Au nanoparticle modified TiO 2 Nanotube light trapping structure and gallium arsenide Schottky junction solar cell and preparation method thereof
By forming Au nanoparticle-modified TiO2 nanotube light-trapping structures on GaAs/graphene Schottky junction solar cells, the problem of low photoelectric conversion efficiency of gallium arsenide Schottky junction solar cells is solved, and short-circuit current density and Significant improvement in photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202210428328.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-04-22
AI Technical Summary
The photoelectric conversion efficiency of existing gallium arsenide Schottky junction solar cells is still not ideal, and there is room for optimization.
Au nanoparticles are used to modify the light-trapping structure of TiO2 nanotubes. Ti is evaporated on the GaAs/graphene Schottky junction solar cell window layer, and the TiO2 nanotube array is grown using an anodizing method, and photoinduced on the TiO2 nanotubes. Au nanoparticles are deposited by the reduction method to form a light trapping structure of Au nanoparticles modified TiO2 nanotubes.
The short-circuit current density and photoelectric conversion efficiency of the solar cell are significantly improved, with the short-circuit current density increased by 21.3% and the photoelectric conversion efficiency increased by 22%.
Smart Images

Figure CN114823962B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solar cells, and more specifically to an Au nanoparticle-modified TiO2 nanotube light-trapping structure and a gallium arsenide Schottky junction solar cell and a preparation method thereof. Background Art
[0002] III-V solar cells based on GaAs have been widely used in the aerospace field due to their advantages such as direct band gap, excellent photoelectric conversion efficiency and radiation resistance. Theoretical calculations show that the efficiency of GaAs single-junction solar cells can reach 30%, while the maximum efficiency of multi-junction solar cells prepared with GaAs-based systems can reach 50%. However, in practical applications, it is difficult for the efficiency of solar cells to reach the theoretical value. In GaAs single-junction solar cells, the GaAs / graphene Schottky junction has a simpler manufacturing process than the traditional PN junction, which can greatly reduce the manufacturing cost. However, there is still a lot of room for optimization of solar cells with this structure. Relevant researchers have improved the photoelectric conversion efficiency of solar cells by optimizing methods such as doping and depositing anti-reflection films and improving the performance of anti-reflection films.
[0003] The prior art discloses a solar cell enhanced by a plasma excitation composite anti-reflection film and a preparation method thereof. The plasma excitation composite anti-reflection film enhanced solar cell comprises, from bottom to top, a solar cell, a metal nanoparticle layer and an anti-reflection film layer; the metal nanoparticles in the metal nanoparticle layer are silver nanoparticles, gold nanoparticles or platinum metal nanoparticles; the anti-reflection film layer is TiO2; and the solar cell is a Schottky junction solar cell. The invention achieves a high photoelectric conversion efficiency of the cell by spin-coating metal nanoparticles on the surface of the solar cell to enhance the scattering effect of sunlight and the light absorption of the solar cell; by spin-coating the TiO2 anti-reflection film, the reflection of light is effectively reduced, the absorption of light by the solar cell is enhanced, the size of the photocurrent of the solar cell is increased, and the photoelectric conversion efficiency of the solar cell is finally improved.
[0004] The prior art discloses a method for preparing a transparent electrode based on TiO2 nanotubes, wherein TiO2 nanotube films of different thicknesses are peeled off from a titanium metal substrate by a re-anodization method, the quality and crystallinity of the TiO2 nanotube films are improved, and the TiO2 nanotube films are adhered to different transparent conductive substrates to form a single-layer or multi-layer transparent electrode based on TiO2 nanotubes. The present invention realizes the preparation of a high-quality, high-crystallinity, single-layer or multi-layer structure transparent electrode based on TiO2 nanotubes, has the characteristics of being simple, reliable and highly flexible, and is conducive to the application of TiO2 nanotubes in different fields including dye-sensitized solar cells.
[0005] The prior art discloses an Au nanoparticle-modified Nd-doped BiFeO3 thin film photoelectrode and a preparation method thereof, wherein Au nanoparticles are loaded on the surface of a Nd-doped BFO thin film prepared by a sol-gel method by a photoreduction method, wherein the Nd-doped BFO thin film is stacked with nanoparticles having a particle size of about 300 to 500 nm, and the Au nanoparticles are relatively evenly distributed on the surface of the Nd-doped BFO thin film photoelectrode. After modification by Au nanoparticles and Nd element doping, the light absorption capacity of the BFO thin film can be improved, the migration and separation efficiency of photogenerated carriers can be promoted, and the photoelectrochemical performance of the BFO thin film photoelectrode can be greatly improved. Summary of the invention
[0006] In order to overcome the problem that the photoelectric conversion efficiency of gallium arsenide Schottky junction solar cells described in the prior art is still not ideal, the present invention provides an Au nanoparticle-modified TiO2 nanotube light trapping structure.
[0007] At the same time, the present invention also provides a GaAs Schottky junction solar cell with a Au nanoparticle-modified TiO2 nanotube light-trapping structure.
[0008] At the same time, the present invention also provides a method for preparing a GaAs Schottky junction solar cell with a Au nanoparticle-modified TiO2 nanotube light-trapping structure.
[0009] In order to solve the above technical problems, the technical solution of the present invention is as follows:
[0010] An Au nanoparticle-modified TiO2 nanotube light trapping structure is prepared by the following preparation method:
[0011] Step 1. Evaporating a layer of Ti on the surface of the graphene layer on the window layer of the GaAs / graphene Schottky junction solar cell;
[0012] Step 2. In a two-electrode electrochemical cell with a platinum foil as a cathode and a GaAs substrate as an anode, anodization is performed at a constant potential to grow a TiO2 nanotube array structure in an NH4F glycerol solution or an ethylene glycol solution to obtain a GaAs / graphene Schottky junction solar cell with a TiO2 nanotube array structure;
[0013] Step 3. Immerse the GaAs / graphene Schottky junction solar cell with the TiO2 nanotube array structure in the HAuCl4 solution, irradiate it with a xenon lamp as a light source, and form Au on the TiO2 nanotube array structure. 3+ The Au nanoparticles are reduced to Au nanoparticles, and then vacuum dried to obtain the Au nanoparticle-modified TiO2 nanotube light-trapping structure.
[0014] Preferably, the inner diameter of a single nanotube in the TiO2 nanotube array structure in step 2 is 20-40 nm, and the thickness is 130-170 nm.
[0015] Preferably, the anodizing conditions in step 2 are as follows: the control voltage is 20 to 30 V, and the power-on reaction time is 500 to 800 s at room temperature.
[0016] Preferably, the mass fraction of the NH4F glycerol solution in step 2 is 0.4% to 1.0%.
[0017] Preferably, the mass fraction of the ethylene glycol solution in step 2 is 0.4% to 1.0%.
[0018] Preferably, in step 3, a 300W xenon lamp is used as the light source for irradiation for 0.5 to 4 hours.
[0019] Preferably, before vacuum drying in step 3, the surface is cleaned alternately with water and ethanol or with water and ethylene glycol solution, in order to clean off the residual Au film.
[0020] A gallium arsenide Schottky junction solar cell with an Au nanoparticle-modified TiO2 nanotube light-trapping structure comprises, from bottom to top, a back electrode, an n-type GaAs substrate, an insulating layer, and a front electrode. The insulating layer and the front electrode are sequentially prepared around the n-type GaAs substrate so that the n-type GaAs substrate retains a window layer. A graphene layer and an anti-reflection layer are sequentially prepared on the window layer. The graphene layer is also in direct contact with the front electrode. The anti-reflection layer is an Au nanoparticle-modified TiO2 nanotube light-trapping structure prepared by the technology of the present invention.
[0021] Preferably, the back electrode (1) has a thickness of 100 to 180 nm.
[0022] Preferably, the insulating layer has a thickness of 100-300 nm.
[0023] Preferably, the front electrode has a thickness of 80-150 nm.
[0024] Preferably, the graphene layer has a thickness of 1 to 10 atoms.
[0025] Preferably, the Au nanoparticles have a particle size of 10 to 30 nm.
[0026] Further preferably, the thickness of the back electrode is 120 nm, the thickness of the insulating layer is 200 nm, the thickness of the front electrode is 100 nm, the thickness of the graphene layer is 3 atoms, and the particle size of the Au nanoparticles is 20 nm.
[0027] A method for preparing a GaAs Schottky junction solar cell with Au nanoparticle-modified TiO2 nanotube light-trapping structure comprises the following steps:
[0028] Step 1, evaporating a back electrode on the bottom surface of the cleaned n-type GaAs substrate, and then annealing to obtain a back electrode / GaAs substrate;
[0029] Step 2, preparing an insulating layer around the front surface of the n-type GaAs substrate in step 1, and then preparing a front electrode on the insulating layer, so that the n-type GaAs substrate retains a window layer;
[0030] Step 3, transferring the graphene sheet to the surface of the window layer retained by the n-type GaAs substrate in step 2 to obtain a graphene layer, wherein the graphene layer is also in direct contact with the front electrode in step 2;
[0031] Step 4: vapor-deposit Ti with an inner diameter of 20 to 40 nm and a thickness of 80 to 120 nm on the graphene layer on the n-type GaAs substrate window layer in step 3, then perform anodic oxidation at a constant potential in a double-electrode electrochemical cell with a platinum foil as a cathode and a GaAs substrate as an anode, grow a TiO2 nanotube array structure in an NH4F glycerol solution or an ethylene glycol solution, and obtain a gallium arsenide Schottky junction solar cell containing a TiO2 nanotube array structure;
[0032] Step 5: immerse the GaAs Schottky junction solar cell containing the TiO2 nanotube array structure in step 4 in a HAuCl4 solution, irradiate it with a xenon lamp as a light source, and form Au on the TiO2 nanotube array structure. 3+ The Au nanoparticles are reduced to Au nanoparticles and then vacuum dried to obtain Au nanoparticle modified TiO2 nanotube light trapping structure GaAs Schottky junction solar cells.
[0033] Preferably, the back electrode / GaAs substrate obtained in step 1 is immersed in an acid or alkaline solution for 1 to 30 minutes and then blown dry for later use.
[0034] Further preferably, the acid solution is any one of HCl, HNO3 or H2SO4, and the alkaline solution is KOH or NaOH, which cleans the oxide impurities on the surface of the back electrode / GaAs substrate to avoid affecting the conductivity of the product.
[0035] Preferably, the graphene sheet of step three is first immersed in a FeCl3 solution with a concentration of 0.1 mol / L until the protective film copper foil is completely dissolved, and then washed with deionized water for 2 to 3 times. Then, the graphene sheet is transferred to the window layer surface of the n-type GaAs substrate of step two on the water surface to obtain a GaAs substrate containing a graphene layer, and the graphene layer is also in direct contact with the front electrode. After the GaAs substrate containing the graphene layer is dried, it is placed in the center of the glue homogenizer, PMMA is added dropwise and rotated at a speed of 1000 rpm for 1 min to dissolve the protective film PMMA on the graphene layer, and then immersed in an acetone solution to remove the residual PMMA, and dried for use.
[0036] Preferably, the inner diameter of a single nanotube in the TiO2 nanotube array structure in step 4 is 20-40 nm, and the thickness is 130-170 nm.
[0037] Preferably, the mass fraction of the NH4F glycerol solution in step 4 is 0.4% to 1.0%.
[0038] Preferably, the mass fraction of the ethylene glycol solution in step 4 is 0.4% to 1.0%.
[0039] Step 4: Using NH4F glycerol solution or ethylene glycol solution as the electrolyte can effectively suppress the fluctuation of local ion concentration and the change of pH value, making the surface of the grown TiO2 nanotubes smoother. By adjusting its concentration, the morphology of the TiO2 nanotubes can be further optimized.
[0040] More preferably, the mass fraction of the NH4F glycerol solution is 0.6%. The mass fraction of the ethylene glycol solution is 0.6%.
[0041] Preferably, before vacuum drying in step 5, the gallium arsenide Schottky junction solar cell containing the TiO2 nanotube array structure is alternately cleaned with water and ethanol or water and ethylene glycol solution are alternately cleaned to remove the residual Au film, thereby preventing impurities from affecting the photoelectric conversion efficiency of the product.
[0042] Preferably, in step 5, a 300W xenon lamp is used as a light source for 0.5 to 4 hours. 3+ It is reduced to Au single substance and modified on the TiO2 nanotube array structure, giving the TiO2 nanotube array structure a plasma excitation effect, which can significantly enhance the light absorption efficiency of the device.
[0043] Preferably, the concentration of the HAuCl4 solution in step five is 0.09 mmol / L.
[0044] Preferably, the back electrode is any single electrode of gold, palladium, silver, titanium, copper, platinum, chromium, nickel, ITO or AZO, or a composite electrode consisting of two or more of the above.
[0045] Preferably, the front electrode is any single electrode of gold, palladium, silver, titanium, copper, platinum, chromium, nickel, ITO or AZO, or a composite electrode consisting of two or more of the above.
[0046] Preferably, the insulating layer is a SiO2 insulating layer or an Al2O3 insulating layer.
[0047] Preferably, the n-type GaAs substrate is a Si-doped n-type GaAs substrate with a crystal orientation of (100) and a Si doping concentration of 10 18 / cm 3 Order of magnitude.
[0048] Preferably, the n-type GaAs substrate cleaning method in step 1 is as follows: wipe off visible dust on the surface with a dust-free cloth dipped in ethanol, then put it into a beaker and ultrasonically clean it with acetone and ethanol for 5 minutes in sequence, and finally ultrasonically clean it with water for 3 minutes.
[0049] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0050] The solar cell of the present invention adopts a top window design structure, and a TiO2 nanotube anti-reflection layer is prepared by a thermal evaporation method combined with an anodic oxidation method. The TiO2 nanotube light-trapping structure is highly ordered, vertically oriented, and has a large specific surface area, so that the incident light is continuously reflected in the nanotube light-trapping structure and finally absorbed by the device, thereby greatly reducing light reflection, enhancing light absorption, improving the short-circuit current density of the device, and enhancing the photoelectric conversion efficiency of the device. Au nanoparticles are modified on the TiO2 nanotube light-trapping structure by a xenon lamp using a photoreduction method, and combined with the surface plasmon effect of the Au nanoparticles, the light absorption efficiency of the device can be further enhanced, thereby significantly improving the photoelectric conversion efficiency. The short-circuit current density of the solar cell prepared by the present invention is increased by as much as 21.3%. The photoelectric conversion efficiency is increased by as much as 22%. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 The schematic diagram of the structure of the Au nanoparticle-modified TiO2 nanotube light-trapping structure gallium arsenide Schottky junction solar cell of the present invention includes: 1. back electrode; 2. n-type GaAs substrate; 3. graphene layer; 4. insulating layer; 5. front electrode; 6. TiO2 nanotube array structure; and 7. Au nanoparticles.
[0052] Figure 2 It is the JV curve diagram of the solar cells of Examples 1 to 3 and Comparative Examples 1 to 2. DETAILED DESCRIPTION
[0053] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0054] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0055] An Au nanoparticle modified TiO2 nanotube light trapping structure gallium arsenide Schottky junction solar cell comprises the following steps:
[0056] Step 1: on the bottom surface of the cleaned and dried n-type GaAs substrate, a back electrode with a thickness of 100 to 180 nm is deposited by electron beam evaporation, and then annealed to obtain a back electrode / GaAs substrate, and the back electrode / GaAs substrate is cracked into 10 mm×10 mm blocks with a diamond pen, and immersed in any one solution of HCl, HNO3, H2SO4, KOH or NaOH for 1 to 30 minutes, and then taken out and dried for use;
[0057] Step 2, preparing a SiO2 insulating layer or an Al2O3 insulating layer with a thickness of 100 to 300 nm around the front of the n-type GaAs substrate in step 1, and then preparing a front electrode with a thickness of 80 to 150 nm on the SiO2 insulating layer or the Al2O3 insulating layer, so that the n-type GaAs substrate retains a window layer;
[0058] Step three, immerse the graphene sheet with copper foil and PMMA protected on both sides respectively in a FeCl3 solution with a concentration of 0.1 mol / L until the copper foil is completely dissolved, and then wash it with deionized water 2 to 3 times. Then transfer the graphene sheet on the water surface to the n-type GaAs substrate window layer in step two to obtain a GaAs substrate with a graphene layer, and the graphene layer is also in direct contact with the front electrode in step two. After drying the GaAs substrate with the graphene layer, place it in the center of a homogenizer, add PMMA and rotate it at 1000 rpm for 1 minute to dissolve the PMMA on the graphene layer, and then immerse it in an acetone solution to remove the residual PMMA. After drying, the thickness of the obtained graphene layer is 1 to 10 atoms;
[0059] Step 4: With the help of a mask, a single Ti with an inner diameter of 20 to 40 nm and a thickness of 80 to 120 nm is evaporated on the graphene layer on the surface of the window layer of the n-type GaAs substrate in step 3, and then placed in a 0.4 to 1.0% NH4F glycerol solution or ethylene glycol solution, with a platinum foil as a cathode and an n-type GaAs substrate as an anode, at room temperature, the voltage is adjusted to 20 to 30 V, and an anodic oxidation reaction is performed for 500 to 800 seconds to grow a single TiO2 nanotube array structure with an inner diameter of 20 to 40 nm and a thickness of 130 to 170 nm, thereby obtaining a gallium arsenide Schottky junction solar cell containing a TiO2 nanotube array structure;
[0060] Step 5: immerse the GaAs Schottky junction solar cell containing the TiO2 nanotube array structure in step 4 in a quartz glass tube filled with a HAuCl4 solution with a concentration of 0.09 mmol / L, and irradiate it from the bottom of the quartz glass tube with a 300 W xenon lamp as a light source for 0.5 to 4 hours to form Au on the TiO2 nanotube array structure. 3+ The Au nanoparticles are reduced to a particle size of 10 to 30 nm, and then washed alternately with deionized water and ethanol or deionized water and ethylene glycol solution to remove the residual Au film, and then placed in a vacuum hood for drying to obtain Au nanoparticle-modified TiO2 nanotube light-trapping structure gallium arsenide Schottky junction solar cells.
[0061] Specifically, the n-type GaAs substrate refers to a Si-doped n-type GaAs substrate with a crystal orientation of (100) and a Si doping concentration of 10 18 / cm 3 Order of magnitude, thickness is 350μm.
[0062] Specifically, in step 1, the cleaning method of the n-type GaAs substrate is as follows: wipe off the visible dust on the surface with a dust-free cloth dipped in ethanol, then put it into a beaker and use acetone and ethanol for ultrasonic cleaning for 5 minutes in sequence, and finally use water for ultrasonic cleaning for 3 minutes.
[0063] Specifically, the back electrode is any single electrode of gold, palladium, silver, titanium, copper, platinum, chromium, nickel, ITO or AZO, or a composite electrode composed of two or more thereof.
[0064] Specifically, the front electrode is any single electrode of gold, palladium, silver, titanium, copper, platinum, chromium, nickel, ITO or AZO, or a composite electrode composed of two or more thereof.
[0065] Example 1
[0066] An Au nanoparticle modified TiO2 nanotube light trapping structure gallium arsenide Schottky junction solar cell comprises the following steps:
[0067] Step 1: On the bottom surface of the cleaned and dried n-type GaAs substrate 2, an Ag back electrode 1 with a thickness of 100 nm is deposited by electron beam evaporation, and then annealed at 330° C. for 3 min to obtain an Ag back electrode / GaAs substrate, which is then cracked into 10 mm×10 mm blocks with a diamond pen, immersed in a NaOH solution for 30 min, and taken out and dried for later use;
[0068] Step 2: stick a 5×5 mm adhesive tape on the middle of the front side of the n-type GaAs substrate 2 in step 1, and use electron beam evaporation to evaporate an Al2O3 insulating layer 4 with a thickness of 100 nm around the front side of the n-type GaAs substrate 2 in step 1, and then evaporate a Cu front electrode 5 with a thickness of 150 nm on the Al2O3 insulating layer 4, and then peel off the adhesive tape to retain a window layer in the middle of the front side of the n-type GaAs substrate 2;
[0069] Step 3, immersing the graphene sheet protected by copper foil and PMMA on both sides in a FeCl3 solution with a concentration of 0.1mol / L until the copper foil is completely dissolved, washing 3 times with deionized water, and then transferring the graphene sheet on the water surface to the window layer of the n-type GaAs substrate 2 of step 2 to obtain an n-type GaAs substrate with a graphene layer 3, the graphene layer 3 is also in direct contact with the Cu front electrode 5 of step 2, and the n-type GaAs substrate 2 with the graphene layer 3 is dried and placed in the center of a homogenizer, PMMA is dripped and rotated at a speed of 1000rpm for 1min to dissolve the PMMA on the graphene layer 3, and then immersed in an acetone solution to remove residual PMMA. After drying, the thickness of the obtained graphene layer is 1 atom;
[0070] Step 4: With the help of a mask, a single Ti with an inner diameter of 20 nm and a thickness of 100 nm is evaporated on the graphene layer 3 on the surface of the window layer of the n-type GaAs substrate 2 in step 3, and then placed in a 0.4% by mass NH4F glycerol solution, with a platinum foil as a cathode and an n-type GaAs substrate as an anode, at room temperature, the voltage is adjusted to 20 V, and power is turned on for an anodic oxidation reaction for 800 s to grow a single TiO2 nanotube array structure 6 with an inner diameter of 20 nm and a thickness of 170 nm, to obtain a gallium arsenide Schottky junction solar cell containing the TiO2 nanotube array structure 6;
[0071] Step 5: immerse the GaAs Schottky junction solar cell containing the TiO2 nanotube array structure 6 in step 4 in a quartz glass tube filled with a 0.09 mmol / L HAuCl4 solution, and irradiate it from the bottom of the quartz glass tube with a 300 W xenon lamp as a light source for 0.5 h, and form Au on the TiO2 nanotube array structure 6. 3+The Au nanoparticles 7 were reduced to a particle size of 10 nm, and then washed alternately with deionized water and ethylene glycol to remove the residual Au film. Finally, the Au nanoparticles were placed in a vacuum hood for drying to obtain a GaAs Schottky junction solar cell with a TiO2 nanotube light trapping structure.
[0072] Specifically, the n-type GaAs substrate 2 is a Si-doped n-type GaAs substrate with a crystal orientation of (100) and a Si doping concentration of 10 18 / cm 3 Order of magnitude, thickness is 350μm.
[0073] Specifically, in step 1, the n-type GaAs substrate cleaning method is as follows: wipe off the visible dust on the surface with a dust-free cloth dipped in ethanol, then put it into a beaker and use acetone and ethanol for ultrasonic cleaning for 5 minutes in sequence, and finally use water for ultrasonic cleaning for 3 minutes.
[0074] Example 2
[0075] An Au nanoparticle modified TiO2 nanotube light trapping structure gallium arsenide Schottky junction solar cell comprises the following steps:
[0076] Step 1: On the bottom surface of the cleaned and dried n-type GaAs substrate 2, an Au back electrode 1 with a thickness of 120 nm is deposited by electron beam evaporation, and then annealed at 330° C. for 3 min to obtain an Au back electrode / GaAs substrate, which is then cracked into 10 mm×10 mm blocks with a diamond pen, immersed in an HCl solution for 1 min, and taken out and dried for later use;
[0077] Step 2: stick a 5×5 mm adhesive tape on the middle of the front side of the n-type GaAs substrate 2 in step 1, and use electron beam evaporation to evaporate a SiO2 insulating layer 4 with a thickness of 200 nm around the front side of the n-type GaAs substrate 2 in step 1, and then evaporate an Ag front electrode 5 with a thickness of 100 nm on the SiO2 insulating layer 4, and then peel off the adhesive tape to leave a window layer in the middle of the front side of the n-type GaAs substrate 2;
[0078] Step 3, immersing the graphene sheet with copper foil and PMMA protected on both sides in a FeCl3 solution with a concentration of 0.1mol / L until the copper foil is completely dissolved, washing 3 times with deionized water, and then transferring the graphene sheet on the water surface to the window layer of the n-type GaAs substrate 2 of step 2 to obtain an n-type GaAs substrate with a graphene layer 3, the graphene layer 3 is also in direct contact with the Ag front electrode 5 of step 2, and the n-type GaAs substrate 2 with the graphene layer 3 is dried and placed in the center of a homogenizer, PMMA is dripped and rotated at a speed of 1000rpm for 1min to dissolve the PMMA on the graphene layer 3, and then immersed in an acetone solution to remove residual PMMA. After drying, the thickness of the obtained graphene layer is 3 atoms;
[0079] Step 4: With the help of a mask, a single Ti with an inner diameter of 40 nm and a thickness of 80 nm is evaporated on the graphene layer 3 on the surface of the window layer of the n-type GaAs substrate 2 in step 3, and then placed in a 0.6% by mass NH4F glycerol solution, with a platinum foil as a cathode and an n-type GaAs substrate as an anode, at room temperature, the voltage is adjusted to 30 V, and an anodic oxidation reaction is performed for 600 s to grow a single TiO2 nanotube array structure 6 with an inner diameter of 40 nm and a thickness of 130 nm, thereby obtaining a gallium arsenide Schottky junction solar cell containing the TiO2 nanotube array structure 6;
[0080] Step 5: immerse the GaAs Schottky junction solar cell containing the TiO2 nanotube array structure 6 in step 4 in a quartz glass tube filled with a 0.09 mmol / L HAuCl4 solution, and irradiate it from the bottom of the quartz glass tube with a 300 W xenon lamp as a light source for 4 hours to form Au on the TiO2 nanotube array structure 6. 3+ The Au nanoparticles were reduced to Au nanoparticles with a particle size of 20 nm 7. Then, the Au film was removed by washing with deionized water and ethanol alternately, and then dried in a vacuum hood to obtain Au nanoparticle-modified TiO2 nanotube light-trapping structure GaAs Schottky junction solar cells.
[0081] Specifically, the n-type GaAs substrate 2 is a Si-doped n-type GaAs substrate with a crystal orientation of (100) and a Si doping concentration of 10 18 / cm 3 Order of magnitude, thickness is 350μm,
[0082] Specifically, in step 1, the n-type GaAs substrate cleaning method is as follows: wipe off the visible dust on the surface with a dust-free cloth dipped in ethanol, then put it into a beaker and use acetone and ethanol for ultrasonic cleaning for 5 minutes in sequence, and finally use water for ultrasonic cleaning for 3 minutes.
[0083] Example 3
[0084] An Au nanoparticle modified TiO2 nanotube light trapping structure gallium arsenide Schottky junction solar cell comprises the following steps:
[0085] Step 1: On the bottom surface of the cleaned and dried n-type GaAs substrate 2, an ITO back electrode 1 with a thickness of 180 nm is deposited by electron beam evaporation, and then annealed at a temperature of 330° C. for 3 min to obtain an ITO back electrode / GaAs substrate, and the substrate is cracked into 10 mm×10 mm blocks with a diamond pen, immersed in a HNO3 solution for 20 min, and taken out and dried for use;
[0086] Step 2: stick a 5×5 mm adhesive tape on the middle of the front side of the n-type GaAs substrate 2 in step 1, and use electron beam evaporation to evaporate a SiO2 insulating layer 4 with a thickness of 300 nm around the front side of the n-type GaAs substrate 2 in step 1, and then evaporate an AZO front electrode 5 with a thickness of 80 nm on the SiO2 insulating layer 4, and then peel off the adhesive tape to leave a window layer in the middle of the front side of the n-type GaAs substrate 2;
[0087] Step 3, immersing the graphene sheet with copper foil and PMMA protected on both sides in a FeCl3 solution with a concentration of 0.1mol / L until the copper foil is completely dissolved, washing with deionized water twice, and then transferring the graphene sheet to the n-type GaAs substrate 2 window layer of step 2 on the water surface to obtain an n-type GaAs substrate with a graphene layer 3, the graphene layer 3 is also in direct contact with the AZO front electrode 5 of step 2, and the n-type GaAs substrate 2 with the graphene layer 3 is dried and placed in the center of a homogenizer, PMMA is dripped and rotated at a speed of 1000rpm for 1min to dissolve the PMMA on the graphene layer 3, and then immersed in an acetone solution to remove residual PMMA. After drying, the obtained graphene layer has a thickness of 10 atoms;
[0088] Step 4, with the help of a mask, a single Ti with an inner diameter of 30nm and a thickness of 120nm is evaporated on the graphene layer 3 on the surface of the window layer of the n-type GaAs substrate 2 in step 3, and then placed in an ethylene glycol solution with a mass fraction of 1.0%, with a platinum foil as a cathode and an n-type GaAs substrate as an anode, at room temperature, the voltage is adjusted to 25V, and power is turned on for an anodic oxidation reaction for 500S to grow a single TiO2 nanotube array structure 6 with an inner diameter of 30nm and a thickness of 140nm, to obtain a gallium arsenide Schottky junction solar cell containing the TiO2 nanotube array structure 6;
[0089] Step 5: immerse the GaAs Schottky junction solar cell containing the TiO2 nanotube array structure 6 in step 4 in a quartz glass tube filled with a 0.09 mmol / L HAuCl4 solution, and irradiate it from the bottom of the quartz glass tube with a 300 W xenon lamp as a light source for 2 hours to form Au on the TiO2 nanotube array structure 6. 3+ The Au nanoparticles 7 were reduced to a particle size of 30 nm, and then washed alternately with deionized water and ethanol to remove the residual Au film. The Au nanoparticles were then dried in a vacuum hood to obtain a GaAs Schottky junction solar cell with a TiO2 nanotube light-trapping structure modified with Au nanoparticles.
[0090] Specifically, the n-type GaAs substrate 2 is a Si-doped n-type GaAs substrate with a crystal orientation of (100) and a Si doping concentration of 10 18 / cm 3 Order of magnitude, thickness is 350μm.
[0091] Specifically, in step 1, the cleaning method of the n-type GaAs substrate 2 is as follows: wipe off the visible dust on the surface with a dust-free cloth dipped in ethanol, then put it into a beaker and use acetone and ethanol for ultrasonic cleaning for 5 minutes in sequence, and finally use water for ultrasonic cleaning for 3 minutes.
[0092] Comparative Example 1
[0093] The preparation method of Comparative Example 1 is similar to that of Example 1, except that step 4 of growing the TiO2 nanotube array structure 6 is not performed.
[0094] Comparative Example 2
[0095] The preparation method of Comparative Example 2 is similar to that of Example 1, except that the TiO 2 nanotube array structure 6 is not modified with Au nanoparticles 7 .
[0096] Performance Testing
[0097] The electrical properties of the solar cells obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were measured. Figure 2 and Table 1.
[0098] Table 1 Comparison of parameters of solar cells in Examples 1 to 3 and Comparative Examples 1 to 2
[0099] Experimental Group <![CDATA[Short-circuit current density (mA / cm 2 )]]> Photoelectric conversion efficiency (%) Example 1 15.08 5.86 Example 2 16.05 6.05 Example 3 15.85 5.94 Comparative Example 1 13.23 5.41 Comparative Example 2 13.85 4.96
[0100] From the test results in Table 1, it can be seen that the short-circuit current density of the solar cell of the present invention is from 13.23 mA / cm 2 Significantly increased to 16.05mA / cm 2 , an increase of up to 21.3%.
[0101] The photoelectric conversion efficiency increased from 4.96% to 6.05%, an increase of 22%, indicating that Au nanoparticle-modified TiO2 nanotube anti-reflection film can significantly improve the electrical performance of solar cells and have a higher photoelectric conversion efficiency.
[0102] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. An Au nanoparticle-modified TiO2 nanotube light trapping structure, characterized in that: Prepared by the following preparation method: Step 1. Evaporating a layer of Ti on the surface of the graphene layer on the window layer of the GaAs / graphene Schottky junction solar cell; Step 2. In a two-electrode electrochemical cell with a platinum foil as a cathode and a GaAs substrate as an anode, anodization is performed at a constant potential to grow a TiO2 nanotube array structure (6) in an NH4F glycerol solution or an ethylene glycol solution to obtain a GaAs / graphene Schottky junction solar cell having a TiO2 nanotube array structure (6); Step 3. Immerse the GaAs / graphene Schottky junction solar cell with the TiO2 nanotube array structure (6) in step 2 in a HAuCl4 solution, irradiate it with a xenon lamp as a light source, and form Au on the TiO2 nanotube array structure (6). 3+ Reducing to Au nanoparticles (7), and vacuum drying to obtain Au nanoparticle-modified TiO2 nanotube light-trapping structure; The anodizing conditions in step 2 are as follows: the control voltage is 20 to 30 V, and the power-on reaction time is 500 to 800 s at room temperature; The inner diameter of a single nanotube of the TiO2 nanotube array structure (6) in step 2 is 20-40 nm, and the thickness is 130-170 nm.
2. The Au nanoparticle-modified TiO2 nanotube light trapping structure according to claim 1, characterized in that: The mass fraction of the NH4F glycerol solution or ethylene glycol solution in step 2 is 0.4% to 1.0%.
3. The Au nanoparticle-modified TiO2 nanotube light trapping structure according to claim 1, characterized in that: In step 3, a 300W xenon lamp is used as a light source for irradiation for 0.5 to 4 hours.
4. The Au nanoparticle-modified TiO2 nanotube light trapping structure according to claim 1, characterized in that: In step 3, the process is performed by alternately washing with water and ethanol or alternately washing with water and ethylene glycol solution before vacuum drying.
5. An Au nanoparticle modified TiO2 nanotube light trapping structure gallium arsenide Schottky junction solar cell, characterized in that: From bottom to top, it comprises a back electrode (1), an n-type GaAs substrate (2), an insulating layer (4), and a front electrode (5); the insulating layer (4) and the front electrode (5) are sequentially prepared around the n-type GaAs substrate (2) so that the n-type GaAs substrate (2) retains a window layer; a graphene layer (3) and an anti-reflection layer are sequentially prepared on the surface of the window layer, and the graphene layer (3) is also in direct contact with the front electrode (5); the anti-reflection layer is the Au nanoparticle-modified TiO2 nanotube light trapping structure according to any one of claims 1 to 4.
6. The Au nanoparticle modified TiO2 nanotube light trapping structure GaAs Schottky junction solar cell according to claim 5, characterized in that: The thickness of the back electrode (1) is 100 to 180 nm, the thickness of the insulating layer (4) is 100 to 300 nm, the thickness of the front electrode (5) is 80 to 150 nm, the thickness of the graphene layer (3) is 1 to 10 atoms, and the particle size of the Au nanoparticles (7) is 10 to 30 nm.
7. The Au nanoparticle modified TiO2 nanotube light trapping structure GaAs Schottky junction solar cell according to claim 5, characterized in that: The back electrode (1) and the front electrode (5) are any single electrode or a composite electrode composed of two or more of gold, palladium, silver, titanium, copper, platinum, chromium, nickel, ITO or AZO; the insulating layer (4) is a SiO2 insulating layer or an Al2O3 insulating layer; The n-type GaAs substrate (2) is a Si-doped n-type GaAs substrate with a crystal orientation of (100) and a Si doping concentration of 10 18 / cm 3 Order of magnitude.
8. A method for preparing the Au nanoparticle-modified TiO2 nanotube light-trapping structure GaAs Schottky junction solar cell according to any one of claims 5 to 7, characterized in that: The following steps are involved: Step 1, evaporating a back electrode (1) on the bottom surface of a cleaned n-type GaAs substrate (2), and then annealing to obtain a back electrode / GaAs substrate; Step 2, preparing an insulating layer (4) around the front surface of the n-type GaAs substrate (2) in step 1, and then preparing a front electrode (5) on the insulating layer (4), so that the n-type GaAs substrate (2) retains a window layer; Step 3, transferring the graphene sheet to the surface of the window layer retained by the n-type GaAs substrate in step 2 to obtain a graphene layer (3), wherein the graphene layer (3) is also in direct contact with the front electrode (5) in step 2; Step 4: vapor-depositing Ti with an inner diameter of 20 to 40 nm and a thickness of 80 to 120 nm on the graphene layer (3) on the surface of the window layer of the n-type GaAs substrate (2) in step 3, and then performing anodization at a constant potential in a two-electrode electrochemical cell with a platinum foil as a cathode and a GaAs substrate as an anode, growing a TiO2 nanotube array structure (6) in an NH4F glycerol solution or an ethylene glycol solution, and obtaining a gallium arsenide Schottky junction solar cell containing the TiO2 nanotube array structure (6); Step 5: immerse the GaAs Schottky junction solar cell containing the TiO2 nanotube array structure (6) in step 4 in a HAuCl4 solution, irradiate it with a xenon lamp as a light source, and form Au on the TiO2 nanotube array structure (6). 3+ The Au nanoparticles (7) are reduced and then vacuum dried to obtain Au nanoparticle-modified TiO2 nanotube light-trapping structure GaAs Schottky junction solar cells.