A device and method for simulating liquid permeability of blast furnace charge column

By arranging coke and iron-containing minerals according to particle size gradients in the simulated blast furnace material column, and simulating reverse air flow and high pressure conditions at high temperature to react, the existing technology solves the problem of effectively simulating the liquid permeability of the internal blast furnace material column. problem, providing new evaluation indicators to ensure the stable production of blast furnaces.

CN114741859BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD +1

Patent Information

Application Number
CN202210328783.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-10-22
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively simulate the liquid permeability of the material column inside the blast furnace, especially during the reduction reaction of iron-containing minerals and coke, which affects the stable and forward production of the blast furnace.

Method used

A device and method are designed to simulate the liquid permeability of the blast furnace material column. By arranging coke and iron-containing minerals according to particle size gradient in the reaction chamber, and simulating reverse air flow and high pressure conditions at high temperature to react, the gas mixture is used. The chamber and flue gas detection devices measure changes in gas composition, calculate the liquid permeability index, and provide new evaluation indicators.

Benefits of technology

The liquid permeability and reduction characteristics of the material column inside the blast furnace were successfully simulated, which provided new technical parameters for the selection of blast furnace coke and ensured the stable production of the blast furnace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114741859B_ABST
    Figure CN114741859B_ABST
Patent Text Reader

Abstract

The present invention relates to a device and method for simulating the liquid permeability of a blast furnace charge column, comprising the following steps: 1) raw material distribution; coke and iron-containing minerals are sequentially loaded from the top into the reaction chamber of the device for simulating the liquid permeability of a blast furnace charge column, the coke is arranged from bottom to top according to the particle size gradient, and the coke particle size near the porous support pad below the reaction chamber is the smallest; or coke and iron-containing minerals are staggered and layered, and the bottom layer is the coke layer; 2) high temperature reaction; the reaction chamber is heated by a heating couple outside the reaction chamber, and gas is transported to the slag iron cooling and storage chamber; 3) liquid and gas collection and reaction analysis; 4) after cooling, the slag iron mass is weighed, and the liquid permeability index of the blast furnace charge column is calculated. The advantages are: it can simulate the actual liquid permeability of the blast furnace with iron ore and coke as the main raw materials, and under the condition of reverse airflow and simulated blast furnace internal pressure, thereby providing a new evaluation index for the selection of blast furnace coke.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ironmaking raw materials and relates to a device and a method for simulating the liquid permeability of a blast furnace material column. Background Art

[0002] The quality of metallurgical coke is crucial to the stable and smooth operation of blast furnaces. In the past, the quality evaluation of coke mainly focused on the cold and hot strength of coke, and it was believed that high-strength coke was conducive to reducing the generation of coke powder, thereby ensuring that the blast furnace column had good gas permeability and liquid permeability of molten slag. At present, the hot strength evaluation method of coke is to react for 2 hours under the reaction conditions of 1100℃ and 100% CO2 atmosphere, and then rotate it using an I-type drum to measure the mass percentage of coke with a particle size greater than 10mm in the residual slag after high-temperature reaction. However, the temperature inside the blast furnace, especially the lower column, is higher than 1100℃, and the particle size of the coke in the column gradually decreases. During the descent of the charge, the gas flow flows upstream and reacts with the column to reduce it. At the same time, the iron-containing minerals will also react directly with the coke in the column to reduce it. These reactions will affect the liquid permeability of the blast furnace column and affect the stable and smooth production of the blast furnace. Summary of the invention

[0003] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a device and method for simulating the liquid permeability of a blast furnace charge column, simulating the liquid permeability of a charge column inside a blast furnace containing iron minerals and coke as main raw materials and in the presence of a reverse airflow, thereby providing a new evaluation index for the selection of blast furnace coke.

[0004] To achieve the above object, the present invention is implemented through the following technical solutions:

[0005] A method for simulating the liquid permeability of a blast furnace charge column comprises the following steps:

[0006] 1) Raw material fabric

[0007] Coke and iron-containing minerals are sequentially loaded from the top into the reaction chamber of the device simulating the permeability of the blast furnace charge column, and the coke is arranged from bottom to top according to the particle size gradient, the coke particle size near the porous support pad at the bottom of the reaction chamber is the smallest, and the iron-containing mineral is placed above the coke with the largest particle size; or the coke and the iron-containing mineral are placed in staggered layers, the bottom layer is the coke layer, and the coke is arranged from bottom to top according to the particle size gradient, and the coke particle size near the porous support pad at the bottom of the reaction chamber is the smallest;

[0008] 2) High temperature reaction

[0009] The reaction chamber is gradually heated to 1300-1500°C by a heating couple outside the reaction chamber, and the temperature is kept constant for 0-5 hours; during the heating or constant temperature process, the gas inlet bottle is opened, and when the inlet gas is multiple gases, the different gases provided by the gas inlet bottle are mixed and pre-added by a gas mixing chamber, and then transported to the slag iron cooling and storage chamber through the gas inlet by a gas delivery pump; when the inlet gas is one gas, the gas provided by the gas inlet bottle is preheated by a gas mixing chamber, and then the gas is transported to the slag iron cooling and storage chamber through the gas inlet by a gas delivery pump;

[0010] 3) Liquid and gas collection and reaction analysis

[0011] The iron-containing mineral melted at high temperature reacts with coke at the interface during the dripping process, and then drips through the coke layer into the slag crucible. At the same time, the gas in the slag cooling and storage chamber passes through the porous support pad, carrying the gas generated by the reaction of the iron-containing mineral and the coke into the flue gas detection device through the exhaust port, or the gas in the slag cooling and storage chamber passes through the porous support pad and directly reacts with the iron-containing mineral, and the tail gas after the reaction enters the flue gas detection device through the exhaust port; the gas composition change curve is measured by the flue gas detection device, and finally enters the tail gas collection and treatment device, and the CO gas emission amount and emission rate can reflect the reducibility and reduction rate of the iron-containing mineral;

[0012] By controlling the inlet flow rate of the gas inlet bottle and the exhaust flow rate of the tail gas outlet, the pressure inside the device is stable and controllable, and the furnace top pressure inside the device is controlled at 100kPa~500kPa, thereby simulating the air and liquid permeability of the material column under the pressure conditions inside the blast furnace;

[0013] 4) After the slag and the storage cavity are cooled, weigh the mass of the slag in the slag crucible and calculate the liquid permeability index r of the blast furnace charge column:

[0014] Among them, m 液滴 is the mass of slag iron in the slag iron crucible, g; m 铁矿 Is the iron mineral content of the raw material, g.

[0015] The iron-containing mineral is one or a mixture of sintered ore, pelletized ore and iron ore.

[0016] The gas in the gas mixing chamber is one or more of N2, CO2, CO, H2, H2O, and the gas flow rate is controlled at 0.5-5 L / min.

[0017] A device for simulating the liquid permeability of a blast furnace material column, comprising a reaction chamber, a porous support pad, a slag iron cooling and storage chamber, a slag iron crucible, a support base, an air inlet, a gas delivery pump, a gas mixing chamber, an air inlet bottle, a smoke detection device, an exhaust gas collection and treatment device, and an exhaust port;

[0018] The reaction chamber is heated by a peripheral heating couple, the bottom of the reaction chamber is connected to the slag iron cooling and storage chamber, the lower part of the reaction chamber is fixedly connected to a porous support pad, and the reaction chamber is filled with iron-containing minerals and coke from top to bottom; a slag iron crucible is arranged in the slag iron cooling and storage chamber, the bottom of the slag iron cooling and storage chamber is fixedly connected to a support base, and a slag iron crucible is fixedly connected to the support base; the slag iron crucible is used to hold the drippings of the molten slag iron after passing through the coke layer under high temperature conditions;

[0019] The mixing chamber is connected to the gas inlet bottle, and the gas in the mixing chamber is transported from the air inlet to the slag cooling and storage chamber through the gas delivery pump, and is discharged from the exhaust port on the top of the reaction chamber. The smoke detection device is connected to the exhaust port, and the smoke detection device is connected to the exhaust gas collection and treatment device.

[0020] The connection between the reaction chamber and the slag iron cooling and storage chamber is a nested structure or a spiral structure.

[0021] The inner wall of the reaction chamber is made of heat-insulating refractory material.

[0022] The bottom of the slag iron cooling and storage chamber is provided with symmetrically distributed air inlets, which are one pair or more pairs.

[0023] A thermal resistor is arranged in the gas mixing chamber, and the heating temperature of the gas mixing chamber is between 25 and 300°C.

[0024] The smoke detection device is used to detect the smoke components discharged from the exhaust port at the top of the reaction chamber and the furnace top gas pressure.

[0025] The porous support pad is made of high temperature resistant graphite or corundum.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention can simulate the liquid permeability of the actual material column inside a blast furnace with iron ore and coke as main raw materials, under the condition of reverse airflow and simulated internal pressure of the blast furnace, thereby providing a new evaluation index for the selection of blast furnace coke, providing a technical parameter basis for guiding the selection of blast furnace raw materials and production operations, and ensuring the liquid permeability and reduction characteristics of the blast furnace material column. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a structural schematic diagram of the present invention.

[0029] Figure 2 This is the CO concentration emission curve of Example 1.

[0030] Figure 3 This is the CO concentration emission curve of Example 2.

[0031] Figure 4This is the CO concentration emission curve of Example 3.

[0032] In the figure: 1-reaction chamber 2-iron-containing minerals 3-coke 4-insulating refractory materials 5-porous support pads 6-slag cooling and storage chamber 7-slag crucible 8-support base 9-air inlet 10-gas delivery pump 11-gas mixing chamber 12-gas inlet bottle 13-smoke detection device 14-exhaust collection and treatment device 15-exhaust port. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.

[0034] See Figure 1 , a device for simulating the liquid permeability of a blast furnace charge column, comprising a reaction chamber 1, a porous support pad 5, a slag iron cooling storage chamber 6, a slag iron crucible 7, a support base 8, an air inlet 9, a gas delivery pump 10, a gas mixing chamber 11, an air inlet bottle 12, a smoke detection device 13, an exhaust gas collection and treatment device 14, and an exhaust port 15;

[0035] The reaction chamber 1 is heated to a high temperature by a peripheral heating couple, the bottom of the reaction chamber 1 is connected to the slag iron cooling storage chamber 6, the reaction chamber 1 and the slag iron cooling storage chamber 6 are detachable, a porous support pad 5 is fixedly installed at the lower part of the reaction chamber 1, and the reaction chamber 1 is filled with iron-containing minerals 2 and coke 3 from top to bottom; a slag iron crucible 7 is arranged in the slag iron cooling storage chamber 6, a support base 8 is fixedly connected to the bottom of the slag iron cooling storage chamber 6, and the slag iron crucible 7 is fixed on the support base 8; the slag iron crucible 7 is used to hold the slag iron dripping after the molten slag iron passes through the coke layer under high temperature conditions;

[0036] The mixing chamber 11 is connected to the gas inlet bottle 12. The gas in the mixing chamber 11 is transported from the air inlet to the slag cooling storage chamber 6 through the gas delivery pump 10, and is discharged from the exhaust port 15 at the top of the reaction chamber 1. The smoke detection device 13 is connected to the exhaust port 15. The smoke detection device 13 is connected to the exhaust port 15. The smoke detection device 13 is connected to the exhaust gas collection and treatment device 14. The smoke detection device 14 can also measure the pressure of the furnace top exhaust port, and then simulate the high-pressure reaction conditions of the blast furnace by controlling the stable furnace top pressure.

[0037] The lower edge of the reaction chamber 1 and the connection with the slag cooling storage chamber 6 are nested structures or spiral structures, thereby ensuring that the reaction chamber 1 and the slag cooling storage chamber 6 are detachable and sealed after connection. The inner side wall of the reaction chamber 1 is composed of a heat-insulating refractory material 4. To ensure that the liquid slag dripping in the reaction chamber 1 does not stick to the inner wall of the reaction chamber 1, the bottom 6 of the slag cooling storage chamber is provided with symmetrically distributed air inlets 9, which can be one pair or more pairs to ensure the stability and uniformity of the rising airflow in the reaction chamber 1. The mixing chamber 11 also has a preheating function for the gas, mainly through resistance heating in the mixing chamber, and the heating temperature is 25 to 300 ° C. On the one hand, it can ensure the uniformity of the mixing of multiple gases, and on the other hand, it ensures that the incoming gases are all in gaseous state, which is consistent with the internal state of the blast furnace. When CO2 is contained in the gas, the porous support pad uses a high-temperature resistant corundum material, and when CO2 is not contained in the gas, the porous support pad uses a high-temperature resistant graphite material. Prevent CO2 from carbonizing with the graphite pad under high temperature conditions.

[0038] A method for simulating the liquid permeability of a blast furnace charge column comprises the following steps:

[0039] 1) Raw material fabric

[0040] Coke 3 and iron-containing mineral 2 are sequentially loaded from the top into the reaction chamber 1 of the device simulating the permeability of the blast furnace charge column, and the coke 3 is arranged from bottom to top according to the particle size gradient, and the particle size of the coke 3 near the porous support pad 5 below the reaction chamber 1 is the smallest, and the iron-containing mineral 2 is placed above the coke 3 with the largest particle size; or the coke 3 and the iron-containing mineral 2 are placed in layers, and the bottom layer is the coke layer, and the coke 3 is arranged from bottom to top according to the particle size gradient, and the particle size of the coke near the porous support pad 5 below the reaction chamber 1 is the smallest. The iron-containing mineral 2 is one or a mixture of sintered ore, pelletized ore, and iron-containing lump ore.

[0041] 2) High temperature reaction

[0042] The reaction chamber 1 is gradually heated to 1300-1500°C by a heating couple on the periphery of the reaction chamber 1, and the temperature is kept constant for 0-5h; during the heating or constant temperature process, the gas inlet bottle 12 is opened, and when the intake gas is a variety of gases, the different gases provided by the gas inlet bottle 12 are mixed and preheated to 25-300°C by the mixing chamber 11, and then the gas delivery pump 10 delivers the mixed gas to the slag iron cooling storage chamber 6 through the air inlet 9; when the intake gas is one gas, the gas provided by the gas inlet bottle 12 is preheated to 25-300°C by the mixing chamber 11, and then the gas delivery pump 10 delivers the gas to the slag iron cooling storage chamber 6 through the air inlet 9; the gas in the mixing chamber 11 is one or more of N2, CO2, CO, H2, and H2O, and the gas flow rate is controlled at 0.5-5L / min.

[0043] 3) Liquid and gas collection and reaction analysis

[0044] The molten iron-containing mineral 2 at high temperature reacts with the coke 3 at the interface during the dripping process, and then drips into the slag crucible 7 through the coke layer. At the same time, the gas in the slag cooling and storage chamber 6 passes through the porous support pad 5, and carries the gas generated by the reaction of the iron-containing mineral 2 and the coke 3 into the flue gas detection device 13 through the exhaust port 15, or the gas in the slag cooling and storage chamber 6 passes through the porous support pad 5 and directly reacts with the iron-containing mineral 2, and the tail gas after the reaction enters the flue gas detection device 13 through the exhaust port 15; the gas composition change curve is measured by the flue gas detection device 13, and finally enters the tail gas collection and treatment device 14, and the CO gas emission amount and emission rate can reflect the reducibility and reduction rate of the iron-containing mineral 2; by controlling the intake flow rate of the gas inlet bottle 12 and the exhaust flow rate of the tail gas exhaust port 15, the pressure in the device is stable and controllable, and the furnace top pressure in the device can be controlled at 100KPa~500KPa, thereby simulating the air permeability and liquid permeability of the material column under the pressure conditions in the blast furnace;

[0045] 4) Liquid permeability index calculation

[0046] After the slag and the storage chamber are cooled, weigh the mass of the slag in the slag crucible and calculate the liquid permeability index r of the blast furnace charge column:

[0047] Among them, m 液滴 is the mass of slag iron in the slag iron crucible, g; m 铁矿 Is the iron mineral content of the raw material, g.

[0048] Embodiment 1:

[0049] See Figure 1 , a device and method for simulating the liquid permeability of a blast furnace column, simulating the reduction of an iron-containing mineral 2 in a coke 3 column and detecting the liquid phase flow characteristics, specifically comprising the following steps:

[0050] 1) Raw material loading

[0051] 350g of coke with particle sizes of 10-15mm, 350g of coke with particle sizes of 15-20mm, 20g of 10-15mm pellets and 20g of 10-15mm sintered ore are sequentially loaded into the reaction chamber 1 from the top, with the 10-15mm coke placed on the porous corundum pad 5, the 15-20mm coke placed above the 10-15mm coke, and the pellets and sintered ore placed above the 10-15mm coke.

[0052] 2) High temperature reaction

[0053] The reaction chamber 1 is gradually heated to 1350°C and kept at a constant temperature for 5 hours. During the heating process, the gas inlet bottle 12 is opened, and the gas delivered during the heating is N2, which is preheated to 200°C in the gas mixing chamber 11, and the mixed gas is delivered from the gas inlet 9 to the slag cooling storage chamber 6 through the gas delivery pump 10. When the temperature rises to 1350°C, the delivered gas is a mixed gas of N2 and CO, which is mixed and preheated to 200°C in the gas mixing chamber 11. The mixed volume ratio of N2 to CO is 9:1, and the furnace top pressure is controlled at 200KPa. The gas flow rate during the entire heating process is 0.5L / min.

[0054] 3) Liquid and gas collection and reaction analysis

[0055] After the pellets react with the coke 3 under high temperature conditions, molten liquid slag iron is formed and drips through the coke 3 layer into the slag iron crucible 7. The tail gas after the reaction is transported to the smoke detection device 13 through the exhaust port 15, and then the gas composition change curve is measured by the smoke detection device 13, see Figure 2 The total amount of CO in the tail gas is obtained by curve integration, and the amount of CO entering the air inlet is removed. The remaining is the CO generated during the high-temperature direct reduction process, and the pellet reduction rate is then obtained. From the figure, it can also be known that the most intense reaction time corresponding to different reaction materials, and then the corresponding reaction temperature is obtained. Finally, the tail gas enters the tail gas collection and treatment device 14.

[0056] 4) Liquid permeability index calculation

[0057] After cooling, the mass of slag in the slag crucible is weighed, and the proportion of liquid slag to iron-containing minerals in the raw materials is calculated to be 50%. At this time, the liquid permeability index of the blast furnace charge column is 50%.

[0058] Example 2

[0059] A method for simulating the liquid permeability of a blast furnace charge column comprises the following steps:

[0060] 1) Raw material loading

[0061] 350g of 10-15mm coke, 350g of 15-20mm coke and 40g of 10-12mm sintered ore are loaded into the reaction chamber 1 in layers from bottom to top, namely 350g of 10-15mm coke, 20g of 10-12mm sintered ore, 350g of 15-20mm coke and 20g of 10-12mm sintered ore.

[0062] 2) High temperature reaction

[0063] Gradually heat to 1500℃ and keep constant temperature for 2h. During the heating and constant temperature process, the conveying gas is N2, the gas inlet bottle 12 is opened, the gas mixing chamber 11 is preheated to 300℃, and the mixed gas is conveyed from the gas inlet 9 to the slag iron cooling storage chamber 6 through the gas delivery pump 10. During the whole heating and constant temperature process, the furnace top pressure is controlled at 200KPa, and the gas flow rate is 1.0L / min.

[0064] 3) Liquid and gas collection and reaction analysis

[0065] After the sintered ore reacts with the coke 3 under high temperature conditions, molten liquid slag iron is formed and drips through the coke 3 layer into the slag iron crucible 7. The tail gas after the reaction enters the flue gas detection device 13 through the exhaust port 15. The flue gas detection device 13 measures the gas composition change curve, see Figure 3 The total amount of CO in the tail gas is obtained by curve integration, which is the amount of CO produced by the high-temperature reduction reaction of iron-containing minerals and coke. From the figure, we can also know the most intense reaction time of different reaction materials, and then the corresponding reaction temperature is obtained. Finally, the tail gas enters the tail gas collection and treatment device 14.

[0066] 4) Liquid permeability index calculation

[0067] After cooling, the mass of the slag in the slag crucible is weighed, and the proportion of the liquid slag to the raw material sintered ore is calculated to be 30%. At this time, the liquid permeability index of the blast furnace charge column is 30%.

[0068] Example 3

[0069] A method for simulating the liquid permeability of a blast furnace charge column comprises the following steps:

[0070] 1) Raw material loading

[0071] 200g of 5-10mm coke, 200g of 10-20mm coke, 200g of 20-22mm coke and 40g of 10-12mm sintered ore are sequentially loaded into the reaction chamber 1 from the top, with the 5-10mm coke placed on the porous corundum pad 5, the 10-20mm coke placed above the 5-10mm coke, the 20-22mm coke placed above the 10-20mm coke, and the sintered ore on the top.

[0072] 2) High temperature reaction

[0073] Gradually heat up to 1300℃ and keep the temperature constant for 2h. During the heating process, open the gas inlet bottle 12, and after the mixing chamber is preheated to 100℃, the mixed gas is transported from the gas inlet 9 to the slag iron cooling storage chamber 6 through the gas delivery pump 10. During the heating process from 0 to 1300℃, 1.0L / min N2 is delivered. When the temperature rises to the 1300℃ constant temperature section, the delivery gas is 0.5L / min CO2+4.5L / min N2. After being mixed and preheated to 300℃ in the mixing chamber, it is delivered from the gas inlet 9 to the slag iron cooling storage chamber 6. During the entire constant temperature process, the furnace top pressure is controlled at 500KPa and the gas flow rate is 5L / min.

[0074] 3) Liquid and gas collection and reaction analysis

[0075] After the sintered ore reacts with the coke 3 under high temperature conditions, molten liquid slag iron is formed and drips through the coke 3 layer into the slag iron crucible 7. The tail gas after the reaction enters the flue gas detection device 13 through the exhaust port 15. The flue gas detection device 13 measures the gas composition change curve, see Figure 4 The total amount of CO in the tail gas is obtained by curve integration, which is the amount of CO produced by the high-temperature reduction reaction of iron-containing minerals and coke and the gasification reaction of coke. The amount of CO produced is obtained by comparative tests without sintered ore and other reaction conditions are the same. The amount of CO produced by the high-temperature reduction reaction of iron-containing minerals and coke is calculated, and the reduction rate of sintered ore is calculated. Figure 4 It is also possible to know the most intense reaction time of different reaction materials, and then obtain the corresponding reaction temperature, and finally the tail gas enters the tail gas collection and treatment device 14.

[0076] 4) Liquid permeability index calculation

[0077] After cooling, the mass of the slag in the slag crucible is weighed, and the proportion of the liquid slag to the raw material sintered ore is calculated to be 30%. At this time, the liquid permeability index of the blast furnace charge column is 30%.

Claims

1. A method for simulating the liquid permeability of a blast furnace charge column, characterized in that: The following steps are involved: 1) Raw material fabric Coke and iron-containing minerals are sequentially loaded from the top into the reaction chamber of the device simulating the permeability of the blast furnace charge column, and the coke is arranged from bottom to top according to the particle size gradient, the coke particle size near the porous support pad at the bottom of the reaction chamber is the smallest, and the iron-containing mineral is placed above the coke with the largest particle size; or the coke and the iron-containing mineral are placed in staggered layers, the bottom layer is the coke layer, and the coke is arranged from bottom to top according to the particle size gradient, and the coke particle size near the porous support pad at the bottom of the reaction chamber is the smallest; 2) High temperature reaction The reaction chamber is gradually heated to 1300-1500°C by a heating couple outside the reaction chamber, and the temperature is kept constant for 0-5 hours; during the heating or constant temperature process, the gas inlet bottle is opened, and when the inlet gas is a plurality of gases, the different gases provided by the gas inlet bottle are mixed and preheated by a gas mixing chamber, and then transported to the slag iron cooling and storage chamber through the gas inlet by a gas delivery pump; when the inlet gas is a single gas, the gas provided by the gas inlet bottle is preheated by a gas mixing chamber, and then transported to the slag iron cooling and storage chamber through the gas inlet by a gas delivery pump; 3) Liquid and gas collection and reaction analysis The iron-containing mineral melted at high temperature reacts with coke at the interface during the dripping process, and then drips through the coke layer into the slag crucible. At the same time, the gas in the slag cooling and storage chamber passes through the porous support pad, carrying the gas generated by the reaction of the iron-containing mineral and the coke into the flue gas detection device through the exhaust port, or the gas in the slag cooling and storage chamber passes through the porous support pad and directly reacts with the iron-containing mineral, and the tail gas after the reaction enters the flue gas detection device through the exhaust port; the gas composition change curve is measured by the flue gas detection device, and finally enters the tail gas collection and treatment device, and the CO gas emission amount and emission rate can reflect the reducibility and reduction rate of the iron-containing mineral; By controlling the inlet flow rate of the gas inlet bottle and the exhaust flow rate of the tail gas outlet, the pressure inside the device is stable and controllable, and the furnace top pressure inside the device is controlled at 100kPa~500kPa, thereby simulating the air and liquid permeability of the material column under the pressure conditions inside the blast furnace; 4) After the slag and storage chamber have cooled, weigh the mass of the slag in the slag crucible and calculate the liquid permeability index of the blast furnace charge column. r : ,in, m 液滴 is the mass of slag iron in the slag iron crucible, g; m 铁矿 Is the iron mineral mass of the raw material, g.

2. A method for simulating the liquid permeability of a blast furnace charge column according to claim 1, characterized in that: The iron-containing mineral is one or a mixture of sintered ore, pelletized ore and iron ore.

3. The method for simulating the liquid permeability of a blast furnace charge column according to claim 1, characterized in that: The gas in the gas mixing chamber is one or more of N2, CO2, CO, H2, H2O, and the gas flow rate is controlled at 0.5~5L / min.

4. A device for simulating the liquid permeability of a blast furnace charge column to implement the method of claim 1, characterized in that: It includes a reaction chamber, a porous support pad, a slag iron cooling and storage chamber, a slag iron crucible, a support base, an air inlet, a gas delivery pump, a gas mixing chamber, an air inlet bottle, a smoke detection device, an exhaust gas collection and treatment device, and an exhaust port; The reaction chamber is heated by a peripheral heating couple, the bottom of the reaction chamber is connected to the slag iron cooling and storage chamber, the lower part of the reaction chamber is fixedly connected to a porous support pad, and the reaction chamber is filled with iron-containing minerals and coke from top to bottom; a slag iron crucible is arranged in the slag iron cooling and storage chamber, the bottom of the slag iron cooling and storage chamber is fixedly connected to a support base, and a slag iron crucible is fixedly connected to the support base; the slag iron crucible is used to hold the drippings of the molten slag iron after passing through the coke layer under high temperature conditions; The mixing chamber is connected to the gas inlet bottle, and the gas in the mixing chamber is transported from the air inlet to the slag cooling and storage chamber through the gas delivery pump, and is discharged from the exhaust port on the top of the reaction chamber. The smoke detection device is connected to the exhaust port, and the smoke detection device is connected to the exhaust gas collection and treatment device.

5. The device for simulating the liquid permeability of a blast furnace charge column according to claim 4, characterized in that: The connection between the reaction chamber and the slag iron cooling and storage chamber is a nested structure or a spiral structure.

6. The device for simulating the liquid permeability of a blast furnace charge column according to claim 4, characterized in that: The inner wall of the reaction chamber is made of heat-insulating refractory material.

7. The device for simulating the liquid permeability of a blast furnace charge column according to claim 4, characterized in that: The bottom of the slag iron cooling and storage chamber is provided with symmetrically distributed air inlets, which are one pair or more pairs.

8. The device for simulating the liquid permeability of a blast furnace charge column according to claim 4, characterized in that: A thermal resistor is arranged in the gas mixing chamber, and the heating temperature of the gas mixing chamber is between 25 and 300°C.

9. The device for simulating the liquid permeability of a blast furnace charge column according to claim 4, characterized in that: The smoke detection device is used to detect the smoke components discharged from the exhaust port at the top of the reaction chamber and the gas pressure at the furnace top.

10. The device for simulating the liquid permeability of a blast furnace charge column according to claim 4, characterized in that: The porous support pad is made of high temperature resistant graphite or corundum.

Citation Information

Patent Citations

  • Method for testing and evaluating influence of ore reduction in blast furnace on air permeability of stock column

    CN102410966A

  • Method for judging liquid permeability of lower part of blast furnace

    CN104805240A

  • Apparatus for simulating reaction of coke in blast furnace, and method thereof

    CN106053758A

  • Method and device for evaluating liquid permeability of blast furnace stock column

    CN107643242A

  • Device and method for simulating blast furnace high-temperature section coke reaction

    CN111638316A

Cited By

  • Method for preparing industrial pure iron through green low-carbon smelting reduction

    CN119956012A