Electroluminescent device and method for preparing the same
By doping MgO and MnO in the electron transport layer of the quantum dot light-emitting diode to form a ZnMgMnO structure, the problem of high electron transport rate is solved, a balance of electron and hole injection rates is achieved, and the performance of the electroluminescent device is improved.
Patent Information
- Application Number
- CN202210286597.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-03-22
AI Technical Summary
When the electron transfer rate of existing quantum dot light-emitting diodes is higher than the hole transfer rate, charge injection is unbalanced, which in turn affects the aging and luminescence performance of the device.
By doping MgO and MnO into ZnO in the electron transport layer, a ZnMgMnO structure is formed, the bandgap width is adjusted to reduce the electron transport rate, and specific layer structures and preparation methods are used in electroluminescent devices to ensure that electrons and holes Injection rate balance.
It effectively reduces the electron transmission rate, achieves a balance between the electron transmission rate and the hole injection rate, and improves the overall performance of the electroluminescent device.
Smart Images

Figure CN114784203B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor technology, and in particular relates to an electroluminescent device and a preparation method thereof. Background Art
[0002] Quantum dots are a kind of low-dimensional semiconductor material, generally composed of IV, II-VI, IV-VI or III-V elements. Since the 1980s, after more than 30 years of development, great progress has been made in the preparation and application of quantum dots. The size of quantum dots is generally 2-100nm, and they are quantum confined in three dimensions. Due to its own quantum effect, size confinement will cause size effect, quantum confinement effect, macroscopic quantum tunneling effect and surface effect, thus showing physical and chemical properties different from those of macroscopic bulk materials. Quantum dots have a wide excitation spectrum and a narrow emission spectrum, and the emission spectrum can be controlled by the size of the quantum dots. Quantum dots have the characteristics of large Stokes shift, excellent photostability, long fluorescence lifetime, good biocompatibility, etc., and have extremely broad application prospects in optoelectronics, solar cells and biomedicine.
[0003] The study of quantum dots as luminescent materials is currently the most extensive research field. Generally speaking, there are two luminescence mechanisms of quantum dots, photoluminescence and electroluminescence. At present, photoluminescence has been commercialized on quantum dot optical films, such as organic light-emitting semiconductors (OLEDs), while quantum dots, as a semiconductor material, are still in the laboratory research stage for electroluminescence technology. The material prepared using electroluminescence technology is called a quantum dot light-emitting diode (QLED). QLED and OLED have similar structures, generally including a cathode, an electron transport layer, a luminescent layer, a hole transport layer, a hole injection layer and an anode. When an external electric field is applied, electrons and holes enter the quantum dot film luminescent layer through the electron transport layer and the hole transport layer respectively, and recombine to emit photons. Therefore, the quantum dot luminescent layer determines the most fundamental performance of the quantum dot light-emitting diode. In addition, the transmission barrier and transmission rate between the functional layers will affect the luminescence performance of the quantum dots. At present, the electron transfer rate of quantum dot light-emitting diodes is often an order of magnitude higher than the hole transfer rate. Unbalanced charge injection often causes serious charge accumulation in the device. Thermal and electrical effects ultimately lead to aging of the quantum dot light-emitting device and quenching of the quantum dot light-emitting layer.
[0004] Therefore, existing quantum dot light-emitting diodes need to be improved. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide an electroluminescent device and a preparation method thereof, wherein the electroluminescent device has a lower electron transfer rate, thereby balancing the electron transfer rate and the hole injection rate as a whole, thereby improving the performance of the electroluminescent device.
[0006] In one aspect of the present invention, the present invention provides an electroluminescent device. According to an embodiment of the present invention, the electroluminescent device comprises:
[0007] anode;
[0008] A hole injection layer, the hole injection layer is disposed on the anode;
[0009] A hole transport layer, the hole transport layer being disposed on the hole injection layer;
[0010] A light-emitting layer, the light-emitting layer being disposed on the hole transport layer;
[0011] An electron transport layer, the electron transport layer being disposed on the light-emitting layer;
[0012] a cathode, the cathode being disposed on the electron transport layer,
[0013] Wherein, the electron transport layer includes ZnO, MgO and MnO.
[0014] According to the electroluminescent device of the embodiment of the present invention, MgO and MnO are doped into the electron transport layer ZnO to form a ZnMgMnO structure. The band gap width of MgO is 7.8 eV, and the band gap width of ZnO is 3.37 eV. 2+ and Zn 2+ With similar radius and small lattice mismatch, the bandgap width becomes adjustable by adjusting the ratio of Zn and Mg. In addition, the bandgap width of MnO is 3.6ev. As a doping ion, the bandgap width can be adjusted to introduce trap energy levels. The bandgap width of MnO is smaller than that of ZnMgO. During the electronic energy level transition process, MnO can capture electrons, thereby reducing the electronic transmission rate of the device, thereby balancing the overall electronic transmission rate and hole injection rate, and improving the device performance.
[0015] In addition, the electroluminescent device according to the above embodiment of the present invention may also have the following additional technical features:
[0016] In some embodiments of the present invention, the molar ratio of ZnO, MgO and MnO in the electron transport layer is (8-12): (80-98): (1-4), thereby effectively reducing the electron transport rate of the device.
[0017] In some embodiments of the present invention, the thickness of the electron transport layer is 20-60 nm, thereby effectively reducing the electron transport rate of the device.
[0018] In some embodiments of the present invention, the electron transport layer is prepared by the following steps: zinc oxide, magnesium oxide and manganese oxide are mixed to obtain a mixed powder; and the mixed powder is deposited on a silicon wafer by pulsed laser deposition technology under an inert atmosphere to obtain an electron transport layer. Thus, the electron transport rate of the device can be effectively reduced.
[0019] In some embodiments of the present invention, the thickness of the silicon wafer is 1-2 mm.
[0020] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned electroluminescent device. According to an embodiment of the present invention, the method comprises:
[0021] (1) spin coating a PEDOT:PSS solution on an anode plate, followed by annealing, to form a hole injection layer on the anode plate;
[0022] (2) spin coating a TFB solution on the hole injection layer, and then annealing to form a hole transport layer on the hole injection layer;
[0023] (3) spin coating a QD quantum dot solution containing CdSe, ZnS and n-octane on the hole transport layer, and then annealing to form a light-emitting layer on the hole transport layer;
[0024] (4) forming an electron transport layer containing ZnO, MgO and MnO on the glass substrate on the light-emitting layer;
[0025] (5) A cathode plate is packaged on the electron transport layer to obtain the electroluminescent device.
[0026] According to the method for preparing an electroluminescent device according to an embodiment of the present invention, a hole injection layer can be formed on the anode plate by spin coating a PEDOT solution on the anode plate and then annealing. Then, a TFB solution is spin coated on the hole injection layer and then annealed to form a hole transport layer on the hole injection layer. Then, a QD quantum dot solution containing CdSe, ZnS and n-octane is spin coated on the hole transport layer and then annealed to form a light-emitting layer on the hole transport layer. An electron transport layer containing ZnO, MgO and MnO is further formed on the glass substrate on the light-emitting layer. Finally, a cathode plate is packaged on the electron transport layer to obtain an electroluminescent device, wherein a ZnMgMnO structure is formed by doping MgO and MnO into the electron transport layer ZnO. The bandgap width of MgO is 7.8ev, and the bandgap width of ZnO is 3.37ev, wherein Mg 2+ and Zn2+ They have similar radii and small lattice mismatch, and the bandgap width becomes adjustable by adjusting the ratio of Zn and Mg. In addition, the bandgap width of MnO is 3.6ev. As a doping ion, the bandgap width can be adjusted to introduce trap energy levels, and the bandgap width of MnO is smaller than that of ZnMgO. During the electronic energy level transition process, MnO can capture electrons, thereby reducing the electron transfer rate of the device, thereby balancing the electron transfer rate and hole injection rate as a whole, thereby improving the device performance.
[0027] In addition, the method for preparing an electroluminescent device according to the above embodiment of the present invention may also have the following additional technical features:
[0028] In some embodiments of the present invention, in step (1), the annealing temperature is 140-180° C., and the annealing time is 20-40 min.
[0029] In some embodiments of the present invention, in step (2), the annealing temperature is 100-160° C., and the annealing time is 25-50 min.
[0030] In some embodiments of the present invention, in step (3), the annealing temperature is 70-90° C., and the annealing time is 20-40 min.
[0031] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0033] Figure 1 is a schematic structural diagram of an electroluminescent device according to an embodiment of the present invention;
[0034] Figure 2 is a schematic flow chart of a method for preparing an electroluminescent device according to one embodiment of the present invention;
[0035] Figure 3 It is a schematic diagram of reducing the electron transport rate by using an electron transport layer including ZnO, MgO and MnO according to the present invention. DETAILED DESCRIPTION
[0036] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0037] In one aspect of the present invention, the present invention provides an electroluminescent device. According to an embodiment of the present invention, referring to Figure 1 The electroluminescent device includes: an anode 100, a hole injection layer 200, a hole transport layer 300, a light-emitting layer 400, an electron transport layer 500 and a cathode 600.
[0038] It should be noted that the anode 100 is made of conventional materials in the art, and those skilled in the art can select the material according to actual needs. For example, the anode 100 is made of indium tin oxide (ITO).
[0039] According to an embodiment of the present invention, referring to Figure 1 The hole injection layer 200 is disposed on the surface of the anode 100. It should be noted that those skilled in the art can select the specific composition of the hole injection layer 200 according to actual needs, such as using PEDOT:PSS.
[0040] According to an embodiment of the present invention, referring to Figure 1 The hole transport layer 300 is disposed on the hole injection layer 200 on a side surface away from the anode 100. It should be noted that those skilled in the art can select the specific composition of the hole transport layer 300 according to actual needs, such as using TFB.
[0041] According to an embodiment of the present invention, referring to Figure 1 The light-emitting layer 400 is disposed on the hole transport layer 300 on a side surface away from the anode 100. It should be noted that those skilled in the art can select the specific composition of the light-emitting layer 400 according to actual needs, such as using a QD quantum dot solution of CdSe, ZnS and n-octane.
[0042] According to an embodiment of the present invention, referring to Figure 1 The electron transport layer 500 is disposed on the surface of the light emitting layer 400 away from the anode 100, and the electron transport layer 500 includes ZnO, MgO and MnO. The inventors found that by doping MgO and MnO into ZnO, a ZnMgMnO structure is formed. The band gap width of MgO is 7.8 eV, and the band gap width of ZnO is 3.37 eV. 2+ and Zn 2+ With similar radius and small lattice mismatch, the bandgap width can be adjusted by adjusting the ratio of Zn and Mg. Figure 3 The band gap of MnO is 3.6ev. As a doping ion, it can adjust the band gap and introduce trap energy levels. The band gap of MnO is smaller than that of ZnMgO. During the electron energy level transition process, MnO can capture electrons. The ZnMgMnO structure formed as an electron transport layer can reduce the electron transport rate of the device, thereby balancing the electron transport rate and hole injection rate as a whole and improving the device performance.
[0043] Furthermore, the molar ratio of ZnO, MgO and MnO in the above-mentioned electron transport layer 500 is (8-12): (80-98): (1-4). The inventors found that if the amount of ZnO added is too high, it will not play a role in reducing the electron transport rate; at the same time, if the amount of MgO or MnO added is too high, it will affect the morphology of the ZnO crystal, thereby seriously affecting the electron transport rate of ZnO, resulting in the inability to achieve carrier transport balance. At the same time, the thickness of the above-mentioned electron transport layer 500 is 20-60nm. The inventors found that if the thickness of the electron transport layer 500 is too low, the electron transport rate will be increased, and if the thickness of the electron transport layer 500 is too high, the electron transport rate will be reduced.
[0044] Furthermore, the electron transport layer 500 is prepared by the following steps: zinc oxide, magnesium oxide and manganese oxide are mixed in proportion to obtain a mixed powder; then, under an inert atmosphere, the mixed powder is deposited on a silicon wafer using a pulsed laser deposition technique to obtain the electron transport layer 500. Wherein, the thickness of the silicon wafer is 1 to 2 mm. The inventors found that if the thickness of the silicon wafer is too low, it cannot better carry the electron transport layer, and it will be more difficult to peel off the electron transport layer later. If the thickness of the silicon wafer is too high, the production cost will be increased. If the thickness of the silicon wafer is too low, it cannot better carry the electron transport layer, and it will be more difficult to peel off the electron transport layer later, and an overly thick silicon wafer will increase the preparation cost.
[0045] According to an embodiment of the present invention, referring to Figure 1 The cathode 600 is disposed on the surface of the electron transport layer 500 away from the anode 100. It should be noted that those skilled in the art can select the specific material of the cathode 600 according to actual needs, such as Al.
[0046] In the second aspect of the present invention, the present invention provides a method for preparing the above electroluminescent device. Figure 2 , the method comprising:
[0047] S100: Spin coating of PEDOT:PSS solution on the anode plate followed by annealing
[0048] In this step, a PEDOT:PSS solution is spin-coated on the anode plate and then annealed, and the PEDOT:PSS solution forms a hole injection layer on the anode plate.
[0049] Furthermore, the annealing time is 20 to 40 minutes, and the annealing temperature is 140 to 180° C. The inventors found that if the annealing time is too long, it will affect the morphology and flatness of the film surface, thereby affecting the efficiency life. If the annealing time is too short, it is easy to cause insufficient volatilization of the solution. If the annealing temperature is too high, it will affect the morphology and flatness of the film surface, thereby affecting the efficiency life. If the annealing temperature is too low, it is easy to cause insufficient volatilization of the solution.
[0050] S200: Spin coating TFB solution on the hole injection layer, followed by annealing
[0051] In this step, the TFB solution is spin-coated on the hole injection layer and then annealed, and the TFB solution forms a hole transport layer on the hole injection layer.
[0052] Furthermore, the annealing time is 25 to 50 minutes, and the annealing temperature is 100 to 160° C. The inventors found that if the annealing time is too long, it will affect the morphology and flatness of the film surface, thereby affecting the efficiency life. If the annealing time is too short, it is easy to cause insufficient volatilization of the solution. If the annealing temperature is too high, it will affect the morphology and flatness of the film surface, thereby affecting the efficiency life. If the annealing temperature is too low, it is easy to cause insufficient volatilization of the solution.
[0053] S300: Spin coating a QD quantum dot solution containing CdSe, ZnS and n-octane on the hole transport layer, followed by annealing
[0054] In this step, a QD quantum dot solution containing CdSe, ZnS and n-octane is spin-coated on the hole transport layer, and then annealed to form a light-emitting layer on the hole transport layer.
[0055] Furthermore, the annealing time is 20 to 40 minutes, and the annealing temperature is 70 to 90° C. The inventors found that if the annealing time is too long, it will affect the morphology and flatness of the film surface, thereby affecting the efficiency life. If the annealing time is too short, it is easy to cause insufficient volatilization of the solution. If the annealing temperature is too high, it will affect the morphology and flatness of the film surface, thereby affecting the efficiency life. If the annealing temperature is too low, it is easy to cause insufficient volatilization of the solution.
[0056] S400: forming an electron transport layer containing ZnO, MgO and MnO on the glass substrate on the light emitting layer
[0057] In this step, an electron transport layer containing ZnO, MgO and MnO is formed on the glass substrate on the light-emitting layer. Specifically, by mixing ZnO powder, MgO powder and MnO powder, using Si as the substrate, a ZnMgMnO structure containing metal Mg and metal Mn is obtained under PLD technology. The inventors found that by doping MgO and MnO into the electron transport layer ZnO, a ZnMgMnO structure is formed. The band gap width of MgO is 7.8ev, and the band gap width of ZnO is 3.37ev. 2+ and Zn 2+ With similar radius and small lattice mismatch, the bandgap width becomes adjustable by adjusting the ratio of Zn and Mg. In addition, the bandgap width of MnO is 3.6ev. As a doping ion, the bandgap width can be adjusted to introduce trap energy levels. The bandgap width of MnO is smaller than that of ZnMgO. During the electronic energy level transition process, MnO can capture electrons, thereby reducing the electronic transmission rate of the device, thereby balancing the overall electronic transmission rate and hole injection rate, and improving the device performance.
[0058] It should be noted that the mixing ratio of ZnO, MgO and MnO in the electron transport layer and its thickness are the same as described above and will not be repeated here.
[0059] S500: Encapsulate the cathode plate on the electron transport layer
[0060] In this step, a cathode plate is packaged on the electron transport layer to obtain an electroluminescent device.
[0061] According to the method for preparing an electroluminescent device according to an embodiment of the present invention, a hole injection layer can be formed on the anode plate by spin coating a PEDOT solution on the anode plate and then annealing. Then, a TFB solution is spin coated on the hole injection layer and then annealed to form a hole transport layer on the hole injection layer. Then, a QD quantum dot solution containing CdSe, ZnS and n-octane is spin coated on the hole transport layer and then annealed to form a light-emitting layer on the hole transport layer. An electron transport layer containing ZnO, MgO and MnO is further formed on the glass substrate on the light-emitting layer. Finally, a cathode plate is packaged on the electron transport layer to obtain an electroluminescent device, wherein a ZnMgMnO structure is formed by doping MgO and MnO into the electron transport layer ZnO. The bandgap width of MgO is 7.8ev, and the bandgap width of ZnO is 3.37ev, wherein Mg 2+ and Zn 2+It has a similar radius and a small lattice mismatch. The bandgap width becomes adjustable by adjusting the ratio of Zn and Mg. In addition, the bandgap width of MnO is 3.6ev. As a doping ion, the bandgap width can be adjusted to introduce trap energy levels, and the bandgap width of MnO is smaller than that of ZnMgO. During the electronic energy level transition process, MnO can capture electrons, thereby reducing the electron transfer rate of the device, thereby balancing the electron transfer rate and the hole injection rate as a whole, thereby improving the device performance. It should be noted that the above-described features and advantages for the electroluminescent device are also applicable to the method for preparing the electroluminescent device, which will not be repeated here.
[0062] The present invention will be described below with reference to specific examples, which should be noted that these examples are merely illustrative and do not limit the present invention in any way. In addition, unless otherwise expressly stated, all reagents used in the following examples are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also readily available to those skilled in the art.
[0063] Example 1
[0064] The method for preparing an electroluminescent device comprises the following steps:
[0065] (1) Spin coating a PEDOT:PSS solution on an ITO glass substrate, and annealing at 150°C for 30 min to obtain a hole injection layer;
[0066] (2) Spin coating the TFB solution on the hole injection layer, and annealing at 150° C. for 30 min to form a hole transport layer;
[0067] (3) spin coating a QD quantum dot solution containing CdSe, ZnS and n-octane on the hole transport layer, wherein the quantum dot solution is prepared according to a ratio of 20 mg of the total mass of CdSe and ZnS dispersed in 1 mL of n-octane solution. After the spin coating is completed, annealing is performed at 80° C. for 15 min to form a light-emitting layer;
[0068] (4) ZnO powder, MgO powder and MnO powder were mixed in a molar ratio of 10:88:2, and then a ZnMgMnO structure film (thickness 50 nm) was prepared by PLD technology at a pressure of 1.0 Pa and N2 atmosphere using Si as a substrate, and the ZnMgMnO structure film was attached to the light-emitting layer as an electron transport layer;
[0069] (5) Encapsulating an Al cathode plate on the electron transport layer to obtain an electroluminescent device.
[0070] Example 2
[0071] The molar ratio of ZnO powder, MgO powder and MnO powder in step (4) is changed to 9:90:3, and the rest of the process is the same as in Example 1.
[0072] Example 3
[0073] The molar ratio of ZnO powder, MgO powder and MnO powder in step (4) is changed to 11:96:3, and the rest of the process is the same as in Example 1.
[0074] Comparative Example 1
[0075] The ZnO powder, MgO powder and MnO powder in step (4) are replaced by ZnO powder, and the rest of the process is the same as in Example 1.
[0076] Comparative Example 2
[0077] The ZnO powder, MgO powder and MnO powder in step (4) are replaced by ZnO powder and MgO powder, and the rest of the process is the same as in Example 1.
[0078] The EL, EQE, electron mobility, current efficiency and lifetime of the electroluminescent devices obtained in Examples 1-3 and Comparative Examples 1-2 were evaluated.
[0079] The evaluation results of the electroluminescent devices obtained in Examples 1-3 and Comparative Examples 1-2 are shown in Table 1.
[0080] Table 1 Evaluation results of the electroluminescent devices obtained in Examples 1-3 and Comparative Examples 1-2
[0081]
[0082]
[0083] Based on the above measurement results, it can be seen that the electron transport layer with a ZnMgMnO structure obtained in Examples 1-3 of the present invention has a significantly reduced electron mobility compared with the electron transport layer obtained in Comparative Examples 1-2, thereby balancing the injection balance of carriers and improving the performance of the electroluminescent device.
[0084] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0085] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. An electroluminescent device, characterized in that: include: anode; A hole injection layer, the hole injection layer is disposed on the anode; A hole transport layer, the hole transport layer being disposed on the hole injection layer; A light-emitting layer, the light-emitting layer being disposed on the hole transport layer; An electron transport layer, the electron transport layer being disposed on the light-emitting layer; a cathode, the cathode being disposed on the electron transport layer, Wherein, the electron transport layer comprises ZnO, MgO and MnO; The molar ratio of ZnO, MgO and MnO in the electron transport layer is (8-12): (80-98): (1-4); The electron transport layer is prepared by the following steps: mixing zinc oxide, magnesium oxide and manganese oxide to obtain a mixed powder; In an inert atmosphere, the mixed powder is deposited on a silicon wafer using a pulsed laser deposition technique to dope MgO and MnO into the electron transport layer ZnO to form a ZnMgMnO structure.
2. The electroluminescent device according to claim 1, characterized in that The thickness of the electron transport layer is 20-60 nm.
3. The electroluminescent device according to claim 2, characterized in that: The thickness of the silicon wafer is 1-2 mm.
4. A method for preparing the electroluminescent device according to any one of claims 1 to 3, characterized in that: include: (1) spin coating a PEDOT:PSS solution on an anode plate, followed by annealing, to form a hole injection layer on the anode plate; (2) spin coating a TFB solution on the hole injection layer, and then annealing to form a hole transport layer on the hole injection layer; (3) spin coating a QD quantum dot solution containing CdSe, ZnS and n-octane on the hole transport layer, and then annealing to form a light-emitting layer on the hole transport layer; (4) forming an electron transport layer containing ZnO, MgO and MnO on the glass substrate on the light-emitting layer; (5) A cathode plate is packaged on the electron transport layer to obtain the electroluminescent device.
5. The method according to claim 4, characterized in that In step (1), the annealing temperature is 140-180° C., and the annealing time is 20-40 min.
6. The method according to claim 4, characterized in that In step (2), the annealing temperature is 100-160° C., and the annealing time is 25-50 min.
7. The method according to claim 4, characterized in that In step (3), the annealing temperature is 70-90° C. and the annealing time is 20-40 min.