780nm is taken. The larger the average value, the stronger the visible light reflectivity. The transmittance values ​​at the wavelengths of 850nm and 940nm are taken. The larger the value, the stronger the transmittance.

[0110] Adhesion test: According to the standard of GB 1720-1979 "Determination of adhesion of paint films", the adhesion of the functional layer to the substrate is tested, where 100 / 100 means no film peeling, and 90 / 100 means 10% peeling.

[0111] Warpage value test: The sample size should be 12cm long and 6cm wide. Place the sample on a marble table and use a plug gauge to test the warpage values ​​of the four corners of the sample. The maximum value is taken as the warpage value of the sample. The smaller the value, the better the anti-warpage performance. A warpage value of less than 1mm is considered qualified.

[0112] Table 1 Performance test results of the light guide plates provided in Examples 1-7 and Comparative Examples 1-2:

[0113]

[0114] As can be seen from Table 1, compared with Example 1, Comparative Example 1 lacks argon plasma bombardment of the substrate and no pretreatment of the substrate, resulting in poor adhesion between the coating and the substrate, so the argon plasma pretreatment process is very necessary. Since the number of coating layers in Comparative Example 2 is already large, the internal stress of the coating is also increased accordingly, the adhesion of the coating is reduced, and about 20% of the test area has fallen off. Therefore, under the premise of meeting the optical performance, the coating cycle has a certain upper limit.

[0115] It can be seen from Examples 1-7 that as the coating cycle increases, the number of coating layers continues to increase, and the light guide plate with the function of transmitting infrared rays and reflecting visible light gradually enhances its reflection of visible light. In particular, the light guide plate provided in Example 7 of the present invention has the best performance, with an average reflectivity exceeding 95% in the 380nm-780nm band, while the transmittance at 850nm and 940nm remains at a level greater than 85%. The light guide plate provided in Example 7 satisfies the high-efficiency reflection of visible light and ensures the transmission of infrared rays, which can well meet the requirements for visible light reflection in the field of LCD backlight sources, and at the same time well meet the signal collection of the fingerprint recognition device.

[0116] It can be seen from Examples 1-7 and Comparative Example 2 that as the coating cycle increases and the number of coating layers increases, the warping caused by the increased stress in the coating layer gradually becomes prominent, but the warping value is still less than 1 mm, and the warping is qualified. Therefore, the light guide plate has good anti-warping ability.

[0117] The thickness of the backlight module with a conventional reflective film is 0.766 mm, while the thickness of the backlight module with the present invention is reduced to 0.686 mm, and the overall thickness is reduced by 10.4%, which better meets the market demand for lightweight and ultra-thin backlight modules.

[0118] Examples 5-7 are preferred embodiments of the present invention, having high visible light reflectivity and good infrared transmittance. Among them, Example 7 has excellent performances and is the most preferred technical solution of the present invention.

[0119] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A backlight module, characterized in that: The backlight module includes a light guide plate with the function of transmitting infrared rays and reflecting visible light, and the light guide plate includes a substrate and a functional layer from top to bottom, the substrate is made of polycarbonate, and the thickness of the substrate is 0.36 mm; the functional layer is an inorganic coating, and the inorganic coating is composed of a high-refractive-index inorganic substance A and a low-refractive-index inorganic substance B; the thickness of the inorganic coating A is 190 nm, and the material of the inorganic coating A is niobium pentoxide; the thickness of the inorganic coating B is 270 nm, and the material of the inorganic coating B is silicon oxide; the inorganic coating A and the inorganic coating B are alternately deposited on the surface of the light guide plate, and the deposition order is ABABA...BAB, and the number of deposited layers is 48.

2. The backlight module according to claim 1, characterized in that: The backlight module comprises a light source, a light guide plate having the function of transmitting infrared rays and reflecting visible light, a diffusion film and a brightness enhancement film.

Citation Information

Patent Citations

  • Biometric detection module, backlight module, display and electronic device

    CN110073366A

  • Infrared ray filter lens

    CN203606527U

  • Reflecting film, backlight module, liquid crystal screen and under-screen fingerprint recognition device

    CN210894926U

  • Infra-red transmitting mirror

    GB722006A