A polymer composite solid electrolyte and preparation method thereof
By adding lithiated polyvinyl formaldehyde, lithium salt, polyvinylidene fluoride, porous organic covalent materials and lithium lanthanum zirconate to the solid electrolyte, the composite electrolyte is formed, which solves the problems of single material and low conductivity, and significantly improves the The performance and life of lithium batteries.
Patent Information
- Application Number
- CN202210372709.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-04-11
AI Technical Summary
The existing solid electrolytes prepared based on polyvinyl formaldehyde (PVFM) polymers have the problem of single material and low room temperature conductivity, which affects the rate discharge performance and cycle life of all solid lithium batteries.
Using polymer composite solid electrolytes, including lithiated polyvinyl formaldehyde polymers, lithium salts, polyvinylidene fluoride, porous organic covalent materials and lithium lanthanum zirconate, the room temperature conductivity and machinery of solid electrolytes are significantly improved through synergistic action. Elasticity, forming a bilithium polymer to increase the lithium source and enhancing the transmission channels and mechanical strength of the lithium ions using porous organic covalent materials and lanthanum zirconate.
It significantly improves the room temperature conductivity and mechanical elasticity of solid electrolytes, greatly improves the rate discharge performance and cycle life of all-solid lithium batteries, and enhances the safety and performance stability of the battery.
Smart Images

Figure GDA0005022061180000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a polymer composite solid electrolyte and a preparation method thereof. Background Art
[0002] At present, lithium-ion secondary batteries have become a widely used green chemical energy source due to their many advantages such as high operating voltage, long cycle life, and low environmental pollution. The new generation of high-energy lithium batteries is the development direction of future energy storage devices. However, due to the use of organic electrolytes, high-energy-density lithium batteries have a series of safety hazards such as leakage, fire, and explosion, which seriously limit the application of secondary batteries in the field of long-cycle, high-safety energy storage. In order to solve these problems, some all-solid-state electrolytes for lithium-ion batteries have been developed one after another. Among solid-state electrolytes, solid polymer electrolytes (SPEs) have the advantages of no electrolyte leakage, low flammability, good flexibility, and easy processing, and are widely used.
[0003] Among the materials for preparing solid polymer electrolytes (SPEs), polyvinyl formal (PVFM) polymer has the advantages of low crystallinity, good film-forming properties, adjustable intramolecular structure, etc., and the ether ring groups it contains have high solubility and good lithium salt resolution, thus becoming an ideal material for preparing solid polymer electrolytes (SPEs). For example, in Chinese patent literature, a polymer porous membrane and its preparation method and application in gel polymer electrolytes are disclosed, which are authorized with publication number CN103804892B and application number CN201310231733.1, which discloses that the gelation of the polyvinyl formal polymer PVFM system is achieved by adsorbing and swelling electrolyte, improving mechanical properties and compatibility with electrodes, and improving the safety of solid batteries. And in Chinese patent literature, a polymer solid electrolyte and battery with publication number CN101176233A and application number CN200680016615.7, which discloses that the electrolyte leakage problem is improved and the battery performance is improved by utilizing the polymerization of polyvinyl acetal alcohol and its derivatives. However, the polyvinyl acetal (PVFM) polymer solid electrolytes prepared in these patent documents have the problem of single material and low conductivity of the solid electrolyte at room temperature, which is not conducive to the optimization of the performance of the solid electrolyte and solid battery, and further affects the rate discharge performance and cycle life of the all-solid lithium battery. Summary of the invention
[0004] 1. Technical problem to be solved by the invention
[0005] In view of the technical problems of single material and low room temperature conductivity of solid electrolytes prepared based on polyvinyl formal (PVFM) polymer in the prior art, the present invention provides a polymer composite solid electrolyte and a preparation method thereof, which can significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte, and greatly improve the rate discharge performance and cycle life of the all-solid-state lithium battery.
[0006] 2. Technical solution
[0007] To solve the above problems, the technical solution provided by the present invention is:
[0008] A polymer composite solid electrolyte comprises lithiated polyvinyl formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate, wherein the mass ratio of the lithiated polyvinyl formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate is 50-70:5-10:1-5:3-5:10-30.
[0009] In the present application, by utilizing the synergistic effect between the components of lithiated polyvinyl alcohol formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lanthanum zirconate, the room temperature conductivity and mechanical elasticity of the solid electrolyte can be significantly improved, and the rate discharge performance and cycle life of the all-solid lithium battery can be greatly improved. Among them, the lithiated polyvinyl alcohol formal polymer can be used as a single lithium ion conductor, and the lithium salt is combined to form a double lithium polymer, which increases the lithium source; at the same time, the added porous organic covalent material is a protonic material, which has excellent affinity with lithium ions, and because the porous organic covalent material has a high specific surface area, the addition of the porous organic covalent material can not only accelerate the further dissociation of lithium ions in the lithiated polyvinyl alcohol formal polymer, but also significantly enhance the transmission channel of lithium ions, thereby significantly reducing the interface internal resistance; in addition, the addition of polyvinylidene fluoride can effectively improve the mechanical elasticity of the polymer film layer, increase the stability of the film layer and the surface smoothness during the cycle, and lanthanum zirconate as an excellent lithium ion conductor can further enhance the mechanical strength and lithium ion transmission performance of the polymer solid electrolyte. It can be seen that compared with pure polyvinyl formal-based solid electrolytes, the polymer composite solid electrolyte using a multi-component matrix in the present application can not only significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte, but also greatly improve the rate discharge performance and cycle life of the all-solid lithium battery.
[0010] Optionally, the raw materials of the lithiated polyvinyl formal polymer include polyvinyl formal polymer, dimethyl sulfoxide, boric acid, lithium carbonate and oxalic acid; wherein the mass ratio of the polyvinyl formal polymer to dimethyl sulfoxide is 0.5-1:8-12; and the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.8-1.0:0.5-1.5:1.5-2.0. By adopting polyvinyl alcohol formal polymer, the mechanical elasticity and anti-lithium dendrite ability of polyvinyl alcohol formal can be improved, which is beneficial to improving the cycle life and safety of solid batteries. At the same time, the polyvinyl alcohol formal polymer is dissolved in dimethyl sulfoxide and gradually reacted with boric acid, lithium carbonate and oxalic acid to form a polyvinyl alcohol acetal polymer as the main chain, and the monooxalic acid lithium borate structure is directly grafted on the polymer molecular chain to achieve chemical cross-linking, and the "coordination" and "decoordination" process between the oxygen atom groups contained in the polymer main chain and the boron atom groups in the monooxalic acid lithium borate structure on the side chain and lithium ions is used to achieve lithium ion conduction, so that the lithiated polyvinyl alcohol formal polymer can be used as a single lithium ion conductor, thereby improving the conductivity of the solid electrolyte.
[0011] Optionally, the raw materials of the polyvinyl formal polymer include polyvinyl formal and 4,4'-diphenylmethane diisocyanate, and the concentrations of the polyvinyl formal and 4,4'-diphenylmethane diisocyanate are 0.5-4.5 mol / L and 0.05-0.5 mol / L, respectively. The polyvinyl formal polymer prepared using the raw materials with the above concentration setting has a very high molecular weight compared to polyvinyl formal. The increase in molecular weight is beneficial to improving the mechanical elasticity and anti-lithium dendrite ability of polyvinyl formal, which is beneficial to improving the cycle life and safety of solid batteries.
[0012] Optionally, the molecular weight of the polyvinyl formal is 50,000-70,000, and the molecular weight of the polyvinyl formal polymer is 200,000-500,000. Generally, if the molecular weight of the polyvinyl formal polymer is lower than 200,000, the material viscosity is too high, which will significantly increase the difficulty of solid battery assembly and increase manufacturing costs; if it is higher than 500,000, the hardness of the polyvinyl formal polymer material will be too high, resulting in the brittleness of the polymer composite solid electrolyte membrane, reducing the contact performance with the positive and negative electrode interfaces, and causing battery safety performance. By limiting the molecular weight of polyvinyl formal, the molecular weight of the polyvinyl formal polymer can be obtained to be 200,000-500,000, ensuring the mechanical elasticity and anti-lithium dendrite ability of the solid electrolyte.
[0013] Optionally, the lithium salt is selected from one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium hexafluoroborate, lithium perchlorate, lithium difluorobis(oxalatoborate), lithium triethylborohydride, lithium diisopropylamide, lithium acetoacetate, bis(trimethylsilyl)lithium, pentamethylcyclopentadiene lithium, 4,5-dicyano-2-trifluoromethylimidazole lithium, (fluorosulfonyl) (perfluorobutylsulfonyl)imide lithium, and tert-butyl lithium.
[0014] At the same time, the present application also provides a method for preparing a polymer composite solid electrolyte, which is used to prepare the polymer composite solid electrolyte described above, comprising the following steps:
[0015] S1, dissolving lithiated polyvinyl formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate in an organic solvent, stirring and mixing, and ultrasonically dispersing to obtain a mixed slurry;
[0016] S2. The mixed slurry obtained in S1 is coated on a glass plate and vacuum dried to obtain a polymer composite solid electrolyte.
[0017] Optionally, the mass ratio of the lithiated polyvinyl alcohol formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate is 50-70:5-10:1-5:3-5:10-30, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide, the organic solvent is anhydrous acetonitrile, the stirring time is 1-3h, the ultrasonic time is 1-2h, the drying temperature is 60-80°C, the drying time is 20-30h, and the coating thickness is 50-200μm. By limiting each parameter, the prepared polymer composite solid electrolyte has higher room temperature conductivity and mechanical elasticity, which can greatly improve the rate discharge performance and cycle life of the all-solid lithium battery.
[0018] Optionally, in step S1, the method for preparing the lithiated polyvinyl formal polymer comprises the following steps:
[0019] a. dissolving polyvinyl formal in an organic solvent, stirring and mixing, adding 4,4′-diphenylmethane diisocyanate, continuing to stir and mix, then adding deionized water, continuing to stir and mix, obtaining a slurry, and finally precipitating the obtained slurry to obtain a polyvinyl formal polymer;
[0020] b. dissolving the polyvinyl formal polymer obtained in a in an organic solvent, adding boric acid, stirring and mixing, then sequentially adding lithium carbonate and oxalic acid, ultrasonically mixing to obtain a mixed solution, and finally freeze-drying the obtained mixed solution to obtain a lithiated polyvinyl formal polymer.
[0021] Optionally, step a is as follows: dissolve polyvinyl formal in N-methylpyrrolidone, stir magnetically for 1-2 hours, continue stirring at 65-85°C for 20-60 minutes, then add 4,4′-diphenylmethane diisocyanate, and continue stirring at 40-55°C for 1-2 hours to dissolve it completely, wherein the concentrations of polyvinyl formal and 4,4′-diphenylmethane diisocyanate are 0.5-4.5 mol / L and 0.05-0.5 mol / L, respectively, then add deionized water, continue stirring and mixing, obtain slurry, and finally place the obtained slurry in a coagulation tank for precipitation to obtain polyvinyl formal polymer. The polyvinyl formal polymer prepared by this method has a very high molecular weight compared to polyvinyl formal, and the increase in molecular weight is conducive to improving the mechanical elasticity and anti-lithium dendrite ability of polyvinyl formal, which is conducive to improving the cycle life and safety of solid batteries.
[0022] Optionally, step b is as follows: the polyvinyl alcohol formal polymer obtained in a is dissolved in dimethyl sulfoxide, the mass ratio of the polyvinyl alcohol formal polymer to dimethyl sulfoxide is 0.5-1:8-12, to obtain a light yellow uniform transparent solution, boric acid with a concentration of 0.05-0.3 mol / L is added, and magnetic stirring is carried out at 70-90°C for 3-5 hours. After uniform mixing, lithium carbonate and oxalic acid are added in sequence, and ultrasonic mixing is carried out at 50°C-90°C for 4-8 hours to obtain a mixed solution, wherein the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.8-1.0:0.5-1.5:1.5-2.0; finally, the obtained mixed solution is rinsed with anhydrous ethanol or isopropanol for 3-4 times, dried at 50-70°C for 3-5 hours, and then vacuum freeze-dried for 3-6 hours to obtain a lithiated polyvinyl alcohol formal polymer. The lithiated polyvinyl formal polymer can act as a single lithium ion conductor, thereby improving the conductivity of the solid electrolyte.
[0023] 3. Beneficial effects
[0024] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0025] (1) A polymer composite solid electrolyte proposed in an embodiment of the present application can significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte by utilizing the synergistic effect among the components of lithiated polyvinyl formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate, thereby greatly improving the rate discharge performance and cycle life of the all-solid-state lithium battery. Among them, the lithiated polyvinyl alcohol formal polymer can be used as a single lithium ion conductor, and can be combined with lithium salts to form a double lithium polymer, which increases the lithium source; at the same time, the added porous organic covalent material is a protonic material, which has excellent affinity with lithium ions, and because the porous organic covalent material has a high specific surface area, the addition of the porous organic covalent material can not only accelerate the further dissociation of lithium ions in the lithiated polyvinyl alcohol formal polymer, but also significantly enhance the transmission channel of lithium ions, thereby significantly reducing the interface internal resistance; in addition, the addition of polyvinylidene fluoride can effectively improve the mechanical elasticity of the polymer film layer, increase the stability of the film layer and the surface flatness during the cycle, and lithium lanthanum zirconate as an excellent lithium ion conductor can further enhance the mechanical strength and lithium ion transmission performance of the polymer solid electrolyte. It can be seen from this that compared with pure polyvinyl alcohol formal-based solid electrolytes, the polymer composite solid electrolyte of the multi-component matrix used in this application can not only significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte, but also greatly improve the rate discharge performance and cycle life of the all-solid lithium battery.
[0026] (2) A polymer composite solid electrolyte proposed in an embodiment of the present application can improve the mechanical elasticity and anti-lithium dendrite ability of polyvinyl formal by adopting polyvinyl formal polymer, which is beneficial to improving the cycle life and safety of solid batteries. At the same time, the polyvinyl formal polymer is dissolved in dimethyl sulfoxide and gradually reacted with boric acid, lithium carbonate and oxalic acid to form a polyvinyl acetal polymer as the main chain, and the monooxalic acid lithium borate structure is directly grafted on the polymer molecular chain to achieve chemical cross-linking. The "coordination" and "decoordination" process between the oxygen atom groups contained in the polymer main chain and the boron atom groups in the monooxalic acid lithium borate structure on the side chain and lithium ions is utilized to achieve lithium ion conduction, so that the lithiated polyvinyl formal polymer can be used as a single lithium ion conductor, thereby improving the conductivity of the solid electrolyte.
[0027] (3) A polymer composite solid electrolyte proposed in an embodiment of the present application, by limiting the use of the above-mentioned concentration, has a very high molecular weight compared to polyvinyl formal. The increase in molecular weight is beneficial to improving the mechanical elasticity and resistance to lithium dendrites of polyvinyl formal, which is beneficial to improving the cycle life and safety of solid batteries.
[0028] (4) A polymer composite solid electrolyte proposed in an embodiment of the present application can obtain a molecular weight of 200,000-500,000 polyvinyl formal polymer by limiting the molecular weight of polyvinyl formal, thereby ensuring the mechanical elasticity and anti-lithium dendrite ability of the solid electrolyte.
[0029] (5) A method for preparing a polymer composite solid electrolyte is proposed in an embodiment of the present application. The polymer composite solid electrolyte prepared by this method has higher room temperature conductivity and mechanical elasticity, and can greatly improve the rate discharge performance and cycle life of all-solid-state lithium batteries. DETAILED DESCRIPTION
[0030] To further understand the content of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present application provides a polymer composite solid electrolyte, comprising a lithiated polyvinyl formal polymer, a lithium salt, polyvinylidene fluoride, a porous organic covalent material and lithium lanthanum zirconate, wherein the mass ratio of the lithiated polyvinyl formal polymer, the lithium salt, polyvinylidene fluoride, the porous organic covalent material and the lithium lanthanum zirconate is 50-70:5-10:1-5:3-5:10-30. By utilizing the synergistic effect between the components of the lithiated polyvinyl formal polymer, the lithium salt, polyvinylidene fluoride, the porous organic covalent material and the lithium lanthanum zirconate, the room temperature conductivity and mechanical elasticity of the solid electrolyte can be significantly improved, and the rate discharge performance and cycle life of the all-solid lithium battery can be greatly improved. Among them, the lithiated polyvinyl alcohol formal polymer can be used as a single lithium ion conductor, and can be combined with lithium salts to form a double lithium polymer, which increases the lithium source; at the same time, the added porous organic covalent material is a protonic material, which has excellent affinity with lithium ions, and because the porous organic covalent material has a high specific surface area, the addition of the porous organic covalent material can not only accelerate the further dissociation of lithium ions in the lithiated polyvinyl alcohol formal polymer, but also significantly enhance the transmission channel of lithium ions, thereby significantly reducing the interface internal resistance; in addition, the addition of polyvinylidene fluoride can effectively improve the mechanical elasticity of the polymer film layer, increase the stability of the film layer and the surface flatness during the cycle, and lithium lanthanum zirconate as an excellent lithium ion conductor can further enhance the mechanical strength and lithium ion transmission performance of the polymer solid electrolyte. It can be seen from this that compared with pure polyvinyl alcohol formal-based solid electrolytes, the polymer composite solid electrolyte of the multi-component matrix used in this application can not only significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte, but also greatly improve the rate discharge performance and cycle life of the all-solid lithium battery.
[0032] Specifically, the raw materials of the lithiated polyvinyl formal polymer include polyvinyl formal polymer, dimethyl sulfoxide, boric acid, lithium carbonate and oxalic acid; wherein the mass ratio of the polyvinyl formal polymer to dimethyl sulfoxide is 0.5-1:8-12; and the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.8-1.0:0.5-1.5:1.5-2.0. By adopting polyvinyl alcohol formal polymer, the mechanical elasticity and anti-lithium dendrite ability of polyvinyl alcohol formal can be improved, which is beneficial to improving the cycle life and safety of solid batteries. At the same time, the polyvinyl alcohol formal polymer is dissolved in dimethyl sulfoxide and gradually reacted with boric acid, lithium carbonate and oxalic acid to form a polyvinyl alcohol acetal polymer as the main chain, and the monooxalic acid lithium borate structure is directly grafted on the polymer molecular chain to achieve chemical cross-linking. The "coordination" and "decoordination" process between the oxygen atom groups contained in the polymer main chain and the boron atom groups in the monooxalic acid lithium borate structure on the side chain and lithium ions is used to achieve lithium ion conduction, so that the lithiated polyvinyl alcohol formal polymer can be used as a single lithium ion conductor, thereby improving the conductivity of the solid electrolyte. In addition, the molecular weight of the polyvinyl alcohol formal polymer is 200000-500000. Generally, if the molecular weight of the polyvinyl alcohol formal polymer is lower than 200000, the material viscosity is too high, which will significantly increase the difficulty of solid battery assembly and increase the manufacturing cost; if it is higher than 500000, the hardness of the polyvinyl alcohol formal polymer material is too high, resulting in the brittleness of the polymer composite solid electrolyte membrane, reducing the contact performance with the positive and negative electrode interfaces, and causing battery safety performance. The molecular weight of the polyvinyl alcohol formal polymer is 200000-500000, which ensures the mechanical elasticity and anti-lithium dendrite ability of the solid electrolyte.
[0033] Specifically, the raw materials of the polyvinyl formal polymer include polyvinyl formal and 4,4'-diphenylmethane diisocyanate, the concentrations of the polyvinyl formal and 4,4'-diphenylmethane diisocyanate are 0.5-4.5 mol / L and 0.05-0.5 mol / L respectively, and the molecular weight of the polyvinyl formal is 50000-70000. The polyvinyl formal polymer prepared by using the raw materials with the above concentration setting has a very high molecular weight compared with polyvinyl formal, and the increase in molecular weight is conducive to improving the mechanical elasticity and anti-lithium dendrite ability of polyvinyl formal, which is conducive to improving the cycle life and safety of solid batteries.
[0034] The lithium salt is selected from one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium hexafluoroborate, lithium perchlorate, lithium difluorobis(oxalatoborate), lithium triethylborohydride, lithium diisopropylamide, lithium acetoacetate, bis(trimethylsilyl)lithium, pentamethylcyclopentadiene lithium, 4,5-dicyano-2-trifluoromethylimidazole lithium, (fluorosulfonyl) (perfluorobutylsulfonyl) imide lithium, and tert-butyl lithium.
[0035] At the same time, the present application also provides a method for preparing a polymer composite solid electrolyte, which is used to prepare the polymer composite solid electrolyte described above, comprising the following steps:
[0036] S1. Dissolve lithiated polyvinyl alcohol formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate in an organic solvent, stir and mix, and ultrasonically disperse to obtain a mixed slurry; wherein the mass ratio of the lithiated polyvinyl alcohol formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate is 50-70:5-10:1-5:3-5:10-30, the lithium salt is lithium bistrifluoromethanesulfonyl imide, the organic solvent is anhydrous acetonitrile, the stirring time is 1-3h, and the ultrasonic time is 1-2h. By limiting each parameter, the prepared polymer composite solid electrolyte has higher room temperature conductivity and mechanical elasticity, which can greatly improve the rate discharge performance and cycle life of all-solid lithium batteries.
[0037] Specifically, the method for preparing the lithiated polyvinyl formal polymer comprises the following steps:
[0038] a. Dissolve polyvinyl formal in N-methylpyrrolidone, stir magnetically for 1-2 hours, continue stirring at 65-85°C for 20-60 minutes, then add 4,4′-diphenylmethane diisocyanate, and continue stirring at 40-55°C for 1-2 hours to completely dissolve it, wherein the concentrations of polyvinyl formal and 4,4′-diphenylmethane diisocyanate are 0.5-4.5 mol / L and 0.05-0.5 mol / L, respectively, then add deionized water as a non-organic solvent to precipitate white particles, continue stirring until the precipitated turbid liquid becomes a transparent and viscous slurry, that is, obtain a slurry, and finally place the obtained slurry in a coagulation tank for precipitation to obtain a polyvinyl formal polymer with a molecular weight of 50,000-70,000. The polyvinyl formal polymer prepared by the method has a very high molecular weight compared to polyvinyl formal. The increase in molecular weight is beneficial to improving the mechanical elasticity and resistance to lithium dendrites of polyvinyl formal, which is beneficial to improving the cycle life and safety of solid batteries.
[0039] b. The polyvinyl alcohol formal polymer obtained in a is dissolved in dimethyl sulfoxide, wherein the mass ratio of the polyvinyl alcohol formal polymer to dimethyl sulfoxide is 0.5-1:8-12, to obtain a light yellow uniform transparent solution, boric acid having a concentration of 0.05-0.3 mol / L is added, and the solution is placed at 70-90° C. for magnetic stirring for 3-5 hours. After uniform mixing, lithium carbonate and oxalic acid are added in sequence, and the solution is placed at 50° C. for ultrasonic mixing for 4-8 hours to obtain a mixed solution, wherein the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.8-1.0:0.5-1.5:1.5-2.0; finally, the obtained mixed solution is rinsed 3-4 times with anhydrous ethanol or isopropanol, dried at 50-70° C. for 3-5 hours, and then freeze-dried in a vacuum environment cold pump for 3-6 hours to obtain a lithiated polyvinyl alcohol formal polymer with a molecular weight of 200000-500000. The lithiated polyvinyl formal polymer can act as a single lithium ion conductor, thereby improving the conductivity of the solid electrolyte.
[0040] S2. The mixed slurry obtained in S1 is coated on a glass plate by a doctor blade method, with a coating thickness of 50-200 μm, and placed in a vacuum oven at 60-80 ° C for 20-30 hours, and the solvent is completely removed by vacuum drying to obtain a polymer composite solid electrolyte. Generally, if the coating thickness is too low, the actual energy density of the solid battery is reduced, resulting in excessive battery costs; if the coating thickness is too high, the lithium ion transmission path increases, the internal resistance of the solid battery is increased, and it is not conducive to the power performance. In this application, by limiting the coating thickness, the energy density of the solid battery and the smoothness of lithium ion transmission can be guaranteed.
[0041] In addition, the present application also provides a method for preparing a solid battery, which is as follows: adding lanthanum zirconate lithium particles (particle size of 100-500nm), positive electrode active materials and carbon black conductive agents in a mass ratio of 0.5-1.0:1-2.5:0.05-0.1 to a high-energy vibration ball mill, ball milling at room temperature for 30-45min to obtain a mixture, and then the mixture is transferred into a molybdenum-based alloy mold, and pressed into a film at 300-400 standard atmospheres as a composite positive electrode sheet, wherein the positive electrode material used is any one of lithium iron phosphate LFP, lithium cobalt oxide LCO and layered ternary material NCM; then using the composite positive electrode sheet obtained above as the positive electrode sheet, and lithium indium alloy as the negative electrode sheet (lithium atomic percentage of 40-60%), the positive and negative electrode sheets are respectively pressed on both sides of the polymer composite solid electrolyte prepared above at 20-40 standard atmospheres to prepare a solid battery.
[0042] Example 1
[0043] Preparation of lithiated polyvinyl formal polymer: dissolve polyvinyl formal in N-methylpyrrolidone, stir magnetically for 1.5 hours, continue stirring at 75°C for 45 minutes, then add 4,4′-diphenylmethane diisocyanate, and continue stirring at 45°C for 1.5 hours to completely dissolve it, wherein the concentrations of polyvinyl formal and 4,4′-diphenylmethane diisocyanate are 2.8 mol / L and 0.22 mol / L, respectively, then add deionized water as a non-organic solvent to precipitate white particles, continue stirring until the precipitated turbid liquid becomes a transparent and viscous slurry, that is, obtain a slurry, and finally place the obtained slurry in a coagulation tank for precipitation to obtain a polyvinyl formal polymer with a molecular weight of 50,000; then obtain The obtained polyvinyl alcohol formal polymer is dissolved in dimethyl sulfoxide, the mass ratio of the polyvinyl alcohol formal polymer to dimethyl sulfoxide is 0.8:10, and a light yellow uniform transparent solution is obtained. Then, boric acid with a concentration of 0.16 mol / L is added, and the mixture is placed at 80°C for magnetic stirring for 4 hours. After uniform mixing, lithium carbonate and oxalic acid are added in sequence, and the mixture is placed at 70°C for ultrasonic mixing for 6 hours to obtain a mixed solution, wherein the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.9:0.9:1.7; finally, the obtained mixed solution is rinsed 3 times with anhydrous ethanol, and then dried at 65°C for 4 hours, and then freeze-dried in a vacuum environment cold pump for 5 hours to obtain a lithiated polyvinyl alcohol formal polymer with a molecular weight of 200,000.
[0044] Preparation of polymer composite solid electrolyte: The above-obtained lithiated polyvinyl formal polymer, lithium bis(trifluoromethanesulfonic acid) amide, polyvinylidene fluoride, porous COFs particles and lithium lanthanum zirconate particles (particle size of 500 nm) were dissolved in anhydrous acetonitrile at a mass ratio of 65:8:3:4:17, first magnetically stirred at room temperature for 2 h, and then ultrasonically dispersed at room temperature for 1.5 h to obtain a uniformly mixed slurry, which was coated on a glass plate using a scraper method with a coating thickness of 120 μm, and dried in a vacuum oven at 70°C for 26 h. After completely removing the solvent, a polymer composite solid electrolyte was obtained (the water and oxygen content in the above preparation process needs to be controlled below 10 ppm).
[0045] Example 2
[0046] Preparation of lithiated polyvinyl formal polymer: dissolve polyvinyl formal in N-methylpyrrolidone, stir magnetically for 2 hours, continue stirring at 75°C for 20 minutes, then add 4,4′-diphenylmethane diisocyanate, and continue stirring at 55°C for 2 hours to completely dissolve it, wherein the concentrations of polyvinyl formal and 4,4′-diphenylmethane diisocyanate are 4.5 mol / L and 0.05 mol / L, respectively, then add deionized water as a non-organic solvent to precipitate white particles, continue stirring until the precipitated turbid liquid becomes a transparent and viscous slurry, that is, obtain a slurry, and finally place the obtained slurry in a coagulation tank for precipitation to obtain a polyvinyl formal polymer with a molecular weight of 60,000; then obtain The obtained polyvinyl alcohol formal polymer is dissolved in dimethyl sulfoxide, the mass ratio of the polyvinyl alcohol formal polymer to dimethyl sulfoxide is 1:8, and a light yellow uniform transparent solution is obtained. Then, boric acid with a concentration of 0.3 mol / L is added, and the mixture is placed at 80°C for magnetic stirring for 4 hours. After uniform mixing, lithium carbonate and oxalic acid are added in sequence, and the mixture is placed at 70°C for ultrasonic mixing for 6 hours to obtain a mixed solution, wherein the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.8:1.5:1.5; finally, the obtained mixed solution is rinsed 4 times with anhydrous ethanol, and then dried at 70°C for 3 hours, and then freeze-dried in a vacuum environment cold pump for 3 hours to obtain a lithiated polyvinyl alcohol formal polymer with a molecular weight of 350,000.
[0047] Preparation of polymer composite solid electrolyte: The above-obtained lithiated polyvinyl alcohol formal polymer, lithium bis(trifluoromethanesulfonic acid) imide, polyvinylidene fluoride, porous COFs particles and lithium lanthanum zirconate particles (particle size of 500nm) were dissolved in anhydrous acetonitrile at a mass ratio of 50:6:2:3:12, first magnetically stirred at room temperature for 1.5h, and then ultrasonically dispersed at room temperature for 1h to obtain a uniformly mixed slurry, which was coated on a glass plate using a doctor blade method with a coating thickness of 80μm, dried in a vacuum oven at 65°C for 22h, and after completely removing the solvent, a polymer composite solid electrolyte was obtained. (The water and oxygen content in the above preparation process needs to be controlled below 10ppm).
[0048] Example 3
[0049] Preparation of lithiated polyvinyl formal polymer: dissolving polyvinyl formal in N-methylpyrrolidone, stirring magnetically for 1 hour, stirring continuously at 75°C for 60 minutes, then adding 4,4′-diphenylmethane diisocyanate, and stirring continuously at 40°C for 1.5 hours to completely dissolve it, wherein the concentrations of polyvinyl formal and 4,4′-diphenylmethane diisocyanate are 0.5 mol / L and 0.5 mol / L, respectively, then adding deionized water as a non-organic solvent to precipitate white particles, stirring continuously until the precipitated turbid liquid becomes a transparent and viscous slurry, that is, obtaining a slurry, and finally placing the obtained slurry in a coagulation tank for precipitation to obtain a polyvinyl formal polymer with a molecular weight of 70,000; then obtaining The polyvinyl alcohol formal polymer is dissolved in dimethyl sulfoxide, the mass ratio of the polyvinyl alcohol formal polymer to dimethyl sulfoxide is 0.5:12, and a light yellow uniform transparent solution is obtained. Then, boric acid with a concentration of 0.05 mol / L is added, and the mixture is placed at 80°C for magnetic stirring for 4 hours. After uniform mixing, lithium carbonate and oxalic acid are added in sequence, and the mixture is placed at 50°C for ultrasonic mixing for 8 hours to obtain a mixed solution, wherein the molar ratio of the boric acid, lithium carbonate and oxalic acid is 1.0:0.5:2.0; finally, the obtained mixed solution is rinsed 3 times with anhydrous ethanol, and then dried at 50°C for 5 hours, and then freeze-dried in a vacuum environment cold pump for 6 hours to obtain a lithiated polyvinyl alcohol formal polymer with a molecular weight of 400,000.
[0050] Preparation of polymer composite solid electrolyte: The above-obtained lithiated polyvinyl alcohol formal polymer, lithium bis(trifluoromethanesulfonic acid) imide, polyvinylidene fluoride, porous COFs particles and lithium lanthanum zirconate particles (particle size 700nm) were dissolved in anhydrous acetonitrile at a mass ratio of 70:10:5:5:25, first magnetically stirred at room temperature for 3h, and then ultrasonically dispersed at room temperature for 2h to obtain a uniformly mixed slurry, which was coated on a glass plate by a doctor blade method with a coating thickness of 130μm, dried in a vacuum oven at 80℃ for 30h, and after completely removing the solvent, a polymer composite solid electrolyte was obtained. (The water and oxygen content in the above preparation process needs to be controlled below 10ppm).
[0051] Example 4
[0052] Compared with Example 1, the difference is that the polymer composite solid electrolyte is prepared by dissolving the lithiated polyvinyl alcohol formal polymer, lithium bistrifluoromethanesulfonate imide, polyvinylidene fluoride, porous COFs particles and lithium lanthanum zirconate particles (particle size of 700nm) obtained in step 1 of Example 1 in anhydrous acetonitrile according to a mass ratio of 70:5:1:3:10, first magnetically stirring at room temperature for 1 hour, and then continuing ultrasonic dispersion at room temperature for 1 hour to obtain a uniformly mixed slurry, and coating the slurry on a glass plate by a doctor blade method with a coating thickness of 200μm, drying in a vacuum oven at 60°C for 20 hours, and completely removing the solvent to obtain a polymer composite solid electrolyte. (The water and oxygen content in the above preparation process needs to be controlled below 10ppm).
[0053] Comparative Example 1
[0054] Compared with Example 1, the difference is that non-lithiated polyvinyl formal is used in Comparative Example 1, and the other conditions are the same as those in Example 1.
[0055] Comparative Example 2
[0056] Compared with Example 1, the difference is that no lithium bis(trifluoromethanesulfonic acid) amide is added in Comparative Example 2, and the other conditions are the same as those in Example 1.
[0057] Comparative Example 3
[0058] Compared with Example 1, the difference is that no porous COFs particles are added in Comparative Example 3, and the other conditions are the same as those in Example 1.
[0059] Comparative Example 4
[0060] Compared with Example 1, the difference is that no polyvinylidene fluoride is added in Comparative Example 4, and the other conditions are the same as those in Example 1.
[0061] Comparative Example 5
[0062] Compared with Example 1, the difference is that Comparative Example 5 uses polyvinyl formal to prepare the polymer solid electrolyte, and the other conditions are the same as those of Example 1.
[0063] Comparative Example 6
[0064] Compared with Example 1, the difference is that the molecular weight of the lithiated polyvinyl formal polymer in Comparative Example 6 is 800,000, and the other conditions are the same as those in Example 1.
[0065] Comparative Example 7
[0066] Compared with Example 1, the difference is that the coating thickness in Comparative Example 7 is 200 μm, and the other conditions are the same as those in Example 1.
[0067] Various performance test evaluations
[0068] In the present application, lanthanum zirconate lithium particles (particle size of 300nm), lithium cobalt oxide and carbon black conductive agent are added to a high-energy vibration ball mill in a mass ratio of 0.8:1.7:0.09, ball-milled at room temperature for 37 minutes, and then transferred to a molybdenum-based alloy mold, and pressed into a film at 350 standard atmospheres as a composite positive electrode sheet. Then, the composite positive electrode sheet obtained as above is used as the positive electrode sheet, and the lithium indium alloy is used as the negative electrode sheet (lithium atomic percentage is 50%). The positive and negative electrodes are respectively pressed on both sides of the three-dimensional polymer composite solid electrolyte prepared in Examples 1-4 and the solid electrolyte prepared in Comparative Examples 1-7 at 35 standard atmospheres to prepare the corresponding solid full battery. Then, the AC internal resistance of the solid full battery prepared as above is tested at 30°C and 60°C respectively using AC impedance spectroscopy. The applied voltage amplitude is 5-10mV, and the frequency range is 1-10 6 HZ; in the voltage range of 2.5-4.0V, the rate discharge performance of the battery was tested; at the same time, at a temperature of 30°C and 60°C, the charge and discharge rate was 0.3C, and in the voltage range of 2.5-4.0V, the battery cycle life was tested by continuous charge and discharge cycles until the voltage short-circuited (voltage drop rate> 5mV / S). As shown in Table 1, the room temperature and high temperature electrochemical performance of the three-dimensional polymer composite solid electrolytes prepared in Examples 1-4 and the solid electrolytes prepared in Comparative Examples 1-7 were compared.
[0069] Table 1: Comparison of room-temperature and high-temperature electrochemical performance of solid electrolytes prepared in Examples 1-4 and Comparative Examples 1-7
[0070]
[0071] As shown in Table 1, combined with the data of Examples 1-4, the lithiated polyvinyl formal polymer and polymer composite solid electrolyte prepared in the present application can significantly improve the rate performance and cycle life of the polymer solid battery, among which Example 1 has the best effect. Specifically, combined with the data of Example 1 and Comparative Examples 1-5, it can be seen that the present application can significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte by utilizing the synergistic effect between the components of the lithiated polyvinyl formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate, and greatly improve the rate discharge performance and cycle life of the all-solid lithium battery. Among them, the lithiated polyvinyl alcohol formal polymer can be used as a single lithium ion conductor, and can be combined with lithium salts to form a double lithium polymer, thereby increasing the lithium source; at the same time, the added porous organic covalent material is a protonic material, and has excellent affinity with lithium ions, and because the porous organic covalent material has a high specific surface area, the addition of the porous organic covalent material can not only accelerate the further dissociation of lithium ions in the lithiated polyvinyl alcohol formal polymer, but also significantly enhance the transmission channel of lithium ions, thereby significantly reducing the interface internal resistance; in addition, the addition of polyvinylidene fluoride can effectively improve the mechanical elasticity of the polymer film layer, increase the stability of the film layer and the surface flatness during the cycle, and lithium lanthanum zirconate as an excellent lithium ion conductor can further enhance the mechanical strength and lithium ion transmission performance of the polymer solid electrolyte. Compared with pure polyvinyl alcohol formal-based solid electrolytes, the present application adopts a polymer composite solid electrolyte with a multi-component matrix, which can not only significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte, but also greatly improve the rate discharge performance and cycle life of the all-solid lithium battery.
[0072] Combining the data of Example 1 and Comparative Examples 6-7, it can be seen that limiting the molecular weight of the lithiated polyvinyl formal polymer and the thickness of the prepared polymer composite solid electrolyte membrane can greatly improve the rate discharge performance and cycle life of the all-solid lithium battery. It can be seen that the polymer composite solid electrolyte prepared by the present application can significantly improve the room temperature conductivity and mechanical elasticity of the solid electrolyte, greatly improve the rate discharge performance and cycle life of the all-solid lithium battery, and significantly improve the performance of the all-solid battery at room temperature and high temperature, providing effective technical support for the development of high-performance solid sizing.
[0073] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A polymer composite solid electrolyte, It is characterized in that It includes lithiated polyvinyl alcohol formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate, wherein the mass ratio of the lithiated polyvinyl alcohol formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate is 50-70: 5-10: 1-5: 3-5: 10-30; The raw materials of the lithiated polyvinyl formal polymer include polyvinyl formal polymer, dimethyl sulfoxide, boric acid, lithium carbonate and oxalic acid; wherein the mass ratio of the polyvinyl formal polymer to dimethyl sulfoxide is 0.5-1:8-12; the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.8-1.0:0.5-1.5:1.5-2.0; The raw materials of the polyvinyl formal polymer include polyvinyl formal and 4,4'-diphenylmethane diisocyanate, and the concentrations of the polyvinyl formal and 4,4'-diphenylmethane diisocyanate are 0.5-4.5 mol / L and 0.05-0.5 mol / L respectively.
2. The polymer composite solid electrolyte according to claim 1, It is characterized in that The molecular weight of the polyvinyl formal is 50,000-70,000, and the molecular weight of the polyvinyl formal polymer is 200,000-500,000.
3. The polymer composite solid electrolyte according to claim 1, It is characterized in that The lithium salt is selected from one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium hexafluoroborate, lithium perchlorate, lithium difluorobis(oxalatoborate), lithium triethylborohydride, lithium diisopropylamide, lithium acetoacetate, lithium bis(trimethylsilyl)lithium, lithium pentamethylcyclopentadiene, lithium 4,5-dicyano-2-trifluoromethylimidazole, lithium (fluorosulfonyl)(perfluorobutylsulfonyl)imide, and tert-butyl lithium.
4. A method for preparing a polymer composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1, dissolving lithiated polyvinyl formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate in an organic solvent, stirring and mixing, and ultrasonically dispersing to obtain a mixed slurry; S2. The mixed slurry obtained in S1 is coated on a glass plate and vacuum dried to obtain a polymer composite solid electrolyte.
5. The method for preparing the polymer composite solid electrolyte according to claim 4, It is characterized in that The mass ratio of the lithiated polyvinyl alcohol formal polymer, lithium salt, polyvinylidene fluoride, porous organic covalent material and lithium lanthanum zirconate is 50-70:5-10:1-5:3-5:10-30, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide, the organic solvent is anhydrous acetonitrile, the stirring time is 1-3 h, the ultrasonic time is 1-2 h, the drying temperature is 60-80°C, the drying time is 20-30 h, and the coating thickness is 50-200 μm.
6. The method for preparing the polymer composite solid electrolyte according to claim 4, It is characterized in that In step S1, the method for preparing the lithiated polyvinyl formal polymer comprises the following steps: a. dissolving polyvinyl formal in an organic solvent, stirring and mixing, adding 4,4′-diphenylmethane diisocyanate, continuing to stir and mix, then adding deionized water, continuing to stir and mix, obtaining a slurry, and finally precipitating the obtained slurry to obtain a polyvinyl formal polymer; b. dissolving the polyvinyl formal polymer obtained in a in an organic solvent, adding boric acid, stirring and mixing, then sequentially adding lithium carbonate and oxalic acid, ultrasonically mixing to obtain a mixed solution, and finally freeze-drying the obtained mixed solution to obtain a lithiated polyvinyl formal polymer.
7. The method for preparing the polymer composite solid electrolyte according to claim 6, It is characterized in that Step a is specifically as follows: dissolving polyvinyl formal in N-methylpyrrolidone, stirring magnetically for 1-2 hours, and then continuing to stir at a temperature of 65-85°C for 20-60 minutes, then adding 4,4′-diphenylmethane diisocyanate, and continuing to stir at a temperature of 40-55°C for 1-2 hours to completely dissolve it, wherein the concentrations of the polyvinyl formal and 4,4′-diphenylmethane diisocyanate are 0.5-4.5 mol / L and 0.05-0.5 mol / L, respectively, then adding deionized water, and continuing to stir and mix to obtain a slurry, and finally placing the obtained slurry in a coagulation tank for precipitation to obtain a polyvinyl formal polymer.
8. The method for preparing the polymer composite solid electrolyte according to claim 6, It is characterized in that Step b is as follows: dissolving the polyvinyl alcohol formal polymer obtained in step a in dimethyl sulfoxide, wherein the mass ratio of the polyvinyl alcohol formal polymer to dimethyl sulfoxide is 0.5-1:8-12, to obtain a light yellow uniform transparent solution, adding boric acid with a concentration of 0.05-0.3 mol / L, placing the solution at a temperature of 70-90°C for magnetic stirring for 3-5 h, and after uniform mixing, adding lithium carbonate and oxalic acid in sequence, placing the solution at a temperature of 50°C-90°C for ultrasonic mixing for 4-8 h, to obtain a mixed solution, wherein the molar ratio of the boric acid, lithium carbonate and oxalic acid is 0.8-1.0:0.5-1.5:1.5-2.0; finally, the obtained mixed solution is rinsed 3-4 times with anhydrous ethanol or isopropanol, placed at a temperature of 50-70°C for drying for 3-5 h, and then vacuum freeze-dried for 3-6 h to obtain a lithiated polyvinyl alcohol formal polymer.
Citation Information
Patent Citations
Polymer electrolyte and battery using it
CN101176233A
A polymer porous membrane, its preparation method, and its application in gel polymer electrolytes.
CN103804892B
All-solid-state polyelectrolyte film, its preparation and application method
CN103367799A
Porous polymer membrane, preparation method thereof and application of porous polymer membrane as gel polymer electrolyte
CN103804892A
High-strength solid electrolyte membrane
CN112768764A