Preparation method of polytetrafluoroethylene stretch tape, stretch tape and preparation device
By adding heating stretching and heating calendering steps in the preparation process of polytetrafluoroethylene stretch tapes, the problems of insufficient density and tensile strength in the existing technology were solved, and ultra-fine PTFE tapes with high density and tensile strength were successfully prepared. PTFE stretch tape.
Patent Information
- Application Number
- CN202210426465.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-04-22
AI Technical Summary
Existing polytetrafluoroethylene stretch tapes have low density, thick thickness, and low tensile strength, making it difficult to meet actual needs.
A preparation method including mixing polytetrafluoroethylene resin and lubricating oil, pressing, extruding, heating calendering, heating stretching and sintering stretching is adopted. The steps of heating stretching and heating calendering are added to improve the drawing efficiency. Stretch and density.
An ultra-fine, high-strength and high-density polytetrafluoroethylene stretch tape with a thickness of 1 to 15 μm, a width of 8 to 50 mm, a density greater than or equal to 1.8g/cm3, and a tensile strength greater than or equal to 400MPa is prepared.
Smart Images

Figure CN114770992B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polytetrafluoroethylene materials, and in particular to a method for preparing an ultra-fine high-strength high-density polytetrafluoroethylene stretch tape, an ultra-fine high-strength high-density polytetrafluoroethylene stretch tape, and a device for preparing an ultra-fine high-strength high-density polytetrafluoroethylene stretch tape. Background Art
[0002] At present, there are two main processing methods for polytetrafluoroethylene (PTFE) stretching tape: semi-sintered body stretching process and sintered body stretching process. Among them, the semi-sintered body stretching process is mixing-pressing-extrusion-calendering-deoiling-semi-sintering stretching-winding, and the sintered body stretching process is mixing-pressing-extrusion-calendering-deoiling-sintering stretching-winding. However, the density of the PTFE stretching tape obtained by the semi-sintered body stretching process is low, and the thickness of the PTFE stretching tape obtained by the sintered body stretching process is thicker, and the tensile strength is low, which is difficult to meet actual needs. Summary of the invention
[0003] Based on this, it is necessary to provide a method for preparing an ultra-fine, high-strength, high-density polytetrafluoroethylene stretch tape.
[0004] In addition, it is also necessary to provide an ultra-fine high-strength and high-density polytetrafluoroethylene stretched tape prepared by the above preparation method.
[0005] In addition, it is also necessary to provide a device for preparing the above-mentioned ultra-fine high-strength and high-density polytetrafluoroethylene stretched tape.
[0006] In one aspect, the present invention provides a method for preparing a polytetrafluoroethylene stretched tape, comprising the following steps:
[0007] Mixing polytetrafluoroethylene resin and lubricating oil to obtain a mixed material;
[0008] Performing green compaction processing on the mixed material to obtain a green body;
[0009] Extruding the embryo to obtain a polytetrafluoroethylene tape;
[0010] Performing a heating and calendering process on the polytetrafluoroethylene-based tape to obtain a first intermediate base tape;
[0011] performing a heating and stretching process on the first intermediate base band to obtain a second intermediate base band;
[0012] performing a heating and calendering process on the second intermediate base band to obtain a third intermediate base band; and
[0013] The third intermediate base tape is subjected to sintering and stretching treatment to obtain the polytetrafluoroethylene stretched tape.
[0014] Further, the temperature of the heating and stretching treatment on the first intermediate base band is 300° C. to 340° C., and / or the stretching ratio of the heating and stretching treatment on the first intermediate base band is 10 to 15 times.
[0015] Furthermore, the temperature of the heating and calendering treatment of the second intermediate base tape is 50°C to 100°C.
[0016] Further, the temperature of the sintering and stretching treatment for the third intermediate base band is 360° C. to 430° C., and / or the stretching ratio of the sintering and stretching treatment for the third intermediate base band is 3 to 12 times.
[0017] Furthermore, after the third intermediate base tape is sintered and stretched, the method for preparing the polytetrafluoroethylene stretched tape further comprises:
[0018] The third intermediate base tape is subjected to a heating and stretching treatment to obtain the polytetrafluoroethylene stretched tape.
[0019] Further, the temperature of the heating and stretching treatment for the third intermediate base band is 280° C. to 360° C., and / or the stretching ratio of the heating and stretching treatment for the third intermediate base band is 1.5 to 3 times.
[0020] Furthermore, the thickness of the polytetrafluoroethylene stretch tape is 1 to 15 μm, the width of the polytetrafluoroethylene stretch tape is 8 to 50 mm, and the density of the polytetrafluoroethylene stretch tape is greater than or equal to 1.8 g / cm 3 , the tensile strength of the polytetrafluoroethylene stretch tape is greater than or equal to 400 MPa.
[0021] Another aspect of the present invention provides a polytetrafluoroethylene stretched tape prepared by the method for preparing the polytetrafluoroethylene stretched tape.
[0022] Furthermore, the thickness of the polytetrafluoroethylene stretch tape is 1 to 15 μm, the width of the polytetrafluoroethylene stretch tape is 8 to 50 mm, and the density of the polytetrafluoroethylene stretch tape is greater than or equal to 1.8 g / cm 3 , the tensile strength of the polytetrafluoroethylene stretch tape is greater than or equal to 400 MPa.
[0023] Another aspect of the present invention provides a device for preparing a polytetrafluoroethylene stretched tape, comprising:
[0024] A mixer, used for mixing polytetrafluoroethylene resin and lubricating oil to obtain a mixed material;
[0025] A molding machine, used for pressing the mixed material into a green body to obtain a green body;
[0026] An extruder, used for extruding the embryo to obtain a polytetrafluoroethylene tape;
[0027] A first calender, used for heating and calendering the polytetrafluoroethylene-based tape to obtain a first intermediate base tape;
[0028] a first stretching machine, used for performing a heating and stretching treatment on the first intermediate base band to obtain a second intermediate base band;
[0029] a second calender, used for performing a heating and calendering treatment on the second intermediate base band to obtain a third intermediate base band; and
[0030] The second stretching machine is used to perform sintering and stretching treatment on the third intermediate base tape to obtain the polytetrafluoroethylene stretched tape.
[0031] The present invention adds the steps of heating stretching and heating calendering after subjecting the polytetrafluoroethylene based tape to the heating calendering treatment step and before the sintering stretching treatment step, thereby improving the stretching ratio, tensile strength and density of the polytetrafluoroethylene stretched tape, thereby obtaining an ultra-fine high-strength and high-density polytetrafluoroethylene stretched tape. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention provides a flow chart for preparing a polytetrafluoroethylene stretch tape.
[0033] Figure 2 This is a module composition diagram of a device for preparing a polytetrafluoroethylene stretch tape provided by the present invention.
[0034] Icon: 100 - preparation device; 10 - mixer; 20 - molding machine; 30 - extruder; 40 - first calender; 50 - first stretching machine; 60 - second calender; 70 - second stretching machine. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0037] See also Figure 1 The present invention provides a method for preparing an ultra-fine high-strength and high-density polytetrafluoroethylene stretch tape, comprising the following steps:
[0038] Step S11, mixing polytetrafluoroethylene resin and lubricating oil to obtain a mixed material.
[0039] Specifically, the polytetrafluoroethylene dispersion and the lubricating oil are mixed evenly and aged to obtain the mixed material, wherein the weight ratio between the polytetrafluoroethylene dispersion and the lubricating oil can be adjusted as required.
[0040] Step S12, pressing the mixed material into a green body.
[0041] Specifically, the matured mixed material is pressed to obtain the round rod-shaped embryo body. According to actual needs, the shape of the embryo body is not limited to the round rod shape, and can also be other shapes.
[0042] Step S13, extruding the embryo to obtain a polytetrafluoroethylene tape.
[0043] Specifically, the embryo is extruded into a flat film by an extruder, to obtain the polytetrafluoroethylene-based tape. It can be understood that the polytetrafluoroethylene-based tape in the present invention is a flat film. The size of the film, such as thickness, can be adjusted within a certain range according to actual needs.
[0044] Step S14, heating and calendering the polytetrafluoroethylene-based tape to obtain a first intermediate base tape.
[0045] Specifically, the polytetrafluoroethylene-based tape may be heated to 60° C., and the polytetrafluoroethylene may be calendered at 60° C. to obtain the first intermediate base tape.
[0046] In other embodiments, the temperature of the heating and calendering treatment is not limited to 60° C., and may be other temperatures, such as 59° C. or 61° C. It can be understood that the temperature of the heating and calendering treatment can be selected according to needs.
[0047] Step S15, heating and stretching the first intermediate baseband to obtain a second intermediate baseband.
[0048] Before the first intermediate base belt is subjected to the heating and stretching treatment, the first intermediate base belt may be subjected to a deoiling treatment to remove lubricating oil in the first intermediate base belt, thereby facilitating subsequent stretching.
[0049] In one embodiment, the temperature of the heating and stretching treatment on the first intermediate base band may be 300° C. to 340° C. Specifically, the temperature of the heating and stretching treatment on the first intermediate base band may be 320° C.
[0050] In one embodiment, the stretching ratio of the first intermediate base band during the heating and stretching process may be 10 to 15 times. Specifically, the stretching ratio of the first intermediate base band during the heating and stretching process may be 12 times.
[0051] Step S16, performing a heating and calendering process on the second intermediate base band to obtain a third intermediate base band.
[0052] In one embodiment, the temperature of the heating and calendering treatment on the second intermediate base belt may be 50° C. to 100° C. Specifically, the temperature of the heating and calendering treatment on the second intermediate base belt may be 75° C.
[0053] In the present invention, the second intermediate base band is subjected to a heating and calendering treatment to increase the density of the second intermediate substrate. Compared with the conventional method of increasing the substrate density by sintering, the method of increasing the substrate density by heating and calendering in the present invention is more efficient. At the same time, the heating and calendering treatment of the second intermediate base band can also increase the stretching ratio of the second intermediate substrate, thereby facilitating the production of a thinner product.
[0054] In addition, in the present invention, since the temperature for heating and calendering the second intermediate base band is relatively low, compared with the traditional high-temperature sintering method, the present invention is conducive to reducing energy consumption, thereby facilitating energy conservation and emission reduction.
[0055] Step S17, performing sintering and stretching treatment on the third intermediate base tape to obtain the polytetrafluoroethylene stretched tape.
[0056] In one embodiment, the temperature for sintering and stretching the third intermediate base band may be 360° C. to 430° C. Specifically, the temperature for sintering and stretching the third intermediate base band may be 395° C.
[0057] In one embodiment, the stretching ratio of the third intermediate base band during the sintering and stretching process may be 3 to 12 times. Specifically, the stretching ratio of the third intermediate base band during the sintering and stretching process may be 3 times.
[0058] In other embodiments, after the third intermediate base tape is subjected to the sintering and stretching treatment, the third intermediate base tape may be subjected to the heating and stretching treatment to improve the tensile strength of the third intermediate base tape, thereby obtaining the polytetrafluoroethylene stretch tape. It is understood that adding the heating and stretching treatment step after the sintering and stretching treatment can further improve the tensile strength of the polytetrafluoroethylene stretch tape.
[0059] In one embodiment, the temperature at which the third intermediate baseband is heated and stretched may be 280° C. to 360° C. Specifically, the temperature at which the third intermediate baseband is heated and stretched may be 310° C.
[0060] In one embodiment, the stretching ratio of the third intermediate base band during the heating and stretching process may be 1.5 to 3 times. Specifically, the stretching ratio of the third intermediate base band during the heating and stretching process may be 2 times.
[0061] In one embodiment, after the polytetrafluoroethylene stretch tape is obtained, the obtained polytetrafluoroethylene stretch tape can be rolled up to facilitate storage of the polytetrafluoroethylene stretch tape.
[0062] In one embodiment, the thickness of the polytetrafluoroethylene stretch tape may be 1 to 15 μm, and the width of the polytetrafluoroethylene stretch tape may be 8 to 50 mm. In one embodiment, the density of the polytetrafluoroethylene stretch tape may be greater than or equal to 1.8 g / cm 3 .
[0063] In one embodiment, the tensile strength of the polytetrafluoroethylene stretch tape may be greater than or equal to 400 MPa. Preferably, the tensile strength of the polytetrafluoroethylene stretch tape may be greater than or equal to 1000 MPa.
[0064] The present invention also provides an ultra-fine high-strength high-density polytetrafluoroethylene stretch tape prepared by the above preparation method. In one embodiment, the thickness of the polytetrafluoroethylene stretch tape can be 1 to 15 μm, and the width of the polytetrafluoroethylene stretch tape can be 8 to 50 mm. In one embodiment, the density of the polytetrafluoroethylene stretch tape can be greater than or equal to 1.8 g / cm 3 .
[0065] In one embodiment, the tensile strength of the polytetrafluoroethylene stretch tape may be greater than or equal to 400 MPa. Preferably, the tensile strength of the polytetrafluoroethylene stretch tape may be greater than or equal to 1000 MPa.
[0066] See also Figure 2 The present invention also provides a device 100 for preparing an ultra-fine high-strength high-density polytetrafluoroethylene stretch tape, which is used to prepare the ultra-fine high-strength high-density polytetrafluoroethylene stretch tape. In one embodiment, the preparation device 100 includes a mixer 10, a molding machine 20, an extruder 30, a first calender 40, a first stretching machine 50, a second calender 60, and a second stretching machine 70.
[0067] In one embodiment, the mixer 10 is used to mix polytetrafluoroethylene resin and lubricating oil to obtain a mixed material.
[0068] In one embodiment, the molding machine 20 is used to perform a compacting process on the mixed material to obtain a green body.
[0069] In one embodiment, the extruder 30 is used to extrude the embryo to obtain a polytetrafluoroethylene-based tape.
[0070] In one embodiment, the first calender 40 is used to perform heating and calendering treatment on the polytetrafluoroethylene-based tape to obtain a first intermediate base tape.
[0071] In one embodiment, the first stretching machine 50 is used to perform a heating and stretching process on the first intermediate base band to obtain a second intermediate base band.
[0072] In one embodiment, the second calender 60 is used to perform a heating and calendering process on the second intermediate base band to obtain a third intermediate base band.
[0073] In one embodiment, the second stretching machine 70 is used to perform a sintering and stretching process on the third intermediate base tape to obtain a stretched polytetrafluoroethylene tape.
[0074] In other embodiments, the preparation device 100 may include a third stretching machine (not shown). The third stretching machine is used to heat and stretch the third intermediate matrix after sintering and stretching to obtain the polytetrafluoroethylene stretched tape.
[0075] The present invention is further described below by means of specific examples.
[0076] Example 1
[0077] In the first step, 100 parts of polytetrafluoroethylene dispersion and 20 to 25 parts of lubricating oil are mixed evenly by weight, and then aged to obtain a mixed material.
[0078] In the second step, the matured mixed material is pressed into a green body to form a round rod-shaped embryo.
[0079] The third step is to extrude the round rod-shaped embryo into a paste to form a polytetrafluoroethylene-based tape, wherein the polytetrafluoroethylene-based tape is a flat film, and the thickness of the polytetrafluoroethylene-based tape is 1.0 mm, and the width of the polytetrafluoroethylene-based tape is 120-150 mm.
[0080] The fourth step is to heat the polytetrafluoroethylene tape to 60° C. for calendering to obtain a first intermediate base tape, wherein the thickness of the first intermediate base tape is 80 to 150 μm, and the width of the first intermediate base tape is 120 to 150 mm.
[0081] The fifth step is to de-oil the first intermediate base tape.
[0082] In the sixth step, the deoiled first intermediate base is subjected to a heating and stretching treatment in a group of rollers or multiple groups of rollers heated to 300°C to 340°C to obtain a second intermediate base. The stretching ratio is 10 to 15 times, the thickness of the second intermediate base is 15 to 60 μm, the width of the second intermediate base is 50 to 90 mm, and the density of the second intermediate base is less than or equal to 0.7 g / cm 3 .
[0083] In the seventh step, the second intermediate base is subjected to a heating and calendering treatment in a group of rollers heated to 50°C to 100°C to obtain a third intermediate base. The thickness of the third intermediate base is 10 to 30 μm, the width of the third intermediate base is 40 to 80 mm, and the density of the third intermediate base is greater than or equal to 1.9 g / cm 3 .
[0084] In the eighth step, the third intermediate base tape is sintered and stretched in an oven heated to 360° C. to 430° C. and an external stretching roller to obtain a polytetrafluoroethylene stretched tape, wherein the stretching ratio is 3 to 8 times.
[0085] Step 9: Roll up the polytetrafluoroethylene stretch tape.
[0086] Example 2
[0087] In the first step, 100 parts of polytetrafluoroethylene dispersion and 20 to 25 parts of lubricating oil are mixed evenly by weight, and then aged to obtain a mixed material.
[0088] In the second step, the matured mixed material is pressed into a green body to form a round rod-shaped embryo.
[0089] The third step is to extrude the round rod-shaped embryo into a paste to form a polytetrafluoroethylene-based tape, wherein the polytetrafluoroethylene-based tape is a flat film, and the thickness of the polytetrafluoroethylene-based tape is 1.0 mm, and the width of the polytetrafluoroethylene-based tape is 120-150 mm.
[0090] The fourth step is to heat the polytetrafluoroethylene tape to 60° C. for calendering to obtain a first intermediate base tape, wherein the thickness of the first intermediate base tape is 70 to 150 μm, and the width of the first intermediate base tape is 120 to 150 mm.
[0091] The fifth step is to de-oil the first intermediate base tape.
[0092] In the sixth step, the deoiled first intermediate base is subjected to a heating and stretching treatment in a group of rollers or multiple groups of rollers heated to 300°C to 340°C to obtain a second intermediate base. The stretching ratio is 10 to 15 times, the thickness of the second intermediate base is 12 to 60 μm, the width of the second intermediate base is 50 to 90 mm, and the density of the second intermediate base is less than or equal to 0.7 g / cm 3 .
[0093] Step 7: Heat and calender the second intermediate base belt in a group of rollers heated to 50°C to 100°C to obtain a third intermediate base belt. The thickness of the third intermediate base belt is 8 to 30 μm, the width of the third intermediate base belt is 40 to 80 mm, and the density of the third intermediate base belt is greater than or equal to 1.9 g / cm 3 .
[0094] In the eighth step, the third intermediate base tape is sintered and stretched in an oven heated to 360° C. to 430° C. and an external stretching roller to obtain a polytetrafluoroethylene stretched tape, wherein the stretching ratio is 3 to 12 times.
[0095] Step 9: Roll up the polytetrafluoroethylene stretch tape.
[0096] Example 2 is now summarized as follows:
[0097] The preparation method of Example 2 is substantially the same as that of Example 1, except that:
[0098] In the fourth step, the thickness of the first intermediate base is 70 to 150 μm; in the sixth step, the thickness of the second intermediate base is 12 to 60 μm; in the seventh step, the thickness of the third intermediate base is 8 to 30 μm; in the eighth step, the stretching ratio is 3 to 12 times.
[0099] Example 3
[0100] In the first step, 100 parts of polytetrafluoroethylene dispersion and 20 to 25 parts of lubricating oil are mixed evenly by weight, and then aged to obtain a mixed material.
[0101] In the second step, the matured mixed material is pressed into a green body to form a round rod-shaped embryo.
[0102] The third step is to extrude the round rod-shaped embryo into a paste to form a polytetrafluoroethylene-based tape, wherein the polytetrafluoroethylene-based tape is a flat film, and the thickness of the polytetrafluoroethylene-based tape is 1.0 mm, and the width of the polytetrafluoroethylene-based tape is 120-150 mm.
[0103] The fourth step is to heat the polytetrafluoroethylene tape to 60° C. for calendering to obtain a first intermediate base tape, wherein the thickness of the first intermediate base tape is 70 to 150 μm, and the width of the first intermediate base tape is 120 to 150 mm.
[0104] The fifth step is to de-oil the first intermediate base tape.
[0105] In the sixth step, the deoiled first intermediate base is subjected to a heating and stretching treatment in a group of rollers or multiple groups of rollers heated to 300°C to 340°C to obtain a second intermediate base. The stretching ratio is 10 to 15 times, the thickness of the second intermediate base is 12 to 60 μm, the width of the second intermediate base is 50 to 90 mm, and the density of the second intermediate base is less than or equal to 0.7 g / cm 3 .
[0106] Step 7: Heat and calender the second intermediate base belt in a group of rollers heated to 50°C to 100°C to obtain a third intermediate base belt. The thickness of the third intermediate base belt is 8 to 30 μm, the width of the third intermediate base belt is 40 to 80 mm, and the density of the third intermediate base belt is greater than or equal to 1.9 g / cm 3 .
[0107] In the eighth step, the third intermediate base tape is sintered and stretched in an oven heated to 360° C. to 430° C. and an external stretching roller to obtain a polytetrafluoroethylene stretched tape, wherein the stretching ratio is 3 to 12 times.
[0108] In the ninth step, the third intermediate base tape after sintering and stretching is heated and stretched in multiple groups of rollers heated to 280° C. to 360° C. to obtain a polytetrafluoroethylene stretched tape, wherein the stretching ratio is 1.5 to 3 times.
[0109] The tenth step is to roll up the polytetrafluoroethylene stretch tape.
[0110] Example 3 is now summarized as follows:
[0111] The steps from the first step to the eighth step in Example 3 are respectively the same as the steps from the first step to the eighth step in Example 2.
[0112] The thickness, width, density and tensile strength of the polytetrafluoroethylene stretched tapes prepared in Examples 1 to 3 were tested respectively. The test results are shown in Table 1 below.
[0113] Table 1
[0114]
[0115]
[0116] From Table 1 above, it can be seen that the thickness of the polytetrafluoroethylene stretched tape prepared by this method is 1-15 μm and the width is 8-50 mm. Among them, the density of the polytetrafluoroethylene stretched tape prepared in Examples 1-3 is greater than or equal to 1.8 g / cm 3 This indicates that the polytetrafluoroethylene stretched tape prepared by this method has a higher density.
[0117] In addition, it can be seen from Table 1 above that the tensile strength of the polytetrafluoroethylene stretched tapes prepared in Examples 1 to 3 is greater than or equal to 400 MPa. Among them, the tensile strength of the polytetrafluoroethylene stretched tapes prepared in Examples 2 and 3 even exceeds 1000 MPa. This shows that the polytetrafluoroethylene stretched tape prepared by this method has a high tensile strength.
[0118] In addition, the stretching ratio in the present invention is 80 to 150 times, while the stretching ratio in the traditional process is generally 10 to 30 times, so that the present invention can obtain a thinner polytetrafluoroethylene stretched tape product with greater tensile strength.
[0119] The present invention adds the steps of heating stretching and heating calendering after subjecting the polytetrafluoroethylene based tape to the heating calendering treatment step and before the sintering stretching treatment step, thereby improving the stretching ratio, tensile strength and density of the polytetrafluoroethylene stretched tape, thereby obtaining an ultra-fine high-strength and high-density polytetrafluoroethylene stretched tape.
[0120] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0121] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a polytetrafluoroethylene stretched tape, characterized in that: The following steps are involved: Mixing polytetrafluoroethylene resin and lubricating oil to obtain a mixed material; Performing green compaction processing on the mixed material to obtain a green body; Extruding the green body to obtain a polytetrafluoroethylene tape; Performing a heating and calendering process on the polytetrafluoroethylene-based tape to obtain a first intermediate base tape; performing a heating and stretching process on the first intermediate base band to obtain a second intermediate base band; performing a heating and calendering process on the second intermediate base band to obtain a third intermediate base band; and Performing sintering and stretching treatment on the third intermediate base tape to obtain the polytetrafluoroethylene stretched tape; The temperature of the heating and stretching treatment of the first intermediate base belt is 320°C to 340°C, and the stretching ratio of the heating and stretching treatment of the first intermediate base belt is 10 to 15 times; the temperature of the sintering and stretching treatment of the third intermediate base belt is 360°C to 395°C, and the stretching ratio of the sintering and stretching treatment of the third intermediate base belt is 3 to 12 times; After the third intermediate base tape is sintered and stretched, the method further comprises the following steps: Performing a heating and stretching treatment on the third intermediate base tape to obtain the polytetrafluoroethylene stretched tape; The temperature of the heating and stretching treatment of the third intermediate base band is 280° C. to 310° C., and the stretching ratio of the heating and stretching treatment of the third intermediate base band is 1.5 to 2 times; The thickness of the polytetrafluoroethylene stretch tape is 1 to 15 μm, the width of the polytetrafluoroethylene stretch tape is 8 to 50 mm, and the density of the polytetrafluoroethylene stretch tape is greater than or equal to 1.8 g / cm 3 , the tensile strength of the polytetrafluoroethylene stretch tape is greater than or equal to 400 MPa.
2. The method for preparing a polytetrafluoroethylene stretched tape according to claim 1, characterized in that: The temperature of the heating and calendering treatment of the second intermediate base tape is 50° C. to 100° C.
3. A polytetrafluoroethylene stretched tape prepared by the method for preparing a polytetrafluoroethylene stretched tape as claimed in any one of claims 1 to 2.
4. A device for preparing the polytetrafluoroethylene stretched tape as claimed in claim 3, characterized in that: include: A mixer, used for mixing polytetrafluoroethylene resin and lubricating oil to obtain a mixed material; A molding machine, used for pressing the mixed material into a green body to obtain a green body; An extruder, used for extruding the blank to obtain a polytetrafluoroethylene-based tape; A first calender, used for heating and calendering the polytetrafluoroethylene-based tape to obtain a first intermediate base tape; a first stretching machine, used for performing a heating and stretching treatment on the first intermediate base band to obtain a second intermediate base band; a second calender, used for performing a heating and calendering treatment on the second intermediate base band to obtain a third intermediate base band; as well as The second stretching machine is used to perform sintering and stretching treatment on the third intermediate base tape to obtain a polytetrafluoroethylene stretched tape.