Package and method of manufacturing the same
By providing a side metallization layer on the ceramic portion of the package and forming a surface oxide film, the problem of solder outflow is solved, material cost is reduced and electrical connection stability is ensured.
Patent Information
- Application Number
- CN202111360843.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-26
- Filing Date
- 2021-11-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-11-17
AI Technical Summary
When the prior art uses solder to cover the metallized conductor layer, the metallized layer for sealing and the exposed surface of the metallized conductor column, the solder material is easily discharged from the upper surface to the side in large quantities, increasing material costs.
The encapsulation body composed of a ceramic part and a metallization part is provided with a side metallization layer on the side of the ceramic part, and a surface oxide film is formed in the middle part of the side metallization layer, and the plating layer is not covered to prevent the solder from flowing out. Ensure electrical connection between the upper and lower surfaces.
It effectively prevents the solder from unnecessarily flowing out of the upper surface to the side, reduces the material cost, and ensures the electrical connection between the upper surface and the lower surface.
Smart Images

Figure CN114696777B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a package and a method for manufacturing the same, and in particular to a package for electronic components and a method for manufacturing the same. Background Art
[0002] Japanese Patent Publication No. 2000-312060 (Patent Document 1) discloses an electronic component mounting substrate for mounting electronic components such as crystal oscillators. The electronic component mounting substrate has a lower insulating layer and an upper insulating layer. The lower insulating layer has a mounting portion for mounting electronic components on the upper surface, and a plurality of metallized conductor layers for connecting the electrodes of the electronic components to the outside are formed from the mounting portion to the lower surface. The upper insulating layer is frame-shaped and is stacked on the lower insulating layer in a manner surrounding the mounting portion, and a sealing metallized layer for joining a cover body is formed on its upper surface. A notch portion that passes through the upper insulating layer from top to bottom is formed on the outer peripheral surface of the upper insulating layer. The metallized conductor post that electrically connects the metallized conductor layer to the sealing metallized layer is buried in the notch portion in a manner such that its upper end surface becomes flush with the upper surface of the upper insulating layer.
[0003] According to the above configuration, the sealing metallization layer is electrically connected to the metallization conductor layer via the metallization conductor post. Therefore, by connecting the metallization conductor layer to the ground potential, the sealing metallization layer can also be connected to the ground potential.
[0004] In addition, the above-mentioned bulletin discloses the following technology, namely: a metal having excellent wettability with the solder, such as gold (Au), is coated on the exposed surface of the metallized conductor layer, the sealing metallized layer, and the metallized conductor column by a plating method. By this plating, oxidative corrosion can be prevented. Furthermore, by this plating, the bonding between the sealing metallized layer and the metal cover via the solder can be made firm. The solder is composed of, for example, a gold-tin (Au-Sn) alloy.
[0005] Prior Art Literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2000-312060 Summary of the invention
[0008] (Problems to be solved by the invention)
[0009] According to the technology described in the above-mentioned bulletin, a metal layer with excellent wettability to the solder is provided in a manner that covers the exposed surface of the metallized conductor layer, the metallized layer for sealing, and the metallized conductor post. Thus, as described above, the bonding of the metallized layer for sealing and the metal cover via the solder can be made firm. On the other hand, since the solder is covered by the metallized layer with excellent wettability to the solder, the solder tends to flow out in large quantities from the metallized layer for sealing located on the upper surface to the metallized conductor post located on the side in a useless manner. In particular, in most cases, the content of expensive materials such as gold in the solder is high. In this case, the useless outflow of the solder in large quantities will lead to a significant increase in material costs.
[0010] The present invention has been made to solve the above-mentioned problems, and an object thereof is to provide a package and a method for manufacturing the same, which can ensure electrical connection between the upper surface and the lower surface and prevent the solder from flowing out unnecessarily in large quantities from the upper surface to the side surface.
[0011] (Methods for solving problems)
[0012] A package in one embodiment is a package for electronic components, and a cover is mounted using solder. The package has a ceramic portion, a metallized portion, and a metal layer. The ceramic portion has an outer edge when viewed from above. The ceramic portion has: an upper surface, a lower surface opposite to the upper surface, and a side surface that is arranged at the outer edge and connects the upper surface and the lower surface to each other when viewed from above. The upper surface includes a sealing surface for supporting the cover, and a cavity for accommodating electronic components is provided on the inner side of the sealing surface. The metallized portion is provided on the ceramic portion and is composed of a metallized material. The metallized portion includes: a sealing metallized layer provided on the sealing surface; a lower surface metallized layer provided on the lower surface of the ceramic portion; and a side metallized layer provided on the side of the ceramic portion. The side metallized layer includes: an upper portion connected to the sealing metallized layer, a lower portion connected to the lower surface metallized layer, and an intermediate portion that connects the upper portion and the lower portion to each other. The metal layer is composed of a metal material having a higher wettability to solder than the metallized material. The metal layer covers the sealing metallization layer of the metallization part, and the middle part of the side metallization layer of the metallization part is not covered.
[0013] In addition, the metal material constituting the above-mentioned metal layer can be any one of a pure metal and an alloy. The metal layer can cover the upper part of the side metallization layer. The metal layer can have an end portion with a gradually decreasing thickness. In a top view, the outer edge of the ceramic portion has a first corner, a second corner, and an edge connecting the first corner and the second corner to each other, and the side metallization layer can leave the first corner and the second corner and connect to one edge. A surface oxide film composed of an oxide of a metallization material can be provided in the middle portion of the side metallization layer. The surface of the middle portion of the side metallization layer is a fracture surface. The outer edge can have a recessed portion configured with a side metallization layer. The recessed portion can be filled with the side metallization layer within the height range of the middle portion configured with the side metallization layer. The recessed portion can be filled with the side metallization layer and a filling portion composed of ceramic facing the ceramic portion through the side metallization layer within the height range of the middle portion configured with the side metallization layer.
[0014] The manufacturing method of the package body of one of the above-mentioned embodiments comprises: (a) a process of forming a green body laminated body having a ceramic green body portion and a metallized green body portion, wherein the ceramic green body portion includes a portion to be a ceramic portion, the metallized green body portion includes a portion to be a metallized portion, and the ceramic green body portion and the metallized green body portion respectively span an imaginary line that is at least a portion of the outer edge of the ceramic portion, and the manufacturing method of the package body also comprises: (b) a process of forming a groove in the green body laminated body along the imaginary line; (c) a process of forming a fired body including a ceramic portion and a metallized portion by firing the green body laminated body; (d) a process of plating the metallized portion of the fired body in order to form a metal layer; and (e) a process of generating a crack in the fired body with the groove as a starting point after the process of plating the metallized portion, thereby breaking the ceramic portion while forming a surface of the middle portion of the side metallized layer of the metallized portion.
[0015] (Effects of the Invention)
[0016] According to the package body of one of the above-mentioned methods, first, the metallization part includes: a sealing metallization layer arranged on the sealing surface; a lower surface metallization layer arranged on the lower surface of the ceramic part; and a side metallization layer arranged on the side of the ceramic part. Thus, the electrical connection between the upper surface provided with the sealing metallization layer and the lower surface provided with the lower surface metallization layer can be ensured. Second, the sealing metallization layer of the metallization part is covered by a metal layer composed of a metal material having a high wettability to the solder in a molten state, but the middle part of the side metallization layer of the metallization part is not covered. Thus, the situation that the solder flows out from the upper surface to the side in a large amount unnecessarily can be prevented. According to the above, the electrical connection between the upper surface and the lower surface can be ensured, and the situation that the solder flows out from the upper surface to the side in a large amount unnecessarily can be prevented.
[0017] The objects, features, aspects and advantages of the present invention will become more apparent from the following detailed description and accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a plan view schematically showing the structure of the electronic device in the first embodiment.
[0019] Figure 2 It is along Figure 1 A schematic partial cross-sectional view taken along line II-II.
[0020] Figure 3 This is a plan view schematically showing the structure of the package in the first embodiment.
[0021] Figure 4 It is along Figure 3 A schematic partial cross-sectional view taken along line IV-IV.
[0022] Figure 5 It is along Figure 3 A schematic partial cross-sectional view taken along line V-V of FIG.
[0023] Figure 6 This is a partial plan view schematically showing a first step of the method for manufacturing a package in the first embodiment.
[0024] Figure 7 It is along Figure 6 A schematic partial cross-sectional view taken along line VII-VII.
[0025] Figure 8 This is a partial plan view schematically showing a second step of the method for manufacturing a package in the first embodiment.
[0026] Fig. 9 It is along Figure 8 A schematic partial cross-sectional view taken along line IX-IX.
[0027] Fig.10 This is a partial plan view schematically showing a third step of the method for manufacturing the package in the first embodiment.
[0028] Fig.11 It is along Fig.10 A schematic partial cross-sectional view taken along line XI-XI.
[0029] Fig.12 This is a partial plan view schematically showing a fourth step of the method for manufacturing the package in the first embodiment.
[0030] Fig.13 It is along Fig.12 A schematic partial cross-sectional view taken along line XIII-XIII.
[0031] Fig.14 This is a partial plan view schematically showing a fifth step of the method for manufacturing the package in the first embodiment.
[0032] Fig.15 It is along Fig.14 A schematic partial cross-sectional view taken along line XV-XV of .
[0033] Fig.16 This is a partial plan view schematically showing a sixth step of the method for manufacturing a package in the first embodiment.
[0034] Fig.17 It is along Fig.16 A schematic partial cross-sectional view taken along line XVII-XVII.
[0035] Fig.18 This is a partial cross-sectional view schematically showing a seventh step of the method for manufacturing a package in the first embodiment.
[0036] Fig.19 It is a partial cross-sectional view schematically showing the structure of an electronic device in a comparative example.
[0037] Fig. 20 This is a plan view schematically showing the structure of a package in the second embodiment.
[0038] Fig.21 It is along Fig. 20 A schematic partial cross-sectional view taken along line XXI-XXI.
[0039] Fig. 22 This is a partial plan view schematically showing a third step of the method for manufacturing a package in the second embodiment.
[0040] Fig.23 It is along Fig. 22 A schematic partial cross-sectional view along line XXIII-XXIII.
[0041] Fig.24 This is a partial plan view schematically showing a fourth step of the method for manufacturing a package in the second embodiment.
[0042] Fig.25 It is along Fig.24 A schematic partial cross-sectional view along line XXV-XXV.
[0043] Fig.26 This is a partial plan view schematically showing a fifth step of the method for manufacturing a package in the second embodiment.
[0044] Fig. 27 It is along Fig.26A schematic partial cross-sectional view along line XXVII-XXVII.
[0045] Fig.28 This is a partial plan view schematically showing a sixth step of the method for manufacturing a package in the second embodiment.
[0046] Fig.29 It is along Fig.28 A schematic partial cross-sectional view along line XXIX-XXIX.
[0047] Fig.30 This is a partial plan view schematically showing a seventh step of the method for manufacturing a package in the second embodiment.
[0048] Fig.31 It is along Fig.30 A schematic partial cross-sectional view taken along line XXXI-XXXI.
[0049] Fig.32 This is a partial plan view schematically showing an eighth step of the method for manufacturing a package in the second embodiment.
[0050] Fig.33 It is along Fig.32 A schematic partial cross-sectional view along line XXXIII-XXXIII.
[0051] Fig.34 This is a partial cross-sectional view schematically showing a ninth step of the method for manufacturing a package in the second embodiment.
[0052] Fig.35 The sixth step ( Fig.29 ) is a partial cross-sectional view of a modified example.
[0053] Fig.36 This is a partial cross-sectional view schematically showing the structure of a package in the third embodiment.
[0054] Fig.37 This is a plan view schematically showing the structure of a package in the fourth embodiment.
[0055] Fig.38 So with Figure 2 The corresponding view schematically shows a partial cross-sectional view of the structure of the electronic device in the fifth embodiment. DETAILED DESCRIPTION
[0056] Hereinafter, embodiments will be described based on the drawings.
[0057] <Implementation method 1>
[0058] Figure 1It is a plan view schematically showing the structure of electronic device 900 in the first embodiment. Figure 2 It is along Figure 1 The electronic device 900 includes a package 801 , an electronic component 910 , a solder 930 , and a lid 920 .
[0059] Figure 3 It is a plan view schematically showing the structure of the package 801. Figure 4 as well as Figure 5 Along the Figure 3 The package 801 is a package for the electronic component 910, and in this embodiment, has an electrode pad 400 bonded to the electronic component 910. Figure 1 as well as Figure 2 As shown, the cover 920 is mounted on the package 801 using a solder 930. The cover 920 is preferably made of a metal having a thermal expansion coefficient similar to that of ceramics, and specifically, preferably made of an alloy containing Fe (iron) and Ni (nickel) as main components, for example, a Fe-Ni-Co (cobalt) alloy or a Fe-Ni alloy. The solder 930 preferably has Au as the main component, more preferably an Au alloy, typically an Au-Sn alloy. In addition, the material of the solder 930 is not limited to these, for example, it may also be an Ag (silver)-Cu (copper) alloy, a Pb (lead)-Sn solder, or a Pb-free solder. The shape of the cover may be a flat plate.
[0060] The package 801 includes a ceramic part 100, a metallization part 200 disposed on the ceramic part 100, and a plating layer 300 (metal layer). The metallization part 200 includes a sealing metallization layer 210, a lower surface metallization layer 220, and a side metallization layer 230. The plating layer 300 includes an upper plating layer 310 and a lower plating layer 320. The upper plating layer 310 and the lower plating layer 320 are separated from each other.
[0061] The ceramic part 100 is made of ceramic, for example, aluminum oxide or aluminum nitride. In the case of ceramic made of aluminum oxide, 10 to 20 wt% of zirconium oxide may be added to improve the mechanical strength. Figure 3 As shown, the ceramic part 100 has an outer edge EO in a top view. Figure 4 As shown, the ceramic part 100 has an upper surface P1, a lower surface P2 opposite to the upper surface P1, and a side surface P3 connecting the upper surface P1 and the lower surface P2. The side surface P3 is arranged at the outer edge EO ( Figure 3The outer edge EO has a recessed portion CC. In the present embodiment, the recessed portion CC has a substantially semicircular shape. The upper surface P1 includes a cover 920 ( Figure 2 ) of the sealing surface SS. In addition, on the upper surface P1, inside the sealing surface SS, a cavity CV for accommodating the electronic component 910 is provided. The ceramic part 100 is viewed from above ( Figure 3 ) and has a frame portion surrounding the chamber CV. In addition, the ceramic portion 100 is provided with internal wiring (not shown) connecting the inside and the outside of the chamber CV. The internal wiring, for example, connects the electrode pad 400 provided in the chamber CV with the electrode pad (not shown) provided on the lower surface P2.
[0062] The metallization part 200 is composed of a metallization material. The main component of the metallization material is preferably a high melting point metal, such as W (tungsten), Mo (molybdenum) or a mixture thereof. Alternatively, the main component of the metallization material may also be an alloy composed of W and Mo. The sealing metallization layer 210 is disposed on the sealing surface SS. The lower surface metallization layer 220 is disposed on the lower surface P2 of the ceramic part 100. The side metallization layer 230 is disposed on the side P3 of the ceramic part 100. Specifically, the side metallization layer 230 is disposed in the recess CC of the outer edge EO. In the present embodiment, the recess CC is surrounded by the side metallization layer 230 ( Figure 4 ) is filled. Here, the direction mentioned in the above “height range” is the thickness direction of the package 801 ( Figure 4 The side metallization layer 230 has an upper portion 231 connected to the sealing metallization layer 210, a lower portion 232 connected to the lower surface metallization layer 220, and a middle portion 233 connecting the upper portion 231 and the lower portion 232. The surface of the middle portion 233 of the side metallization layer 230 is not an as-fired surface, but a fracture surface SF ( Fig.18 ).
[0063] Looking down ( Figure 3), the outer edge EO of the ceramic part 100 has a rectangular shape with 4 sides and 4 corners. In addition, a square is a kind of rectangle. Specifically, the outer edge EO has: a first corner N1 (in the figure, the upper right corner), a second corner N2 (in the figure, the lower right corner), and an edge connecting the first corner N1 and the second corner N2 to each other (in the figure, the right side). The side metallization layer 230 leaves the first corner N1 and the second corner N2 and connects to an edge. Correspondingly, the recess CC leaves the first corner N1 and the second corner N2 and connects to an edge. In addition, in the present embodiment, another side metallization layer 230 (and the recess CC configured with the side metallization layer) is connected to the side opposite to the one side, that is, the left side in the figure. In addition, the number of side metallization layers (and the number of recesses CC) possessed by a package is arbitrary.
[0064] The upper plating layer 310 of the plating layer 300 covers the sealing metallization layer 210 of the metallization part 200. On the other hand, the plating layer 300 does not cover the middle portion 233 of the side metallization layer 230 of the metallization part 200. In this embodiment, the upper plating layer 310 covers the upper portion 231 of the side metallization layer 230. The interface between the upper portion 231 and the upper plating layer 310 may include a thickness direction ( Figure 4 The interface may also be formed only by the inclined surface. In addition, the lower plating layer 320 of the plating layer 300 covers the lower surface metallization layer 220 of the metallization part 200. In addition, the lower plating layer 320 of the plating layer 300 covers the lower part 232 of the side metallization layer 230 of the metallization part 200.
[0065] The upper plating layer 310 of the plating layer 300 has an end portion where the thickness gradually decreases ( Figure 4 Similarly, the lower plating layer 320 of the plating layer 300 has an end portion where the thickness gradually decreases ( Figure 4 right end in the middle).
[0066] The plating layer 300 is composed of a metal material having higher wettability to the molten solder 930 than the metallization material. In other words, the wettability of the metal material of the plating layer 300 is higher than that of the metallization material. The metal material of the plating layer 300 preferably has Au as a main component, for example, substantially Au.
[0067] In addition, in order to make the plating layer 300 difficult to peel off, it is preferred that a base layer (not shown) composed of a conductive material different from the above-mentioned metal material is formed between the plating layer 300 and the metallization part 200. The base layer can also be a plating layer. The material of the base layer can be mainly Ni, for example, Ni or Ni-Co alloy.
[0068] Figure 5It is a partial cross-sectional view of a portion where the concave portion CC is not provided.
[0069] Next, refer to Figure 6 to Figure 18 A method for manufacturing a plurality of packages 801 at once is described. Figure 6 , Figure 8 , Fig.10 , Fig.12 , Fig.14 as well as Fig.16 The following are partial top views schematically showing the first to sixth steps. Figure 7 , Fig. 9 , Fig.11 , Fig.13 , Fig.15 as well as Fig.17 Along line VII-VII( Figure 6 ), line IX-IX( Figure 8 ), line XI-XI( Fig.10 )、Line XIII-XIII( Fig.12 )、Line XV-XV( Fig.14 ) and line XVII-XVII( Fig.16 ) is a schematic partial cross-sectional view of the Fig.18 It is a partial cross-sectional view schematically showing the seventh step.
[0070] Reference Figure 6 as well as Figure 7 The ceramic green body part 100G is formed by stacking a plurality of green sheets. The ceramic green body part 100G includes a ceramic part 100 ( Figure 4 Although not shown in the figure, a portion that becomes an internal wiring (not shown) of the ceramic part 100 may be provided in the ceramic green part 100G.
[0071] Reference Figure 8 as well as Fig. 9 In the ceramic green body 100G, a through hole HL extending in the thickness direction is formed. The through hole HL spans over an imaginary line LV that is at least a portion of the outer edge EO of the ceramic body 100. The through hole HL includes a concave portion CC ( Figure 3 ) part. The through hole HL is formed by machining using a mold. In addition, as a modified example, the through hole HL can also be formed by machining using a laser.
[0072] Reference Fig.10 as well as Fig.11By printing the metal paste, a metallized green part 200G including a sealing metallized green layer 210G, a lower surface metallized green layer 220G, and a side metallized green layer 230G is formed on the ceramic green part 100G. The metallized green part 200G includes a portion that becomes the metallized part 200 through the firing process described later. Specifically, the sealing metallized green layer 210G, the lower surface metallized green layer 220G, and the side metallized green layer 230G respectively include portions that become the sealing metallized layer 210, the lower surface metallized layer 220, and the side metallized layer 230 through the firing process described later. As a result, a green laminate 500G including a ceramic green part 100G and a metallized green part 200G including a portion that becomes the ceramic part 100 is formed.
[0073] The side metallized green layer 230G of the ceramic green part 100G and the metallized green part 200G respectively crosses the imaginary line LV ( Fig.10 Specifically, the ceramic green part 100G crosses the imaginary line LV outside the through hole HL. In addition, the side metallized green layer 230G of the metallized green part 200G crosses the imaginary line LV inside the through hole HL.
[0074] Reference Fig.12 as well as Fig.13 , along the imaginary line LV( Fig.10 ) A groove TR is formed in the green laminate 500G. The step of forming the groove TR is performed by pressing the tip of the knife against the green laminate 500G along the imaginary line LV. In addition, as a modified example, the step of forming the groove TR may also be performed by irradiating the green laminate 500G with a laser along the imaginary line LV.
[0075] Next, the green laminate 500G ( Fig.12 as well as Fig.13 ) for firing. Fig.14 as well as Fig.15 By this firing, a fired body 500 including the ceramic portion 100 and the metallized portion 200 is formed. Fig.16 as well as Fig.17 The metallized portion 200 of the sintered body 500 is plated. Thus, the plated layer 300 is formed.
[0076] Reference Fig.18 After the above plating process, cracks are generated in the sintered body 500 starting from the trench TR. Thus, the ceramic part 100 is fractured, and the surface (fracture surface SF) of the middle part 233 of the side metallization layer 230 of the metallization part 200 is formed. Through the above process, a plurality of packages 801 are obtained.
[0077] Fig.19 FIG. 1 is a partial cross-sectional view schematically showing the structure of an electronic device 990 in a comparative example. Figure 2 ), the entire side of the side metallization layer 230 is provided with a plating layer 390. As a result, when the cover 920 is installed using the solder 930, the solder 930 tends to flow out from the upper surface to the side in a large amount, as shown by the arrow in the figure. In addition, if a member for preventing the flow of the solder 930 as shown by the arrow in the figure is added, the structure and the manufacturing method will be complicated.
[0078] Although not shown in the figure, as another comparative example, it is conceivable that Figure 3 In a top view, a through hole is formed in the frame of the ceramic part 100, which is away from the outer edge EO and the cavity CV, and a conductor member for electrically connecting the upper surface P1 and the lower surface P2 is formed in the through hole. In this case, the size of the through hole needs to be sufficiently smaller than the width of the frame. Therefore, when the width of the frame is small, the difficulty of forming the through hole is high. For example, in the case of mechanical processing using a mold with tiny pins, the tiny pins corresponding to the tiny through holes are easily broken. When a laser is used instead of a mold, the productivity will be greatly reduced. Furthermore, even if it is assumed that a tiny through hole can be formed, the difficulty of filling the conductor member therein is also high.
[0079] According to the package 801 of this embodiment, first, the metallization part 200 ( Figure 4 ) includes: a sealing metallization layer 210 disposed on the sealing surface SS; a lower surface metallization layer 220 disposed on the lower surface P2 of the ceramic part 100; and a side surface metallization layer 230 disposed on the side surface P3 of the ceramic part 100. Thus, the electrical connection between the upper surface P1 configured with the sealing metallization layer 210 and the lower surface P2 configured with the lower surface metallization layer 220 can be ensured. Second, by applying the solder 930 ( Figure 2 ) covers the sealing metallization layer 210 of the metallization part 200, but does not cover the middle part 233 of the side metallization layer 230 of the metallization part 200. Fig.19 ) is different, and the solder 930 can be prevented from flowing out of a large amount from the upper surface to the side surface unnecessarily. According to the above, the electrical connection between the upper surface P1 and the lower surface P2 can be ensured, and the solder 930 can be prevented from flowing out of a large amount from the upper surface to the side surface unnecessarily.
[0080] The upper plating layer 310 ( Figure 4) covers the upper portion 231 of the side metallization layer 230. Thus, the solder 930 ( Figure 2 ) is easily outflowed from the edge of the sealing metallization layer 210 is limited to the range of the upper portion 231 of the side metallization layer 230. Therefore, by sufficiently reducing the size of the upper portion 231 of the side metallization layer 230, the amount of solder 930 outflow can be suppressed. Furthermore, by slightly extending the solder 930 from the edge of the sealing metallization layer 210, the solder 930 is more firmly bonded to the plating layer 300. In addition, the surface of the middle portion 233 of the side metallization layer 230 is subjected to the cracking process ( Fig.18 ) and defines the position of the cleavage process. Fig.12 ) is formed before the firing step, the plating layer 300 is formed by a plating step ( Fig.17 ) is carried out efficiently. In this case, the portion of the plating layer 300 formed in the trench TR corresponds to the portion covering the upper portion 231 of the side metallization layer 230. Therefore, by allowing the plating layer 300 to cover the upper portion 231 of the side metallization layer 230, the plating layer 300 in this embodiment can be efficiently formed.
[0081] The upper plating layer 310 has an end portion with a gradually decreasing thickness ( Figure 4 The right end portion in the middle of the side metallization layer 230 is formed by the cleavage process ( Fig.18 ) and defines the position of the cleavage process. Fig.12 ) is formed before the firing step, the plating layer 300 is formed by a plating step ( Fig.17 ) is efficient. In this case, the portion of the end of the plating layer 300 of the package 801 after completion is located at the bottom of the groove TR at the time point of the plating process. Since it is difficult to plate at the bottom of the groove TR, the plating layer 300 has an end with a gradually decreasing thickness. Therefore, by allowing the plating layer 300 to have an end with a gradually decreasing thickness, the plating layer 300 in this embodiment can be efficiently formed.
[0082] Regarding the outer edge EO ( Figure 3), the side metallization layer 230 is separated from the first corner N1 and the second corner N2 and connected to one side. The side metallization layer 230 is easily peeled off at the corner of the outer edge EO, but this structure can suppress such peeling. In particular, compared with the case where the side metallization layer 230 is located at the corner of the outer edge EO, the cracking process ( Fig.18 ) and thus cause damage to the side metallization layer 230. However, when this effect is not particularly required, that is, when the adhesion strength between the side metallization layer 230 and the ceramic part 100 is sufficiently high, the configuration of the side metallization layer 230 is not limited thereto, and the side metallization layer 230 may also be configured at a corner.
[0083] The surface of the middle portion 233 of the side metallization layer 230 is a fracture surface SF ( Fig.18 ). Thus, the surface can be formed by a cleavage process.
[0084] The side metallization layer 230 is disposed on the outer edge EO ( Figure 3 Thus, the side metallization layer 230 can be prevented from protruding from the outer edge EO of the ceramic part 100.
[0085] Concave CC ( Figure 3 ) in the middle portion 233 ( Figure 4 ) is filled with the side metallization layer 230. Thus, as a component for filling the recess CC, there is no need to form a component other than the side metallization layer 230. In addition, by filling the recess CC, it is possible to avoid a situation where the area to which the cover body 920 is joined becomes smaller due to the recess CC, thereby causing poor sealing. Furthermore, since the rigidity is improved, it is also possible to prevent the destruction of the frame portion surrounding the cavity CV starting from the recess CC. This is effective when the width dimension of the frame portion surrounding the cavity CV of the ceramic portion 100 is only 100μm or less even in a portion away from the recess CC. It should be noted that, particularly in an ultra-small package having an outer edge EO so small as to be contained in an area of 1mm square, it is often required in design that the width dimension of the frame portion be set to 100μm or less. Typically, in the electronic component 910( Figure 1 ) is an ultra-small crystal blank (with electrodes), such an ultra-small package is sought.
[0086] According to the method for manufacturing the package 801 of the present embodiment, the package 801 can be manufactured by a simple method. Specifically, the fracture surface SF ( Fig.18 ) is used as a surface for suppressing further flow of the solder 930. Therefore, it is not necessary to form a special member for suppressing the flow of the solder 930. In addition, the through hole HL ( Figure 8 as well as Fig. 9 ) is divided into a concave portion CC for a castellated electrode ( Figure 3 ). Therefore, the diameter of the through hole HL can be set larger than the case where a through hole away from both the outer edge EO and the cavity CV is formed in the frame of the ceramic part 100 for a through-hole electrode, which is different from the present embodiment. Therefore, the diameter of the pin of the mold for forming the through hole HL can also be set larger. Therefore, the through hole HL can be easily formed by mechanical processing using a mold. Thus, productivity can be improved compared to the case of using laser processing.
[0087] According to the manufacturing method of the electronic device 900 of the present embodiment, first, the package 801 is manufactured as described above. Then, the electronic component 910 is joined to the electrode pad 400 of the package 801. Then, the cover 920 is installed to the package 801 by soldering using the solder 930. Thus, the electronic device 900 is obtained. Soldering can be performed by a known method. In this case, as the solder 930, an Au alloy, in particular an Au-Sn alloy, is typically used. However, the soldering method is not limited to this, and for example, it can be performed as follows. First, a layer of solder composed of an Ag-Cu alloy is formed on one surface of the cover 920. Then, the cover 920 provided with a layer of solder is placed on the sealing metallization layer 210 in such a manner that the layer of solder is in contact with the sealing metallization layer 210. Then, the solder is melted by heating by energization. Thus, the electronic device 900 is obtained.
[0088] In addition, the electronic device 900 ( Figure 2 ) is mounted on an external substrate (not shown) using electrode pads (not shown) provided on the lower surface P2 as described above. In this installation, the electrode pads are joined to the external substrate using solder. In this solder joining, if the solder flows out from the lower surface to the side unnecessarily, the joining between the electrode pads and the external substrate is likely to become poor. According to this embodiment, the plating layer 300 composed of a metal material having high wettability to the solder in a molten state covers the lower surface metallization layer 220 of the metallization part 200, but the middle part 233 of the side metallization layer 230 of the metallization part 200 is not covered. Thereby, it is possible to prevent the solder in a molten state from flowing out from the lower surface to the side unnecessarily.
[0089] <Implementation method 2>
[0090] Fig. 20 It is a plan view schematically showing the structure of the package 802 in the second embodiment. Fig.21 It is along Fig. 20A schematic partial cross-sectional view along line XXI-XXI of . In the present embodiment, the recess CC is filled with the side metallization layer 230 and the filling portion 150 within the height range of the middle portion 233 where the side metallization layer 230 is disposed. The filling portion 150 faces the ceramic portion 100 through the side metallization layer 230 and is made of ceramic. The main component of the material of the filling portion 150 is preferably the same as the main component of the material of the ceramic portion 100. For example, the filling portion 150 and the ceramic portion 100 may both be made of aluminum oxide, or the filling portion 150 and the ceramic portion 100 may both be made of aluminum nitride. The surface of the filling portion 150 is not a fired surface but a fracture surface SG. In addition, Fig.21 The cross section shown is taken along line XXI-XXI ( Fig. 20 ) section, along line AA( Fig. 20 ) and Figure 4 (Implementation method 1) is roughly the same.
[0091] Next, a method for manufacturing a plurality of packages 802 at once is described below. Figure 6 to Figure 9 ) is also commonly performed in this embodiment, so its description is omitted. Fig. 22 , Fig.24 , Fig.26 , Fig.28 , Fig.30 as well as Fig.32 The following are partial top views schematically showing the third step to the eighth step, respectively. Fig.23 , Fig.25 , Fig. 27 , Fig.29 , Fig.31 as well as Fig.33 Along the line XXIII-XXIII ( Fig. 22 ), line XXV-XXV( Fig.24 ), line XXVII-XXVII( Fig.26 ), line XXIX-XXIX( Fig.28 )、Line XXXI-XXXI( Fig.30 ) and line XXXIII-XXXIII( Fig.32 ) is a schematic partial cross-sectional view of the Fig.34 It is a partial cross-sectional view schematically showing the ninth step.
[0092] Reference Fig. 22 as well as Fig.23 By printing the metal paste, the side metallization green layer 230G is formed on the inner surface of the through hole HL of the ceramic green part 100G in such a manner that the through hole HL is only partially filled. Fig.24 as well as Fig.25Then, by printing the ceramic paste, the filling green part 150G is filled into the through hole HL via the side metallization green layer 230G so as to fill the through hole HL. Fig.26 as well as Fig. 27 By printing the metal paste, a sealing metallized green layer 210G and a lower surface metallized green layer 220G are formed on the ceramic green part 100G. Figure 22 to Figure 27 In the step of forming the metallized green part 200G including the portion to be the metallized part 200 on the ceramic green part 100G, the green laminated body 500G is formed, which includes the ceramic green part 100G including the portion to be the ceramic part 100, the metallized green part 200G including the portion to be the metallized part 200, and the filling green part 150G including the portion to be the filling part 150.
[0093] The side metallized green layer 230G and the filling green part 150G of the ceramic green part 100G and the metallized green part 200G respectively cross the imaginary line LV ( Fig.26 Specifically, the ceramic green part 100G crosses the imaginary line LV outside the through hole HL. In addition, the side metallization green layer 230G and the filling green part 150G cross the imaginary line LV inside the through hole HL.
[0094] Reference Fig.28 as well as Fig.29 , along the imaginary line LV( Fig.26 ) The groove TR is formed in the green laminate 500G. The step of forming the groove TR is performed by pressing the tip of the knife against the green laminate 500G along the imaginary line LV. When the groove TR is formed using the tip of the knife, as shown in FIG. Fig.29 As shown in FIG. 1 , the sealing metallization green layer 210G easily extends to the side of the trench TR. This is because the sealing metallization green layer 210G is caught by the blade tip when the trench TR is formed. As a result, in the plating step ( Fig.32 as well as Fig.33 ), the plating layer 300 is also easily formed on the surface of the filling portion 150 made of ceramic.
[0095] Next, the green laminate 500G ( Fig.28 as well as Fig.29 ) for firing. Fig.30 as well as Fig.31 By this firing, a fired body 500 including the ceramic portion 100 and the metallized portion 200 is formed.
[0096] Reference Fig.32 as well as Fig.33The metallized portion 200 of the sintered body 500 is plated. Thus, the plated layer 300 is formed.
[0097] Reference Fig.34 After the above plating, cracks are generated in the sintered body 500 starting from the trench TR. As a result, the ceramic part 100 and the filling part 150 are snapped, and the surface of the middle part 233 of the side metallization layer 230 of the metallization part 200 is formed ( Fig. 20 Through the above, a plurality of packages 802 are obtained.
[0098] Note that, other than the above, since the present invention is substantially the same as the above-mentioned first embodiment, the same or corresponding elements are denoted by the same reference numerals, and description thereof will not be repeated.
[0099] According to the package 802 of this embodiment, the concave portion CC ( Fig. 20 ) in the middle portion 233 ( Fig.21 ) is filled with the side metallization layer 230 and the filling portion 150 made of ceramic facing the ceramic portion 100 through the side metallization layer 230. Thus, the side metallization layer 230 can be protected by the filling portion 150. In addition, the filling portion 150 (made of ceramic) is formed in the through hole HL including the portion to be the concave portion CC. Fig.33 ), so the proportion of ceramic materials constituting the frame portion increases, the homogeneity improves, and thus the fracture process can be generated more stably ( Fig.34 ) in the recess CC.
[0100] According to the method for manufacturing the package 802 of the present embodiment, the trench TR ( Fig.29 ). As described above, the sealing metallization green layer 210G easily extends to the side of the trench TR. As a result of the sealing metallization green layer 210G extending to the side of the trench TR, the sealing metallization layer 210 of the package 802 also extends to the side of the trench TR. Figure 4 In the same manner as in the case of (Embodiment 1), an upper plating layer 310 ( Fig.21 ).
[0101] <Variation of Embodiment 2>
[0102] Fig.35 It is schematically shown Fig.29 A partial cross-sectional view of a modified example of the process. Fig.29 In the process of forming the groove TR using a tool tip, in this modification, the groove TR is formed by laser processing (i.e., irradiation with laser). Fig.29 Unlike the case of the sealing metallization green layer 210G, it is difficult for the sealing metallization green layer 210G to extend onto the side surface of the trench TR. According to this modification, by using a laser instead of a blade tip, a fine trench TR can be formed.
[0103] <Implementation method 3>
[0104] Fig.36 2 is a partial cross-sectional view schematically showing the structure of the package 801M in the third embodiment. In the present embodiment, a surface oxide film 233X composed of an oxide of a metallization material is provided in the middle portion 233 of the side metallization layer 230. The surface oxide film 233X may be a natural oxide film of the middle portion 233. In addition, regarding other structures, since the above-mentioned embodiment 1 ( Figure 4 ) have substantially the same structure, and therefore the same or corresponding elements are denoted by the same reference numerals and their descriptions are not repeated.
[0105] According to this embodiment, it is also possible to obtain substantially the same effects as those of Embodiment 1. Furthermore, according to this embodiment, the surface oxide film 233X can further reduce the wettability of the middle portion 233 of the brazing material 930. In particular, when the surface oxide film 233X is a natural oxide film of the middle portion 233, the surface oxide film 233X can be easily formed.
[0106] <Implementation method 4>
[0107] Fig.37 1 is a top view schematically showing the structure of the package 802M in the fourth embodiment. In the present embodiment, a surface oxide film 233X composed of an oxide of a metallization material is provided in the middle portion 233 of the side metallization layer 230. The surface oxide film 233X may be a natural oxide film of the middle portion 233. In addition, since the other structures are substantially the same as those in the second embodiment described above, the same or corresponding elements are denoted by the same reference numerals, and their descriptions are not repeated.
[0108] According to this embodiment, it is possible to obtain substantially the same effects as those of Embodiment 2. Furthermore, according to this embodiment, it is possible to obtain the same effects as those peculiar to Embodiment 3 described above.
[0109] <Implementation method 5>
[0110] Fig.38 So with Figure 2(Electronic device 900: Embodiment 1) The corresponding view schematically shows a partial cross-sectional view of the structure of an electronic device 900M in Embodiment 5. In addition to the components of the electronic device 900, the electronic device 900M further includes a metal frame 940. The shape of the metal frame 940 is substantially the same as the shape of the sealing metallization layer 210 in a plan view. Therefore, the metal frame 940 surrounds the cavity CV in a plan view.
[0111] The metal frame 940 is preferably made of a metal having a thermal expansion coefficient close to that of ceramics, and specifically, is preferably made of an alloy containing Fe (iron) and Ni (nickel) as main components, such as a Fe-Ni-Co (cobalt) alloy or a Fe-Ni alloy.
[0112] Next, the manufacturing method of the electronic device 900M is described. First, prepare the package 801 described in the aforementioned embodiment 1. Then, use the solder 930 to install the metal frame 940 on the sealing metallization layer 210 of the package 801. In other words, the metal frame 940 is brazed to the sealing metallization layer 210. The brazing method can be the same as the method of brazing the cover 920 to the sealing metallization layer 210 in the aforementioned embodiment 1 or its modified example. In particular, in this embodiment, the material of the solder 930 is preferably an Ag-Cu alloy. Next, install the cover 920 on the metal frame 940. The installation is preferably performed by welding.
[0113] In the present embodiment, the cover 920 is mounted on the package 801 using the solder 930 and the metal frame 940 brazed by the solder 930. In other words, the package 801 is a package in which the cover 920 is mounted using the solder 930 and the metal frame 940 brazed to the solder 930. Therefore, in the present embodiment, the sealing surface SS of the package 801 is used to support the cover 920 via the metal frame 940.
[0114] In addition, as a modification, the package 801 in the electronic device 900M may be replaced with any package in the above-described first to fourth embodiments and their modifications other than the package 801 .
[0115] The above-mentioned embodiments and variations can be combined freely with each other. The present invention has been described in detail, but the above description is illustrative in all aspects and the present invention is not limited thereto. It should be understood that countless variations that are not exemplified can be thought of without departing from the scope of the present invention.
[0116] Explanation of symbols
[0117] 100: Ceramics Department
[0118] 100G: Ceramic green body
[0119] 150: Filling
[0120] 150G: Filling green part
[0121] 200: Metallization Department
[0122] 200G: Metallized green part
[0123] 210: Sealing metallization layer
[0124] 210G: Sealed metallized green layer
[0125] 220: Bottom surface metallization layer
[0126] 220G: Lower surface metallization green layer
[0127] 230: Side metallization layer
[0128] 230G: Side metallization green layer
[0129] 231: Upper part
[0130] 232: Lower part
[0131] 233: Middle part
[0132] 233X: Surface oxide film
[0133] 300: Plating layer (metal layer)
[0134] 310: Upper plating layer
[0135] 320: Bottom plating layer
[0136] 500: Sintered
[0137] 500G: Green laminate
[0138] 801, 801M, 802, 802M: Encapsulation
[0139] 900, 900M: Electronic equipment
[0140] 910: Electronic components
[0141] 920: Cover
[0142] 940: Metal frame
[0143] 930: Brazing material
[0144] CC: Concave
[0145] CV: Chamber
[0146] EO: Outer Edge
[0147] HL: Through hole
[0148] LV: Imaginary Line
[0149] N1, N2: first angle and second angle
[0150] P1: Top surface
[0151] P2: Lower surface
[0152] P3: Side
[0153] SF: Fracture surface
[0154] SG: fracture surface
[0155] SS: Sealing surface
[0156] TR: Groove.
Claims
1. A package for an electronic component having a cover body mounted thereon using solder, in, The package includes a ceramic portion having an outer edge in a plan view, The ceramic part has: an upper surface, comprising a sealing surface for supporting the cover, wherein a cavity for accommodating the electronic component is provided inside the sealing surface; a lower surface opposite to the upper surface; and a side surface, which is arranged at the outer edge in the plan view and connects the upper surface and the lower surface to each other, The package further comprises a metallization portion, which is disposed on the ceramic portion and is made of a metallization material. The metallization portion comprises: A sealing metallization layer disposed on the sealing surface; a lower surface metallization layer disposed on the lower surface of the ceramic portion; and a side metallization layer, which is disposed on the side of the ceramic part and has an upper portion connected to the sealing metallization layer, a lower portion connected to the lower surface metallization layer, and a middle portion connecting the upper portion and the lower portion to each other, The package further includes a metal layer, the metal layer being made of a metal material having higher wettability to the solder than the metallization material, the metal layer covering the sealing metallization layer of the metallization portion, and the middle portion of the side metallization layer of the metallization portion being uncovered.
2. The package according to claim 1, in, The metal layer covers the upper portion of the side metallization layer.
3. The package according to claim 1 or 2, in, The metal layer has an end portion with a gradually decreasing thickness.
4. The package according to claim 1 or 2, in, In the plan view, the outer edge of the ceramic portion has a first corner, a second corner, and a side connecting the first corner and the second corner, and the side metallization layer is separated from the first corner and the second corner and connected to the side.
5. The package according to claim 1 or 2, in, A surface oxide film composed of an oxide of the metallization material is provided at the middle portion of the side metallization layer.
6. The package according to claim 1 or 2, in, The surface of the middle portion of the side metallization layer is a fracture surface.
7. The package according to claim 1 or 2, in, The outer edge has a recessed portion in which the side metallization layer is disposed.
8. The package according to claim 7, in, The recess is filled with the side metallization layer within a height range of the middle portion where the side metallization layer is disposed.
9. The package according to claim 7, in, The recessed portion is filled with the side metallization layer and a filling portion made of ceramic within a height range of the middle portion where the side metallization layer is arranged, and the filling portion faces the ceramic portion with the side metallization layer interposed therebetween.
10. The package according to claim 1 or 2, in, The package is a package in which the cover is mounted using the solder and a metal frame brazed with the solder. The sealing surface is used to support the cover body via the metal frame.
11. A method for manufacturing a package, which is the method for manufacturing a package according to any one of claims 1 to 10, wherein the method for manufacturing a package include: (a) forming a green laminate having a ceramic green portion and a metallized green portion, wherein the ceramic green portion includes a portion to be the ceramic portion, the metallized green portion includes a portion to be the metallized portion, the ceramic green portion and the metallized green portion each straddling an imaginary line that is at least a portion of the outer edge of the ceramic portion, The method for manufacturing the package further comprises: (b) forming a groove in the green laminate along the imaginary line; (c) a step of forming a fired body including the ceramic portion and the metallized portion by firing the green laminate; (d) a step of plating the metallized portion of the sintered body to form the metal layer; and (e) After the step of plating the metallized portion, a step of generating a crack in the sintered body starting from the groove to thereby fracture the ceramic portion while forming a surface of the intermediate portion of the side metallized layer of the metallized portion.