A composite environmentally friendly catalyst for polyester resin synthesis and its preparation method and application
By using a composite catalyst of stannous hydroxide and stannous oxalate in the synthesis of polyester resin, the problem of the formation of blooming substances in polyester resin is solved, low-temperature curing and no-blooming performance are achieved, and the cost and process complexity are reduced. , improving the curing efficiency.
Patent Information
- Application Number
- CN202210609692.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-05-31
AI Technical Summary
Polyester resin easily forms blooming substances in powder coatings, causing frost-like substances to precipitate on the surface of the coating, affecting the decorative and mechanical properties. At the same time, the cost is high and the process is complicated under high-temperature curing conditions, and the curing accelerator is in the polyester resin. Uneven dispersion affects curing activity.
A composite environmentally friendly catalyst of stannous hydroxide and stannous oxalate is used. By synthesizing the catalyst and using it in the polyester resin synthesis process, the formation of blooming substances is avoided, and it also functions as a curing accelerator, reducing the viscosity of the polyester resin. Cost and process complexity.
It achieves low-temperature curing of polyester resin with no blooming performance, maintains the transparency and mechanical properties of the coating, reduces the cost of polyester resin, simplifies the process flow, and improves curing efficiency.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester resin synthesis and polyester resin application, and in particular to a composite environmentally friendly catalyst suitable for polyester resin synthesis and a preparation method and application thereof. Background Art
[0002] Powder coating is a solvent-free solid coating with no VOC emissions during use, making it one of the ideal environmentally friendly coatings. Powder coating requires high-temperature baking for melting, leveling and curing to form a film, especially in the engineering machinery coating industry. The mechanical parts are heavy, and the substrate and coating absorb a lot of heat during curing. The workpiece stores heat after leaving the drying oven, and the residual heat is released slowly. A layer of powdery frost will precipitate on the surface of the powder coating, reducing the gloss of the coating and affecting the decorative performance, processing performance and mechanical properties of the coating. The white frost substance is a ring-forming product of two terephthalic acids and two neopentyl glycols. The product has no reactive groups and exists in a free form in the coating. The molecular weight is 468.18. It migrates to the coating surface under the action of heat. When the temperature is greater than 120°C, the white frost migrates from the coating to the coating surface. When the temperature is greater than 160°C, the white frost desorbs from the coating surface.
[0003] To solve the problem of frosting of powder coating, there are two ways: first, there is no frosting substance; second, there is frosting substance, but the frosting substance cannot precipitate, volatilize, or sublimate out of the coating. Polyester resin is mainly based on raw materials PTA (terephthalic acid) and NPG (neopentyl glycol). PTA and NPG are important raw materials for polyester synthesis. In order to reduce the cost of powder coating formulation, it is almost inevitable to use a large amount of PTA and NPG, because NPG is the main polyol to ensure wetting and weather resistance, and PTA is the main polyacid to ensure Tg, cost, and flexibility. Therefore, it is inevitable to use a large amount of PTA and NPG in the production of polyester resin. Frosting substances will be produced under the usual catalytic system. The para-structure of PTA is easy for NPG to form C22 cyclic compounds. The C22 cyclic substances remain in polyester, which will reduce the melt viscosity of polyester and plasticize the powder coating. During the UV aging process, the C22 cyclic substances migrate to the surface of the coating, increase the cavities and water absorption rate of the powder coating, and accelerate the hydrolysis of the powder coating. In order to reduce the content of frosting substances, there are generally two ways: 1. Reduce the amount of NPG added to the polyester resin, which reduces weather resistance; 2. Use high weather resistance polyester with low or no PTA, but the cost of polyester resin is high; mixing the above two polyesters can reduce the requirements for frosting substances, but it is cumbersome to use and requires readjustment and verification of various indicators of powder coatings and coatings.
[0004] The synthesis process of polyester resin is generally divided into three stages. The first stage is esterification reaction to produce hydroxyl-terminated polyester resin, wherein the stirring rate (150±50r / min), heating method (programmed heating), heating rate (5-15 / ℃h) and the first stage endpoint control (acid value 10-15mgKOH / g; the second stage is to add alcoholysis agent, the reaction temperature is 245-255℃ until the product is clear and transparent, and the acid value is controlled at 40-45mgKOH / g at the end point; the third stage is vacuum polycondensation, the reaction temperature is 220-230℃, time 2-3h, vacuum degree -0.095-0.098Mpa, acid value 32-38mgKOH / g, Tg≥60℃, softening point 100-120℃, melt viscosity 5000-7000mPa.s / 200℃, then add antioxidants and other additives, stir and disperse evenly, cool and discharge. At present, there are two main problems with anti-blooming polyester resin: one is that the cost is greatly increased after optimizing the polyester formula, and the other is that the coating construction process has high requirements and cumbersome operation.
[0005] In order to meet the reaction activity of powder coatings and meet the baking and curing conditions, it is necessary to add a curing accelerator so that the coating performance meets the index requirements. Adding a curing accelerator reduces the curing temperature and shortens the curing time, reduces energy consumption, improves efficiency, and expands the application range of powder coatings, expanding the application in areas where the substrate is not heat-resistant, such as the wooden furniture industry. The curing accelerator can be added during the powder making process or in the polyester resin. Due to the small amount added, it is difficult to disperse evenly when added during the powder making process. If the local concentration is too high, gel is easily generated, forming defects on the coating surface. If added to the synthetic polyester resin, the viscosity of the polyester resin is relatively small at this time, and the curing accelerator is easy to disperse evenly. There are the following problems when adding in the late stage of polyester resin synthesis: (1) The viscosity of the polyester resin in the late stage is very high, and a small amount of curing accelerator is not mixed evenly, resulting in large differences in the curing activity of the same batch of polyester resins; (2) Generally, curing accelerators are small molecular compounds, which are easy to absorb water and lose activity.
[0006] At present, the field of powder coatings mainly focuses on meeting the performance requirements of conventional powder coatings, such as good fluidity, impact resistance and mechanical properties. In order to improve the anti-blooming performance of powder coatings, the coatings industry has solved the problem from the aspects of polyester resin formula, powder coating formula and coating construction technology, such as selecting polyester resins specially used for anti-blooming; adjusting the reactivity and cross-linking density of powder coatings, rapidly cooling the workpiece after leaving the drying oven, and reducing the residence time of the workpiece at 120-150℃. The invention patent application with publication number CN 102365321 A discloses a composition of a thermosetting powder coating comprising a crosslinking agent and a polyester, and solves the problem of frosting to frost-free of the powder coating by adjusting the polyester resin formula and selecting the crosslinking agent. However, the raw material prices of the acid and alcohol selected for preparing the polyester resin are generally higher than those of the conventional polyester, resulting in an increase in the cost of the polyester resin, and secondly, the process needs to be changed; the invention patent applications with publication numbers CN 103755934 A, CN 105254860 A, CN 1072266666A, CN 110511365A, CN 111533892A, and CN 11621007A reduce or eliminate the frosting phenomenon by optimizing the polyester formula, but the above-mentioned problems still exist; the invention patent application with publication number CN 104109452A optimizes the powder coating formula, i.e., adds a mica additive to enhance the coating performance, such as the adhesion between the coating and the substrate, the strength and mechanical properties of the coating, but the powder coating preparation process needs to be adjusted to adapt to the powder coating and increase the cost of the powder coating. At present, there are two main problems with anti-blooming polyester resins: one is that the cost is greatly increased after optimizing the polyester formula, and the other is that the coating construction process has high requirements and cumbersome operations. Therefore, how to select a suitable catalyst to prepare polyester resins without blooming substances without adjusting or optimizing the current polyester resin formula process, powder coating formula process and coating construction process has become a problem that needs to be solved. Summary of the invention
[0007] Purpose of the invention: In order to solve the technical problem of preparing polyester resin without white frost substances, the present invention provides a preparation method of a composite environmentally friendly catalyst and its application. The composite environmentally friendly catalyst is easy to prepare and does not require adjustment of the polyester resin formula and process in the production of polyester resin. The prepared polyester resin does not contain frosting substances and meets the application fields of low-temperature curing and no frosting. At the same time, experiments have found that the composite environmentally friendly catalyst also has the function of a curing accelerator.
[0008] In order to solve the above technical problems, the present invention discloses a composite environmentally friendly catalyst for polyester resin synthesis, wherein the catalyst comprises stannous hydroxide and stannous oxalate.
[0009] Preferably, the mass ratio of stannous hydroxide to stannous oxalate is 9:1 to 5:5.
[0010] The present invention further provides a method for preparing the above-mentioned composite environmentally friendly catalyst, comprising the following steps:
[0011] (1) Synthesis of stannous hydroxide: weigh tin dichloride dihydrate and add a small amount of water to prepare an aqueous solution of tin dichloride dihydrate; weigh an appropriate amount of ammonia solution; add the ammonia solution dropwise to the prepared aqueous solution of tin dichloride dihydrate, preferably, no obvious lumps are formed during the dropwise addition process, the reaction temperature is controlled below 50-80° C., the pH value at the reaction end point is controlled between 6-8, the temperature is kept at 50-80° C. for 3 hours, the upper water layer is removed, the product is dehydrated at 100-110° C. under negative pressure, filtered, and dried to obtain stannous hydroxide. The purity of the final product obtained by the above method is above 98%;
[0012] (2) Synthesis of stannous oxalate: weigh tin dichloride dihydrate and add a small amount of water to prepare an aqueous solution of tin dichloride dihydrate, weigh an appropriate amount of sodium oxalate and add water to prepare an aqueous solution of sodium oxalate, add the aqueous solution of tin dichloride dropwise to the aqueous solution of sodium oxalate at a molar ratio of sodium oxalate to tin dichloride of 1.1-1.3:1, control the reaction temperature to be below 40-60°C, react at 40-60°C for 1-2h after the addition is completed, filter, wash, and dry to obtain the product stannous oxalate, and the purity of the final product is above 99%;
[0013] (3) The stannous hydroxide obtained in step (1) and the stannous oxalate obtained in step (2) are mixed according to a formula amount to obtain a composite environmentally friendly catalyst.
[0014] Wherein, in step (1), the concentration of the aqueous solution of tin dichloride dihydrate is 60-80wt%, and the concentration of the aqueous ammonia solution is 10-20wt%.
[0015] In step (2), the concentration of the aqueous solution of tin dichloride dihydrate is 30%-50wt%, and the concentration of the aqueous solution of sodium oxalate is 30-50wt%.
[0016] The present invention further proposes the use of the above-mentioned composite environmentally friendly catalyst for polyester resin synthesis in the preparation of polyester resin.
[0017] Specifically, the polyester resin preparation process is as follows: add polyols, polyacids and composite environmentally friendly catalysts into the reactor according to the ratio, slowly heat up to 240-255°C and maintain, take samples for analysis, when the acid value is 5-10 mgKOH / g, cool to 210-230°C, add acid for acid blocking, when the acid value of the polyester resin is 40-45 mgKOH / g, cool to 210°C for vacuum condensation, when the acid value of the polyester resin is 32-38 mgKOH / g, cool to 180°C, add additives, stir for 1 hour and then discharge.
[0018] The polyacid is any one of TA, IPA, AA and SA; the polyol is any one of EG, DEG and 1,2-PG. Taking into account the cost, Tg, flexibility, weather resistance and other indicators, PTA and NPG are preferred as the main raw materials for polyester resin synthesis.
[0019] The present invention further proposes the use of the polyester resin prepared above in preparing powder coatings.
[0020] Specifically, the process comprises the following steps: preparing the powder coating according to the formula, premixing, extruding, tableting, crushing and screening, spraying the prepared powder coating onto the sample plate by electrostatic spraying, and then baking and curing the sample plate in an oven at 200°C for 10 minutes to obtain the coating.
[0021] Beneficial effects: Compared with the prior art, the stannous hydroxide in the environmentally friendly composite catalyst provided by the present invention has higher catalytic activity, the synthetic polyester has high transparency, and has the function of a curing accelerator; stannous oxalate also has higher catalytic activity, and the synthetic polyester is slightly turbid; stannous oxalate and stannous hydroxide do not support the occurrence of cyclization reaction, thus avoiding the formation of frosting substance C22 cyclic compounds, and stannous oxalate has higher cost performance than stannous hydroxide. By adjusting the appropriate ratio of stannous oxalate and stannous hydroxide, the amount of stannous oxalate can be increased as much as possible under the premise that the polyester resin is clear and transparent, so that the composite catalyst has higher cost performance. DETAILED DESCRIPTION
[0022] The present invention is described in detail below through specific embodiments.
[0023] Through the study of a large number of catalytic mechanisms, the synthesis of tin compounds and practical proof, it is found that the catalysts used in the preparation of polyester resins without white frost need to meet several conditions:
[0024] (1) The prepared catalyst is thermally stable, resistant to hydrolysis, non-corrosive, non-toxic, does not need to be separated after the reaction, and does not affect the quality of the final product;
[0025] (2) In the process of preparing polyester resin, the product has high catalytic activity, gentle reaction process, low degradation reaction and low adhesion; the product quality of polyester resin has no blooming substances, low discoloration and high transparency.
[0026] Through a large number of experiments, it was found that a mixture of stannous hydroxide and stannous oxalate meets the above conditions and can be used in the preparation of polyester resins and powder coatings to prepare low-temperature curing and frosting-free materials.
[0027] In the following examples, the stannous hydroxide and stannous oxalate used were prepared by the following method:
[0028] Synthesis of stannous hydroxide: weigh tin dichloride dihydrate and add a small amount of water to prepare an aqueous solution of tin dichloride dihydrate, the concentration of which is 60-80wt%; weigh an appropriate amount of ammonia solution, the concentration of which is 10-20wt%; drop the ammonia solution into the prepared aqueous solution of tin dichloride dihydrate, and no obvious lumps are formed during the dropwise addition process, the reaction temperature is controlled below 80°C, the pH value at the reaction end point is controlled between 6-8, the reaction is continued to be kept warm for 1h, the upper water layer is separated, the product is stannous hydroxide, and the purity of the final product is obtained by negative pressure dehydration at 105°C, suction filtration, and drying.
[0029] (2) Synthesis of stannous oxalate: Weigh tin dichloride dihydrate and add a small amount of water to prepare an aqueous solution of tin dichloride dihydrate with a concentration of 30%-50wt%, weigh an appropriate amount of sodium oxalate and add water to prepare an aqueous solution of sodium oxalate with a concentration of 30-50wt%, add the aqueous solution of tin dichloride dropwise to the aqueous solution of sodium oxalate at a molar ratio of sodium oxalate:tin dichloride of 1.1:1, control the reaction temperature to be below 60°C, react at 60°C for 1h after the addition is completed, filter, wash and dry to obtain the product stannous oxalate, and the purity of the final product is above 99%.
[0030] Example 1
[0031] The specific synthetic process of the polyester resin is as follows: polyol, polyacid and catalyst monobutyl tin oxide according to the formula amount are added into a four-mouth glass reactor equipped with a heating device, a stirrer, a distillation column and a condenser, stirring is started, and the temperature is gradually raised to 245-255° C. and maintained in a nitrogen environment, and the material temperature is 160-190° C., the esterification reaction begins, and distillate flows out of the condenser, and the temperature at the top of the distillation column is controlled at 100±2° C. When the top temperature of the distillation column is lower than 80° C. and the amount of distillate reaches more than 95% of the theoretical water amount, the acid value reaches 5-15 (mgKO H / g), adding alcoholysis agent isophthalic acid and maintaining the temperature at 240-250° C. for 90-120 min to carry out acidolysis and end-capping, and after the acid value of the polyester resin reaches the set value, cooling by 230-240° C. and carrying out vacuum polycondensation, and reducing the vacuum degree to -0.097-0.098 MPa, and reacting for 90-120 min under vacuum conditions; after the vacuum reaction is completed, the acid value and hydroxyl value of the polyester resin are within the target value range, cooling to 200° C., adding an antioxidant, stirring for 15-30 min, discharging, cooling, and crushing to obtain a granular polyester resin.
[0032] Among them, the formula combination and dosage of each component are:
[0033] The polyol component is neopentyl glycol, the polyacid component is terephthalic acid, the catalyst component is monobutyl tin oxide, the alcoholysis agent is isophthalic acid, the antioxidants are TPP and 1010, and the curing accelerator is triphenylethylphosphonium bromide.
[0034] Specifically, according to mass fraction (g), the dosage is:
[0035] 638 parts of neopentyl glycol, 428 parts of terephthalic acid, 1 part of monobutyltin oxide, 90 parts of isophthalic acid, 1.4 parts of TPP, 2 parts of 1010, and 1 part of triphenylethylphosphonium bromide.
[0036] The acid value of polyester resin is tested according to GB / T 6743-2008 standard; the glass transition temperature is tested according to GB / T19466.2-2004 standard, using nitrogen atmosphere and a heating rate of 10°C / min; the softening point (Sp) is tested according to GB / T12007.6-1989 standard; and the resin melt viscosity is measured at 200°C using a cone plate viscometer.
[0037] The performance of polyester resin is characterized by preparing powder coating. The preparation process of powder coating is as follows: polyester resin and other raw materials are pre-evenly mixed according to the formula ratio, and powder coating is prepared through double-screw foundation and extrusion, tableting, cooling, crushing, and screening. The powder coating is then sprayed on the sample by electrostatic spraying, and various properties of the coating are tested after heating and curing.
[0038] Specifically, according to mass fraction (g), the powder coating formula is:
[0039] 558 parts of polyester resin, 42 parts of curing agent TGIC, 200 parts of titanium dioxide, 200 parts of barium sulfate, 3 parts of benzoin, 10 parts of leveling agent, 3 parts of matting agent, and the curing conditions are 180°C for 10 minutes.
[0040] Coating performance test: gel time is tested according to GB / T 16995-1997; horizontal fluidity is tested according to GB6551-1986; coating thickness test is tested according to GB / T 13452.2-2008; coating impact performance test is tested according to GB-T 1732-1993; coating gloss is tested according to GB / T 1743-1979; anti-blooming test method, constant temperature test method: place the baked and cured sample in an oven at 120℃, keep the constant temperature for 24h, take out the sample, check with a red cloth after curing, and observe the frosting of the coating.
[0041] The preparation process of Examples 2 to 11 is the same as that of Example 1, except that:
[0042] The catalyst of Example 2 is dibutyltin oxide, and the rest is the same as that of Example 1;
[0043] The catalyst of Example 3 is stannous hydroxide, and the rest is the same as that of Example 1;
[0044] In Example 4, the catalyst is stannous oxalate, and the rest is the same as in Example 1;
[0045] Example 5, the catalyst is stannous hydroxide: stannous oxalate = 9:1 (mass ratio), and the rest is the same as Example 1;
[0046] Example 6, the catalyst is stannous hydroxide: stannous oxalate = 8:2 (mass ratio), and the rest is the same as Example 1;
[0047] Example 7, the catalyst is stannous hydroxide: stannous oxalate = 7:3 (mass ratio), and the rest is the same as Example 1;
[0048] Example 8, the catalyst is stannous hydroxide: stannous oxalate = 6:4 (mass ratio), and the rest is the same as Example 1;
[0049] Example 9, the catalyst is stannous hydroxide: stannous oxalate = 5:5 (mass ratio), and the rest is the same as Example 1;
[0050] In Example 10, the catalyst is stannous hydroxide, no curing accelerator is added, and the rest is the same as in Example 1;
[0051] Example 11, the catalyst is stannous oxalate, no curing accelerator is added, and the rest is the same as Example 1;
[0052] Example 12, the catalyst is stannous hydroxide: stannous oxalate = 9:1 (mass ratio), no curing accelerator is added, and the rest is the same as Example 1;
[0053] Example 13, the catalyst is stannous hydroxide: stannous oxalate = 7:3 (mass ratio), no curing accelerator is added, and the rest is the same as Example 1;
[0054] In Example 14, the catalyst is stannous hydroxide: stannous oxalate = 5:5 (mass ratio), no curing accelerator is added, and the rest is the same as in Example 1.
[0055] The polyester resins prepared above are labeled 1-14, and the coatings further prepared from the resins 1-14 are labeled coatings 1-14 respectively.
[0056] The properties of the polyester resin prepared in the above examples and the obtained powder coating are shown in Table 1 and Table 2 below.
[0057] Table 1 Properties of polyester resin
[0058]
[0059] Wherein, A is the acid value (mgKOH / g); B is the glass transition temperature (°C); C is the softening point (°C); and D is the melt rotational viscosity (mPa.s / 200°C).
[0060] Table 2 Coating properties
[0061]
[0062]
[0063] It can be seen from Tables 1 and 2 that the polyester resin synthesized using the composite catalyst meets the index requirements of polyester resin, is made into powder coatings, maintains the appearance and mechanical properties of the powder coatings, eliminates the frosting phenomenon, and the composite catalyst has the function of a curing accelerator.
[0064] The present invention provides a concept and method for a composite environmentally friendly catalyst suitable for polyester resin synthesis. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A composite environmentally friendly catalyst for polyester resin synthesis, characterized in that: The catalyst comprises stannous hydroxide and stannous oxalate, wherein the mass ratio of stannous hydroxide to stannous oxalate is 9:1 to 5:
5.
2. The method for preparing the composite environmentally friendly catalyst according to claim 1, characterized in that: The steps include: (1) Synthesis of stannous hydroxide: weigh tin dichloride dihydrate and add water to prepare an aqueous solution of tin dichloride dihydrate; weigh an appropriate amount of ammonia solution; add the ammonia solution dropwise to the prepared aqueous solution of tin dichloride dihydrate, control the reaction temperature to be below 50-80°C, control the pH at the reaction end point to be between 6-8, continue to keep the temperature at 50-80°C for 3 hours, remove the upper water layer, dehydrate at 100-110°C under negative pressure, filter and dry to obtain the product of stannous hydroxide; (2) Synthesis of stannous oxalate: weigh tin dichloride dihydrate and add a small amount of water to prepare an aqueous solution of tin dichloride dihydrate, weigh an appropriate amount of sodium oxalate and add water to prepare an aqueous solution of sodium oxalate, add the aqueous solution of tin dichloride dropwise to the aqueous solution of sodium oxalate at a molar ratio of sodium oxalate:tin dichloride of 1.1-1.3:1, control the reaction temperature to be below 40-60°C, react at 40-60°C for 1-2h after the addition is completed, filter, wash, and dry to obtain the product stannous oxalate; (3) The stannous hydroxide obtained in step (1) and the stannous oxalate obtained in step (2) are mixed according to the formula amount to obtain a composite environmentally friendly catalyst.
3. The preparation method according to claim 2, characterized in that: In step (1), the concentration of the aqueous solution of tin dichloride dihydrate is 60-80wt%, and the concentration of the aqueous ammonia solution is 10-20wt%.
4. The preparation method according to claim 2, characterized in that: In step (2), the concentration of the aqueous solution of tin dichloride dihydrate is 30%-50wt%, and the concentration of the aqueous solution of sodium oxalate is 30-50wt%.
5. Use of the composite environmentally friendly catalyst for polyester resin synthesis according to claim 1 in the preparation of polyester resin.
6. The use according to claim 5, characterized in that: The polyester resin preparation process is as follows: polyol, polyacid and the composite environmentally friendly catalyst according to claim 1 are added to a reaction kettle according to a ratio, the temperature is slowly raised to 240-255°C and maintained, sampling and analysis are performed, when the acid value is 5-10 mgKOH / g, the temperature is lowered to 210-230°C, acid is added for acid blocking, when the acid value of the polyester resin is 40-45 mgKOH / g, the temperature is lowered to 210°C for vacuum polycondensation, when the acid value of the polyester resin is 32-38 mgKOH / g, the temperature is lowered to 180°C, an auxiliary agent is added, and the material is discharged after stirring for 1 hour.
7. The use according to claim 6, characterized in that: The polyacid is any one of TA, IPA, AA, and SA; the polyol is any one of EG, DEG, and 1,2-PG.
8. Use of the polyester resin prepared according to claim 5 in preparing powder coatings.
9. The use according to claim 8, characterized in that: The method comprises the following steps: preparing ingredients according to a formula, premixing, extruding, tableting, crushing and screening to obtain a powder coating, spraying the prepared powder coating onto a sample plate by electrostatic spraying, and then placing the sample plate in an oven for baking and curing at 200°C for 10 minutes to obtain a coating.