A modification method for retired lithium-ion battery negative electrode material
Through homogeneous dispersion, calcination and washing of the negative electrode materials of retired lithium-ion batteries, the problem of poor electrochemical performance of graphite materials is solved, and the morphology and performance improvement of the material are achieved, and the process is simple and environmentally friendly.
Patent Information
- Application Number
- CN202210549841.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-05-20
AI Technical Summary
The prior art is difficult to effectively modify the negative electrode graphite material of retired lithium-ion batteries, resulting in poor electrochemical performance, and traditional methods and processes are complex, high costs and serious environmental pollution.
By mixing the negative electrode powder of the decommissioned lithium-ion battery with an ethanol solution for homogeneous dispersion, washing with ethanol after calcination, the graphite surface morphology modification and electrochemical performance optimization are achieved, and fluorine-containing components and debris inclusions are removed.
This method is simple and low-cost, effectively improving the electrochemical charging and discharging performance of recycled graphite materials, improving the surface morphology, reducing fluorine content and debris, and improving the recycling value of the material.
Smart Images

Figure CN114709506B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling negative electrode materials of lithium ion batteries, and in particular to a method for modifying negative electrode materials of retired lithium ion batteries. Background Art
[0002] Lithium-ion batteries are widely used in electric vehicles, energy storage and 3C electronic devices due to their high operating voltage, recyclability and environmental friendliness. Globally, the installed capacity of lithium-ion batteries is showing an explosive growth trend; accordingly, the number of retired lithium-ion batteries at the end of their product life cycle has also increased sharply.
[0003] At present, the recycling of retired lithium-ion batteries is mainly focused on the recycling of valuable metals in the positive electrode materials. However, in the traditional lithium-ion battery recycling method, graphite, which accounts for 10-21% of the waste lithium-ion batteries, is usually used for energy utilization by high-temperature combustion or as filter residue storage and landfill, which aggravates the particulate pollution and greenhouse effect. Therefore, realizing the high-value closed-loop recycling of graphite powder in retired lithium-ion batteries is of great significance to the sustainable development of new energy vehicles and energy storage industries.
[0004] At present, the research on lithium battery graphite negative electrode in the market mainly improves the electrochemical performance of graphite materials through modification treatment. There is not much research on the influence of fluorine-containing components and surface morphology in the recycled graphite materials on the performance of graphite, which results in poor initial charge and discharge performance of graphite negative electrode materials. Patent CN200910226670B discloses a method for recycling and repairing waste lithium-ion battery anode graphite. After acid leaching and impurities removal, it is calcined at high temperature, and cellulose acetate is used as a coating material and acetone is used as a solvent to coat and modify the graphite, thereby obtaining a carbonaceous material with high purity and amorphous carbon coated on the surface. However, the patent process is relatively complicated, requiring the use of a large amount of acid, and the wastewater generated needs additional treatment, which increases the cost.
[0005] Therefore, how to obtain a surface modification method for the negative electrode graphite of retired lithium-ion batteries that is simple in process, environmentally friendly, and can improve the electrochemical properties of graphite materials is a technical problem that needs to be solved at present. Summary of the invention
[0006] The purpose of the present invention is to provide a method for modifying the negative electrode material of retired lithium-ion batteries, so as to achieve modification of the graphite surface morphology and optimization of the electrochemical performance.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for modifying a negative electrode material of a retired lithium-ion battery, comprising the following steps:
[0009] 1) mixing retired lithium-ion battery negative electrode powder and ethanol solution and performing homogenization and dispersion treatment to obtain graphite powder;
[0010] 2) calcining the graphite powder in a mixed atmosphere to obtain a calcined product;
[0011] 3) Wash the roasted product with ethanol, separate the solid and liquid, and then dry the solid product.
[0012] Furthermore, in step 1), the retired lithium-ion battery negative electrode powder is a graphite negative electrode powder obtained by recovering Li, Fe and P elements from retired lithium iron phosphate batteries, and the carbon content of the graphite negative electrode powder is 76-84wt%, and the fluorine content is 2-3.6wt%.
[0013] Furthermore, in step 1), the volume concentration of the ethanol solution is 10-40%, and the mass volume ratio of the retired lithium-ion battery negative electrode powder to the ethanol solution is 1 g: 2-8 mL.
[0014] Furthermore, the temperature of the homogenous dispersion is 20 to 80° C., the rotation speed of the homogenous dispersion is 2000 to 6000 rpm, and the time of the homogenous dispersion is 5 to 30 minutes.
[0015] Furthermore, in step 2), the mixed atmosphere is O 2 and N 2 .
[0016] Furthermore, in step 2), the calcination temperature is 200-480° C., and the calcination time is 0.5-3 h.
[0017] Furthermore, in step 3), the washing temperature is 30 to 80° C., and the washing time is 10 to 50 minutes.
[0018] Furthermore, in step 3), the drying temperature is 60-80° C., and the drying time is 5-10 hours.
[0019] Beneficial effects of the present invention:
[0020] (1) The method of the present invention can effectively remove fluorine-containing components and debris inclusions with small particle size and irregular morphology in graphite, improve the surface morphology of the regenerated graphite material, and effectively enhance its electrochemical charge and discharge performance.
[0021] (2) The method of the present invention is simple to operate, low in cost, and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the SEM image of the graphite powder obtained in Example 1;
[0023] Figure 2 This is the SEM image of the graphite powder obtained in Example 2;
[0024] Figure 3 This is the SEM image of the graphite powder obtained in Example 3;
[0025] Figure 4 This is the SEM image of the graphite powder obtained in Example 4;
[0026] Figure 5 This is the SEM image of the graphite powder obtained in Example 5;
[0027] Figure 6 This is the SEM image of the graphite powder obtained in Comparative Example 1;
[0028] Figure 7 The first charge and discharge curves of half-cells assembled with graphite powders obtained in Examples 1 to 5 and Comparative Example 1 are shown, wherein 1 is Example 1, 2 is Example 2, 3 is Example 3, 4 is Example 4, 5 is Example 5, and 6 is Comparative Example 1. DETAILED DESCRIPTION
[0029] The present invention provides a method for modifying a negative electrode material of a retired lithium-ion battery, comprising the following steps:
[0030] 1) mixing retired lithium-ion battery negative electrode powder and ethanol solution and performing homogenization and dispersion treatment to obtain graphite powder;
[0031] 2) calcining the graphite powder in a mixed atmosphere to obtain a calcined product;
[0032] 3) Wash the roasted product with ethanol, separate the solid and liquid, and then dry the solid product.
[0033] In the present invention, in step 1), the retired lithium-ion battery negative electrode powder is a graphite negative electrode powder obtained by recovering Li, Fe and P elements from retired lithium iron phosphate batteries, and the carbon content of the graphite negative electrode powder is 76-84wt%, and the fluorine content is 2-3.6wt%; preferably, the carbon content of the graphite negative electrode powder is 78-82wt%, and the fluorine content is 2.5-3.0wt%; further preferably, the carbon content of the graphite negative electrode powder is 80wt%, and the fluorine content is 2.8wt%.
[0034] In the present invention, in step 1), the volume concentration of the ethanol solution is 10-40%, preferably 15-35%, and more preferably 20-30%.
[0035] In the present invention, in step 1), the mass volume ratio of the retired lithium ion battery negative electrode powder and the ethanol solution is 1g:2-8mL, preferably 1g:4-6mL, and more preferably 1g:5mL.
[0036] In the present invention, the temperature of the homogeneous dispersion is 20-80°C, the rotation speed of the homogeneous dispersion is 2000-6000rpm, and the time of the homogeneous dispersion is 5-30min; preferably, the temperature of the homogeneous dispersion is 40-60°C, the rotation speed of the homogeneous dispersion is 3000-5000rpm, and the time of the homogeneous dispersion is 10-25min; further preferably, the temperature of the homogeneous dispersion is 50°C, the rotation speed of the homogeneous dispersion is 4000rpm, and the time of the homogeneous dispersion is 15-20min.
[0037] In the present invention, the homogenous dispersion is preferably carried out in a high shear homogenizing emulsifier.
[0038] In the present invention, in step 2), the mixed atmosphere is O 2 and N 2 The volume ratio is preferably 0.2-0.5:0.5-0.8, and more preferably 0.3-0.4:0.6-0.7.
[0039] In the present invention, in step 2), the calcination temperature is 200-480°C, and the calcination time is 0.5-3h; preferably, the calcination temperature is 250-420°C, and the calcination time is 1-2.5h; further preferably, the calcination temperature is 300-380°C, and the calcination time is 1.5-2h.
[0040] In the present invention, in step 3), the washing temperature is 30-80°C, and the washing time is 10-50 min; preferably, the washing temperature is 35-75°C, and the washing time is 20-40 min; further preferably, the washing temperature is 40-60°C, and the washing time is 30-35 min.
[0041] In the present invention, in step 3), the drying temperature is 60-80°C, and the drying time is 5-10 hours; preferably, the drying temperature is 65-75°C, and the drying time is 6-9 hours; further preferably, the drying temperature is 70°C, and the drying time is 8 hours.
[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] Example 1
[0044] The retired lithium-ion battery negative electrode powder (fixed carbon content 78wt%, fluorine content 2.6wt%) was mixed with 10% ethanol solution and sheared for 25min using a high shear homogenizer at 6000rpm, 80℃, and a liquid-to-solid ratio of 2mL:1g to obtain graphite powder with less organic residue and better dissociation degree. The graphite powder was then placed in an electric furnace and O was introduced at a volume ratio of 0.6:0.4 at 200℃. 2 With N 2 The mixed gas was kept warm for 3 hours, and then the graphite powder was taken out and cooled naturally in the air. It was then washed with ethanol at 30°C for 50 minutes to remove the fluoride and organic phase remaining on the surface of the graphite after calcination. Finally, it was dried at 60°C for 10 hours to obtain regenerated graphite powder 1.
[0045] Comparative Example 1
[0046] The retired lithium-ion battery negative electrode powder (fixed carbon content 78wt%, fluorine content 2.6wt%) was mixed with 15% ethanol solution and sheared for 10min at 50℃ and liquid-solid ratio 7mL:1g using a high shear homogenizer. The obtained graphite powder 6 had a rough surface, many debris inclusions, and obvious agglomeration, such as Figure 6 Its electrochemical performance is shown in Table 1 and Figure 7 shown.
[0047] After testing, the fluorine content in the regenerated graphite powder 1 was reduced from 2.6wt% to 0.12wt%. Figure 1 As shown, the regenerated graphite powder 1 is better than the comparative example 1 (such as Figure 6 ) The surface of graphite powder is relatively smooth, the debris inclusions are reduced, and the morphology is improved; after testing, its particle size is concentrated between 15 and 20 μm, and its D 10 , D 50 and D 90 The regenerated graphite powder 1 was assembled into a half-cell with metal lithium sheet, separator, electrolyte, etc., and its first charge and discharge specific capacity was measured to be 282.89 mAh g -1 、393.60mAh·g -1 The first cycle coulombic efficiency is 71.87%, which is 4.8% higher than that of the battery in comparative example 1. The results are shown in Table 1 and Figure 7 .
[0048] Example 2
[0049] The retired lithium-ion battery negative electrode powder (fixed carbon content 78wt%, fluorine content 2.6wt%) was mixed with 18% ethanol solution and sheared for 18 minutes using a high shear homogenizer at 5000rpm, 60℃, and a liquid-to-solid ratio of 3mL:1g to obtain graphite powder with less organic residue and better dissociation degree. The graphite powder was then placed in an electric furnace and O was introduced at a volume ratio of 0.3:0.7 at 300℃. 2 With N 2 After keeping the temperature for 2.5 hours, the graphite powder was taken out and cooled naturally in the air, and then washed with ethanol at 40°C for 40 minutes to remove the fluoride and organic phase remaining on the surface of the graphite after calcination. Finally, it was dried at 65°C for 9 hours to obtain regenerated graphite powder 2.
[0050] After testing, the fluorine content in graphite decreased from 2.6wt% to 0.094wt%. Figure 2 As shown, the regenerated graphite powder 2 is better than the comparative example 1 (such as Figure 6 ) surface is relatively smooth, the debris inclusions are reduced, and the morphology is improved; after testing, its particle size is concentrated between 22 and 34 μm, and its D 10 , D 50 and D 90 The regenerated graphite powder 2 was assembled into a half-cell with metal lithium sheet, separator, electrolyte, etc., and its first charge and discharge specific capacity was measured to be 316.41 mAh·g -1 、415.22mAh·g -1 The first cycle coulombic efficiency is 76.20%, which is a significant improvement over the charge and discharge performance of the untreated material. The results are shown in Table 1 and Figure 7 .
[0051] Example 3
[0052] The retired lithium-ion battery negative electrode powder (fixed carbon content 78wt%, fluorine content 2.6wt%) was mixed with 25% ethanol solution and sheared for 15min using a high shear homogenizer at 4000rpm, 50℃, and a liquid-to-solid ratio of 5mL:1g to obtain graphite powder with less organic residue and better dissociation degree. The graphite powder was then placed in an electric furnace and O was introduced at a volume ratio of 0.25:0.75 at 350℃. 2 With N 2 After keeping the temperature for 2.0 h, the graphite powder was taken out and cooled naturally in the air, and then washed with ethanol at 50 ° C for 30 min to remove the fluoride and organic phase remaining on the surface of the graphite after calcination, and finally dried at 70 ° C for 8 h to obtain regenerated graphite powder 3.
[0053] After testing, the fluorine content in the regenerated graphite powder 3 is 0.067wt%. Figure 3As shown, the regenerated graphite powder 3 is better than the comparative example 1 (such as Figure 6 ) The graphite layer structure is obvious, the surface debris is significantly reduced, and the morphology is well improved; after testing, its particle size is concentrated between 20 and 35 μm, and its D 10 , D 50 and D 90 The regenerated graphite powder 3 was assembled into a half-cell with metal lithium sheet, separator, electrolyte, etc., and its first charge and discharge specific capacity was measured to be 349.62 mAh g -1 、439.33mAh·g -1 The first cycle Coulomb efficiency is 79.58%, and the results are shown in Table 1 and Figure 7 .
[0054] Example 4
[0055] The retired lithium-ion battery negative electrode powder (fixed carbon content 78wt%, fluorine content 2.6wt%) was mixed with 30% ethanol solution and sheared for 10 min using a high shear homogenizer at 3000rpm, 40℃, and a liquid-to-solid ratio of 6mL:1g to obtain graphite powder with less organic residue and better dissociation degree. The graphite powder was then placed in an electric furnace and O was introduced at a volume ratio of 0.40:0.60 at 400℃. 2 With N 2 After keeping the mixture for 1.5 hours, the graphite powder was taken out and cooled naturally in the air, and then washed with ethanol at 60°C for 25 minutes to remove the fluoride and organic phase remaining on the surface of the graphite after calcination. Finally, it was dried at 80°C for 6 hours to obtain regenerated graphite powder 4.
[0056] After testing, the fluorine content in the regenerated graphite powder 4 is 0.049wt%. Figure 4 As shown, the surface of the regenerated graphite powder 4 is smooth and regular, with almost no debris; after testing, its particle size is concentrated between 20 and 35 μm, and its D 10 , D 50 and D 90 The regenerated graphite powder 4 was assembled into a half-cell with metal lithium sheet, separator, electrolyte, etc., and its first charge and discharge specific capacity was measured to be 355.74 mAh·g -1 、432.54mAh·g -1 The first cycle Coulomb efficiency is 82.24%, and the results are shown in Table 1 and Figure 7 The graphite in Example 4 has a relatively high charge-discharge specific capacity and is capable of being reused as a negative electrode material for lithium-ion batteries.
[0057] Example 5
[0058] The retired lithium-ion battery negative electrode powder (fixed carbon content 78wt%, fluorine content 2.6wt%) was mixed with 40% ethanol solution and sheared for 5 min at 2000rpm, 20℃, and liquid-to-solid ratio 8mL:1g using a high shear homogenizer to obtain graphite powder with less organic residue and better dissociation degree. The graphite powder was then placed in an electric furnace and O was introduced at a volume ratio of 0.15:0.85 at 480℃. 2 With N 2 The mixed gas was kept warm for 1.0 h, then the graphite powder was taken out and cooled naturally in the air, and then washed with ethanol at 80 ° C for 50 min to remove the fluoride and organic phase remaining on the surface of the graphite after calcination, and finally dried at 75 ° C for 7 h to obtain regenerated graphite powder 5.
[0059] According to the test, the fluorine content in the regenerated graphite powder 5 is 0.039 wt%. Figure 5 As shown in the figure, the regenerated graphite powder 5 has an obvious layered structure, with few surface debris, but ablation holes appear on the surface; after testing, its particle size is concentrated between 25 and 40 μm, and its D 10 , D 50 and D 90 The regenerated graphite powder 5 was assembled into a half-cell with metal lithium sheet, separator, electrolyte, etc., and its first charge and discharge specific capacity was measured to be 319.51 mAh·g -1 、413.24mAh·g -1 The first cycle Coulomb efficiency is 77.32%, and the results are shown in Table 1 and Figure 7 .
[0060] The modified negative electrode regenerated graphite powder obtained in Examples 1 to 5 and Comparative Example 1 was assembled into a half-cell, and the electrochemical performance of the obtained half-cell was tested. The results are shown in Table 1:
[0061] Table 1: Electrochemical performance test table of half-cells of Examples 1 to 5 and Comparative Example 1
[0062] sample Charge capacity (mAh / g) Discharge specific capacity (mAh / g) Coulomb efficiency (%) 1 282.89 393.60 71.87 2 316.41 415.22 76.20 3 349.62 439.33 79.58 4 355.74 432.54 82.24 5 319.51 413.24 77.32 6 262.67 391.59 67.07
[0063] It can be seen from the above embodiments that the present invention provides a method for modifying the negative electrode material of retired lithium-ion batteries. The present invention uses the graphite negative electrode powder after recycling Li, Fe, and P elements from retired lithium iron phosphate batteries as raw materials, and conducts monomer enhanced dissociation and oxidative roasting heat treatment for the fluorine-containing components remaining in the graphite powder and the debris inclusions with small particle size and irregular morphology without adding other chemical reagents. While efficiently removing the fluorine-containing components, the debris inclusions are fully burned at low temperature to achieve surface morphology modification of the graphite powder. The regenerated graphite powder obtained by the present invention has a regular morphology, a low impurity fluorine content, and an effectively improved electrochemical charge and discharge performance. The method of the present invention also has the advantages of simple operation and low cost.
[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for modifying a negative electrode material of a retired lithium-ion battery, characterized in that: The following steps are involved: 1) mixing retired lithium-ion battery negative electrode powder and ethanol solution and performing homogenization and dispersion treatment to obtain graphite powder; 2) calcining the graphite powder in a mixed atmosphere to obtain a calcined product; 3) washing the roasted product with ethanol, and drying the solid product after solid-liquid separation; In step 2), the mixed atmosphere is O2 and N2 in a volume ratio of 0.25-0.4:0.6-0.75; In step 2), the calcination temperature is 350-400°C and the calcination time is 0.5-3h; The rotation speed of the homogenous dispersion is 3000-4000 rpm.
2. The method for modifying the negative electrode material of retired lithium-ion batteries according to claim 1, characterized in that: In step 1), the retired lithium-ion battery negative electrode powder is a graphite negative electrode powder obtained by recovering Li, Fe and P elements from retired lithium iron phosphate batteries, and the carbon content of the graphite negative electrode powder is 76-84wt%, and the fluorine content is 2-3.6wt%.
3. The method for modifying the negative electrode material of retired lithium-ion batteries according to claim 1 or 2, characterized in that: In step 1), the volume concentration of the ethanol solution is 10-40%, and the mass volume ratio of the retired lithium-ion battery negative electrode powder to the ethanol solution is 1 g: 2-8 mL.
4. The method for modifying the negative electrode material of retired lithium-ion batteries according to claim 3, characterized in that: The homogenous dispersion temperature is 20 to 80° C., and the homogenous dispersion time is 5 to 30 minutes.
5. The method for modifying the negative electrode material of retired lithium-ion batteries according to claim 1 or 4, characterized in that: In step 3), the washing temperature is 30 to 80° C., and the washing time is 10 to 50 minutes.
6. The method for modifying the negative electrode material of retired lithium-ion batteries according to claim 5, characterized in that: In step 3), the drying temperature is 60-80° C. and the drying time is 5-10 hours.