Method for regenerating a hydrogenation catalyst

By using low temperature and low oxygen concentration gas flow to regenerate the catalyst in the ring hydrogenation of aromatic compounds and aromatic esters, the problem of poor catalyst activity recovery effect is solved, and the rapid regeneration of the catalyst and the improvement of the ring hydrogenation conversion rate are achieved. Improved, avoiding risks caused by high temperatures.

CN114713220BActive Publication Date: 2024-10-18EVONIK OXENO GMBH & CO KG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111550235.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-17
Publication Date
2024-10-18
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

In the current catalyst regeneration process, especially in the ring hydrogenation of aromatic compounds and aromatic esters, the catalyst activity recovery effect is not good, especially in the presence of water and other substances that reduce hydrogenation activity, and high-temperature regeneration may cause Excessive energy consumption or damaged catalyst.

Method used

By regenerating the catalyst using a gas stream containing 100 ppm to 20,000 ppm oxygen at a temperature of 15 to 170°C, avoiding high-temperature calcination, utilizing a gas stream with a low oxygen concentration to entrain sediments, improve catalyst activity, and improve catalyst activity in multiple reactions. Stagger or perform regeneration simultaneously in the reactor to improve conversion rate.

Benefits of technology

It achieves rapid and effective regeneration of the catalyst, improves the ring hydrogenation conversion rate, avoids catalyst damage caused by temperature rise during the oxidation process, and improves production efficiency and product value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 729255DEST_PATH_IMAGE002
    Figure 729255DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The present invention provides a process for regenerating a catalyst for the ring hydrogenation of aromatic compounds, in particular aromatic esters, wherein a gas stream comprising a certain amount of oxygen is used for the regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a process for regenerating a catalyst for the ring hydrogenation of aromatic compounds, in particular aromatic esters, wherein a gas stream comprising a certain amount of oxygen is used for the regeneration. Background Art

[0002] The hydrogenation of aromatic compounds, in particular the hydrogenation of aromatic esters, which hydrogenates aromatic rings is known and is also referred to as ring hydrogenation. In such ring hydrogenation, catalysts comprising, for example, transition metals are used. Suitable catalysts are known to those skilled in the art. Corresponding hydrogenation processes are also used on an industrial scale.

[0003] As the duration of the cyclohydrogenation increases, the catalyst used loses activity, which may be due to clogging, loss or poisoning of the active centers of the catalyst. If the activity loss is too great and / or it is no longer possible to operate the hydrogenation process economically enough, the activity of the catalyst must be increased. This is achieved by means of a regeneration process in which the catalyst is freed of deposits and adhering materials. In this case, the catalyst can be calcined, wherein the deposits are removed at high temperatures (> 200° C.), which, however, may be problematic for certain catalysts or purely from an energetic point of view due to the high temperatures.

[0004] However, the catalyst can also be regenerated by passing a gas stream through it, thereby entraining the deposits and thus removing them. Such a method for regenerating a ruthenium catalyst is described, for example, in WO 2008 / 015103 A1. The regeneration disclosed there is characterized in that the catalyst is purged with an inert gas until the catalyst partially or even completely regains its activity. The removal of water, i.e. drying of the catalyst, is mentioned as the reason for the regeneration described there by means of hydrogenation of benzene.

[0005] However, the known methods have the problem that the regeneration effect may be too small, especially when not only water has to be removed from the catalyst, or not only water but also other substances which reduce the hydrogenation activity are present on the catalyst. Summary of the invention

[0006] It is therefore an object of the present invention to provide a method for regenerating catalysts for the ring hydrogenation of aromatic compounds, in particular aromatic esters, with which method an acceptable activity can be obtained more quickly and better.

[0007] The object is achieved by the method as claimed in claim 1. Preferred embodiments are given in the dependent claims. The method according to the invention is a method for regenerating a catalyst for the ring hydrogenation of aromatic compounds in at least one reactor, wherein the regeneration is carried out as follows:

[0008] - at a temperature of 15 to 170° C., preferably 25 to 150° C., particularly preferably 25 to 120° C., very particularly preferably 25 to 110° C.;

[0009] - passing a gas stream through the catalyst to be regenerated, the gas stream having an oxygen content of from 100 ppm, preferably 250 ppm, particularly preferably 380 ppm to 20,000 ppm, preferably 13,000 ppm, particularly preferably 9,000 ppm; and

[0010] - The catalyst is not removed from the at least one reactor.

[0011] By means of the process according to the invention, in which a small amount of oxygen is present in the gas stream (regeneration medium), an advantageous regeneration of the hydrogenation catalyst can be achieved. The catalyst activity is improved by this regeneration, which according to the invention can already be carried out at low oxygen concentrations. The regeneration described here makes it possible to subsequently restart the cyclohydrogenation at an increased conversion, thereby producing actual valuable products and thus proceeding more efficiently. At the same time, the relatively low oxygen concentration prevents the occurrence of strongly (optionally even only locally) elevated temperatures in the reactor due to the oxidation process, which would damage the catalyst or, in the worst case, lead to damage to the reactor.

[0012] The ring hydrogenation of aromatic compounds, in particular aromatic esters, described here is usually carried out in at least one reactor, i.e. the ring hydrogenation can be carried out in one or more reactors, each of which contains a suitable catalyst. The regeneration according to the invention of the catalyst used can be carried out in each reactor present. In the case of the presence of a plurality of reactors, the regeneration can be carried out in a time-staggered manner or simultaneously for each reactor, wherein preferably all catalysts are regenerated simultaneously in all reactors present.

[0013] According to the invention, the method is applicable to all catalysts used in the ring hydrogenation of aromatic compounds, especially aromatic esters. However, the catalyst preferably comprises at least one transition metal on a support material or consists of at least one transition metal on a support material. Suitable catalysts are also familiar to those skilled in the art and can be learned, for example, from WO 03 / 103830 A1.

[0014] The transition metal of the catalyst to be regenerated is preferably a metal selected from the following: iron, ruthenium, nickel, rhodium, platinum, palladium or a mixture thereof. Ruthenium is a particularly preferred transition metal for the catalyst in the present invention. The content of the transition metal in the catalyst to be regenerated is generally 0.1 to 30% by mass. The ruthenium content calculated as metal is preferably 0.1 to 10% by mass, in particular 0.3 to 5% by mass, and very particularly 0.4 to 2.5% by mass.

[0015] The carrier material on which the transition metal is located is preferably selected from activated carbon, silicon carbide, aluminum oxide, silicon dioxide, aluminosilicate, titanium dioxide, zirconium dioxide, magnesium oxide, zinc oxide or a mixture thereof. Preferred carrier materials are aluminum oxide, silicon dioxide, titanium dioxide and a mixture thereof. In addition, these carrier materials may contain alkali metals, alkaline earth metals and / or sulphur. In a particularly preferred embodiment of the present invention, the catalyst to be regenerated is a shell-type catalyst.

[0016] According to the present invention, a gas stream is used as the regeneration medium. The gas stream is preferably composed of an inert gas and oxygen, wherein the oxygen content of the gas stream is 100 ppm, preferably 250 ppm, particularly preferably 380 ppm to 20,000 ppm, preferably 13,000 ppm, particularly preferably 9,000 ppm. The inert gas can be nitrogen, helium, neon, argon, carbon dioxide and mixtures thereof. Particularly preferably, nitrogen is used as the inert gas. Based on the flow direction during cyclohydrogenation, the gas stream during regeneration can be directed to pass through the catalyst in the same or opposite flow direction, preferably in the same flow direction.

[0017] In the case of multiple hydrogenation reactors, the regeneration medium can be fed only to the first reactor. The regeneration medium will then also be sent from the first reactor to the subsequent reactor or reactors in order to also regenerate the catalyst there. However, it is preferred that, in the case of multiple reactors, the regeneration medium is sent to each individual reactor separately. The regeneration medium is therefore sent directly to each individual reactor and does not first pass through the upstream reactor or reactors.

[0018] According to the claim, the regeneration is carried out at a temperature of 15 to 170° C., preferably 25 to 150° C., particularly preferably 25 to 120° C. In this connection, it is important that no combustion of the catalyst takes place, wherein the impurities are removed at high temperatures. The pressure during the regeneration is preferably 0.5 to 200 bar, preferably 1 to 110 bar.

[0019] How long the regeneration described here must be carried out in order to improve the catalyst activity to a sufficient degree depends on various factors. Examples of these factors are the type and amount of impurities, the properties of the reactor (size, diameter) or the properties of the catalyst particles (particularly size, shape, surface, pore structure, metal loading and penetration depth of the metal in the support). In a preferred embodiment of the invention, the duration of the regeneration is at least 24 hours. If the regeneration is terminated too early, it may happen that the catalyst has to be regenerated again after a relatively short period of use in the cyclohydrogenation.

[0020] The catalyst used in the ring hydrogenation of aromatic compounds is regenerated according to the invention. In a preferred embodiment, the catalyst used in the ring hydrogenation of aromatic esters is regenerated according to the invention. The aromatic ester is preferably an ester of benzoic acid, an ester of benzodicarboxylic acid, an ester of benzenetricarboxylic acid or an ester of benzenetetracarboxylic acid, preferably an ester of benzodicarboxylic acid or an ester of benzenetricarboxylic acid. These include phthalates, isophthalates, terephthalates and trimellitic acid esters. Preferred esters of benzodicarboxylic acids are phthalates, i.e. phthalates, isophthalates and terephthalates. Among them, C8-C10 alkyl esters, in particular C8-C10 alkyl esters of phthalic acid (e.g., dioctyl phthalate, diethylhexyl phthalate, diisononyl phthalate, dipropylheptyl phthalate) or C8-C10 alkyl esters of terephthalic acid (e.g., dioctyl terephthalate, diethylhexyl terephthalate, diisononyl terephthalate, dipropylheptyl terephthalate) are preferred.

[0021] The cyclohydrogenation is preferably carried out in the liquid phase. The cyclohydrogenation can be carried out continuously or discontinuously over a suspended or massive catalyst arranged in a fixed bed. In the process according to the invention, preference is given to continuous cyclohydrogenation over a catalyst arranged in a fixed bed, wherein the product / reactant phase is predominantly in the liquid state under the reaction conditions. Preferably, one or more reactors are operated as a trickle bed reactor which can be completely or partially overflowed.

[0022] When the cyclohydrogenation is carried out continuously on a catalyst arranged in a fixed bed, it is expedient to convert the catalyst into an active form before the cyclohydrogenation is carried out for the first time. This activation is not absolutely necessary after regeneration. The activation can be carried out by reducing the catalyst with a hydrogen-containing gas according to a temperature program. Here, the reduction can optionally be carried out in the presence of a liquid phase dripping through the catalyst. A solvent or a hydrogenation product can be used as a liquid phase. Under corresponding hydrogenation conditions, this activation can also be omitted, because this is also carried out under the reaction conditions.

[0023] Different process variants can be selected for the ring hydrogenation. It can be carried out adiabatically, variably or almost isothermally (i.e., wherein the temperature rise is generally less than 10° C.) in one or more stages. In the latter case, all reactors, preferably tubular reactors, can be operated adiabatically or almost isothermally, and one or more are operated adiabatically and others are operated almost isothermally. In addition, the aromatic polycarboxylic acid ester can be hydrogenated in a straight-through manner or under product recycle. There can also be two reactors, wherein the first reactor is operated under product recycle and the second reactor is operated in a straight-through manner. The ring hydrogenation can also be carried out as a trickle bed. Here, the reactor can also be partially or completely filled.

[0024] The cyclohydrogenation can be carried out in a liquid / gas mixed phase or in the liquid phase in a three-phase reactor in parallel flow, wherein the hydrogenation gas is distributed in a manner known per se in the liquid reactant / product stream. For uniform liquid distribution, improved removal of the heat of reaction and high space-time yields, the reactor is preferably 15 to 120, in particular 25 to 80 m 3 per m 2 If the reactor is operated in a straight-through mode, a specific catalyst loading (LHSV) value of 0.1 to 10 h -1 .

[0025] The ring hydrogenation can be carried out in the absence of a solvent or preferably in the presence of a solvent. All liquids which form a homogeneous solution with the reactants and products, behave inertly under the hydrogenation conditions and can be easily separated from the products can be used as solvents. The solvent can also be a mixture of various substances and optionally contain water.

[0026] For example, the following can be used as solvents: linear or cyclic ethers, such as tetrahydrofuran or dioxane, and aliphatic alcohols in which the alkyl radical has 1 to 13 carbon atoms. Alcohols which can be preferably used are, for example, isopropanol, n-butanol, isobutanol, n-pentanol, 2-ethylhexanol, nonanol, technical nonanol mixtures, decanol, technical decanol mixtures, tridecanol.

[0027] When an alcohol is used as solvent, it may be appropriate to use the alcohol or alcohol mixture that is formed when the product is saponified. This excludes the formation of by-products due to transesterification. Another preferred solvent is the hydrogenation product itself.

[0028] By using a solvent, the aromatics concentration in the reactor feed can be limited, whereby better temperature control in the reactor can be achieved. This can minimize side reactions and thus increase the product yield. The aromatics content in the reactor feed is preferably 1 to 35%, in particular 5 to 25%. In the case of a reactor operated in loop mode, the desired concentration range can be set via the circulation ratio (amount ratio of recycled hydrogenation output (Austrag) to reactants).

[0029] The ring hydrogenation can be carried out in a pressure range of 20 to 300 bar, preferably 40 to 200 bar. The hydrogenation temperature is preferably 60 to 200°C, in particular 80 to 180°C.

[0030] Any hydrogen-containing gas mixture which does not contain harmful amounts of catalyst poisons such as carbon monoxide or hydrogen sulfide can be used as the hydrogenation gas. The inert gas component can be nitrogen or methane, for example. Preferably, hydrogen is used with a purity of more than 95%, in particular more than 98%. DETAILED DESCRIPTION

[0031] The invention is explained below with the aid of examples. These examples show exemplary embodiments and are not to be understood as limiting.

[0032] Example 1 - Same oxygen concentration

[0033] For the current experiments, the catalyst must first be produced reproducibly and then it should be regenerated. In this case, diisononyl terephthalate (DINT) was hydrogenated continuously for this purpose. The cyclic hydrogenation of DINT was carried out in a tubular reactor in a cyclic operation. The circulating tubular reactor was flowed through by the liquid phase (DINT and hydrogenation products) and the gas phase (hydrogen) in a trickle bed in parallel. As a hydrogenation catalyst, a commercially available ruthenium catalyst (Specialyst® 102: 1% Ru on a TiO2 carrier, Evonik Operations GmbH) was used in Example 1. It was diluted with an equal amount of inert material (TiO2) and used in a tubular reactor with an inner diameter of 40 mm and a length of 378 mm. The feed rate of DINT used in the cyclic hydrogenation was always 130 g / h, and the circulation flow was 80 L / h. H2 regulation was carried out by a constant exhaust gas mode with an exhaust gas flow of 0.5 L / h. The experiments were each carried out at a plant pressure of 100 bar and a tubular reactor temperature of 110°C. The DINT concentration was recorded by means of online Raman analysis. The conversion of DINT decreased continuously over time. Regeneration was then carried out after approximately 3700 to 5700 hours in each case.

[0034] Before regeneration, the circulation pump and the feed of reactants are stopped, and the liquid is discharged from the circulation reactor. Then the respective regeneration conditions (e.g., pressure, temperature) are set and regeneration is performed for a certain time (see Table 1). After regeneration, the circulation pump and the feed of reactants are restarted so that the ring hydrogenation as described in the previous paragraph is performed again. As a basis for evaluating the regeneration effect, sampling is used just before the reactant feed is shut down (DINT conversion before regeneration) and about 20 to 40 hours after the reactant feed is restarted (DINT conversion after regeneration). The results are shown in Table 1 below.

[0035] Table 1: Experimental data of Example 1

[0036] .

[0037] As can be seen from Table 1, neither pressure nor regeneration duration has a significant effect on regeneration.

[0038] Example 2 - Different oxygen concentrations

[0039] The experiment of Example 2 was carried out in a manner similar to the experiment of Example 1. Therefore, only the differences from the method in Example 1 are listed below. The hydrogenation catalyst used was a ruthenium catalyst with a relatively large amount of Ru (2% Ru on a TiO2 support). The feed rate of DINT used in the cyclohydrogenation was always 180 g / h, and the hydrogenation was carried out at a temperature of 92.5°C. Unlike Example 1, in addition to the temperature and pressure, the oxygen concentration during regeneration was also changed here. In order to avoid problems (explosive gas), the reactor was first inerted with N2 before the regeneration experiment with a higher O2 concentration. The results are shown in Table 2.

[0040] Table 2: Experimental data of Example 2

[0041]

[0042] * Not according to the invention.

[0043] As can be seen in Table 2, poor regeneration can be achieved at very low oxygen concentrations. At high oxygen concentrations, regeneration is also better in a short time, but it should be noted here that at such high concentrations there is a risk of catalyst calcination or burning, so only low temperatures or low pressures can be used. For safety reasons, still higher oxygen concentrations (> 20,000 ppm) have proven to be unhelpful in the present case.

Claims

1. A process for regenerating a catalyst for the ring hydrogenation of aromatic esters selected from esters of benzenecarboxylic acid, benzenedicarboxylic acid, benzenetricarboxylic acid or benzenetetracarboxylic acid in at least one reactor, wherein the catalyst comprises at least one transition metal on a support material, wherein the regeneration is carried out by: - at a temperature of 15 to 170°C; - directing a gas stream through the catalyst to be regenerated, said gas stream having an oxygen content of 380 ppm to 9000 ppm; and - The catalyst is not removed from the at least one reactor.

2. The method according to claim 1, wherein the regeneration is carried out at a temperature of 25 to 150°C.

3. The method according to claim 1 or 2, wherein the at least one transition metal is a metal selected from the group consisting of iron, ruthenium, nickel, rhodium, platinum, palladium or mixtures thereof.

4. The method according to claim 1 or 2, wherein the support material is selected from activated carbon, silicon carbide, aluminum oxide, silicon dioxide, aluminosilicate, titanium dioxide, zirconium dioxide, magnesium oxide, zinc oxide or a mixture thereof.

5. The process according to claim 1 or 2, wherein the catalyst used is a shell-type catalyst.

6. The method according to claim 1 or 2, wherein the gas stream is an inert gas having an oxygen content according to claim 1.

7. The method according to claim 6, wherein the inert gas is selected from nitrogen, helium, neon, argon, carbon dioxide and mixtures thereof.

8. The method of claim 1, wherein the aromatic ester is an ester of benzene dicarboxylic acid or benzene tricarboxylic acid.

9. The method of claim 1, wherein the aromatic ester is an ester of benzene dicarboxylic acid.

10. The method according to claim 8, wherein the aromatic ester is a C8 to C10 alkyl ester of phthalic acid or a C8 to C10 alkyl ester of terephthalic acid.

11. The method according to claim 1 or 2, wherein the regeneration is carried out at a pressure of 0.5 to 200 bar.

12. The method of claim 1 or 2, wherein the duration of the regeneration is at least 24 hours.

13. The method according to claim 1 or 2, wherein the gas flow during regeneration is directed through the catalyst in the same or opposite flow direction, based on the flow direction during hydrogenation.

14. The method according to claim 1 or 2, wherein the gas flow during regeneration is directed through the catalyst in the same flow direction as during hydrogenation.

Citation Information

Patent Citations

  • Catalyst and method for hydrogenating aromatic compounds

    WO2003103830A1

  • Process for regenerating ruthenium catalysts which are suitable for hydrogenation

    WO2008015103A2

  • Regeneration of hydrogenation catalysts based on a platinum metal

    CN101959598A

  • Method for hydrogenating organic compounds by means of RU / SIO2 catalysts

    CN1531459A

  • Process for the reactivation of a platinum-group metal catalyst for the hydrogenation of sugars

    EP0037137A2