Sapphire substrate, light-emitting diode chip and method for preparing substrate
By etching on the surface of the sapphire substrate to form a Bragg mirror structure, the problems of low light extraction efficiency of the sapphire substrate and high dislocation density of the nitride film are solved, and the luminous efficiency and service life of the LED are improved.
Patent Information
- Application Number
- CN202210173740.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-02-24
AI Technical Summary
The low light extraction efficiency of sapphire substrate and high dislocation density of nitride films affect the luminous efficiency and service life of LEDs.
The surface of the sapphire substrate is etched to form a plurality of spaced blind holes. The blind holes include countersunk sections and conical hole sections. One end of the countersunk section is connected to the small end of the conical hole section, and the large end of the conical hole section is located on the surface. , the first and second material layers are filled to form a Bragg mirror structure, improving light extraction efficiency and reducing dislocation density.
By forming a Bragg mirror structure, the chance of light refraction into the air is improved, the brightness of the LED chip and the crystal quality of the nitride film are improved, and the service life of the LED is extended.
Smart Images

Figure CN114784161B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of optoelectronic manufacturing technology, and in particular to a sapphire substrate, a light emitting diode chip and a method for preparing the substrate. Background Art
[0002] As a new product with great influence in the optoelectronics industry, light emitting diode (LED) has the characteristics of small size, long service life, rich colors and low energy consumption, and is widely used in lighting, display screens, signal lights, backlight sources, toys and other fields. The core structure of LED is epitaxial wafer, and the production of epitaxial wafer has a great influence on the optoelectronic characteristics of LED.
[0003] In the related art, when growing epitaxial wafers, a sapphire substrate is first placed on a tray in a reaction chamber of a metal organic chemical vapor deposition (MOCVD) device. Then, the sapphire substrate in the tray is heated by a heating wire in the MOCVD device, and raw materials are introduced into the reaction chamber to epitaxially grow on the sapphire substrate to form an epitaxial wafer.
[0004] However, in the related art, sapphire substrates are mostly flat-plate structures, which have the problem of low light extraction efficiency. In addition, the nitride film epitaxially grown on this type of sapphire substrate is also prone to problems of high dislocation density and lattice adaptation, thereby affecting the luminous efficiency and service life of the LED. Summary of the invention
[0005] The embodiments of the present disclosure provide a sapphire substrate, a light-emitting diode chip, and a method for preparing the substrate, which can improve the problem of low light extraction efficiency of the sapphire substrate, reduce the dislocation density of nitride grown on the sapphire substrate, and improve the crystal quality and the light-emitting efficiency of the chip. The technical solution is as follows:
[0006] In a first aspect, an embodiment of the present disclosure provides a sapphire substrate, comprising: a substrate body, a surface of the substrate body having a plurality of blind holes, the plurality of blind holes being arranged at intervals; the blind holes comprising a connected countersunk hole section and a tapered hole section, one end of the countersunk hole section being coaxially connected to the small end of the tapered hole section, and the large end of the tapered hole section being located on the surface of the substrate body; the blind holes comprising at least one group of blind holes arranged at intervals along the same straight line, in the same group of the blind holes, one of two adjacent blind holes has a first material layer in its countersunk hole section, and the other of the two adjacent blind holes has a second material layer in its countersunk hole section, and the refractive index of the first material layer is different from the refractive index of the second material layer.
[0007] In an implementation of the embodiment of the present disclosure, the refractive index of the first material layer is 1 to 3, and the refractive index of the second material layer is 1 to 3.
[0008] In another implementation of the embodiment of the present disclosure, the first material layer is a silicon oxide layer, and the second material layer is a titanium oxide layer.
[0009] In another implementation of the embodiment of the present disclosure, the thickness of the first material layer is not greater than the length of the countersunk section, and the thickness of the second material layer is not greater than the length of the countersunk section.
[0010] In another implementation of the embodiment of the present disclosure, the thickness of the first material layer is the same as the thickness of the second material layer.
[0011] In another implementation of the embodiment of the present disclosure, the pore diameter of the countersink section is 100 nm to 600 nm, and the length of the countersink section is 100 nm to 500 nm.
[0012] In another implementation of the embodiment of the present disclosure, the length of the tapered hole segment is 100nm to 500nm, the diameter of the large end of the tapered hole segment is 800nm to 1200nm, and the diameter of the small end of the tapered hole segment is 500nm to 700nm.
[0013] In another implementation of the embodiment of the present disclosure, the distance between two adjacent blind holes is 800 nm to 1500 nm.
[0014] In a second aspect, an embodiment of the present disclosure provides a method for preparing a sapphire substrate, the method comprising:
[0015] Providing a substrate body;
[0016] A plurality of blind holes are formed by etching on the surface of the substrate body, wherein the plurality of blind holes are arranged at intervals, wherein the blind holes include a countersunk hole section and a tapered hole section connected to each other, wherein one end of the countersunk hole section is coaxially connected to the small end of the tapered hole section, and the large end of the tapered hole section is located on the surface of the substrate body, wherein the blind holes include at least one group of blind holes arranged at intervals along the same straight line, wherein in the same group of the blind holes, the countersunk hole section of one of the two adjacent blind holes comprises a first material layer, and the countersunk hole section of the other of the two adjacent blind holes comprises a second material layer, and the refractive index of the first material layer is different from the refractive index of the second material layer.
[0017] In a third aspect, an embodiment of the present disclosure provides a light emitting diode chip, wherein the light emitting diode chip includes the sapphire substrate as described above.
[0018] The beneficial effects brought by the technical solution provided by the embodiments of the present disclosure include at least:
[0019] The disclosed embodiment provides a sapphire substrate including a substrate body, a surface of the substrate body is provided with a plurality of blind holes arranged at intervals, the blind holes include a countersunk hole section and a conical hole section, one end of the countersunk hole section is connected to the small end of the conical hole section, and the large end of the conical hole section is located on the surface of the substrate body. In this way, a plurality of conical surfaces are formed on the surface of the substrate body, which is conducive to reducing the dislocation density of the nitride film epitaxially grown on the substrate body, so as to improve the crystal quality of the nitride film.
[0020] Furthermore, the blind holes include at least one group of blind holes arranged at intervals along the same straight line. In two adjacent blind holes in the same group of blind holes, the countersink of one blind hole is filled with a first material layer, and the countersink of the other blind hole is filled with a second material layer. Since the refractive indexes of the first material layer and the second material layer are different, the first material layer, the substrate body and the second material layer can form a Bragg reflector structure in the horizontal direction, so that light can be emitted after multiple reflections in the Bragg reflector structure, so as to increase the probability of light being refracted into the air, improve the light extraction efficiency, and increase the brightness of the chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 is a schematic structural diagram of a sapphire substrate provided by an embodiment of the present disclosure;
[0023] Figure 2 is a top view of a sapphire substrate provided by an embodiment of the present disclosure;
[0024] Figure 3 is a flow chart of a method for preparing a sapphire substrate provided by an embodiment of the present disclosure;
[0025] Figure 4 It is a structural schematic diagram of a light emitting diode chip provided in an embodiment of the present disclosure.
[0026] The descriptions of the marks in the figure are as follows:
[0027] 10. Substrate body;
[0028] 20, blind hole; 210, countersunk hole section; 220, tapered hole section;
[0029] 31. first material layer; 32. second material layer;
[0030] 41. Low-temperature AlN layer; 42. High-temperature AlN layer; 43. n-type AlGaN layer; 44. Multiple quantum well layer; 45. p-type AlGaN barrier layer; 46. p-type AlGaN layer; 47. p-type GaN layer. DETAILED DESCRIPTION
[0031] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0032] Unless otherwise defined, the technical terms or scientific terms used herein shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. The words "first", "second", "third" and similar words used in the patent application specification and claims of the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not indicate a quantity limitation, but indicate the existence of at least one. Words such as "include" or "comprise" and similar words mean that the elements or objects appearing before "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. Words such as "connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right", "top", "bottom" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0033] Figure 1 Schematic diagram of the structure of a sapphire substrate provided by an embodiment of the present disclosure. Figure 1 As shown, the sapphire substrate includes: a substrate body 10, a surface of the substrate body 10 has a plurality of blind holes 20, and the plurality of blind holes 20 are arranged at intervals.
[0034] like Figure 1 As shown, the blind hole 20 includes a connected countersunk hole section 210 and a tapered hole section 220 , one end of the countersunk hole section 210 is coaxially connected to the small end of the tapered hole section 220 , and the large end of the tapered hole section 220 is located on the surface of the substrate body 10 .
[0035] The blind holes 20 include at least one group of blind holes 20 arranged at intervals along the same straight line. Figure 1 As shown, in the same group of blind holes 20, the countersink section 210 of one of the two adjacent blind holes 20 has a first material layer 31, and the countersink section 210 of the other of the two adjacent blind holes 20 has a second material layer 32, and the refractive index of the first material layer 31 is different from the refractive index of the second material layer 32.
[0036] The sapphire substrate provided by the embodiment of the present disclosure includes a substrate body 10, and a plurality of blind holes 20 arranged at intervals are provided on the surface of the substrate body 10, and the blind holes 20 include a countersunk hole section 210 and a tapered hole section 220, one end of the countersunk hole section 210 is connected to the small end of the tapered hole section 220, and the large end of the tapered hole section 220 is located on the surface of the substrate body 10. In this way, a plurality of conical surfaces are formed on the surface of the substrate body 10, which is conducive to reducing the dislocation density of the nitride film epitaxially grown on the substrate body 10, so as to improve the crystal quality of the nitride film.
[0037] Furthermore, the blind holes 20 include at least one group of blind holes 20 arranged at intervals along the same straight line. In two adjacent blind holes 20 in the same group of blind holes 20, the countersunk section 210 of one blind hole 20 is filled with the first material layer 31, and the other blind hole 20 is filled with the second material layer 32. Since the refractive indexes of the first material layer 31 and the second material layer 32 are different, the first material layer 31, the substrate body 10 and the second material layer 32 can form a Bragg reflector structure in the horizontal direction, so that light can be emitted after multiple reflections in the Bragg reflector structure, so as to increase the probability of light being refracted into the air, improve the light extraction efficiency, and increase the brightness of the chip.
[0038] Optionally, the refractive index of the first material layer 31 is 1 to 3, and the refractive index of the second material layer 32 is 1 to 3.
[0039] Exemplarily, the first material layer 31 is a silicon oxide layer, and the refractive index of silicon oxide is 1.2. The second material layer 32 is a titanium oxide layer, and the refractive index of titanium oxide is 1.5.
[0040] Thus, in two adjacent blind holes 20, the counterbore section 210 of one blind hole 20 is filled with a silicon oxide layer, and the other blind hole 20 is filled with a silicon nitride layer, so as to form an alternating silicon oxide layer and a silicon nitride layer on the substrate body 10. Since the refractive indexes of the silicon oxide layer and the silicon nitride layer are different, the silicon oxide layer, the substrate body 10 and the silicon nitride layer can form a Bragg reflector structure in the lateral direction, so that the light can be reflected multiple times in the Bragg reflector structure before emitting light, so as to increase the probability of light being refracted into the air, improve the light extraction efficiency, and increase the brightness of the chip.
[0041] Alternatively, if Figure 1 As shown, the thickness of the first material layer 31 is not greater than the length of the countersunk section 210 , and the thickness of the second material layer 32 is not greater than the length of the countersunk section 210 .
[0042] By filling the first material layer 31 and the second material layer 32 in the respective countersunk hole sections 210, and controlling the thickness of the first material layer 31 not to exceed the length of the countersunk hole section 210, and controlling the thickness of the second material layer 32 not to exceed the length of the countersunk hole section 210, it is ensured that the first material layer 31 will not extend to the tapered hole section 220, and the second material layer 32 will not extend to the tapered hole section 220. In this way, it is ensured that there are sufficient first material layers 31 and second material layers 32 on the substrate body 10 to form a Bragg reflector structure, thereby improving the light extraction efficiency of the sapphire substrate; at the same time, since the first material layer 31 and the second material layer 32 will not extend to the tapered hole section 220, the integrity of the tapered surface formed by the tapered hole on the surface of the substrate body 10 can also be ensured, which is beneficial to reducing the dislocation density of the nitride film epitaxially grown on the substrate body 10, so as to improve the crystal quality of the nitride film.
[0043] As an example, in the embodiment of the present disclosure, the thickness of the first material layer 31 can be the same as the length of the countersunk hole section 210, and the thickness of the second material layer 32 can be the same as the length of the countersunk hole section 210. In this way, the first material layer 31 and the second material layer 32 can fill the corresponding countersunk hole sections 210 respectively, so as to ensure that there are sufficient first material layers 31 and second material layers 32 on the substrate body 10 to form a Bragg reflector structure, thereby improving the light extraction efficiency of the sapphire substrate.
[0044] As an example, in the embodiment of the present disclosure, the thickness of the first material layer 31 may be half the length of the countersunk hole section 210, and the thickness of the second material layer 32 may be half the length of the countersunk hole section 210. In this way, by filling the through hole with an appropriate amount of the first material layer 31 and the second material layer 32, while ensuring that there are sufficient first material layers 31 and second material layers 32 on the substrate body 10 to form a Bragg reflector structure, the preparation cost can also be effectively saved.
[0045] Optionally, the thickness of the first material layer 31 is the same as the thickness of the second material layer 32 .
[0046] Exemplarily, the first material layer 31 is a silicon oxide layer, and the second material layer 32 is a titanium oxide layer. The thickness of the silicon oxide layer and the thickness of the second material layer 32 are set to be the same, which can form a Bragg reflector structure with better reflective effect, so as to further increase the probability of light being refracted into the air, improve the light extraction efficiency, and increase the brightness of the chip.
[0047] Optionally, the thickness of the first material layer 31 may be different from the thickness of the second material layer 32 .
[0048] For example, if the manufacturing cost of the first material layer 31 is greater than the manufacturing cost of the second material layer 32, the thickness of the first material layer 31 may be greater than the thickness of the second material layer 32. In this way, by only providing a suitable second material layer 32, while ensuring that there are sufficient first material layers 31 and second material layers 32 on the substrate body 10 to form a Bragg reflector structure, the manufacturing cost can be effectively saved.
[0049] For example, if the manufacturing cost of the first material layer 31 is less than the manufacturing cost of the second material layer 32, the thickness of the first material layer 31 may be less than the thickness of the second material layer 32. In this way, by only providing a suitable first material layer 31, the manufacturing cost can be effectively saved while ensuring that there are sufficient first material layers 31 and second material layers 32 on the substrate body 10 to form a Bragg reflector structure.
[0050] Alternatively, if Figure 1 As shown, the pore diameter of the counterbore section 210 is 100 nm to 600 nm, and the length of the counterbore section 210 is 100 nm to 500 nm.
[0051] Exemplarily, the aperture of the countersunk hole section 210 is 400 nm, and the length of the countersunk hole section 210 is 300 nm. By setting the countersunk hole section 210 to this size, it is ensured that a sufficient amount of the first material layer 31 and the second material layer 32 are filled in the countersunk hole section 210 to form a Bragg reflector structure, thereby improving the light extraction efficiency of the sapphire substrate.
[0052] Alternatively, if Figure 1 As shown, the length of the tapered hole segment 220 is 100 nm to 500 nm, the diameter of the large end of the tapered hole segment 220 is 800 nm to 1200 nm, and the diameter of the small end of the tapered hole segment 220 is 500 nm to 700 nm.
[0053] Exemplarily, the length of the conical hole section 220 is 400 nm, the diameter of the small end of the conical hole section 220 is 400 nm, and the diameter of the large end of the conical hole section 220 is 600 nm. By setting the conical hole section 220 to this size, a suitable conical surface is formed on the surface of the substrate body 10, which is conducive to reducing the dislocation density of the nitride film epitaxially grown on the substrate body 10, so as to improve the crystal quality of the nitride film.
[0054] In the disclosed embodiment, the blind holes 20 on the surface of the substrate body 10 are evenly distributed and cover all surfaces of the substrate body 10 , so that the formed Bragg reflectors can be evenly distributed on the surface of the substrate body 10 , thereby improving light extraction efficiency.
[0055] For example, Figure 2 FIG. 1 is a top view of a sapphire substrate provided by an embodiment of the present disclosure. Figure 2As shown, the blind holes 20 are arranged in an array on the surface of the substrate body 10. The distance between two adjacent blind holes 20 is 800nm to 1500nm.
[0056] As an example, the distance between two adjacent blind holes 20 is 800 nm.
[0057] It should be noted that the blind holes 20 may also be arranged on the surface of the substrate body 10 in other ways, as long as the blind holes 20 are evenly distributed, and the embodiment of the present disclosure does not limit this.
[0058] Figure 3 FIG. 1 is a flow chart of a method for preparing a sapphire substrate provided by an embodiment of the present disclosure. Figure 3 As shown, the preparation method comprises:
[0059] Step S11: providing a substrate body 10 .
[0060] Step S12: etching a plurality of blind holes 20 on the surface of the substrate body 10 .
[0061] Among them, a plurality of blind holes 20 are arranged at intervals, and the blind holes 20 include a connected countersunk hole section 210 and a tapered hole section 220, one end of the countersunk hole section 210 is coaxially connected to the small end of the tapered hole section 220, and the large end of the tapered hole section 220 is located on the surface of the substrate body 10. The blind holes 20 include at least one group of blind holes 20 arranged at intervals along the same straight line, and in the same group of blind holes 20, the countersunk hole section 210 of one of the two adjacent blind holes 20 has a first material layer 31, and the countersunk hole section 210 of the other of the two adjacent blind holes 20 has a second material layer 32, and the refractive index of the first material layer 31 is different from the refractive index of the second material layer 32.
[0062] The sapphire substrate prepared by the preparation method includes a substrate body 10, and a plurality of blind holes 20 arranged at intervals are provided on the surface of the substrate body 10, and the blind holes 20 include a countersunk hole section 210 and a tapered hole section 220, one end of the countersunk hole section 210 is connected to the small end of the tapered hole section 220, and the large end of the tapered hole section 220 is located on the surface of the substrate body 10. In this way, a plurality of conical surfaces are formed on the surface of the substrate body 10, which is conducive to reducing the dislocation density of the nitride film epitaxially grown on the substrate body 10, so as to improve the crystal quality of the nitride film.
[0063] Furthermore, the blind holes 20 include at least one group of blind holes 20 arranged at intervals along the same straight line. Among two adjacent blind holes 20 in the same group of blind holes 20, one blind hole 20 is filled with a first material layer 31, and the other blind hole 20 is filled with a second material layer 32. Since the refractive indexes of the first material layer 31 and the second material layer 32 are different, the first material layer 31, the substrate body 10 and the second material layer 32 can form a Bragg reflector structure in the horizontal direction, so that light can be emitted after multiple reflections in the Bragg reflector structure, so as to increase the probability of light being refracted into the air, improve the light extraction efficiency, and increase the brightness of the chip.
[0064] Optionally, the substrate body 10 is a flat sheet structure made of sapphire material.
[0065] In step S11, the substrate body 10 may be pre-treated, the substrate body 10 may be placed in a MOCVD reaction chamber, and the substrate body 10 may be baked for 12 to 18 minutes. As an example, in the embodiment of the present disclosure, the substrate body 10 may be baked for 15 minutes.
[0066] Specifically, the baking temperature may be 1000° C. to 1200° C., and the pressure in the MOCVD reaction chamber during baking may be 100 mbar to 200 mbar.
[0067] In step S12, the process of forming the blind hole 20 on the surface of the substrate body 10 may include:
[0068] First, an initial countersink is formed on the surface of the substrate body 10 by dry etching. The length of the initial countersink is the sum of the lengths of the countersink section 210 and the tapered hole section 220 .
[0069] Then, dry etching is continued on the basis of the initial countersink to form a tapered hole section 220 , so that the etched initial countersink forms a countersink section 210 to complete the preparation of the blind hole 20 .
[0070] Alternatively, if Figure 1 As shown, the pore diameter of the counterbore section 210 is 100 nm to 600 nm, and the length of the counterbore section 210 is 100 nm to 500 nm.
[0071] Exemplarily, the aperture of the countersunk hole section 210 is 400 nm, and the length of the countersunk hole section 210 is 300 nm. By setting the countersunk hole section 210 to this size, it is ensured that a sufficient amount of the first material layer 31 and the second material layer 32 are filled in the countersunk hole section 210 to form a Bragg reflector structure, thereby improving the light extraction efficiency of the sapphire substrate.
[0072] Alternatively, if Figure 1As shown, the length of the tapered hole segment 220 is 100 nm to 500 nm, the diameter of the large end of the tapered hole segment 220 is 800 nm to 1200 nm, and the diameter of the small end of the tapered hole segment 220 is 500 nm to 700 nm.
[0073] Exemplarily, the length of the conical hole section 220 is 400 nm, the diameter of the small end of the conical hole section 220 is 400 nm, and the diameter of the large end of the conical hole section 220 is 600 nm. By setting the conical hole section 220 to this size, a suitable conical surface is formed on the surface of the substrate body 10, which is conducive to reducing the dislocation density of the nitride film epitaxially grown on the substrate body 10, so as to improve the crystal quality of the nitride film.
[0074] Optionally, the first material layer 31 is a silicon oxide layer, and the refractive index of silicon oxide is 1.2. The second material layer 32 is a titanium oxide layer, and the refractive index of titanium oxide is 1.5.
[0075] In this way, silicon oxide layers and silicon nitride layers are alternately formed on the substrate body 10. Since the refractive indexes of the silicon oxide layer and the silicon nitride layer are different, the silicon oxide layer, the substrate body 10 and the silicon nitride layer can form a Bragg reflector structure in the lateral direction, so that light can be reflected multiple times in the Bragg reflector structure before being emitted, thereby increasing the probability of light being refracted into the air, improving light extraction efficiency, and increasing the brightness of the chip.
[0076] In the disclosed embodiment, after the blind holes 20 are formed by etching the surface of the substrate body 10 , silicon oxide or titanium oxide may be deposited in the counterbore section 210 of each blind hole 20 using atomic layer deposition (ALD) technology.
[0077] Exemplarily, the thickness of the silicon oxide layer is not greater than the length of the counterbore section 210 , and the thickness of the titanium oxide layer is not greater than the length of the counterbore section 210 .
[0078] By filling the silicon oxide layer and the titanium oxide layer in the respective countersunk hole sections 210, and controlling the thickness of the silicon oxide layer not to exceed the length of the countersunk hole section 210, and controlling the thickness of the titanium oxide layer not to exceed the length of the countersunk hole section 210, it is ensured that the silicon oxide layer does not extend to the tapered hole section 220, and the titanium oxide layer does not extend to the tapered hole section 220. It is ensured that there are sufficient silicon oxide layers and titanium oxide layers on the substrate body 10 to form a Bragg reflector structure, thereby improving the light extraction efficiency of the sapphire substrate; and the silicon oxide layer and the titanium oxide layer do not extend to the tapered hole section 220, which can ensure the integrity of the tapered surface formed by the tapered hole on the surface of the substrate body 10, which is conducive to reducing the dislocation density of the nitride film epitaxially grown on the substrate body 10, so as to improve the crystal quality of the nitride film.
[0079] As an example, the thickness of the silicon oxide layer is 300 nm, and the thickness of the titanium oxide layer is 300 nm.
[0080] Figure 4 Schematic diagram of the structure of a light emitting diode chip provided by an embodiment of the present disclosure. Figure 4 As shown, the light emitting diode chip includes the sapphire substrate as described above.
[0081] like Figure 4 As shown, the light-emitting diode chip also includes an epitaxial wafer stacked on a sapphire substrate, and the epitaxial wafer includes a low-temperature AlN layer 41, a high-temperature AlN layer 42, an n-type AlGaN layer 43, a multi-quantum well layer 44, a p-type AlGaN barrier layer 45, a p-type AlGaN layer 46 and a p-type GaN layer 47 stacked in sequence.
[0082] In the disclosed embodiment, a high-temperature MOCVD device is used to grow epitaxial wafers. High-purity hydrogen or high-purity nitrogen or a mixture of high-purity hydrogen and high-purity nitrogen is used as a carrier gas, high-purity ammonia is used as a nitrogen source, trimethylgallium and triethylgallium are used as gallium sources, trimethylindium is used as an indium source, silane is used as an N-type dopant, i.e., a Si source, trimethylaluminum is used as an aluminum source, and dicyclopentadienyl magnesium is used as a P-type dopant, i.e., a Mg source. The pressure of the reaction chamber is 100 torr to 600 torr.
[0083] The specific preparation process is as follows:
[0084] First, the sapphire substrate used as a growth substrate is specially cleaned.
[0085] Then, the substrate is placed in MOCVD to grow a low-temperature AlN layer 41. The process temperature of MOCVD is 1100° C., the pressure is 100 torr, ammonia and trimethylaluminum are introduced as reactants, the V / III molar ratio is 3000, and the process time is 1000 s.
[0086] Next, the temperature is raised to 1350° C. to grow a 2.5 μm thick high-temperature AlN layer 42. The growth pressure is 100 torr, ammonia and trimethylaluminum are introduced as reactants, the V / III molar ratio is 300, and the process time is 5000 s.
[0087] Then, a silane-doped n-type AlGaN layer 43 with a thickness of 700 nm is grown in an environment at a temperature of 1060° C. The growth pressure is 200 torr.
[0088] Next, five cycles of Al were grown in a nitrogen atmosphere at a growth pressure of 150 torr and a temperature of 1040°C. x Ga 1-x N / A y Ga 1-yN(x<y) multiple quantum well layer 44, where Al in the multiple quantum well layer 44 x Ga 1-x N layer and barrier layer Al y Ga 1-y The thicknesses of the N layers are 3 nm and 11 nm respectively.
[0089] Next, a p-type AlGaN barrier layer 45 doped with Mg is grown at a temperature of 980 °C and a growth pressure of 200 torr, with a thickness of 30 nm.
[0090] Then, a p-type AlGaN layer 46 doped with Mg is grown at a temperature of 900 °C and a growth pressure of 300 torr, with a thickness of 25 nm.
[0091] Next, a p-type GaN layer 47 doped with Mg is grown at a temperature of 850 °C and a growth pressure of 400 torr, with a thickness of 5 nm.
[0092] Finally, annealing is performed for 30 minutes in a nitrogen atmosphere to complete the growth process of the epitaxial wafer.
[0093] The above is not any form of limitation to the present disclosure. Although the present disclosure has been disclosed as above through embodiments, it is not intended to limit the present disclosure. Any person skilled in the art, within the scope of the technical solution of the present disclosure, can make some changes or modifications to the above-disclosed technical content to form equivalent embodiments with equivalent changes. However, as long as it does not depart from the technical solution of the present disclosure, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present disclosure still fall within the scope of the technical solution of the present disclosure.
Claims
1. A sapphire substrate, characterized in that: The sapphire substrate comprises: a substrate body (10), a surface of the substrate body (10) having a plurality of blind holes (20), the plurality of blind holes (20) being arranged at intervals; The blind hole (20) comprises a connected countersunk hole section (210) and a tapered hole section (220), one end of the countersunk hole section (210) is coaxially connected to the small end of the tapered hole section (220), and the large end of the tapered hole section (220) is located on the surface of the substrate body (10); The blind holes (20) include at least one group of blind holes (20) arranged at intervals along the same straight line; in the same group of blind holes (20), a first material layer (31) is included in the countersunk hole section (210) of one of the two adjacent blind holes (20); a second material layer (32) is included in the countersunk hole section (210) of the other of the two adjacent blind holes (20); the refractive index of the first material layer (31) is different from the refractive index of the second material layer (32), so that the first material layer, the substrate body and the second material layer form a Bragg reflector structure in the lateral direction.
2. The sapphire substrate according to claim 1, characterized in that The refractive index of the first material layer (31) is 1 to 3, and the refractive index of the second material layer (32) is 1 to 3.
3. The sapphire substrate according to claim 2, characterized in that: The first material layer (31) is a silicon oxide layer, and the second material layer (32) is a titanium oxide layer.
4. The sapphire substrate according to claim 1, characterized in that: The thickness of the first material layer (31) is not greater than the length of the countersunk hole section (210), and the thickness of the second material layer (32) is not greater than the length of the countersunk hole section (210).
5. The sapphire substrate according to claim 4, characterized in that: The thickness of the first material layer (31) is the same as the thickness of the second material layer (32).
6. The sapphire substrate according to any one of claims 1 to 5, characterized in that: The pore diameter of the countersunk hole section (210) is between 100 nm and 600 nm, and the length of the countersunk hole section (210) is between 100 nm and 500 nm.
7. The sapphire substrate according to any one of claims 1 to 5, characterized in that: The length of the conical hole section (220) is 100 nm to 500 nm, the diameter of the large end of the conical hole section (220) is 800 nm to 1200 nm, and the diameter of the small end of the conical hole section (220) is 500 nm to 700 nm.
8. The sapphire substrate according to any one of claims 1 to 5, characterized in that: The distance between two adjacent blind holes (20) is 800 nm to 1500 nm.
9. A method for preparing a sapphire substrate, characterized in that: The preparation method comprises: Providing a substrate body; A plurality of blind holes are formed by etching on the surface of the substrate body, wherein the plurality of blind holes are arranged at intervals, wherein the blind holes include a connected countersunk hole section and a tapered hole section, wherein one end of the countersunk hole section is coaxially connected to the small end of the tapered hole section, and the large end of the tapered hole section is located on the surface of the substrate body, wherein the blind holes include at least one group of blind holes arranged at intervals along the same straight line, wherein in the same group of the blind holes, the countersunk hole section of one of the two adjacent blind holes comprises a first material layer, and the countersunk hole section of the other of the two adjacent blind holes comprises a second material layer, and the refractive index of the first material layer is different from the refractive index of the second material layer, so that the first material layer, the substrate body, and the second material layer form a Bragg reflector structure in the lateral direction.
10. A light emitting diode chip, characterized in that: The light emitting diode chip comprises the sapphire substrate as claimed in any one of claims 1 to 8.