Processing methods for recycling polystyrene waste

Through the dissolution and non-solvent washing technology of umbrella hydrocarbons, the problem of inconsistent properties of polystyrene recovery in the prior art was solved, and the recovery of polystyrene with low melt flow index and low additive content was achieved, and its application scope was expanded and improves the life cycle.

CN114773665BActive Publication Date: 2024-11-29POLYSTYVERT
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210524437.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2015-10-05
Publication Date
2024-11-29
Estimated Expiration
2035-10-05

AI Technical Summary

Technical Problem

The existing polystyrene waste recycling methods cannot produce new polystyrene with the same properties, and the melt flow index and additive content of the polystyrene are not in compliance with the use requirements, limiting its application scope.

Method used

By dissolving the polystyrene waste in the pseudohydrin, precipitating and washing with a non-solvent, dissolving, adding and separating repeatedly, finally recovered polystyrene with a low melt flow index and a low additive content is obtained by drying.

Benefits of technology

The production of recovered polystyrene with properties close to new polystyrene has been achieved, reducing additive and ash content, expanding its application range, and improving the life cycle of recovered polystyrene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114773665B_ABST
    Figure CN114773665B_ABST
Patent Text Reader

Abstract

The present invention relates to a processing method for recycling polystyrene waste. The present invention also relates to the use of a combination of p-cymene and a non-solvent with a boiling point of 98°C to 110°C at a pressure of 1 atm for recycling polystyrene and a composition for producing recycled polystyrene, the composition comprising polystyrene, p-cymene and a non-solvent with a boiling point of 98°C to 110°C at a pressure of 1 atm. The composition and processing method of the present invention allow the life cycle of the recycled polystyrene to be increased, and they have a very low MFI while avoiding the use of a large amount of additives and / or fillers.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a re-divisional application of the Chinese patent divisional application with application number 201910549840.6 and invention title "Processing method for recycling polystyrene waste". This divisional application is a divisional application of the original Chinese patent application with application number 201580065085.4 and invention title "Processing method for recycling polystyrene waste". Technical Field

[0002] The present disclosure relates to a process for recycling polystyrene waste. For example, it relates to a process for recycling polystyrene, the process comprising dissolving the polystyrene waste in a solvent such as p-cymene, and then precipitating and washing the polystyrene with a non-solvent. Background Art

[0003] Polystyrene waste, for example packaging of electronic products or furniture, food trays, merchandise and insulation can for example have an environmental impact.

[0004] For example, most polystyrene waste, whether post-consumer or post-industrial, is buried in landfills. For example, more than 40,000 tons of polystyrene waste is buried annually in Quebec. Further, 60,000 tons of new polystyrene is purchased and consumed annually in Quebec.

[0005] Known processes for recycling polystyrene do not produce recycled polystyrene with the same properties as virgin polystyrene. For example, known processes for recycling polystyrene do not produce recycled polystyrene with a melt flow index (MFI) that meets the technical specifications for using recycled polystyrene for the same applications as virgin polystyrene. To offset this loss in mechanical properties, recycled polystyrene is blended with virgin polystyrene in proportions that can rarely exceed 20%, even for less stringent applications.

[0006] Most industrial polystyrene articles are not composed solely of polystyrene; for example, they may contain chemicals added to the polymer to modify some physical, biological and / or chemical properties. Examples of additives are colorants, fillers, flame retardants, lubricants and plasticizers.

[0007] It would therefore be desirable to provide recycled polystyrene and a process for the processing of recycled polystyrene waste which would at least partially solve one of the problems mentioned or would be an alternative to the known processes for the processing of recycled polystyrene waste. Summary of the invention

[0008] Thus, according to one aspect of the present disclosure, there is provided a recycled polystyrene having a melt flow index of less than about 25 g / 10 min as measured according to ASTM D1238-13.

[0009] According to another aspect of the present disclosure, there is provided a recycled polystyrene having a melt flow index of less than about 25 g / 10 min as measured according to ASTM D1238-13 standard and an additive content of less than about 1 wt%.

[0010] According to another aspect of the present disclosure, there is provided a recycled polystyrene having a melt flow index of less than about 25 g / 10 min as measured according to ASTM D1238-13 and an ash content of less than about 1 wt % as measured according to ASTM D5630-13.

[0011] According to another aspect of the present disclosure, there is provided a recycled polystyrene having a melt flow index of less than about 25 g / 10 min as measured according to ASTM D1238-13 and an ash content of less than about 0.5 wt % as measured according to ASTM D5630-13.

[0012] According to another aspect of the present disclosure, a recycled polystyrene having a melt flow index of less than about 25 g / 10 min is provided.

[0013] According to another aspect of the present disclosure, there is provided a recycled polystyrene having a melt flow index of less than about 25 g / 10 min as measured according to the ASTM D1238-13 standard.

[0014] According to another aspect of the present disclosure, there is provided a processing method for recycling polystyrene waste, comprising:

[0015] dissolving the polystyrene waste in p-cymene under conditions such that a polystyrene / p-cymene mixture is obtained;

[0016] adding the polystyrene / p-cymene mixture to the first portion of the hydrocarbon polystyrene nonsolvent under conditions to obtain precipitated polystyrene and a first portion of hydrocarbon waste liquor;

[0017] separating the precipitated polystyrene from the first portion of the hydrocarbon waste stream;

[0018] optionally repeating the dissolving, adding and separating;

[0019] washing the precipitated polystyrene with a second portion of the hydrocarbon polystyrene nonsolvent under conditions to obtain washed polystyrene and a second portion of hydrocarbon waste liquor;

[0020] separating the washed polystyrene from a second portion of the hydrocarbon waste liquor;

[0021] washing the washed polystyrene with a third portion of a hydrocarbon polystyrene nonsolvent under conditions to obtain a second washed polystyrene and a third portion of hydrocarbon waste liquor;

[0022] separating the second washed polystyrene from a third portion of the hydrocarbon waste stream; and

[0023] Optionally, the second washed polystyrene is dried under conditions to obtain dry polystyrene.

[0024] Therefore, according to another aspect of the present disclosure, there is provided a processing method for recycling polystyrene waste, comprising:

[0025] dissolving the polystyrene waste in p-cymene under conditions such that a polystyrene / p-cymene mixture is obtained;

[0026] adding the polystyrene / p-cymene mixture to the first portion of the hydrocarbon polystyrene nonsolvent under conditions to obtain precipitated polystyrene and a first portion of hydrocarbon waste liquor;

[0027] separating the precipitated polystyrene from the first portion of the hydrocarbon waste stream;

[0028] optionally repeating the dissolving, adding and separating;

[0029] washing the precipitated polystyrene with a second portion of the hydrocarbon polystyrene nonsolvent under conditions to obtain washed polystyrene and a second portion of hydrocarbon waste liquor;

[0030] separating the washed polystyrene from a second portion of the hydrocarbon waste liquor;

[0031] washing the washed polystyrene with a third portion of a hydrocarbon polystyrene nonsolvent under conditions to obtain a second washed polystyrene and a third portion of hydrocarbon waste liquor;

[0032] separating the second washed polystyrene from a third portion of the hydrocarbon waste stream;

[0033] removing the remaining hydrocarbon waste by wringing and / or compressing the secondary washed polypropylene; and

[0034] The second washed polystyrene is dried under conditions such that dry polystyrene is obtained.

[0035] The present disclosure also includes recycled polystyrene prepared according to the processing method of recycling polystyrene waste of the present disclosure.

[0036] Polystyrene waste, such as expanded polystyrene waste, is typically bulky and light, whereas a polystyrene / p-cymene mixture typically has a higher density and can therefore be transported at a lower cost. Thus, if, for example, a polystyrene / p-cymene mixture is obtained at a first location, and the process further comprises transporting the polystyrene / p-cymene mixture to a second location where a subsequent step in the process is performed, the process of the present disclosure can, for example, save on transportation costs.

[0037] The processing methods of the recycled polystyrene waste of the present disclosure can, for example, allow the removal of most additives (e.g., chemicals added to the polymer to modify some physical, biological and / or chemical properties), and can produce recycled polystyrene with properties very close to those of new polystyrene. The recycled polystyrene prepared by the processing methods of the present disclosure can be, for example, suitable for the same uses as new polystyrene, such as for preparing new polystyrene articles. For example, the recycled polystyrene prepared by the processing methods of the present disclosure can have, for example, an MFI within an effective range for such uses.

[0038] The recovered polystyrene and the processing method for obtaining the recovered polystyrene of the present disclosure have been found to be quite useful. In fact, it has been found that such recovered polymers and processing methods allow the provision of recovered polystyrene with very low contents of additives (fillers and / or lubricants). This also results in the production of recovered polystyrene with very low ash contents. For example, when these processing methods are applied to white expanded or extruded polystyrene, the final product is very clear and transparent to light transmission. Such features of the polymers and processing methods of the present disclosure are very interesting because they allow the life cycle of the recovered polystyrene to be significantly improved. In fact, the uses of recovered polystyrene are generally quite limited, considering the various additives contained in the recovered polystyrene, so they do not meet the requirements of certain uses and applications that can be performed with polystyrene. Some manufacturers are also reluctant to use recovered polystyrene because it has too high a content of additives and the additives can affect or reduce the properties of the polystyrene or the properties of the products made with the recovered polystyrene in this way. This is clearly not the case with the polymers and processing methods mentioned in the present disclosure. In contrast, since users of such products are not forced to recycle the products, high levels of additives and / or fillers are almost never obtained, so the very low amounts of additives and / or fillers found in the polymers of the present disclosure allow these recycled polystyrenes to be used in many different applications and to be recycled multiple times and to obtain low MFI values.

[0039] Thus, the polymers and processing methods of the present disclosure allow for an increased life cycle of recycled polystyrene (it is possible to recycle it multiple times while maintaining the desired specifications and properties), and they have very low MFI while avoiding the use of large amounts of additives and / or fillers. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In the following figures, various embodiments of the present disclosure are shown by way of example only:

[0041] Figure 1 is a schematic diagram of a processing method according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0042] Unless otherwise stated, the definitions and embodiments described in this section and other sections are intended to apply to all embodiments and aspects of the disclosure described herein, as understood by those skilled in the art, and are appropriate for all embodiments and aspects of the disclosure.

[0043] As used in this disclosure, the singular forms "a", "an", and "the" include plural references unless the content clearly dictates otherwise. For example, inclusion of "a hydrocarbon polystyrene non-solvent" should be understood to refer to one hydrocarbon polystyrene non-solvent, or certain aspects of two or more additional hydrocarbon polystyrene non-solvents.

[0044] In embodiments comprising an "additional" or "second" component, such as an additional or second hydrocarbon polystyrene non-solvent, the second component as used herein is different from the other components or the first component. The "third" component is different from the other components, the first component, and the second component, and similarly different from the further listed or "additional" components.

[0045] As used herein, the term "additive" refers to a chemical substance added to a polymer to modify at least one physical, biological and / or chemical property. Non-limiting examples of additives are: colorants, fillers, flame retardants, lubricants, and plasticizers.

[0046] In the understanding of the scope of the present disclosure, the term "comprising" and its derivatives as used herein are intended to be open terms specifying the presence of stated features, elements, components, groups, integers and / or steps, but not excluding the presence of other unstated features, elements, components, groups, integers and / or steps. The above also applies to words with similar meanings, such as the terms "including", "having" and their derivatives. As used herein, the term "consisting of" and its derivatives are intended to be closed terms specifying the presence of stated features, elements, components, groups, integers and / or steps, but excluding the presence of other unstated features, elements, components, groups, integers and / or steps. As used herein, the term "consisting essentially of" is intended to specify the presence of stated features, elements, components, groups, integers and / or steps as well as features, elements, components, groups, integers and / or steps that do not substantially affect the basic and novel properties of the features, elements, components, groups, integers and / or steps.

[0047] As used herein, terms of degree such as "about" and "approximately" refer to a reasonable amount of deviation of the modified term that does not result in a significant change in the end result. If the deviation does not negate the meaning of the word it modifies, these terms of degree should be interpreted as including a deviation of at least ± 5% or at least ± 10% of the modified term.

[0048] The term "hydrocarbon polystyrene non-solvent" as used herein refers to, for example, a hydrocarbon-based compound or mixture thereof in which polystyrene is substantially insoluble. The selection of an appropriate hydrocarbon polystyrene non-solvent for the processing method of the present disclosure can be made by a person skilled in the art. For example, a person skilled in the art will appreciate that under the conditions used in the processing method of the present disclosure to obtain precipitated polystyrene and in the step of washing with a hydrocarbon polystyrene non-solvent, most non-polar additives (e.g., hexabromocyclododecane and silicone oil) and para-cymene typically found in polystyrene waste should be substantially soluble in the hydrocarbon polystyrene non-solvent. A person skilled in the art will also appreciate that, for example, a hydrocarbon polystyrene non-solvent having a glass transition temperature (T ) of about or slightly above the glass transition temperature (T ) of the polystyrene waste to be recycled can be selected. g ) are useful as hydrocarbon polystyrene non-solvents.

[0049] The examples provided below are non-limiting and are used to better illustrate the processing methods of the present disclosure.

[0050] An exemplary process flow chart of the processing method disclosed in the present invention is shown in Figure 1 Exemplary process 10 is a process for recycling polystyrene waste. Figure 1In an exemplary processing method 10, polystyrene waste can be dissolved 12 in p-cymene under conditions to obtain a polystyrene / p-cymene mixture. For example, if the polystyrene / p-cymene mixture includes insoluble matter, the polystyrene / p-cymene mixture can be optionally filtered 14 under conditions to remove the insoluble matter. The polystyrene / p-cymene mixture can then be added 16 to a first portion of a hydrocarbon waste liquor under conditions to obtain precipitated polystyrene and a first portion of a hydrocarbon waste liquor. Next, the precipitated polystyrene can be separated from the first portion of the hydrocarbon waste liquor. The precipitated polystyrene can then be washed 18 with a second portion of a hydrocarbon polystyrene non-solvent under conditions to obtain washed polystyrene and a second portion of the hydrocarbon waste liquor. Thereafter, the washed polystyrene can be separated from the second portion of the hydrocarbon waste liquor. The washed polystyrene can then be washed 20 with a third portion of a hydrocarbon polystyrene non-solvent under conditions to obtain a second washed polystyrene and a third portion of the hydrocarbon waste liquor. The second washed polystyrene can be separated from the third portion of the hydrocarbon waste liquor. The remaining hydrocarbon waste liquid may optionally be removed by wringing and / or compressing the secondary washed polystyrene. The secondary washed polystyrene may then optionally be dried 22 under conditions to obtain dried polystyrene. The dried polystyrene may then optionally be packaged 24, for example, the processing method may further include treating the dried polystyrene under conditions to obtain polystyrene particles, and the polystyrene particles may be packaged 24. Para-cymene and / or hydrocarbon polystyrene non-solvent may optionally be recovered 26, for example, by a process including distilling a first portion of the hydrocarbon waste liquid, a second portion of the hydrocarbon waste liquid, and / or a third portion of the hydrocarbon waste liquid under conditions to obtain para-cymene and / or hydrocarbon polystyrene non-solvent. Para-cymene may optionally be recovered for dissolving 12. The hydrocarbon polystyrene non-solvent may optionally be recovered for addition 16, first washing 18, and / or second washing 20.

[0051] For example, the polystyrene / p-cymene mixture can include polystyrene in an amount equal to or less than about 33 wt % based on the total weight of the polystyrene / p-cymene mixture.

[0052] For example, the polystyrene / p-cymene mixture can include polystyrene in an amount of about 10 wt % to about 30 wt %, based on the total weight of the polystyrene / p-cymene mixture.

[0053] For example, the polystyrene / p-cymene mixture can include polystyrene in an amount of about 14 wt % to about 28 wt %, based on the total weight of the polystyrene / p-cymene mixture.

[0054] For example, the polystyrene / p-cymene mixture can include polystyrene in an amount of about 15 wt % to about 27 wt %, based on the total weight of the polystyrene / p-cymene mixture.

[0055] For example, the polystyrene / p-cymene mixture can include polystyrene in an amount of about 16 wt % to about 25 wt %, based on the total weight of the polystyrene / p-cymene mixture.

[0056] For example, polystyrene waste can be dissolved in para-cymene in a container having a chamber containing para-cymene and at least one opening toward the chamber for adding the polystyrene waste to the para-cymene, and the processing method can further include adding the polystyrene waste to the para-cymene contained in the chamber.

[0057] For example, the container may further include an outlet.

[0058] For example, the container may further include means for driving the polystyrene waste into the para-cymene.

[0059] For example, the means for forcing polystyrene waste into para-cymene may include a metal grid inside the container.

[0060] For example, the container may further include means for indicating when the capacity of the chamber has been reached.

[0061] For example, the means for indicating when the capacity of the chamber has been reached may be an indicator light.

[0062] For example, the indicator light can be connected to a float switch in the room.

[0063] For example, the polystyrene / p-cymene mixture may contain insoluble matter, and the method may further include filtering the polystyrene / p-cymene mixture under conditions that remove the insoluble matter before adding the polystyrene / p-cymene mixture to the first portion of the hydrocarbon polystyrene non-solvent. For example, the insoluble matter may be selected from polystyrene / butadiene mixtures, styrene copolymer dust, adhesives, metals, wood, plastics, pollutants, and mixtures thereof. For example, filtering may include multi-stage filtration from coarse to fine. For example, unless butadiene has been heavily cross-linked, it is soluble in p-cymene.

[0064] For example, the conditions for obtaining precipitated polystyrene and a first portion of hydrocarbon waste liquor may include adding a polystyrene / p-cymene mixture to a first portion of the hydrocarbon polystyrene nonsolvent at the boiling point of the hydrocarbon polystyrene nonsolvent, agitating for a period of time to allow the p-cymene to diffuse from the polystyrene / p-cymene mixture into the hydrocarbon polystyrene nonsolvent, and continuing to a sufficient extent.

[0065] For example, the time may be from about 5 minutes to about 10 minutes.

[0066] For example, agitating may include stirring with a mechanical stirrer.

[0067] For example, greater than about 90 weight percent of the p-cymene in the polystyrene / p-cymene mixture, based on the total weight of the polystyrene / p-cymene mixture, can be diffused into the hydrocarbon polystyrene non-solvent.

[0068] For example, the volume ratio of the first portion of the hydrocarbon polystyrene non-solvent to the polystyrene / p-cymene mixture can be from about 2:1 to about 4:1.

[0069] For example, the volume ratio of the first portion of the hydrocarbon polystyrene non-solvent to the polystyrene / p-cymene mixture can be about 3:1.

[0070] For example, the precipitated polystyrene may be separated from the first portion of the hydrocarbon waste liquor by a process that includes decanting the first portion of the hydrocarbon waste liquor from the precipitated polystyrene.

[0071] For example, the conditions for obtaining washed polystyrene and a second portion of hydrocarbon waste liquor may include adding a second portion of the hydrocarbon polystyrene non-solvent to the precipitated polystyrene at the boiling point of the hydrocarbon polystyrene non-solvent, agitating for a period of time to allow diffusion of para-cymene from the precipitated polystyrene into the hydrocarbon polystyrene non-solvent, and continuing to a sufficient extent.

[0072] For example, the time can be about 1 minute to about 15 minutes. For example, the time can be about 10 minutes. For example, the time can be about 2 minutes to about 5 minutes. For example, stirring can include stirring with a mechanical stirrer.

[0073] For example, the washed polystyrene can include less than about 0.3 wt% p-cymene. For example, the washed polystyrene can include less than about 0.1 wt% p-cymene.

[0074] For example, the volume ratio of the second portion of the hydrocarbon polystyrene nonsolvent to the precipitated polystyrene can be about 1:2 to about 2: 1. For example, the volume ratio of the second portion of the hydrocarbon polystyrene nonsolvent to the precipitated polystyrene can be about 1:1.

[0075] For example, the washed polystyrene may be separated from the second portion of the hydrocarbon waste liquor by a process that includes decanting the second portion of the hydrocarbon waste liquor from the washed polystyrene.

[0076] For example, the conditions for obtaining the second washed polystyrene and the third portion of hydrocarbon waste liquor may include adding the third portion of the hydrocarbon polystyrene non-solvent to the washed polystyrene at the boiling point of the hydrocarbon polystyrene non-solvent, agitating for a period of time to allow diffusion of para-cymene from the washed polystyrene into the hydrocarbon polystyrene non-solvent, and continuing to a sufficient extent.

[0077] For example, the time can be about 1 minute to about 10 minutes. For example, the time can be about 5 minutes. For example, agitation can include stirring with a mechanical stirrer.

[0078] For example, the double washed polystyrene can include less than about 0.1 wt% p-cymene. For example, the double washed polystyrene can include less than about 0.05 wt% p-cymene.

[0079] For example, the volume ratio of the third portion of the hydrocarbon polystyrene nonsolvent to the washed polystyrene may be about 1:2 to about 2: 1. For example, the volume ratio of the third portion of the hydrocarbon polystyrene nonsolvent to the washed polystyrene may be about 1:1.

[0080] For example, the secondarily washed polystyrene may be separated from the third portion of the hydrocarbon waste liquor by a process that includes decanting the third portion of the hydrocarbon waste liquor from the secondarily washed polystyrene.

[0081] For example, after separating the secondarily washed polystyrene from the third portion of the hydrocarbon waste liquor and before drying, the processing method may further include removing the remaining hydrocarbon waste liquor by wringing and / or compressing the secondarily washed polystyrene.

[0082] For example, at least one of the first portion of hydrocarbon polystyrene non-solvent, the second portion of hydrocarbon polystyrene non-solvent, and the third portion of hydrocarbon polystyrene non-solvent may include, consist of, or consist essentially of a hydrocarbon polystyrene non-solvent having a boiling point of about 98°C to about 110°C or about 105°C to about 110°C at a pressure of 1 atm.

[0083] For example, the first portion of the hydrocarbon polystyrene non-solvent, the second portion of the hydrocarbon polystyrene non-solvent, and the third portion of the hydrocarbon polystyrene non-solvent may include, consist of, or consist essentially of C6-C8 alkanes or petroleum distillates.

[0084] For example, the first portion of the hydrocarbon polystyrene nonsolvent, the second portion of the hydrocarbon polystyrene nonsolvent, and the third portion of the hydrocarbon polystyrene nonsolvent can include, consist of, or consist essentially of C6-C8 alkanes.

[0085] For example, the first portion of the hydrocarbon polystyrene nonsolvent, the second portion of the hydrocarbon polystyrene nonsolvent, and the third portion of the hydrocarbon polystyrene nonsolvent can include, consist of, or consist essentially of petroleum distillates.

[0086] For example, the first portion of the hydrocarbon polystyrene nonsolvent, the second portion of the hydrocarbon polystyrene nonsolvent, and the third portion of the hydrocarbon polystyrene nonsolvent can include, consist of, or consist essentially of n-heptane.

[0087] For example, the first portion of the hydrocarbon polystyrene nonsolvent, the second portion of the hydrocarbon polystyrene nonsolvent, and the third portion of the hydrocarbon polystyrene nonsolvent can all be the same hydrocarbon polystyrene nonsolvent.

[0088] For example, the first portion of the hydrocarbon polystyrene nonsolvent, the second portion of the hydrocarbon polystyrene nonsolvent, and the third portion of the hydrocarbon polystyrene nonsolvent may all be different hydrocarbon polystyrene nonsolvents.

[0089] For example, the second portion of the hydrocarbon polystyrene nonsolvent and the third portion of the hydrocarbon polystyrene nonsolvent may be the same hydrocarbon polystyrene nonsolvent, and the first portion of the hydrocarbon polystyrene nonsolvent may be a different hydrocarbon polystyrene nonsolvent.

[0090] For example, the second portion of the hydrocarbon polystyrene nonsolvent and the third portion of the hydrocarbon polystyrene nonsolvent may include, consist of, or consist essentially of n-heptane, and the first portion of the hydrocarbon polystyrene nonsolvent may include, consist of, or consist essentially of n-hexane.

[0091] For example, the conditions for obtaining dried polystyrene may include drying the secondary washed polystyrene at a temperature and time for removing the remaining hydrocarbon polystyrene non-solvent, continuing to a sufficient extent. For example, the secondary washed polystyrene may be dried at a temperature of about 115° C. to about 125° C. For example, the secondary washed polystyrene may be dried at a temperature of about 120° C.

[0092] For example, the conditions for obtaining a dried polystyrene may include drying the second washed polystyrene using an infrared dryer for a period of time to remove the remaining hydrocarbon polystyrene non-solvent, continuing to a sufficient degree.

[0093] For example, the polystyrene waste may include polar impurities, and the processing method may further include washing the polystyrene waste with a polar organic solvent under conditions to remove the polar impurities.

[0094] For example, the polar organic solvent may include, consist essentially of, or consist of methanol or ethanol. For example, the polar organic solvent may include, consist essentially of, or consist of methanol. For example, the polar organic solvent may include, consist essentially of, or consist of ethanol.

[0095] For example, the processing method may further include distilling the first portion of the hydrocarbon waste liquid, the second portion of the hydrocarbon waste liquid, and / or the third portion of the hydrocarbon waste liquid under conditions to obtain p-cymene and / or a hydrocarbon polystyrene non-solvent.

[0096] For example, the processing method may further include recovering p-cymene for use in the dissolving step.

[0097] For example, the processing method can further include recovering the hydrocarbon polystyrene non-solvent for use in the adding step, the first washing step, and / or the second washing step.

[0098] For example, the processing method may further include treating the dried polystyrene under conditions to obtain polystyrene particles. For example, the conditions to obtain polystyrene particles may include extruding the dried polystyrene at a temperature of about 140°C to about 160°C.

[0099] For example, the processing method may further include packaging the polystyrene particles. Suitable means for packaging the polystyrene particles may be selected by a person skilled in the art.

[0100] For example, the processing method may further include adding an antioxidant during the dissolving step, the adding step, the first washing step, and / or the second washing step. For example, the processing method may further include adding an antioxidant during the dissolving step.

[0101] For example, the antioxidant can comprise, consist essentially of, or consist of octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate.

[0102] For example, the antioxidant may be added in an amount of about 0.1 wt % to about 2 wt % based on the total weight of the polystyrene. For example, the antioxidant may be added in an amount of about 1 wt % based on the total weight of the polystyrene.

[0103] For example, the antioxidant may be added in an amount of about 0.5 wt % to about 2 wt % based on the total weight of the polystyrene. For example, the antioxidant may be added in an amount of about 1 wt % based on the total weight of the polystyrene.

[0104] For example, the processing method may further include adding an additive for lowering or increasing the melt flow index to the polystyrene / p-cymene mixture.

[0105] For example, the additive for reducing the melt flow index can include, consist essentially of, or consist of lime, talc, silicon dioxide, silicon hydroxide, aluminum oxide, aluminum hydroxide, or a combination thereof. For example, the additive for reducing the melt flow index can include, consist essentially of, or consist of lime. For example, the additive for reducing the melt flow index can include, consist essentially of, or consist of talc.

[0106] For example, the additive for improving the melt flow index may include about 0.0001 wt % to about 1 wt % of silicone oil. For example, about 0.01 wt % to 0.1 wt % of silicone oil may be added.

[0107] For example, based on the total weight of the polystyrene, the additive for reducing the melt flow index can be added in an amount of about 0.5 wt% to about 25 wt%. For example, based on the total weight of the polystyrene, the additive for reducing the melt flow index can be added in an amount of about 0.5 wt% to about 5 wt%. For example, based on the total weight of the polystyrene, the additive for reducing the melt flow index can be added in an amount of about 1 wt%.

[0108] For example, the polystyrene waste can be post-industrial waste, post-consumer waste, or a combination thereof. For example, the polystyrene waste can be post-industrial waste. For example, the polystyrene waste can be post-consumer waste. For example, the polystyrene waste can be a combination of post-industrial waste and post-consumer waste.

[0109] For example, the polystyrene waste may comprise, consist essentially of, or consist of expanded polystyrene. For example, the polystyrene waste may comprise, consist essentially of, or consist of white expanded polystyrene. For example, the polystyrene waste may comprise, consist essentially of, or consist of compressed polystyrene.

[0110] For example, the processing method may further include grinding the polystyrene waste prior to dissolving.

[0111] For example, a polystyrene / p-cymene mixture can be obtained at a first location, and the process can further include transporting the polystyrene / p-cymene mixture to a second location where a subsequent step in the process is performed.

[0112] The present disclosure also includes recycled polystyrene prepared according to the processing method of recycling polystyrene waste of the present disclosure.

[0113] For example, polystyrene waste may include other copolymers. For example, it may include butadiene (HIPS), a copolymer of styrene and acrylonitrile (SAN) or a copolymer of acrylonitrile, butadiene and styrene (ABS).

[0114] For example, the waste polystyrene may be a polystyrene-co-butadiene copolymer.

[0115] For example, embodiments of the present disclosure directed to recycled polystyrene may be varied as discussed herein with respect to the presently disclosed methods of processing recycled polystyrene waste.

[0116] For example, the polystyrene recovered can have a melt flow index of less than about 40 g / 10 min. For example, the polystyrene recovered can have a melt flow index of about 3 to about 30 g / 10 min. For example, the polystyrene recovered can have a melt flow index of about 3 to about 25 g / 10 min. For example, the polystyrene recovered can have a melt flow index of less than about 25 g / 10 min. For example, the polystyrene recovered can have a melt flow index of about 10 to about 20 g / 10 min.

[0117] For example, the polystyrene recovered can have a melt flow index of less than about 40 g / 10 min. For example, the polystyrene recovered can have a melt flow index of about 5 to about 30 g / 10 min. For example, the polystyrene recovered can have a melt flow index of about 5 to about 25 g / 10 min. For example, the polystyrene recovered can have a melt flow index of less than about 25 g / 10 min. For example, the polystyrene recovered can have a melt flow index of about 10 to about 20 g / 10 min.

[0118] For example, the polystyrene recovered can have a melt flow index of less than about 30g / 10min. For example, the polystyrene recovered can have a melt flow index of about 3 to about 25g / 10min. For example, the polystyrene recovered can have a melt flow index of about 1 to about 15g / 10min. For example, the polystyrene recovered can have a melt flow index of about 10 to about 15g / 10min. For example, the polystyrene recovered can have a melt flow index of about 5 to about 12g / 10min. For example, the polystyrene recovered can have a melt flow index of about 2 to about 12g / 10min. For example, the polystyrene recovered can have a melt flow index of less than about 15g / 10min. For example, the polystyrene recovered can have a melt flow index of less than about 12g / 10min.

[0119] For example, recycled polystyrene may have an additive content of less than about 5 wt%.

[0120] For example, recycled polystyrene may have an additive content of less than about 3 wt%.

[0121] For example, recycled polystyrene may have an additive content of less than about 2 wt%.

[0122] For example, recycled polystyrene may have an additive content of less than about 1 wt %.

[0123] For example, recycled polystyrene may have an additive content of less than about 0.5 wt%.

[0124] For example, recycled polystyrene may have an additive content of less than about 0.1 wt%.

[0125] For example, recycled polystyrene may have an additive content of less than about 0.05 wt%.

[0126] For example, the recycled polystyrene may have an additive content of about 0.05 wt % to about 1 wt %.

[0127] For example, the recycled polystyrene may have an additive content of about 0.1 wt % to about 1 wt %.

[0128] For example, recycled polystyrene may have a filler content of less than about 5 wt%.

[0129] For example, recycled polystyrene may have a filler content of less than about 3 wt%.

[0130] For example, recycled polystyrene may have a filler content of less than about 2 wt%.

[0131] For example, recycled polystyrene may have a filler content of less than about 1 wt %.

[0132] For example, recycled polystyrene may have a filler content of less than about 0.5 wt%.

[0133] For example, recycled polystyrene may have a filler content of less than about 0.1 wt%.

[0134] For example, recycled polystyrene may have a filler content of less than about 0.05 wt%.

[0135] For example, recycled polystyrene may have a filler content of about 0.05 wt % to about 1 wt %.

[0136] For example, recycled polystyrene may have a filler content of about 0.1 wt % to about 1 wt %.

[0137] For example, the filler may be an inorganic filler.

[0138] For example, recycled polymers can be obtained by recycling polystyrene waste involving treatment with solvents and non-solvents.

[0139] For example, the recycled polymer can be obtained by recycling polystyrene waste involving treatment with a solvent, p-cymene, and a hydrocarbon polystyrene non-solvent, which is a C6-C8 alkane or a mixture thereof.

[0140] For example, polystyrene waste can include polystyrene having an average molecular weight of about 200,000 to about 350,000 g / mol.

[0141] For example, polystyrene waste can include polystyrene having an average molecular weight of about 230,000 to about 260,000 g / mol.

[0142] For example, polystyrene waste can include polystyrene having an average molecular weight of about 260,000 to about 300,000 g / mol.

[0143] For example, recycled polystyrene can be transparent.

[0144] For example, recycled polystyrene can be clear.

[0145] For example, recycled polystyrene can be substantially transparent.

[0146] For example, recycled polystyrene may be at least substantially transparent.

[0147] For example, recycled polystyrene can be obtained by any of the processes and / or methods described in this disclosure.

[0148] Provided is a use of the recycled polystyrene of the present disclosure for preparing a mixture comprising the recycled polystyrene and virgin polystyrene.

[0149] Also provided are methods of using the recycled polystyrene of the present disclosure, the methods comprising mixing the recycled polystyrene with virgin polystyrene.

[0150] For example, the mixture can include at least about 10 wt%, at least about 15 wt%, at least about 20 wt%, about 1 wt% to about 50 wt%, about 5 wt% to about 50 wt%, or about 5 wt% to about 30 wt% recycled polystyrene.

[0151] For example, recycled polystyrene may include other copolymers. For example, it may include butadiene (HIPS), a copolymer of styrene and acrylonitrile (SAN) or a copolymer of acrylonitrile, butadiene and styrene (ABS).

[0152] For example, the recycled polystyrene may be a styrene-butadiene copolymer.

[0153] According to another aspect of the present disclosure, there is provided a method for controlling the recovery of polystyrene, comprising:

[0154] providing a consumer with at least one container for storing polystyrene waste;

[0155] providing instructions to a consumer on how to dissolve polystyrene waste in at least one container using at least one solvent;

[0156] optionally monitoring the concentration of polystyrene waste entering at least one solvent, and / or the volume of liquid and / or solid contained in at least one container;

[0157] removing at least a portion of liquid contents contained in at least one container, the liquid contents comprising polystyrene waste dissolved in at least one solvent;

[0158] optionally adding an amount of at least one solvent to at least one container;

[0159] At least a portion of the liquid contents contained in the at least one container is transported to a facility where the polystyrene waste is recycled or processed for conversion of the polystyrene waste into recycled polystyrene.

[0160] According to another aspect of the present disclosure, there is provided a method for storing polystyrene waste and recycling polystyrene, the method comprising:

[0161] dissolving polystyrene waste in at least one container by using at least one solvent;

[0162] optionally monitoring the concentration of polystyrene waste entering at least one solvent and / or the volume of liquid and / or solid contained in at least one container;

[0163] removing at least a portion of liquid contents contained in at least one container, the liquid contents comprising polystyrene waste dissolved in at least one solvent;

[0164] optionally adding an amount of at least one solvent to at least one container;

[0165] At least a portion of the liquid contents contained in the at least one container is transported to a facility where the polystyrene waste is recycled or processed for conversion of the polystyrene waste into recycled polystyrene.

[0166] For example, the recycling of polystyrene or the conversion of polystyrene waste into recycled polystyrene is performed by the process as defined in the present disclosure.

[0167] For example, transportation may be carried out by tank truck transport.

[0168] For example, the transport may be carried out by tank train transport.

[0169] For example, transportation can be done with the help of pipelines.

[0170] For example, transport can take place via pipelines.

[0171] Example

[0172] Example 1

[0173] Recycling of polystyrene waste

[0174] In this study, polystyrene waste was recycled using a method that included five main steps according to the following sequence:

[0175] 1. Dissolve polystyrene in para-cymene 2. Filter the PS / para-cymene mixture to remove undissolved material

[0176] 3. Wash with a non-polar solvent that is a non-solvent for PS

[0177] 4. Drying

[0178] 5. Forming and Packaging PS Plastic Beads

[0179] In the first step (dissolution), polystyrene waste, such as post-industrial expanded polystyrene, is dissolved in p-cymene (1-methyl-4-(1-methylethyl)benzene, one of the three possible isomers of cymene and the only one that exists in nature). The solubility limit of polystyrene in p-cymene is 33% (w / w) or 28.5% (v / v) at room temperature, and the density of the polystyrene / p-cymene mixture reaches a value of 1.06 kg / L, which is higher than the density of pure p-cymene, which is 0.86 kg / L. It is possible to reach the solubility limit, but the dissolution rate is reduced to 1 / 3.

[0180] In the dissolution step, polystyrene loses its structural properties and the volume it occupies decreases. Various non-polar additives including hexabromocyclododecane (HBCD) and silicone oil used in the manufacture of polystyrene are dissolved in a p-cymene solvent. This step is performed in a closed ventilated tank called a dissolution assembly. The purpose of this assembly is to maximize the amount of polystyrene that can be dissolved in a given time. For example, a metal grid inside the dissolution assembly can push expanded polystyrene items into p-cymene, which can, for example, reduce the dissolution time from hours to minutes.

[0181] The third step (washing) has the following objectives: (1) precipitating the polystyrene; (2) recovering p-cymene for reuse in step 1; and (3) eliminating various additives that may alter the mechanical properties of the recovered polystyrene.

[0182] This step involves first precipitating the dissolved polystyrene with hexane, heptane, or any other hydrocarbon with an appropriate boiling point. Although heptane was observed to provide the best results in the washing step, other hydrocarbons may also be useful. Hexane and octane were tested in this study. Petroleum distillates with a boiling point of about 100° C. to about 120° C. may also be useful and may provide, for example, reduced process and / or production costs.

[0183] For example, the solvent may have a T of about or slightly higher than that of the polystyrene waste. g Although the T g may vary, for example, according to molecular weight, but the T of polystyrene waste g Typically it is about 98° C. Those skilled in the art will appreciate that for most polystyrenes used in the manufacture of industrial polystyrene articles, T g Typically only minor variations with molecular weight or polydispersity. Thus, the solvent may have a boiling point up to about 110°C, for example about 105°C to 110°C at 1 atm pressure. Suitable hydrocarbon solvents may, for example, allow more than 90% of the p-cymene to migrate into the hydrocarbon solvent and be a non-solvent for polystyrene.

[0184] In order to carry out the first washing step (i.e., precipitating polystyrene), the mixture of dissolved polystyrene in para-cymene is slowly poured into a double-walled stainless steel tank containing hydrocarbons at their boiling temperature. In an exemplary embodiment, hexane at a boiling temperature (69° C.) is used for this step. In other exemplary embodiments, heptane at a boiling temperature (98° C.) is used for this step. The entire mixture is gently stirred using a mechanical stirrer. The volume of the polystyrene / para-cymene solution added to the hydrocarbon is at a volume ratio of polystyrene / para-cymene solution to the hydrocarbon of 1:3. Under these conditions, polystyrene is precipitated in the form of a viscous white paste. The stirring time (about 5 minutes to about 10 minutes) allows a useful amount of para-cymene to diffuse into the hydrocarbon. Then, the solvent mixture supernatant is removed by simple decantation, after which a second washing of the precipitated polystyrene may be performed.

[0185] The second wash is carried out in the same tank with heptane. A determined amount of heptane with a boiling temperature of 98° C. is introduced into the tank, according to a volume ratio of polystyrene:heptane of 1:1. The entire mixture is boiled at atmospheric pressure for about 2 minutes to about 5 minutes under mild mechanical stirring. The use of a different hydrocarbon in the second wash than in the first wash improves the ductility of the polystyrene, for example, by increasing the diffusion of the remaining p-cymene solvent out of the precipitated polystyrene and into the hydrocarbon. Thereafter, the supernatant solvent mixture is removed by simple decantation. According to calculations of the washing efficiency, the remaining p-cymene in the precipitated polystyrene at this stage is less than 0.1%.

[0186] In order to further reduce the p-cymene present in the polystyrene, a third wash is performed using boiling heptane. The presence of residual solvent can, for example, affect the melt index, also known as the melt flow index (MFI). The degree of washing efficiency is inversely proportional to the MFI. The washing conditions used are the same as for the second washing step.

[0187] The recovered solvent mixture contains hexane, heptane, p-cymene and / or other hydrocarbon solvents used, and non-polar additives extracted from PS. The ratio of p-cymene to additives is higher in the first solvent mixture than in the second and third solvent mixtures. Fractional distillation is used to separate the different products. p-cymene is reused in the dissolving step, while hexane and heptane are reused in the washing step. The recovered additives are considered as waste for disposal.

[0188] The fourth step (drying) consists in drying the polystyrene paste, which contains about 5 to 37% heptane, in a desiccator at a temperature of 120° C. The aim is to remove substantially all remaining solvent without changing the quality of the polymer.

[0189] The fifth step (packaging) involves cutting the dried polystyrene into small particles suitable for distributing the product to consumers. The size and shape of the final product is controlled using a pelletizer commonly used in the industry.

[0190] To limit the PS degradation observed during the drying and extrusion steps, mainly due to oxidation, a commercial antioxidant such as Irganox can be added at a rate of about 1% based on the weight of polystyrene. TM 1076 (octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate). This compound is acceptable for food applications, has a melting point of 50°C, and can be added at various times in the process: together with p-cymene, in the washing step and / or in the final extrusion step.

[0191] Table 1 shows the results of recycling various types of waste polystyrene using the process steps described above. [1] .

[0192] Table 1 [1]

[0193]

[0194]

[0195] [1] All experiments were performed using three washes of heptane at volume ratios of 3:1, 1:1 and 1:1 of heptane:PS / cymene mixture, using extraction times of 15 minutes, 10 minutes and 5 minutes, respectively.

[0196] [2] The mixtures used for all tests also included p-cymene to make the total amount 100 wt%.

[0197] [3] The ASTM D1238 standard was used for each result.

[0198] [4] Aluminium plates with a diameter of 8 cm were used in an oven at 120° C. Unless otherwise specified, polystyrene was dried at a thickness of <5 mm.

[0199] [5] The regrind beads come from the tray and already have a lower melt flow index. Due to the high molecular weight, the mass of the polystyrene reduces the melt flow index of the blend.

[0200] [6] Lime and talc were added to the PS cymene mixture before washing.

[0201] Irganox 1076 has the property of protecting from oxidation. Many results show a helpful effect on the color of the product. Adding butadiene to styrene results in the formation of styrene-butadiene copolymers, which show better impact resistance than pure polystyrene. The butadiene units in styrene-butadiene copolymers can be used to build a three-dimensional matrix with polymer chains. By building connections between polymer chains, the molecular weight increases, and the melt flow index must then decrease. Styrene-butadiene copolymer polymers contain 4% butadiene. The small amount of butadiene must be enough to see a difference in the melt flow index, but the results are inconclusive.

[0202] As can be seen in Table 1, the experiments showed better results when the polystyrene-cymene mixture had a lower concentration. Dilution of the mixture in a non-solvent improves diffusion and therefore the extraction of the solvent. Adding solid particles to polymer mixtures is a common practice in the polystyrene industry to reduce costs or improve mechanical properties.

[0203] Table 2 shows the results of including the antioxidant Irganox 1076 at different steps of the process.

[0204] Table 2

[0205]

[0206] [1] For each result the ASTM D1238 standard was used.

[0207] As can be seen in Table 2, the product color for all samples was white. The MFI of the product resulting from the process where Irganox 1076 was added to the polystyrene / p-cymene mixture was the lowest.

[0208] Table 3 shows the effect of changes in mechanical conditioning and drying steps. There is a difference of about 37.5% between washed polystyrene and dried polystyrene. At this time, all the heptane has evaporated. Moreover, it is possible to remove 14% of the heptane from the washed polystyrene with only the extrusion and granulation steps. The heptane is recovered in the process to repeat the washing process. The source of the polystyrene did not have any significant effect in the drying step of these studies.

[0209] Table 3 [1]

[0210]

[0211] [1] All drying was done in an oven at 120°C.

[0212] [2] All tested mixtures also included p-cymene to make the total amount 100 wt%.

[0213] [3] Values ​​are provided as wt % based on the total mass before pelletization.

[0214] Example 2

[0215] Further tests were carried out to prepare recycled polystyrene. Such tests were carried out by using a method similar to that described previously in Example 1 but without the addition of any Irganox. These tests were carried out on a laboratory scale on real white expanded polystyrene used for packaging.

[0216] Thus, the following provides the results of such a test

[0217] DSC (ASTM D3418): T g =108.1℃

[0218] IZOD impact test (ASTM D4812): average impact of 4 tests is 13,78KJ / m 2 and 175,72 J / m, energy = 0,55 J with total fracture

[0219] Table 4: MFI test MFI (ASTM D1238 for Dynisco D4002 at 200°C):

[0220] test MFI(g / 10min) 1 11.44 2 11.01 3 10.70 average 11.05

[0221] Ash content (ASTM D5630): 0.10

[0222] Table 5: VICAT test

[0223] VICAT softening temperature (ASTM D1525):

[0224]

[0225] Table 6: VICAT test

[0226] Traction test (ASTM D638)

[0227]

[0228] Example 3

[0229] Further tests were conducted to prepare recycled polystyrene. Such tests were conducted using a method similar to that previously described in Example 1. The method was performed continuously, scaling up the method from laboratory level to industrial level. For example, the method allowed the preparation of about 10 kg of recycled polystyrene per hour. It should be noted that the limiting factor in the productivity of the method in this case is not in the method itself, but in certain types of equipment used to perform the method. By obtaining some equipment that allows acceptance of larger volumes or larger quantities, the entire method can easily reach about 500 to about 1000 kg of recycled polystyrene per hour.

[0230] Thus, the results of such testing are provided below.

[0231] According to ASTM D1238-13 standard, MFI=22 g / 10 min.

[0232] The description has been made with particular reference to a particular embodiment, but it will be appreciated that many modifications thereto will be apparent to those skilled in the art. Therefore, the above description and the accompanying drawings should be interpreted as specific examples rather than in a limiting sense.

Claims

1. A combined use of p-cymene and a non-solvent having a boiling point of 98° C. to 110° C. at a pressure of 1 atm for recovering polystyrene, in, The non-solvent is an alkane or a mixture of alkanes; and The p-cymene is used to dissolve polystyrene, and the non-solvent is used to precipitate the polystyrene into a paste.

2. The use according to claim 1, wherein The precipitation of polystyrene is carried out at the boiling point of the non-solvent.

3. The use according to claim 1 or 2, wherein The non-solvent was heptane.

4. The use according to claim 1 or 2, wherein Polystyrene was precipitated from a mixture comprising p-cymene, heptane and polystyrene, and the precipitation was performed at a temperature of 98°C.

5. The use according to claim 3, wherein Polystyrene was precipitated from a mixture comprising p-cymene, heptane and polystyrene, and the precipitation was performed at a temperature of 98°C.

6. A composition for producing recycled polystyrene, characterized in that The composition comprises polystyrene, p-cymene and a non-solvent having a boiling point of 98° C. to 110° C. at a pressure of 1 atm, wherein the non-solvent is an alkane or a mixture of alkanes; and The p-cymene is used to dissolve polystyrene, and the non-solvent is used to precipitate the polystyrene into a paste.

7. The composition according to claim 6, wherein The non-solvent was heptane.

Citation Information

Patent Citations

  • Recovering method of polystyrene from foamed syyrene molding containing flame retardant

    JP1995214028A

  • Natural solvent for reducing volume of foamed polystyrene, and method for volume-reducing treatment of foamed polystyrene using the same

    JP2009120682A

  • Method for Recycling Plastic Materials and Use Thereof

    US20080281002A1

  • Fluid formulations for electric-field-driven spinning of fibers

    US20100239861A1

  • Reclamation of polymers, that contain styrene in the polymeric backbone, using a water soluble solvent based reclamation process

    US5594035A