Composite plating material and method for manufacturing the same
By forming a composite coating containing carbon particles and antimony on the conductor raw material, the problem of abrasion and peeling of the silver coating is solved, and a composite plating material with high wear resistance is achieved, specifically including a composite coating containing carbon particles and Sb in the Ag layer. The composite coating composed of materials improves the hardness and wear resistance.
Patent Information
- Application Number
- CN202080083588.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-06-10
AI Technical Summary
In the existing technology, the silver coating is easily worn and peeled off during the sliding process, resulting in insufficient wear resistance.
By forming a composite coating containing carbon particles and antimony on the conductor raw material, the hardness and wear resistance of the coating are improved. The specific method includes forming a composite coating composed of a composite material containing carbon particles and Sb in the Ag layer on the base material. The carbon content is more than 6.0%, S The content of b is more than 0.5%, and the stirring speed and current density are controlled during the electroplating process. The area ratio of surface carbon particles is 15 to 80%, the Vickers hardness is more than 150, the arithmetic mean roughness is more than 0.3 μm, and the micron The crystal size is 40nm or less.
The wear resistance and hardness of composite plating materials are significantly improved, ensuring wear resistance under sliding conditions.
Smart Images

Figure BDA0003673905000000121 
Figure BDA0003673905000000122 
Figure BDA0003673905000000123
Abstract
Description
Technical Field
[0001] The invention relates to a composite plating material and a manufacturing method thereof. Background Art
[0002] Conventionally, silver-plated materials, which are silver-plated conductive materials such as copper and copper alloys, have been used as materials for sliding contact parts such as switches and connectors used in automobiles to prevent oxidation of conductive materials such as copper and copper alloys caused by heat during sliding.
[0003] However, silver plating is soft and easily wears away, and generally has a high coefficient of friction, making it prone to peeling due to sliding. To address this issue, methods have been proposed to improve wear resistance by forming a silver alloy plating film or a composite plating film composed of silver with graphite particles dispersed in a silver matrix on a conductive material through electroplating.
[0004] Patent Document 1, paragraph
[0026] states that in a silver plating solution containing 120 g / L of potassium silver cyanide, 120 g / L of potassium cyanide, 30 g / L of potassium sodium tartrate tetrahydrate, and 7 g / L of potassium antimony (Sb) tartrate, the material to be plated is used as the cathode and the silver electrode plate is used as the anode, while stirring with a stirring rod at 400 rpm and at a liquid temperature of 20°C with a current density of 5 A / dm 2 Electroplating (second silver plating) was performed until the total film thickness of the silver plating layer (the first silver plating layer and the second silver plating layer) reached 3 μm.
[0005] Paragraph
[0033] of Patent Document 2 states that 80 g / L of oxidized carbon particles are added to a silver cyanide plating solution containing 120 g / L of potassium silver cyanide and 100 g / L of potassium cyanide, dispersed and suspended, and then potassium cyanide selenate (KSeCN) is added to prepare a composite plating solution of silver and carbon particles.
[0006] In addition, it is also described that: using this composite plating solution, the solution temperature is 25 ° C, the current density is 1A / dm 2 Electroplating was performed to produce a composite plated material in which a composite plated film of silver and carbon particles having a thickness of 5 μm was formed on a copper plate having a thickness of 0.3 mm as a raw material.
[0007] In order to improve the adhesion of the plated film, as the base plating, an impact plating Ag bath containing 3 g / L of potassium silver cyanide and 100 g / L of potassium cyanide was used at a liquid temperature of 25°C and a current density of 3 A / dm 2 Perform Ag impact plating.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 2013-189680
[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 2007-16250 Summary of the Invention
[0012] Problems to be solved by the invention
[0013] According to the investigation by the present inventors, it has become clear that the plated materials obtained by the methods described in Patent Documents 1 and 2 have room for improvement in terms of wear resistance.
[0014] An object of the present invention is to provide a composite plating material having high wear resistance, a method for producing the same, and related technologies.
[0015] Solutions for solving problems
[0016] The first embodiment of the present invention is a composite plating material.
[0017] A composite coating is formed on a substrate, wherein the composite coating is formed of a composite material containing carbon particles and Sb in an Ag layer.
[0018] The carbon content in the composite plating layer is 6.0 mass % or more, and the Sb content is 0.5 mass % or more.
[0019] The second aspect of the present invention is the aspect described in the first aspect, wherein
[0020] The ratio of the carbon particles on the surface of the composite plating layer is 15 to 80% by area.
[0021] The third aspect of the present invention is the aspect described in the first or second aspect, wherein
[0022] The surface of the composite plating material has a Vickers hardness HV of 150 or greater.
[0023] A fourth aspect of the present invention is the aspect described in any one of the first to third aspects, wherein:
[0024] The surface of the composite plating layer has an arithmetic mean roughness Ra of 0.3 μm or more.
[0025] A fifth aspect of the present invention is the aspect described in any one of the first to fourth aspects, wherein:
[0026] The crystallite size of the composite coating is less than 40 nm.
[0027] A sixth aspect of the present invention is the aspect described in any one of the first to fifth aspects, wherein:
[0028] The carbon content in the composite coating is 30% by mass or less, and the Sb content is 5% by mass or less.
[0029] A seventh aspect of the present invention is the aspect described in any one of the first to sixth aspects, wherein:
[0030] The aforementioned substrate is copper or a copper alloy.
[0031] The eighth aspect of the present invention is the aspect described in any one of the first to seventh aspects, wherein:
[0032] A bottom plating layer is provided between the substrate and the composite plating layer.
[0033] The ninth aspect of the present invention is the aspect described in the eighth aspect, wherein
[0034] The base plating layer is formed of at least one selected from a Ni plating layer and a Cu plating layer.
[0035] A tenth aspect of the present invention is a method for producing a composite plating material.
[0036] In the method, electroplating is performed using a composite plating solution obtained by adding carbon particles to an Ag plating solution containing Sb, thereby forming a composite plating layer on a substrate. The composite plating layer is formed by a composite material containing carbon particles and Sb in an Ag layer, and the carbon content in the composite plating layer is greater than 6.0 mass%, and the Sb content is greater than 0.5 mass%.
[0037] The eleventh aspect of the present invention is the aspect described in the tenth aspect, wherein
[0038] The ratio of the carbon particles on the surface of the composite plating layer is 15 to 80% by area.
[0039] The twelfth aspect of the present invention is the aspect described in the tenth or eleventh aspect, wherein
[0040] The stirring speed of the composite plating solution during formation of the composite plating layer is set to 400 rpm or less.
[0041] A 13th aspect of the present invention is the aspect described in any one of the 10th to 12th aspects, wherein:
[0042] The current density of the electroplating was set to 4 A / dm 2 above.
[0043] A fourteenth aspect of the present invention is the aspect described in any one of the tenth to thirteenth aspects, wherein:
[0044] The carbon particles are oxidized carbon particles.
[0045] A fifteenth aspect of the present invention is the aspect described in any one of the tenth to fourteenth aspects, wherein:
[0046] Before forming the composite plating layer, a base plating layer is formed on the substrate.
[0047] A sixteenth aspect of the present invention is the aspect described in the fifteenth aspect, wherein
[0048] The base plating layer is formed of at least one selected from a Ni plating layer and a Cu plating layer.
[0049] Effects of the Invention
[0050] According to the present invention, a composite plating material having high wear resistance, a method for producing the same, and related technologies can be provided. DETAILED DESCRIPTION
[0051] Hereinafter, this embodiment will be described. In this specification, "to" means a value greater than or equal to a predetermined value and less than or equal to a predetermined value.
[0052] (Composite plating material)
[0053] The composite plating material of this embodiment forms a composite plating layer on a substrate, wherein the composite plating layer is formed of a composite material containing carbon particles and Sb in an Ag layer, wherein the carbon content in the composite plating layer is greater than 6.0 mass % and the Sb content is greater than 0.5 mass %.
[0054] Through this structure, the composite plating material of the present invention can significantly improve the wear resistance compared with the composite plating material in which a composite plating layer composed of a composite material containing carbon particles (and not containing Sb) in an Ag layer is formed on a substrate, and the composite plating material in which a composite plating layer composed of a composite material containing Sb (and not containing carbon particles) in an Ag layer is formed on a substrate (for details, refer to the items of the following embodiments).
[0055] The carbon content in the composite coating is 6.0% by mass or more (preferably 7% by mass or more, and further preferably 8% by mass or more). If it is less than this, the improvement in wear resistance is insufficient. In addition, even if a large amount of carbon particles is included, a significant improvement in wear resistance is not observed. Therefore, the carbon content can be set to 30% by mass or less.
[0056] The Sb content in the composite plating layer is 0.5 mass % or more (suitably 1.0 mass % or more, more preferably 1.5 mass % or more, with an upper limit of 5 mass % or 3 mass %). This improves the hardness of the composite plating layer (plating material).
[0057] The carbon and Sb contents in the composite plating layer can be measured on the surface of the composite plating layer by energy dispersive X-ray analysis using an energy dispersive X-ray analyzer attached to a scanning electron microscope.
[0058] A composite coating formed on a substrate, made of a composite plating material, has a high carbon content and a high amount of surface carbon particles, resulting in excellent wear resistance. The surface carbon particles can be expressed as "the ratio of carbon particles on the surface of the composite coating is 15 to 80% (preferably 18% or more and less than 60%) by area." The definition (measurement and calculation methods) of the ratio of carbon particles on the surface, i.e., the area ratio, is described in the following Examples.
[0059] The Vickers hardness HV of the composite plating material is preferably not less than 150. The definition (measurement method) of the Vickers hardness HV is described in the following examples.
[0060] Considering the ease with which carbon particles are entangled in the composite coating, the arithmetic mean roughness Ra of the composite coating surface is preferably 0.3 μm or greater. The arithmetic mean roughness Ra is preferably 10 μm or less, and more preferably 8 μm or less. The definition (measurement method) of the arithmetic mean roughness Ra of the surface is described in the following Examples.
[0061] The crystallite size of the composite plating layer is preferably 40 nm or less. The definition (measurement method) of the crystallite size is described in the following Examples.
[0062] A bottom plating layer may be formed between the substrate and the composite plating layer. In addition, the bottom plating layer is preferably formed of at least one selected from the group consisting of a Ni plating layer and a Cu plating layer.
[0063] The substrate is not limited, but is preferably copper or a copper alloy.
[0064] A ratio of the mass % of Ag, the mass % of Sb, and the mass % of carbon in the composite coating of 93.5:0.5:6 to 65:5:30 is preferred, as it improves not only wear resistance but also other properties. Specifically, in the composite coating, the mass % of Ag is preferably set between 65 and 93.5 mass %, the mass % of Sb is preferably set between 0.5 and 5 mass %, and the mass % of carbon is preferably set between 6 and 30 mass %.
[0065] In addition, the thickness of the composite coating is preferably 0.5 to 25 μm, more preferably 1 to 20 μm. If it is within the above range, wear resistance can be fully ensured and production efficiency is also good. The definition (measurement method) of the thickness of the composite coating is described in the following examples.
[0066] (Method for manufacturing composite plated material)
[0067] As an embodiment of the method for manufacturing a composite plating material of the present invention, there is a method for manufacturing a composite plating material as follows, wherein electroplating is performed using a composite plating solution obtained by adding carbon particles to an Ag plating solution (Ag alloy plating solution) containing Sb, thereby forming a composite plating layer on a substrate, wherein the composite plating layer is formed by a composite material containing carbon particles and Sb in an Ag layer, and the carbon content in the composite plating layer is greater than 6.0 mass%, and the Sb content is greater than 0.5 mass%.
[0068] The Ag plating solution may be a so-called cyanide bath containing cyanide. "Cyanide" in this specification is a general term for substances containing cyanide ions.
[0069] As an example of the aforementioned Ag plating solution, a plating bath containing 50-150 g / L of sodium silver cyanide, 150-450 g / L of sodium cyanide, and 3-20 g / L of antimony trioxide (Sb) can be used. Potassium antimony tartrate can also be used instead of antimony trioxide.
[0070] Alternatively, the aforementioned Ag plating solution having a selenium concentration of 5 to 15 mg / L and a mass ratio of silver to free cyanide of 0.9 to 1.8 may be used.
[0071] When forming a composite plating layer on a substrate by electroplating, a composite plating solution containing carbon particles added to the aforementioned Ag plating solution is used. The temperature of the composite plating solution during electroplating to form the composite plating layer on the substrate is preferably 10 to 40°C, more preferably 15 to 30°C.
[0072] Furthermore, the composite plating material is preferably formed under conditions such that the ratio of carbon on the surface of the composite plating layer is 15 to 80% by area.
[0073] The stirring speed of the composite plating solution is preferably set to 400 rpm or less when forming the composite plating layer, and the current density is preferably set to 4 A / dm 2 above.
[0074] The stirring speed of the composite plating solution during electroplating can be suitably adjusted by the device used, but it is believed that by adopting a lower value as the stirring speed, the surface roughness of the composite coating increases, and carbon particles are easily involved in the composite coating. The applicable range of the stirring speed is different according to the device used, but is generally less than 400 rpm (suitable for being lower than 400 rpm) (particularly the situation of the stirring rod (cross stirring bar) recorded in the project of the following embodiment).
[0075] The current density during electroplating is preferably 4A / dm 2 More preferably, 4 to 10 A / dm 2It is considered that these regulations increase the surface roughness of the composite plating layer and make it easier for carbon particles to be entangled in the composite plating layer.
[0076] It should be noted that the concentration of carbon particles in the composite plating solution is preferably 10 to 200 g / L, more preferably 20 to 80 g / L. If it is 10 g / L or more, the amount of carbon particles for composite formation is appropriately maintained, and even if an amount exceeding 200 g / L is added, the amount of carbon particles in the composite plating layer is hardly increased.
[0077] Furthermore, a ratio of the Ag concentration to the Sb concentration to the carbon particle concentration in the composite plating solution of 10:1:5 to 40:1:30 is preferred, as demonstrated in the examples below. This improves not only wear resistance but also other properties. Specifically, when the Sb concentration in the composite plating solution is set to 1, the Ag concentration is preferably set to between 10 and 40 times that value. Furthermore, when the Sb concentration is set to 1, the carbon particle concentration is preferably set to between 5 and 30 times that value.
[0078] The carbon particles are preferably oxidized carbon particles. That is, the carbon particles are preferably oxidized (to remove organic matter therefrom) before being added.
[0079] By adding the oxidized carbon particles to the plating solution, a plating solution can be obtained that allows the carbon particles to be well dispersed during plating without using additives such as dispersants or coating the surface of the carbon particles. By using this composite plating solution for electroplating, a composite coating is formed on the substrate, the composite coating comprising a composite material containing carbon particles and Sb in an Ag layer.
[0080] In addition, before forming the composite coating on the base material, a bottom coating can also be formed on the base material. As the bottom coating, it is preferred to form a bottom coating formed by at least one of, for example, a Ni coating and a Cu coating. The Ni coating and the Cu coating of the substrate can also be stacked to form multiple layers. As a specific method for forming the Ni coating and the Cu coating, known methods can be utilized to form them.
[0081] Furthermore, as described in paragraph
[0021] of Patent Document 2, in addition to the oxidized carbon particles, a silver matrix orientation modifier, a brightener, and the like may be added to the composite plating solution. The silver matrix orientation modifier and brightener preferably contain selenium (Se) ions, and may also be added in the form of potassium selenocyanate (KSeCN). Furthermore, the Se concentration in the composite plating solution can be set to 1 to 48 mg / L.
[0082] On the other hand, as shown in the following examples, the present embodiment achieves good hardness test results even without the addition of a silver matrix orientation modifier (in other words, even when selenium (Se ≤ 10 ppm) is substantially absent from the composite coating), which is one of the technical features of the present invention. Whether or not to add a silver matrix orientation modifier depends on the type of plating solution.
[0083] The protection scope of the present invention is not limited to the above-described embodiment, and includes various changes and improvements within the scope of the specific effects obtained by the technical features of the invention and the combination thereof.
[0084] For example, the fact that a hard film can be obtained by adding an element selected from the group consisting of Sn, In, and Te to the plating solution is described in the publication "Surface Technology vol. 70, No. 9, 2019" page 428 "Advances in Precious Metal Plating Technology".
[0085] In addition, as shown in the following embodiments, in order to improve the adhesion of the composite plating layer, the substrate may be subjected to strike plating of Ag before forming the composite plating layer. It should be noted that the strike plating of Ag may also be performed using the known strike plating method of Ag described in paragraph
[0024] of Patent Document 1 and
[0033] of Patent Document 2. It should be noted that, in order to distinguish it from strike plating of Ag, the composite plating (layer) described in this embodiment is also referred to as the "main plating (layer)."
[0086] In addition, a bottom plating layer can be formed before the impact plating. As the bottom plating layer, there is no limitation, for example, a bottom plating formed by at least one selected from a Ni plating layer and a Cu plating layer can also be implemented. The Ni plating layer and the Cu plating layer of the substrate can also be stacked to form a multilayer. As a specific method for forming the Ni plating layer and the Cu plating layer, a known method can be adopted.
[0087] Furthermore, the composite plating solution serving as the basis for the composite plating layer also embodies the technical concept of the present invention and satisfies the invention itself. Specific configurations and suitable examples of the composite plating solution are as described above.
[0088] Example
[0089] Next, the present invention will be described in detail with reference to the following examples. The present invention is not limited to the following examples. It should be noted that the contents not described below are the same as those described in the present embodiment.
[0090] [Example 1]
[0091] 80 g of flaky graphite particles (natural graphite J-CPB, manufactured by Nippon Graphite Industries, Co., Ltd.) with a long diameter of 5 μm, serving as carbon particles, were added to 1.4 L of pure water. The mixed solution was then heated to 50°C while stirring. Next, 0.6 L of an aqueous solution containing 27 g of potassium persulfate as an oxidizing agent was slowly added dropwise to the mixed solution. The mixture was then stirred for 2 hours for oxidation treatment, filtered through filter paper, and washed with water. This oxidation treatment produced carbon particles from which attached hydrophobic substances such as hydrocarbons had been removed.
[0092] Separately, a copper alloy plate (a copper alloy plate containing 1.0 mass% Ni, 0.9 mass% Sn, and 0.05 mass% P, with the remainder being Cu) having a thickness of 0.2 mm was prepared as a substrate. The substrate was immersed in an impact plating Ag solution (cyanide bath) containing 3 g / L of potassium silver cyanide and 90 g / L of potassium cyanide. The substrate was used as a cathode, and a titanium platinum mesh electrode plate (a titanium mesh raw material plated with platinum) was used as an anode. The solution temperature was set to 25° C. and the current density was 5 A / dm 2 , plating time is 30 seconds, and electroplating (Ag impact plating) is performed.
[0093] Separately, a composite plating solution containing Sb and carbon particles in the Ag layer was prepared by adding 30 g / L of carbon particles that had undergone the aforementioned oxidation treatment to a cyanide-based Ag-Sb alloy plating solution containing 10 mass% sodium silver cyanide, 30 mass% sodium cyanide, and 50 mL / L of Nissan BRIGHTN (brightening agent, containing 6 mass% antimony trioxide) (manufactured by Nikken Eigen Co., Ltd.). The Ag concentration in the composite plating solution was 60 g / L, and the antimony (Sb) concentration was 2.5 g / L.
[0094] The substrate with the impact-plated Ag layer was used as the cathode and the Ag electrode plate was used as the anode. The Ag electrode plate was immersed in the composite plating solution at a liquid temperature of 18°C, a stirring speed of 250 rpm, and a current density of 5 A / dm 2 , electroplating (composite plating (main plating)) was performed for 250 seconds, and a composite plating layer with a thickness of 3.8 μm was formed on the substrate with an impact-plated Ag layer, followed by 15 seconds of water washing and drying in a dryer to produce a composite plated material. It should be noted that the composite plating solution was placed in a beaker with a capacity of 1 L and a diameter of 110 mm to prepare a 1 L plating bath, and stirred using a magnetic stirrer REXIM RS-1DN (cross stirring bar, width 38.1 mm, height 15.8 mm) manufactured by AS ONE.
[0095] The “thickness of the composite plating layer” was obtained by measuring a region with a diameter of 1.0 mm at the center of the sample using a fluorescent X-ray film thickness meter (FT9450 manufactured by Hitachi High-Tech Science Corporation).
[0096] "Mass % of Sb" and "Mass % of C" were observed using a desktop microscope (TM4000 Plus manufactured by Hitachi High-Technologies Corporation) serving as an electron microscope at an accelerating voltage of 15 kV and a magnification of 1000 times. In this observation area, the amount of Sb (mass %) and the amount of C (mass %) measured by EDX analysis using an energy dispersive X-ray analyzer (AztecOne manufactured by Oxford Corporation) attached to the above-mentioned desktop microscope were used as the Sb content and carbon content in the composite coating.
[0097] The “arithmetic mean roughness Ra of the surface of the composite plating layer” was measured in accordance with JIS B0601 (2001) by magnifying the surface 1000 times using a laser microscope (VK-X100 manufactured by KEYENCE CORPORATION).
[0098] The “Vickers hardness HV of the surface of the composite plating layer” was measured using a microhardness tester (HM221 manufactured by Mitutoyo Corporation) with a load of 0.1 N applied for 15 seconds in accordance with JIS Z2244, and the average value of three measurements was adopted.
[0099] For the crystallite size of the composite coating, the Bruker D2Phaser2 nd Generation performed X-ray diffraction on the surface of the composite coating (Cu Kα tube, tube voltage 30kV, tube current 10mA). Based on the peaks detected for the (111) and (222) faces of Ag, the full width at half maximum (FWHM) was determined using the analysis software PDXL manufactured by Rigaku Corporation. The crystallite size was then calculated based on the Scherrer equation. To reduce variations due to crystallographic planes, the average of the crystallite sizes for the (111) and (222) faces of Ag was used as the crystallite size of the composite coating.
[0100] It should be noted that the Scherrer formula is as follows.
[0101] D=K·λ / β·cosθ
[0102] D: Crystallite size
[0103] K: Scherrer constant, which is 0.9 due to the use of the full width at half maximum
[0104] λ: Since it is the wavelength of X-rays and CuKα rays, it is
[0105] β: Full width at half maximum (FWHM) (rad)
[0106] θ: Measurement angle (deg)
[0107] The "carbon area ratio of the surface of the composite coating" is obtained by observing the surface of the composite coating. Specifically, the reflected electron composition (COMPO) image magnified 1000 times by the previously mentioned desktop microscope TM4000 Plus (manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 5kV is binarized using GIMP 2.10.10 (image analysis software), and the area ratio occupied by carbon is calculated. More specifically, when the highest brightness of all pixels is set to 255 and the lowest brightness is set to 0, the grayscale is binarized in such a way that pixels with a brightness of 127 or less become black and pixels with a brightness of more than 127 become white, and the grayscale is separated into the silver part (white part) and the carbon particle part (black part), and the ratio Y / X of the number of pixels Y of the carbon particle part to the total number of pixels X of the image is calculated as the carbon area ratio (%) of the surface.
[0108] The "reflection density of the composite coating surface" was measured visually and using a GretagMacbeth RD-918 reflection densitometer. Table 1 shows the apparent color and measured values. In this test example, a silver gloss was considered good. The value is the ratio of the concentration obtained by incident light to the concentration obtained by reflected light, and is preferably 0.7 or greater.
[0109] The “wear resistance” was measured using a sliding tester (CRS-G2050-DWA) manufactured by Yamazaki Seiki Laboratories.
[0110] As an indenter for sliding the flat plate-shaped composite plated material (evaluation sample) of Example 1, the copper alloy plate was subjected to a 1.0 mm inner diameter press process (so-called indentation), and then a 20 μm thick Ag-Sb coating was formed using the Ag-Sb alloy plating solution of Comparative Example 2 described below. The resulting indenter was used as a convex indenter. This indenter was mounted in the aforementioned sliding tester and slid continuously against the composite plated material of Example 1 at a contact load of 2 N, a sliding speed of 3 mm / s, and a sliding distance of 10 mm until 1000 reciprocating strokes were repeated or the substrate was exposed.
[0111] The thickness of the composite coating after the sliding test was measured using the same method as described above for the "composite coating thickness," except that the measurement area was set to a 0.1 mm diameter at the center of the sliding mark (ground portion). The grinding amount was the difference in thickness between the composite coating before and after the sliding test. A grinding amount of 1 μm or less was considered to indicate excellent wear resistance.
[0112] The "average friction coefficient" is calculated by measuring the horizontal force (F) applied when the slide reaches half the outward sliding distance in one reciprocating slide in the aforementioned sliding test. The friction coefficient is calculated using μ(friction coefficient) = F / N (N is 2N, representing the normal force). The friction coefficient is calculated for each test until the 1000th test or until the substrate is exposed, and the average value is used as the average friction coefficient. An average friction coefficient of 0.5 or less is considered good.
[0113] For "average contact resistance (contact reliability)," in the aforementioned sliding test, the contact resistance is measured when the device reaches half the outward sliding distance in one reciprocating sliding motion. The average contact resistance is calculated as the average contact resistance for each reciprocating sliding motion until the 1000th reciprocating motion or until the substrate is exposed. A contact resistance of 3 mΩ or less is considered to be contact reliable.
[0114] The scratch resistance was investigated as follows.
[0115] The composite plated material of Example 1 was subjected to a scratch test using Revetest-RST manufactured by CSM Instruments. A diamond indenter manufactured by Nanotec (R=0.2mm, 120° conical shape) was used to scratch a distance of 10mm. Then, a laser microscope (the same as that used in the "arithmetic mean roughness Ra of the surface of the composite coating") was used to observe the composite plated material after the scratch test, and the position where the set load was applied, that is, the line roughness of the end of the scratch (the end of the scratching direction of the scratch, centered on the end of the scratch, and the length of the width of 1cm perpendicular to the length direction of the scratch) was measured to determine the maximum valley depth Rv. If the thickness of the composite coating is greater than the maximum valley depth Rv of the scratch (in other words, if a composite coating remains after the test), it is considered to have scratch resistance.
[0116] The load was set as follows: the initial load was set to 1 and the load was increased to the set load with a movement distance of 10 mm. The load was set according to the plating thickness so that the set load / plating thickness = 1 (N / μm).
[0117] The following tables summarize the above contents.
[0118] Table 1 summarizes the differences between the composite plating materials in each Example and each Comparative Example as products.
[0119] Table 2 summarizes the differences in the manufacturing methods of the composite plating materials in each of the Examples and Comparative Examples.
[0120] Table 3 summarizes the test results of the composite plating materials in each of the Examples and Comparative Examples.
[0121] [Table 1]
[0122]
[0123] [Table 2]
[0124]
[0125] [Table 3]
[0126]
[0127] [Example 2]
[0128] Before forming the impact plating Ag, the substrate was immersed in a Ni plating bath containing 500 mL / L nickel sulfamate, 25 g / L nickel chloride hexahydrate and 35 g / L boric acid as the cathode, and the Ni electrode plate was used as the anode. The solution temperature was set to 18 ° C and the current density was 4 A / dm 2 A composite-plated material having a composite plating layer with a thickness of 1.8 μm was produced by the same method as in Example 1, except that a Ni primer plating with a thickness of 1 μm was performed on the substrate, a plating time of 140 seconds, and a composite plating time of 100 seconds. Other conditions and evaluation results are shown in Tables 1 to 3.
[0129] [Example 3]
[0130] A composite plated material having a composite plated layer having a thickness of 18.7 μm was produced by the same method as in Example 1, except that the composite plating time was set to 1000 seconds. Other conditions and evaluation results are as described in Tables 1 to 3.
[0131] [Comparative Example 1]
[0132] Except that no graphite particles were added to the Ag—Sb plating solution, an electroplated material having a 5.1 μm-thick Ag—Sb alloy plating layer was prepared in the same manner as in Example 1. Other conditions and evaluation results are as shown in Tables 1 to 3.
[0133] [Comparative Example 2]
[0134] Prepare the same substrate as in Example 1, prepare a sulfonic acid bath (Dyne Silver GPE-ST (Yamato Chemical Industry Co., Ltd.) with an Ag concentration of 3 g / L as a shock plating Ag solution, immerse the substrate as a cathode in the shock plating Ag solution, and use the Ag electrode plate as an anode. Set the current density to 5 A / dm 2 , plating time is 30 seconds, and Ag impact plating is performed on the substrate.
[0135] After the impact plating of Ag, a sulfonic acid-based Ag plating solution (DyneSilver GPE-PL (manufactured by Yamato Chemical Industry Co., Ltd.) containing sulfonic acid Ag and sulfonic acid with an Ag concentration of 30 g / L was added with 30 g / L of carbon particles. The substrate subjected to the impact plating of Ag was used as the cathode and the Ag electrode plate was used as the anode. The reaction was carried out at a liquid temperature of 25°C, a stirring speed of 500 rpm, and a current density of 3 A / dm 2 Electroplating was performed for 250 seconds to produce an electroplated material having a 6.6 μm-thick Ag plating layer formed on the substrate with an Ag strike-plated layer interposed therebetween. Other conditions and evaluation results are as described in Tables 1 to 3.
[0136] [Comparative Example 3]
[0137] The stirring speed was set to 500 rpm and the current density was set to 3 A / dm 2 A composite plated material having a composite plated layer having a thickness of 4.1 μm was produced by the same manufacturing method as in Example 1 except for the above. Other conditions and evaluation results are as described in Tables 1 to 3.
[0138] [Comparative Example 4]
[0139] A composite plated material having a composite plated layer was produced using the same manufacturing method as in Example 1, except that the stirring speed was set at 500 rpm. However, the composite plated layer precipitated from the substrate in a granular form and peeled off from the substrate, making it impossible to evaluate. Other conditions are as described in Tables 1 to 3.
[0140] [Comparative Example 5]
[0141] A Ag plating solution (cyanide bath) containing 150 g / L of potassium silver cyanide, 90 g / L of potassium cyanide, and 3.6 g / L of potassium cyanoselenate (i.e., without Sb) was used, with an Ag concentration of 80 g / L, a stirring speed of 500 rpm, and a current density of 3 A / dm 2 A plated material having a 5.6 μm-thick Ag—C plated layer was produced by the same manufacturing method as in Example 1 except for the above. Other conditions and evaluation results are as shown in Tables 1 to 3.
[0142] [Research]
[0143] As shown in Table 3, each example showed good results in all test items. According to each example, a composite plating layer and a composite plating material having high wear resistance were obtained.
[0144] On the other hand, the wear resistance was poor in Comparative Examples 1 to 3 and 5. In Comparative Example 4, granular electrolytic deposits were generated in the plating film, and the plating film peeled off from the substrate, making measurement impossible.
[0145] In addition, the gloss of the composite plating layer was good in each example, whereas it was poor in Comparative Examples 2 and 5. In addition, the friction coefficient was relatively too high in Comparative Example 1. In Comparative Example 2, the scratch resistance was poor.
Claims
1. A composite plating material, wherein a composite plating layer is formed on a substrate, wherein the composite plating layer is formed of a composite material containing carbon particles and Sb in an Ag layer, The carbon content in the composite plating layer is 8 mass % or more and 30 mass % or less, and the Sb content is 1.5 mass % or more and 3 mass % or less, The ratio of carbon particles on the surface of the composite plating layer is 15 to 80% by area.
2. The composite plating material according to claim 1, in, The Vickers hardness HV of the surface of the composite plating material is 150 or more.
3. The composite plating material according to claim 1 or 2, in, The arithmetic mean roughness Ra of the surface of the composite plating layer is greater than or equal to 0.3 μm.
4. The composite plating material according to claim 1 or 2, in, The crystallite size of the composite coating is less than 40 nm.
5. The composite plating material according to claim 1 or 2, in, The substrate is copper or a copper alloy.
6. The composite plating material according to claim 1 or 2, in, A bottom plating layer is provided between the substrate and the composite plating layer.
7. The composite plating material according to claim 6, in, The base plating layer is formed of at least one selected from a Ni plating layer and a Cu plating layer.
8. A method for manufacturing a composite plating material, in, A composite plating layer is formed on a substrate by electroplating using a composite plating solution obtained by adding carbon particles to an Ag plating solution containing Sb. The composite plating layer is formed by a composite material containing carbon particles and Sb in an Ag layer, and the carbon content in the composite plating layer is greater than 8 mass% and less than 30 mass%, and the Sb content is greater than 1.5 mass% and less than 3 mass%, wherein the ratio of carbon particles on the surface of the composite plating layer is 15 to 80% by area.
9. The method for manufacturing the composite plating material according to claim 8, in, The stirring speed of the composite plating solution during formation of the composite plating layer is set to 400 rpm or less.
10. The method for producing a composite plating material according to claim 8 or 9, in, The current density of the electroplating is 4A / dm 2 above.
11. The method for producing a composite plating material according to claim 8 or 9, in, The carbon particles are carbon particles that have been subjected to oxidation treatment.
12. The method for producing a composite plating material according to claim 8 or 9, in, Before forming the composite plating layer, a bottom plating layer is formed on the substrate.
13. The method for manufacturing the composite plating material according to claim 12, in, The base plating layer is formed of at least one selected from a Ni plating layer and a Cu plating layer.
Citation Information
Patent Citations
Composite plated material and method for producing the same
JP2007016250A
Silver plating material
JP2013189680A
Plating solution, method for preparing plating solution, surface treatment method and contact member
JP2006169609A
Composite plating material and method of manufacturing the same
JP2007254876A