Negative electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

By using a combination of porous metal current collectors and silicon-based materials in non-aqueous electrolyte secondary batteries, the problem of conductive path fracture caused by limited thickness of the negative electrode and expansion and contraction is solved, and high cycle durability and energy density are improved.

CN114824166BActive Publication Date: 2024-10-29HONDA MOTOR CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210048652.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-17
Publication Date
2024-10-29
Estimated Expiration
2042-01-17

AI Technical Summary

Technical Problem

The thickness of the negative electrode in existing non-aqueous electrolyte secondary batteries is limited, resulting in problems such as uneven coating, cracks, and peeling, making it difficult to improve cycle durability and energy density, and the difference in expansion and contraction of the porous metal current collector leads to conductive paths fracture.

Method used

A porous metal body is used as the current collector, and the negative electrode material is filled with silicon-based materials, silicate skeleton forming agents with siloxane bonds, conductive additives and binders, and the negative electrode active material is filled through the pores of the porous metal body. , and set up areas with different filling densities in the current collector to stabilize expansion and contraction.

Benefits of technology

Effectively suppresses durability degradation, improves cycle durability and energy density, prevents breakage of conductive paths, and achieves high-precision anode structure and high capacity density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824166B_ABST
    Figure CN114824166B_ABST
Patent Text Reader

Abstract

The problem to be solved by the present invention is to provide a negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery including the negative electrode for a non-aqueous electrolyte secondary battery, which can suppress durable degradation, improve cycle durability and energy density, and suppress the breakage of the conductive path of the collector composed of a porous metal body in the area that becomes the boundary between the coated area and the uncoated area of ​​the electrode mixture (electrode mixture boundary area). In order to solve the above problems, the negative electrode for a non-aqueous electrolyte secondary battery includes: a collector foil; a pair of collectors, which are arranged on both sides of the collector foil in contact with each other and are composed of a porous metal body; and a negative electrode material, which is arranged in the pores of the porous metal body; and the negative electrode material includes: a negative electrode active material composed of a silicon-based material, a skeleton forming agent containing a silicate having a siloxane bond, a conductive auxiliary agent and a binder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery including the negative electrode. Background Art

[0002] In recent years, non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries have been used more in automobiles and the like because they are small, lightweight and can obtain high output. Non-aqueous electrolyte secondary batteries are a general term for the following power storage devices: a battery system using an electrolyte that is not mainly composed of water in the electrolyte, and can be charged and discharged. For example, known lithium ion batteries, lithium polymer batteries, lithium all-solid-state batteries, lithium-air batteries, lithium-sulfur batteries, sodium ion batteries, potassium ion batteries, multivalent ion batteries, fluoride batteries, sodium-sulfur batteries, etc. The non-aqueous electrolyte secondary battery is mainly composed of a positive electrode, a negative electrode, and an electrolyte. In addition, when the electrolyte has fluidity, a diaphragm is further interposed between the positive electrode and the negative electrode.

[0003] For example, the following technology is disclosed: in order to extend the battery life, a skeleton forming agent containing a silicate having a siloxane bond is present at least on the surface of the active material, and the skeleton forming agent is infiltrated from the surface to the inside (for example, refer to Patent Document 1). According to this technology, since a strong skeleton can be formed on the active material, the battery life can be extended. In addition, the following technology is also disclosed: the above-mentioned skeleton forming agent is applied to a negative electrode containing a silicon (Si)-based active material (for example, refer to Patent Document 2).

[0004] [Prior technical literature]

[0005] (Patent Document)

[0006] Patent Document 1: Japanese Patent No. 6369818

[0007] Patent Document 2: Japanese Patent No. 6149147 Summary of the invention

[0008] [Problems to be solved by the invention]

[0009] However, in the above-mentioned non-aqueous electrolyte secondary battery, it is required to improve the energy density. In order to improve the energy density, it is considered more effective to thicken the film thickness of the negative electrode or to make the amount of the negative electrode active material high-density. However, in the prior art, the thickness of the negative electrode is limited in the production of the negative electrode. Specifically, in the past, the practical thickness of the film thickness of the electrode mixture layer applied on the collector foil was less than 100 μm. When the film thickness is more than 100 μm, problems such as uneven coating, cracks, and peeling will occur, making it difficult to produce a high-precision negative electrode.

[0010] Furthermore, since it is necessary to balance the binding force of the binder with the expansion and contraction of the negative electrode active material, the amount of negative electrode active material per unit area is limited from the perspective of durability. Specifically, the limit of the active material capacity per unit area of ​​the negative electrode is 4 mAh / cm 2 If the active material capacity is less than 4 mAh / cm 2 , then no improvement in energy density can be expected.

[0011] In order to solve the above problems, it is considered that the porous metal body is applied to the collector of the negative electrode of the non-aqueous electrolyte secondary battery, and the porous metal body is impregnated with the electrode mixture. However, it is known that when the collector of the negative electrode is composed of a porous metal body, when the non-aqueous electrolyte secondary battery is charged and discharged, between the coated area coated with the electrode mixture on the collector and the uncoated area (ear area) where the electrode mixture is not coated on the collector, the difference in expansion and contraction is large, and fracture occurs in the area (boundary area) that becomes the boundary of the coated area and the uncoated area.

[0012] Therefore, it is desired to have a negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery including the negative electrode for a non-aqueous electrolyte secondary battery, which can suppress durability degradation, improve cycle durability and energy density, and suppress the breakage of the conductive path of the collector composed of a porous metal body in the area which is the boundary between the coated area and the uncoated area of ​​the electrode mixture (electrode mixture boundary area).

[0013] The present invention has been completed in view of the above situation, and its purpose is to provide a negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery including the negative electrode for a non-aqueous electrolyte secondary battery, which can suppress durability degradation, improve cycle durability and energy density, and suppress the breakage of the conductive path of the collector composed of a porous metal body generated in the area that becomes the boundary between the coated area and the uncoated area of ​​the electrode mixture (electrode mixture boundary area).

[0014] [Technical means to solve the problem]

[0015] (1) In order to achieve the above-mentioned purpose, the present invention provides a negative electrode for a non-aqueous electrolyte secondary battery, comprising: a collector foil; a pair of collectors, which are arranged in contact with each other on both sides of the aforementioned collector foil and are composed of a porous metal body; and a negative electrode material, which is arranged in the pores of the aforementioned porous metal body; and the aforementioned negative electrode material includes: a negative electrode active material composed of a silicon-based material, a skeleton former containing a silicate having a siloxane bond, a conductive aid and a binder.

[0016] (2) In the negative electrode for a nonaqueous electrolyte secondary battery described in (1), at least one of the pair of current collectors may have a region that is in contact with the current collector foil and is not filled with the negative electrode material or a region where the filling density of the negative electrode material is lower than that of other regions.

[0017] (3) In the negative electrode for a nonaqueous electrolyte secondary battery described in (1) or (2), the thickness of a region not filled with the negative electrode material or a region with a lower filling density of the negative electrode material than other regions may be 50 μm or less.

[0018] (4) In the negative electrode for a nonaqueous electrolyte secondary battery according to any one of (1) to (3), the skeleton-forming agent may include a silicate represented by the following general formula (1):

[0019] A2O·nSiO2 Formula (1)

[0020] In the above general formula (1), A represents an alkali metal.

[0021] (5) In the negative electrode for a nonaqueous electrolyte secondary battery according to any one of (1) to (4), the porous metal body may be a foamed metal body.

[0022] (6) Furthermore, the present invention provides a non-aqueous electrolyte secondary battery comprising the negative electrode for a non-aqueous electrolyte secondary battery according to any one of (1) to (5).

[0023] (Effects of the Invention)

[0024] According to the present invention, there can be provided a negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery comprising the negative electrode for a non-aqueous electrolyte secondary battery, which can suppress durability degradation, improve cycle durability and energy density, and suppress the breakage of the conductive path of the collector composed of a porous metal body generated in the area which is the boundary between the coated area and the uncoated area of ​​the electrode mixture (electrode mixture boundary area). BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a diagram schematically showing the structure of the negative electrode for a nonaqueous electrolyte secondary battery according to the first embodiment of the present invention.

[0026] Figure 2 This is a diagram schematically showing the internal structure of the negative electrode for a non-aqueous electrolyte secondary battery of the present invention.

[0027] Figure 3 It is a cross-sectional view schematically showing the structure of a negative electrode for a nonaqueous electrolyte secondary battery according to a second embodiment of the present invention.

[0028] Figure 4This is a graph showing the relationship between the number of cycles and the capacity retention rate of Examples 1 to 3 and Comparative Example 1. DETAILED DESCRIPTION

[0029] Hereinafter, a first embodiment of the present invention will be described in detail with reference to the drawings.

[0030] <First embodiment>

[0031] [negative electrode]

[0032] Figure 1 1 is a diagram schematically showing the structure of the negative electrode 1 for a non-aqueous electrolyte secondary battery according to the present embodiment. The negative electrode 1 for a non-aqueous electrolyte secondary battery according to the present embodiment comprises: a current collector foil 11; and a pair of current collectors 12, which are arranged on both sides of the current collector foil in contact with each other and are composed of a porous metal body.

[0033] and, Figure 2 Schematically shows a state where a negative electrode material 13 is arranged in the pores of a current collector 12 composed of a porous metal body. The negative electrode material 13 includes: a negative electrode active material 14 composed of a silicon-based material, a skeleton forming agent 15 containing a silicate having a siloxane bond, a conductive auxiliary agent 16, and a binder 17. By sandwiching the collector foil 11 with a pair of current collectors 12, even if the negative electrode active material 14 filled in the collector 12 expands and contracts during charging and discharging, the break of the conductive path between the collector foil 11 and the collector 12 composed of a porous metal body can be suppressed. In addition, even if a break occurs, conduction (conductive path) from the collector foil side can be ensured.

[0034] For example, by applying the present embodiment to a negative electrode for a lithium ion secondary battery, a negative electrode for a lithium ion secondary battery and a lithium ion secondary battery including the negative electrode for a lithium ion secondary battery can be provided, which can suppress durable degradation and improve energy density. Below, an example of applying the present embodiment to a negative electrode for a lithium ion secondary battery is described in detail, but various additions, changes or deletions can be made within the scope of the present invention.

[0035] In addition, the pair of current collectors 12 composed of porous metal bodies may be simply referred to as “current collectors.” In this case, both of the pair of current collectors may be referred to, and either one of the pair of current collectors may be referred to.

[0036] As a pair of current collectors 12 arranged in contact with both sides of the current collector foil 11, a current collector composed of a porous metal body can be used. Nets, fabrics, non-woven fabrics, embossed bodies, punched bodies, expanded bodies, foamed bodies, etc. can be exemplified, and a foamed metal body is preferably used. Among them, a foamed metal body having a three-dimensional mesh structure with continuous pores is preferably used, for example, Celmet (registered trademark) (manufactured by Sumitomo Electric Industries, Ltd.) can be used.

[0037] Furthermore, the thicknesses of the pair of current collectors 12 composed of porous metal bodies disposed in contact with both surfaces of the current collector foil 11 may be the same or different.

[0038] The material of the collector foil and the porous metal body is not particularly limited as long as it has electronic conductivity and can conduct electricity to the electrode material held. For example, conductive metals such as Al, Al alloys, Ni, Ni-Cr alloys, Fe, Cu, Ti, Cr, Au, Mo, W, Ta, Pt, Ru, and Rh, and conductive alloys containing two or more of these conductive metals (stainless steel (SUS304, SUS316, SUS316L, YUS270, etc.)) can be used. In addition, when using materials other than the above-mentioned conductive metals or conductive alloys, for example, a multilayer structure of heterogeneous metals such as Cu and Ni coated on Fe can also be used. Among them, Ni or Ni alloys are preferably used because of their excellent electronic conductivity and reduction resistance.

[0039] Furthermore, the materials of the current collector foil and the porous metal body may be the same or different.

[0040] The thickness of the current collector foil is preferably 5 μm or more, more preferably 8 μm or more. The thickness of the current collector foil is preferably 20 μm or less, more preferably 15 μm or less.

[0041] The thickness of the porous metal body is preferably 10 μm or more, more preferably 50 μm or more. The thickness of the porous metal body is preferably 1 mm or less, more preferably 500 μm or less.

[0042] The average pore size of the porous metal body is preferably less than 500 μm. By making the average pore size of the porous metal body within this range, the distance between the negative electrode active material 14 filled in the porous metal body and the metal skeleton is stabilized, the electronic conductivity is improved, and the increase in the internal resistance of the battery is suppressed. In addition, even if the volume changes with charging and discharging, the electrode mixture can be suppressed from falling off.

[0043] The specific surface area of ​​the porous metal body is preferably 200 to 10,000 m 2 / m 3This is 2 to 10 times the specific surface area of ​​conventional collector foils. By keeping the specific surface area of ​​the porous metal body within this range, the contact between the electrode mixture and the collector 12 is improved, and the increase in the internal resistance of the battery is suppressed. The specific surface area is more preferably 500 to 7000 m 2 / m 3 .

[0044] The porosity of the porous metal body is preferably 90 to 99%. By virtue of the porosity of the porous metal body being within this range, the filling amount of the electrode mixture can be increased, and the energy density of the battery is improved. Specifically, if the porosity exceeds 99%, the mechanical strength of the porous metal body is significantly reduced, and it is easy to be damaged due to the volume change of the electrode accompanying the charge and discharge. On the contrary, if it is less than 90%, not only the filling amount of the electrode mixture is reduced, but also the ion conductivity of the electrode is reduced, and it is difficult to obtain sufficient input and output characteristics. From these viewpoints, the porosity is more preferably 93 to 98%.

[0045] The electrode area weight of the porous metal body is preferably 1 to 100 mg / cm 2 When the electrode unit area weight of the porous metal body is within this range, the active material capacity can be fully expressed, and the electrode can exhibit the designed capacity. The electrode unit area weight is more preferably 5 to 60 mg / cm 2 .

[0046] As the negative electrode active material 14, a negative electrode active material that can reversibly absorb and release lithium ions can be used. Specifically, a negative electrode active material 14 composed of a high-capacity silicon-based material can be used. As silicon-based materials, silicon monomers, silicon alloys, silicon oxides, silicon compounds, etc. meet the conditions. Here, silicon monomer refers to crystalline or amorphous silicon with a purity of 95% by mass or more. Silicon alloy refers to a Si-M alloy containing silicon and other transition elements M. As M, for example, Al, Mg, La, Ag, Sn, Ti, Y, Cr, Ni, Zr, V, Nb, Mo, etc. can be listed. It can also be a complete solid solution alloy, eutectic alloy, hypoeutectic alloy, hypereutectic alloy, and peritectic alloy. Silicon oxide refers to silicon oxide or a complex containing silicon monomer and SiO2. The element ratio of Si to O is as long as Si is 1 and O is less than 1.7. Silicon compound refers to a substance in which silicon is chemically bonded with two or more other elements. Among them, silicon monomer is preferred in terms of being able to form the following interface layer well. Alternatively, a carbon-based material may be mixed or composited with a silicon-based material for use.

[0047] The shape of the silicon-based material is not particularly limited, and may be spherical, elliptical, polygonal, ribbon-like, fibrous, flaky, ring-like, or hollow powder. They may be single particles or granules.

[0048] The expansion rate of the negative electrode active material 14 made of silicon-based material due to charge and discharge is 10% or more. That is, when the negative electrode active material 14 greatly expands and contracts during charge and discharge, the use of the skeleton forming agent 15 described below can suppress the durability degradation caused by the expansion and contraction.

[0049] From the viewpoint of achieving excellent cycle characteristics of the electrode and obtaining high input-output characteristics, the particle size of the silicon-based material is preferably 0.01 μm to 10 μm.

[0050] Furthermore, the negative electrode active material 14 may include not only the above-mentioned silicon-based material but also a carbon-based material (graphite, hard carbon, soft carbon, etc.).

[0051] As the skeleton forming agent 15, a skeleton forming agent 15 containing a silicate having a siloxane bond can be used. More specifically, the skeleton forming agent 15 preferably contains a silicate represented by the following general formula (1).

[0052] A2O·nSiO2 formula (1)

[0053] In the above general formula (1), A represents an alkali metal. Among them, A is preferably at least one of lithium (Li), sodium (Na) and potassium (K). By using the alkali metal salt of silicate having a siloxane bond as a skeleton forming agent, a lithium ion secondary battery with high strength, excellent heat resistance and excellent cycle life can be obtained.

[0054] Furthermore, in the above general formula (1), n ​​is preferably greater than 1.6 and less than 3.9. With n within this range, when the composite skeleton forming agent 15 is mixed with water to form a skeleton forming agent liquid, a moderate viscosity can be obtained, and when applied to a negative electrode containing silicon as a negative electrode active material 14 as described below, the skeleton forming agent 15 easily penetrates into the negative electrode material 13. Therefore, a lithium ion secondary battery with high strength, excellent heat resistance and excellent cycle life can be more reliably obtained. n is more preferably greater than 2.0 and less than 3.5.

[0055] The silicate is preferably amorphous. Amorphous silicates are composed of disordered molecular arrangements and thus do not break in a specific direction like crystals. Therefore, by using amorphous silicates as the skeleton forming agent 15, the cycle life characteristics are improved.

[0056] For example, by applying the above-mentioned skeleton forming agent liquid to the negative electrode containing silicon as the negative electrode active material 14, the skeleton forming agent 15 penetrates into the negative electrode active material 14. Therefore, it is speculated that the silicon constituting the negative electrode active material 14 is fused with the above-mentioned silicate constituting the skeleton forming agent 15, for example, the hydrolyzed silicate undergoes a dehydration reaction (condensation reaction of silanol groups) by heating, thereby forming a siloxane bond (-Si-O-Si-). That is, in the negative electrode 1 for lithium ion secondary batteries of the present embodiment, an interface layer composed of inorganic substances is formed at the interface between the negative electrode active material 14 and the skeleton forming agent 15, and the interface layer contains silicon from the siloxane bond and an alkali metal generated by the hydrolysis of the silicate, etc. In addition, it is speculated that due to the presence of this interface layer, the negative electrode active material 14 and the skeleton forming agent 15 are firmly combined, and as a result, excellent cycle life characteristics can be obtained.

[0057] In the present embodiment, the ratio of alkali metal atoms in the interface layer to all constituent atoms of the interface layer is preferably higher than the ratio of alkali metal atoms in the skeleton former 15 to all constituent atoms of the skeleton former 15. More specifically, the ratio of alkali metal atoms in the interface layer to all constituent atoms of the interface layer is preferably more than 5 times the ratio of alkali metal atoms in the skeleton former 15 to all constituent atoms of the skeleton former 15. As a result, the bond between the negative electrode active material 14 and the skeleton former 15 is more firmly established, and the shedding caused by the expansion and contraction of the negative electrode active material 14 during charge and discharge, or the generation of wrinkles or cracks between the collector foil 11 and the collector 12 is further suppressed, and the conductive path will not be broken, so the cycle life is further extended.

[0058] The thickness of the interface layer is preferably 3 to 30 nm. When the thickness of the interface layer is within this range, the negative electrode active material 14 and the skeleton forming agent 15 are more firmly bonded, and the shedding caused by the expansion and contraction of the negative electrode active material 14 during charge and discharge, or the generation of wrinkles or cracks between the collector foil and the collector 12 is further suppressed, and the conductive path will not be broken, so the cycle life is further extended.

[0059] The skeleton forming agent 15 of this embodiment may also include a surfactant. As a result, the lyophilicity of the skeleton forming agent 15 in the negative electrode material 13 is improved, so that the skeleton forming agent 15 is uniformly impregnated into the negative electrode material 13. Therefore, a uniform skeleton is formed between the negative electrode active materials 14 in the negative electrode material 13, and the cycle life characteristics are further improved.

[0060] The content (density) of the skeleton forming agent 15 relative to the negative electrode material 13 is preferably 0.1 to 5.0 mg / cm 2 When the content of the skeleton forming agent 15 relative to the negative electrode material 13 is within this range, the effect of using the skeleton forming agent 15 can be more reliably exerted.

[0061] When the total solid content of the negative electrode active material 14, the skeleton forming agent 15, the conductive auxiliary agent 16 and the binder 17 is set to 100% by mass, the content of the skeleton forming agent 15 is preferably 3.0 to 40.0% by mass. If the content of the skeleton forming agent 15 is within this range, the effect of using the above-mentioned skeleton forming agent 15 can be more reliably exerted. By making the content of the skeleton forming agent 15 in the negative electrode material 13 3.0% by mass or more, the function of the skeleton forming agent 15 can be more fully obtained. In addition, by setting the content of the skeleton forming agent 15 to 40.0% by mass or less, the reduction of energy density can be prevented. The content of the skeleton forming agent 15 is more preferably 5.0 to 30.0% by mass.

[0062] Here, in the negative electrode 1 for a non-aqueous electrolyte secondary battery of the present embodiment, the skeleton forming agent 15 is disposed at least at the interface between the negative electrode material 13 and the current collector 12. More specifically, the skeleton forming agent 15 is not only disposed at the interface between the current collector 12 and the negative electrode material 13, but is also uniformly disposed throughout the negative electrode material 13, and is dispersedly present between the negative electrode active materials 14. In contrast, in the conventional negative electrode for a non-aqueous electrolyte secondary battery, the skeleton forming agent is locally present on the surface of the negative electrode material.

[0063] Furthermore, the negative electrode 1 for lithium ion secondary battery of the present embodiment includes a conductive aid 16. As the conductive aid 16, there is no particular limitation as long as it has electronic conductivity, and metals, carbon materials, conductive polymers, conductive glass, etc. can be used. Specifically, acetylene black (AB), Ketjen black (KB), furnace black (FB), thermal black, lamp black, channel black, roller black, disk black, carbon black (CB), carbon fiber (e.g., vapor grown carbon fiber VGCF (registered trademark)), carbon nanotube (CNT), carbon nanohorn, graphite, graphene, glassy carbon, amorphous carbon, etc. can be listed, and one or more of them can be used.

[0064] When the total amount of the negative electrode active material 14, the conductive aid 16, and the binder 17 contained in the negative electrode material 13 is 100 mass %, the content of the conductive aid 16 is preferably 0 to 20.0 mass %. When the content of the conductive aid 16 is within this range, the conductivity can be improved without reducing the negative electrode capacity density, and a gap that can hold a sufficient skeleton forming agent 15 can be formed inside the negative electrode material 13. The content of the conductive aid 16 is more preferably 8.8 to 25.0 mass %.

[0065] The bulk density of the conductive additive 16 of the present embodiment is preferably 0.04 to 0.25 mg / cm 3 When the volume density of the conductive agent 16 is within this range, the skeleton forming agent 15 can be fully impregnated, thereby fully exerting the effect of the skeleton forming agent 15. The volume density of the conductive agent 16 is more preferably 0.04 to 0.15 mg / cm 3 .

[0066] Furthermore, the negative electrode 1 for lithium ion secondary battery of the present embodiment includes a binder 17. As the binder 17, for example, one of the following organic materials may be used alone, or two or more thereof may be used in combination: polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, aromatic polyamide, polypropylene, styrene-butadiene rubber (SBR), ethylene-vinyl acetate copolymer (EVA), styrene-ethylene-butylene-styrene copolymer (SEBS), carboxymethyl cellulose (CMC), xanthan gum, polyvinyl alcohol (PVA), ethylene-vinyl alcohol, polyvinyl butyral (PVB), polyethylene (PE), polypropylene (PP), polyacrylic acid, lithium polyacrylate, sodium polyacrylate, potassium polyacrylate, ammonium polyacrylate, methyl polyacrylate, ethyl polyacrylate, polypropylene Acrylic amine, polyacrylate, epoxy resin, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), nylon, vinyl chloride, silicone rubber, nitrile rubber, cyanoacrylate, urea-formaldehyde resin, melamine resin, phenolic resin, latex, polyurethane, silanized polyurethane, nitrocellulose, dextrin, polyvinyl pyrrolidone, vinyl acetate, polystyrene, allyl chloride, resorcinol resin, polyaromatic compounds, modified silicone, methacrylic resin, polybutene, butyl rubber, 2-acrylic acid, cyanoacrylate, methyl methacrylate, glycidyl methacrylate, acrylate oligomer, 2-hydroxyethyl acrylate, alginic acid, starch, sumac, sucrose, animal glue, casein, cellulose nanofibers, etc.

[0067] In addition, materials obtained by mixing the above-mentioned various organic binders with inorganic binders can also be used. Examples of inorganic binders include silicate-based, phosphate-based, sol-based, cement-based, and the like. For example, one of the following inorganic materials can be used alone, or two or more of them can be used in combination: lithium silicate, sodium silicate, potassium silicate, cesium silicate, guanidine silicate, ammonium silicate, fluorosilicate, borate, lithium aluminate, sodium aluminate, potassium aluminate, aluminosilicate, lithium aluminate, sodium aluminate, potassium aluminate, polyaluminum chloride, polyaluminum sulfate, polyaluminum sulfate silicate, aluminum sulfate, aluminum nitrate, ammonium alum, lithium alum, sodium alum, potassium alum, chrome alum, iron alum, manganese alum, ammonium nickel sulfate, diatomaceous earth, polyzirconia, polytantaloxane, mullite, white carbon, silica sol, colloidal silica, fumed silica, alumina sol, colloidal alumina, fumed alumina Alumina, zirconia sol, colloidal zirconia, fumed zirconia, magnesia sol, colloidal magnesia, fumed magnesia, calcium oxide sol, colloidal calcium oxide, fumed calcium oxide, titanium dioxide sol, colloidal titanium dioxide, fumed titanium dioxide, zeolite, silicoaluminophosphate zeolite, sepiolite, montmorillonite, kaolin, saponite, aluminum phosphate, magnesium phosphate, calcium phosphate, iron phosphate, copper phosphate, zinc phosphate, titanium phosphate, manganese phosphate, barium phosphate, tin phosphate, low melting point glass, plaster, gypsum, magnesium cement, lead oxide cement, silicate cement, blast furnace cement, fly ash cement, silica cement, phosphate cement, concrete, solid electrolyte, etc.

[0068] In addition, in the present embodiment, the negative electrode active material 14 and the skeleton forming agent 15 are firmly bonded by the above-mentioned interface layer formed by using the skeleton forming agent 15, so all of the above-mentioned binder 17 can be used. When the total amount of the negative electrode active material 14, the conductive auxiliary agent 16 and the binder 17 contained in the negative electrode material 13 is set to 100 mass%, the content of the binder 17 is preferably 0.1 to 60 mass%. By the content of the binder 17 being within this range, the ion conductivity can be improved without reducing the negative electrode capacity density, and a higher mechanical strength can be obtained, and excellent cycle life characteristics can be obtained. The content of the binder 17 is more preferably 0.5 to 30 mass%.

[0069] The thickness of the negative electrode 1 for a non-aqueous electrolyte secondary battery of the present embodiment including the above-mentioned structure is preferably 50 μm to 1000 μm. If the thickness of the negative electrode 1 for a non-aqueous electrolyte secondary battery is within this range, the endurance degradation can be suppressed compared with the past, and the energy density can be improved. The thickness of the negative electrode 1 for a non-aqueous electrolyte secondary battery is more preferably 150 μm to 800 μm.

[0070] Furthermore, in the negative electrode 1 for a non-aqueous electrolyte secondary battery of the present embodiment, the distance between the current collector 12 composed of a porous metal body and the negative electrode active material 14 is preferably 50 μm or less. If the distance between the current collector 12 composed of a porous metal body and the negative electrode active material 14 is 50 μm or less, durable degradation can be suppressed. The distance between the current collector 12 composed of a porous metal body and the negative electrode active material 14 is more preferably 30 μm or less.

[0071] [positive electrode]

[0072] Next, a positive electrode in the case of configuring a lithium ion secondary battery using the above-mentioned negative electrode will be described.

[0073] As the positive electrode active material, there is no particular limitation as long as it is a positive electrode active material commonly used in lithium ion secondary batteries. For example, positive electrode active materials such as alkali metal transition metal oxides, vanadium, sulfur, solid solution systems (lithium excess systems, sodium excess systems, potassium excess systems), carbon systems, and organic systems can be used.

[0074] Similar to the negative electrode, the positive electrode for lithium ion secondary battery of this embodiment may also contain a skeleton forming agent. As the skeleton forming agent, the same substances as those for the negative electrode can be used, and the preferred content of the skeleton forming agent is also the same as that for the negative electrode.

[0075] The positive electrode for lithium ion secondary battery of this embodiment may also contain a conductive auxiliary agent. As the conductive auxiliary agent, various conductive auxiliary agents that can be used in the negative electrode can be used. The preferred content of the conductive auxiliary agent is also the same as that of the negative electrode.

[0076] The positive electrode for lithium ion secondary battery of the present embodiment may also include a binder. As a binder, for example, one of the following organic materials can be used alone, or two or more can be used in combination: polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), hexafluoropropylene, tetrafluoroethylene, polypropylene, alginic acid, etc. In addition, it can also be a material mixed with these organic binders and inorganic binders. As inorganic binders, for example, silicate systems, phosphate systems, sol systems, cement systems, etc. can be listed.

[0077] As a current collector for the positive electrode, as long as it is a material with electronic conductivity and can be energized to the positive electrode active material maintained, it is not particularly limited. Conductive materials such as C, Ti, Cr, Ni, Cu, Mo, Ru, Rh, Ta, W, Os, Ir, Pt, Au, Al, and alloys containing two or more of these conductive materials (for example, stainless steel or Al-Fe alloy) can be used. When using materials other than the above-mentioned conductive materials, for example, a multilayer structure of a heterogeneous metal such as Al coated on iron or a heterogeneous element such as C coated on Al can be used. From the viewpoint of higher conductivity and higher stability in the electrolyte, as a current collector, preferably C, Ti, Cr, Au, Al, stainless steel, etc., further from the viewpoint of oxidation resistance and material cost, preferably C, Al, stainless steel, etc. More preferably, Al or Al alloy coated with carbon, stainless steel coated with carbon.

[0078] In addition, the shape of the current collector for the positive electrode is linear, rod-shaped, plate-shaped, foil-shaped, porous, wherein, in terms of being able to improve the packing density and the skeleton forming agent being easily impregnated into the active material layer, it can be porous. Among the porous shapes, nets, fabrics, nonwovens, embossed bodies, punched bodies, expanded bodies or foamed bodies can be cited. The same porous metal body as the negative electrode can also be used.

[0079] [Diaphragm]

[0080] In the lithium ion secondary battery of the present embodiment, as the separator, a separator commonly used in lithium ion secondary batteries can be used. For example, as the separator, a polyethylene microporous membrane, a polypropylene microporous membrane, a glass nonwoven fabric or an aramid nonwoven fabric, a polyimide microporous membrane, a polyolefin microporous membrane, etc. can be used.

[0081] [Electrolytes]

[0082] In the lithium ion secondary battery of the present embodiment, as the electrolyte, an electrolyte commonly used in lithium ion secondary batteries can be used. Examples thereof include electrolytes formed by dissolving an electrolyte in a solvent, gel electrolytes, solid electrolytes, ionic liquids, and molten salts. Here, the electrolyte refers to an electrolyte in a state where the electrolyte is dissolved in a solvent.

[0083] As the electrolyte of lithium ion secondary battery, it is necessary to contain lithium ions as the carrier for carrying the conductive function. Therefore, as its electrolyte salt, as long as it is an electrolyte salt that can be used in lithium ion secondary battery, it is not particularly limited, preferably lithium salt. As the lithium salt, at least one selected from the group consisting of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO4), bistrifluoromethanesulfonyl imide lithium (LiN(SO2CF3)2), bispentafluoroethanesulfonyl imide lithium (LiN(SO2C2F5)2), lithium bisoxalate borate (LiBC4O8), etc. can be used, or two or more can be used in combination.

[0084] The solvent for the electrolyte can be any solvent that can be used in lithium-ion secondary batteries without particular limitation. For example, at least one selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), γ-butyrolactone (GBL), methyl-γ-butyrolactone, dimethoxymethane (DMM), dimethoxyethane (DME), vinylene carbonate (VC), vinyl ethylene carbonate (EVC), fluoroethylene carbonate (FEC), and vinyl sulfite (ES) can be used, or two or more thereof can be used in combination.

[0085] The concentration of the electrolyte solution (the concentration of the salt in the solvent) is not particularly limited, but is preferably 0.1 to 3.0 mol / L, and more preferably 0.8 to 2.0 mol / L.

[0086] Ionic liquids or molten salts are classified into pyridine, alicyclic amine, aliphatic amine, etc. according to the type of cation. A variety of ionic liquids or molten salts can be synthesized by selecting the type of anion combined with the cation. As cations, there are ammonium, phosphonium ions, inorganic ions, etc. such as imidazolium salts and pyridinium salts, and as examples of anions, there are halogens such as bromide ions or trifluoromethanesulfonate, boron such as tetraphenylborate, phosphorus such as hexafluorophosphate, etc.

[0087] Ionic liquids or molten salts can be obtained, for example, by the following well-known synthesis method: a cation such as imidazolium is reacted with Br - , Cl - , BF 4- PF 6- 、(CF3SO2)2N - CF3SO 3- 、FeCl 4- If it is an ionic liquid or a molten salt, it can function as an electrolyte even without adding an electrolyte.

[0088] Solid electrolytes are classified into sulfide-based, oxide-based, hydride-based, organic polymer-based, etc. Most of them are amorphous or crystalline consisting of salts and inorganic derivatives as carriers. Since no flammable aprotic organic solvent is used like an electrolyte, it is not easy to apply gas or liquid, leak liquid, etc., and thus it can be expected to become a secondary battery with excellent safety.

[0089] [Manufacturing method]

[0090] Next, a method for manufacturing the lithium ion secondary battery of this embodiment will be described.

[0091] The manufacturing method of the negative electrode for lithium-ion secondary battery of the present embodiment includes a first step, by coating a negative electrode material including a negative electrode active material, a conductive aid and a binder on a current collector composed of a porous metal body and drying, to form a negative electrode layer precursor. For example, a nickel porous material with a thickness of 1000 μm is manufactured, and a nickel porous body wound into a roll is prepared in advance. At the same time, the negative electrode active material, the binder, the conductive aid, etc. are mixed to prepare a paste slurry as the negative electrode material. Then, the paste-like negative electrode material is filled and coated inside the nickel porous body, and a voltage adjustment treatment is performed after drying, thereby obtaining a negative electrode layer precursor.

[0092] In addition, as described above, the negative electrode layer precursor may also be maintained in a wet state without drying. In addition to the above-mentioned slurry coating, the following methods may also be cited: for example, using chemical plating or sputtering, evaporation, vapor deposition, impregnation, pressing, etc., a negative electrode material layer is formed inside the porous collector to integrate the negative electrode active material (precursor). Among them, from the perspective of the lyophilicity of the skeleton forming agent and the cost of electrode manufacturing, a slurry filling coating method or an impregnation method is preferred.

[0093] Furthermore, the manufacturing method of the negative electrode for lithium ion secondary battery of the present embodiment includes a second step of forming a negative electrode layer by impregnating the negative electrode layer precursor formed in the first step with a skeleton forming agent containing a silicate having a siloxane bond or a phosphate having a phosphate bond and drying it. For example, a skeleton forming agent liquid including a skeleton forming agent is prepared by purifying a silicate having a siloxane bond or a phosphate having a phosphate bond by a dry or wet method and adjusting it with water. At this time, a surfactant may also be mixed. As a dry method, for example, an alkali metal silicate may be manufactured by adding SiO2 to water in which an alkali metal oxide is dissolved and treating it at 150°C to 250°C in an autoclave. As a wet method, for example, a mixture composed of an alkali metal carbonate and SiO2 may be calcined at 1000°C to 2000°C and dissolved in hot water.

[0094] Next, a skeleton forming agent liquid is applied to the surface of the negative electrode layer precursor, and the negative electrode active material is coated. As a method for applying the skeleton forming agent, in addition to the method of impregnating the negative electrode precursor in a tank storing the skeleton forming agent liquid, a method of dripping and applying the skeleton forming agent on the surface of the negative electrode precursor, spraying, screen printing, curtain coating, spin coating, gravure coating, die coating, etc. can also be used. The skeleton forming agent coated on the surface of the negative electrode layer precursor penetrates into the negative electrode and enters the gaps between the negative electrode active material or the conductive additive. In addition, the skeleton forming agent is cured by drying by heat treatment. Thus, the skeleton forming agent forms the skeleton of the negative electrode active material layer.

[0095] From the viewpoint that the heat treatment time can be shortened when the temperature is high and the strength of the skeleton forming agent is improved, the heat treatment is preferably above 80°C, more preferably above 100°C, and more preferably above 110°C. In addition, the upper limit temperature of the heat treatment is not particularly limited as long as it does not cause the collector to melt, and can be raised to the melting point of copper, i.e., 1000°C. In the case of a conventional electrode, there is a situation where the binder is carbonized or the collector is softened, so it is expected that the upper limit temperature is much less than 1000°C, and in the present embodiment, by using a skeleton forming agent, the skeleton forming agent shows excellent heat resistance, and from the viewpoint that the strength of the collector is more solid, the upper limit of the temperature is 1000°C.

[0096] The heat treatment time may be maintained for 0.5 to 100 hours. The heat treatment atmosphere may be in the air, but in order to prevent oxidation of the current collector, it is preferably treated in a non-oxidizing atmosphere.

[0097] In addition, the manufacturing method of the negative electrode for lithium ion secondary battery of the present embodiment includes a third step of sandwiching the collector foil with a pair of collectors having the negative electrode layer formed in the first step and the second step. Regarding the method of sandwiching the two sides of the collector foil with a pair of collectors, a well-known method can be applied, for example, the following method can be applied: using a roller press, pressing the two sides of the collector foil while sandwiching the collectors.

[0098] Here, in the method for manufacturing a negative electrode for a lithium ion secondary battery of the present embodiment, the ratio B / A of the density B of the negative electrode layer formed in the second step relative to the density A of the negative electrode layer precursor formed in the first step is controlled to be 0.9<B / A<1.4. Specifically, by selecting the type of material, the amount of material, the processing conditions, etc., the ratio B / A (i.e., the density increase ratio) of the density B of the negative electrode layer relative to the density A of the negative electrode layer precursor is controlled within the above range. As a result, the impregnated skeleton forming agent is distributed throughout the negative electrode layer, and as a result, the skeleton forming agent is also configured at the interface between the negative electrode layer and the current collector. Therefore, by forming a skeleton using a skeleton forming agent uniformly configured throughout the negative electrode layer, a higher mechanical strength can be obtained, and the cycle life characteristics are improved.

[0099] In the method for producing a negative electrode for a lithium ion secondary battery of the present embodiment, the density A of the negative electrode layer precursor formed in the first step is set to 0.5 to 2.0 g / cm 3 As a result, the ratio B / A (i.e., density increase ratio) of the density B of the negative electrode layer to the density A of the negative electrode layer precursor can be more reliably set within the above range, thereby improving the effect of the above skeleton forming agent. The range of the density A of the negative electrode layer precursor is more preferably 0.6 to 1.5 g / cm 3 By setting the density A of the negative electrode layer precursor to 0.6 g / cm 3 The above can suppress the decrease in energy density caused by the decrease in electrode density. 3 Hereinafter, a decrease in capacity can be suppressed.

[0100] The manufacturing method of the positive electrode for lithium ion secondary battery of the present invention comprises the following steps: by coating the positive electrode material including positive electrode active material, conductive aid and binder on the collector, drying and rolling, to manufacture the positive electrode. For example, a rolled aluminum foil with a thickness of 10 μm is manufactured, and the aluminum foil wound into a roll is prepared in advance. At the same time, the positive electrode active material, binder, conductive aid, etc. are mixed to prepare a paste slurry as the positive electrode material. Then, the paste-like positive electrode material is coated on the surface of the aluminum, and after drying, a rolling step is performed to obtain the positive electrode. In addition, a foamed porous body composed of metal can also be used as the collector. It is characterized in that the collector is filled with an electrode mixture. The method of filling the electrode mixture into the collector is not particularly limited, and the following methods can be cited: for example, by using a press method, pressure is applied to fill the slurry containing the electrode mixture into the mesh structure of the collector. After the electrode mixture is filled, the filled current collector is dried and then pressed, so that the density of the electrode mixture can be increased and adjusted to a desired density.

[0101] Finally, the obtained negative electrode and positive electrode are cut into required sizes, joined via a separator, and sealed while immersed in an electrolyte, thereby obtaining a lithium-ion secondary battery. As the structure of the lithium-ion secondary battery, it can be applied to existing battery forms or structures such as laminated batteries or wound batteries.

[0102] [Effect]

[0103] According to this embodiment, the following effects are achieved.

[0104] In this embodiment, the negative electrode 1 for a non-aqueous electrolyte secondary battery includes: a collector foil 11; a pair of collectors 12, which are arranged in contact with each other on both sides of the aforementioned collector foil and are composed of a porous metal body; and a negative electrode material 13, which is arranged in the pores of the aforementioned porous metal body; and the negative electrode material 13 includes a negative electrode active material 14 composed of a silicon-based material, a skeleton former 15 containing a silicate having a siloxane bond, a conductive additive 16 and a binder 17.

[0105] First, by using a porous metal body as the current collector 12, the porous metal skeleton can be used to fix the negative electrode material 13 in the micrometer-level region, thereby suppressing the peeling and cracking of the negative electrode. In addition, by using such a current collector 12 to clamp the two sides of the collector foil 11, even if the negative electrode is peeled off, cracked, or broken due to the expansion and contraction of the negative electrode active material 14, the collector foil 11 can be used to ensure conduction (conductive path), thereby suppressing the reduction of battery performance and improving the cycle life.

[0106] Furthermore, by using the skeleton forming agent 15 as the negative electrode material 13, the negative electrode material 13 can be fixed in the nanoscale region. More specifically, by forming a third phase realized by the skeleton forming agent 15 at the interface between the collector 12 composed of a porous metal body and the negative electrode active material 14, the negative electrode active material 14 can be firmly bonded in the negative electrode material 13, thereby suppressing the shedding during expansion and contraction, thereby suppressing the durable degradation.

[0107] Therefore, by making the collector 12 into a double skeleton structure formed by filling the negative electrode material 13 containing the skeleton forming agent 15 into the foamed metal body, and using this collector 12 to clamp the two sides of the collector foil 11, even if the negative electrode active material 14 composed of a silicon-based material with a high capacity and a large expansion and contraction rate is used, even if the negative electrode is peeled off, cracked, or broken due to the expansion and contraction of the negative electrode active material 14, the collector foil 11 can be used to ensure conduction (conductive path). Therefore, even in the case of a full charge and discharge cycle with an SOC (State of Charge) of 0 to 100, the strength of the electrode mixture boundary area is improved, so the negative electrode structure can be maintained. Furthermore, it is possible to suppress the shedding and the breakage of the conductive path when the capacity is high or the unit area weight is high due to the thick film of the negative electrode, so that high cyclability can be achieved, and an overwhelmingly high energy density can be achieved.

[0108] <Second embodiment>

[0109] Furthermore, as another embodiment of the negative electrode for a non-aqueous electrolyte secondary battery of the present invention, a method in which at least one of a pair of current collectors formed by a porous metal body has an area in contact with the collector foil and not filled with negative electrode material or an area in which the filling density of the negative electrode material is lower than that of other areas (hereinafter also referred to as the second embodiment) is described in detail with reference to the accompanying drawings.

[0110] Figure 3 1 is a cross-sectional view schematically showing the structure of the negative electrode 1 for a non-aqueous electrolyte secondary battery according to the present embodiment. In the present embodiment, at least one of a pair of current collectors composed of a porous metal body has a region 18 with a high packing density of the negative electrode material, and a region 19 with no negative electrode material 13 or a low packing density of the negative electrode material 13 arranged in contact with the current collector foil 11. The region 19 with no negative electrode material 13 or a low packing density of the negative electrode material 13 is preferably arranged to be sandwiched between the region 18 with a high packing density of the negative electrode material and the current collector foil 11.

[0111] By providing the above-mentioned region on the current collector, even if the negative electrode active material 14 filled in the pair of current collectors 12 expands and contracts during charge and discharge, the breakage of the conductive path between the current collector foil 11 and the pair of current collectors 12 composed of the porous metal body can be suppressed. Furthermore, even if a breakage occurs, the conduction (conductive path) from the current collector foil side can be ensured.

[0112] In addition, the region 19 where the negative electrode material 13 is not filled or where the negative electrode material 13 is filled with a low density refers to a region (thickness) from the surface of a pair of current collectors 12 formed by a porous metal body to about 50 μm inside each current collector on the side in contact with the current collector 12. Preferably, the region 19 where the negative electrode material 13 is not filled or where the negative electrode material 13 is filled with a low density is set from the surface of the current collector foil on the side in contact with the pair of current collectors 12 formed by a porous metal body to within 50 μm inside each current collector.

[0113] In the current collector 12 composed of a porous metal body, the electrode weight per unit area of ​​the region 18 where the negative electrode material is packed at a high density is preferably 1 to 100 mg / cm 2 The electrode unit area weight of the region 18 with a high negative electrode material filling density in the current collector 12 composed of a porous metal body is within this range, so that the active material capacity can be fully expressed and the electrode can show the designed capacity. The electrode unit area weight is more preferably 5 to 60 mg / cm 2 .

[0114] In the current collector 12 composed of a porous metal body, the electrode weight per unit area of ​​the region not filled with the negative electrode material 13 or the region 19 where the negative electrode material filling density is lower than that of other regions is preferably 0 to 10 mg / cm2 . By having the electrode unit area weight of the region without negative electrode material 13 or the region 19 with a lower negative electrode material filling density than other regions in a pair of current collectors 12 formed of a porous metal body within this range, the active material capacity can be fully demonstrated in the negative electrode for a non-aqueous electrolyte secondary battery, and the designed capacity can be displayed as an electrode. Even if the negative electrode is peeled off, cracked, or broken due to expansion and contraction of the negative electrode active material 14, the collector foil 11 can more reliably ensure conduction (conductive path). The electrode unit area weight of the region without negative electrode material 13 or the region 19 with a lower negative electrode material filling density than other regions is more preferably 0 to 5 mg / cm 2 .

[0115] In addition, "areas with higher filling density of negative electrode materials" and "areas with lower filling density of negative electrode materials than other areas" refer, for example, to setting differences in the concentration of the negative electrode material slurry and filling them into the same current collector, or filling slurries of negative electrode materials with different concentrations into a plurality of different current collectors and then crimping them to achieve integration, thereby making the area of ​​negative electrode material with a higher unit area weight and the area of ​​negative electrode material with a lower unit area weight exist integrally inside the current collector composed of a porous metal body.

[0116] [Manufacturing method]

[0117] Next, a method for manufacturing the lithium ion secondary battery of this embodiment will be described.

[0118] There are many methods for manufacturing the lithium-ion secondary battery of this embodiment. For example, as a manufacturing method, there is method A: a certain surface of a current collector composed of a porous metal body and the other surface on the opposite side are filled with negative electrode materials of different concentrations, and then, after impregnating the negative electrode layer with a skeleton forming agent, the current collector foil is clamped by the pair of current collectors, thereby obtaining the negative electrode for the non-aqueous electrolyte secondary battery of this embodiment. The following is a detailed description.

[0119] [Method A for producing a negative electrode for a non-aqueous electrolyte secondary battery according to the second embodiment]

[0120] The manufacturing method A of the negative electrode for lithium-ion secondary battery of the present embodiment includes, for example, a first step of coating a negative electrode material including a negative electrode active material, a conductive aid and a binder on a current collector composed of a porous metal body in such a manner that the concentration of the negative electrode material is changed according to the surface of the current collector and drying the negative electrode material, thereby forming a negative electrode layer precursor having areas with a higher filling density of the negative electrode material and areas with a smaller filling density of the negative electrode material than other areas.

[0121] For example, to manufacture a nickel porous material with a thickness of 1000 μm, a nickel porous body wound into a roll is prepared in advance, and at the same time, a negative electrode active material, a binder, a conductive aid, etc. are mixed to prepare a paste-like slurry as a negative electrode material. Next, the paste-like negative electrode material is filled and coated only from one side of the collector and in a manner that does not fill all the pores of the collector. Further, from the side opposite to the side filled with the negative electrode material, a slurry of the negative electrode material obtained by diluting the negative electrode material used when filling and coating is applied. After that, drying and voltage regulation treatment are performed, thereby, a negative electrode layer precursor having a region with a higher filling density of the negative electrode material and a region with a smaller filling density of the negative electrode material than other regions can be obtained in the collector. At this time, when it is not filled from the other side, such as the opposite side, a negative electrode layer precursor having a region with a higher filling density of the negative electrode material and a region without filling the negative electrode material can be manufactured.

[0122] In the manufacturing method A, the second step and the subsequent steps can manufacture the negative electrode for the non-aqueous electrolyte secondary battery of the present embodiment by applying the second step and the subsequent manufacturing steps of the first embodiment. In addition, in the negative electrode for the non-aqueous electrolyte secondary battery of the present embodiment, at least one of the pair of collectors sandwiching the collector foil can use the collector manufactured by the manufacturing method of the present embodiment described above.

[0123] In this embodiment, the negative electrode for a nonaqueous electrolyte secondary battery of this embodiment and the positive electrode used in the first embodiment can be used to manufacture a nonaqueous electrolyte secondary battery including the negative electrode for a nonaqueous electrolyte secondary battery of this embodiment.

[0124] [Method B for producing negative electrode for non-aqueous electrolyte secondary battery according to the second embodiment]

[0125] In addition, as another method for manufacturing the negative electrode for lithium ion secondary battery of the present embodiment, there is a manufacturing method B: for example, a plurality of current collectors composed of porous metal bodies are prepared, and each current collector is filled with a negative electrode material of different concentrations to form a negative electrode material precursor with different filling densities of the negative electrode material, which is impregnated with a skeleton forming agent to form a negative electrode layer, and then the current collector foil is sandwiched by the plurality of negative electrode layers, thereby obtaining the negative electrode for non-aqueous electrolyte secondary battery of the present embodiment. The following is a detailed description.

[0126] In manufacturing method B, a first step is included, in which a plurality of current collectors composed of porous metal bodies are prepared, and each current collector is filled with negative electrode materials of different concentrations and dried, thereby forming a negative electrode layer precursor. By means of the first step, a negative electrode layer precursor having an area with a higher filling density of negative electrode materials and a negative electrode layer precursor having an area with a smaller filling density of negative electrode materials than other areas can be manufactured respectively. Regarding the coating method of the negative electrode material, in addition to preparing slurries of negative electrode materials with higher and lower concentrations and a plurality of current collector rolls, the method described in the first embodiment can also be preferably used. Furthermore, when the negative electrode material is not coated on the current collector, a negative electrode layer having an area not filled with the negative electrode material can be manufactured.

[0127] For a negative electrode layer precursor having an area not filled with negative electrode material or an area having a negative electrode material filling density lower than other areas, it is preferable to use a current collector composed of the same porous metal body as that of the negative electrode layer precursor having an area having a higher negative electrode material filling density.

[0128] A manufacturing method B for a negative electrode for a lithium ion secondary battery of the present embodiment, then applies the second step of the first embodiment to the negative electrode layer precursor obtained by the first step, and after obtaining the negative electrode layer, includes a third step, forming a negative electrode layer corresponding to a region with a larger packing density of the negative electrode material, a collector having a region without filling the negative electrode material, or a negative electrode layer having a region with a smaller packing density of the negative electrode material than other regions, with a collector foil. At this time, the negative electrode layer having a region without filling the negative electrode material obtained by not coating the negative electrode material is not impregnated with a skeleton forming agent. In addition, the negative electrode layer having a region without filling the negative electrode material obtained by not coating the negative electrode material can also be subjected to voltage regulation and thickness adjustment using a roller press or the like before preparing the negative electrode for a secondary battery with a non-aqueous electrolyte.

[0129] For example, the negative electrode layer corresponding to the area with a higher filling density of the negative electrode material is arranged on the outside, the negative electrode layer corresponding to the area not filled with the negative electrode material in the collector or the negative electrode layer corresponding to the area with a filling density of the negative electrode material smaller than other areas is arranged on the inside, and the collector foil is arranged in the center, and they are made into a sandwich and pressed using a roller press, etc., thereby obtaining the negative electrode for the non-aqueous electrolyte secondary battery of this embodiment.

[0130] Furthermore, in this embodiment, the nonaqueous electrolyte secondary battery including the negative electrode for nonaqueous electrolyte secondary battery of this embodiment can be manufactured by using the negative electrode for nonaqueous electrolyte secondary battery of this embodiment and the positive electrode produced in the first embodiment.

[0131] Regarding the negative electrode for a non-aqueous electrolyte secondary battery of the present embodiment and the method for manufacturing a non-aqueous electrolyte secondary battery including the negative electrode for a non-aqueous electrolyte secondary battery, as a method for preparing a negative electrode material and a method for coating a collector composed of a porous metal body, the manufacturing method described in the first embodiment can be preferably used, on the premise that attention is paid to setting an area with a higher filling density of the negative electrode material, and an area that is not filled with the negative electrode material and is arranged in contact with the collector foil, or an area where the filling density of the negative electrode material is lower than that of other areas.

[0132] Furthermore, for parts not described in detail in the second embodiment, the configuration and method of the first embodiment can be preferably used as long as they do not hinder the configuration of the second embodiment.

[0133] Here, in the method for manufacturing a negative electrode for a lithium ion secondary battery of the present embodiment, the ratio B / A of the density B of the entire negative electrode layer formed in the second step relative to the density A of the entire negative electrode layer precursor formed in the first step is controlled to be 0.9<B / A<1.4. Specifically, by selecting the type of material, the amount of material, the processing conditions, etc., the ratio B / A (i.e., the density increase ratio) of the density B of the negative electrode layer relative to the density A of the negative electrode layer precursor is controlled within the above range. As a result, the impregnated skeleton forming agent is distributed throughout the negative electrode layer, and as a result, the skeleton forming agent is also configured at the interface with the collector in the negative electrode layer. Therefore, by forming a skeleton using a skeleton forming agent uniformly configured throughout the negative electrode layer, a higher mechanical strength can be obtained, and the cycle life characteristics are improved.

[0134] In the method for producing a negative electrode for a lithium ion secondary battery of the present embodiment, the density A of the entire negative electrode layer formed in the second step is set to 0.5 to 2.0 g / cm 3 As a result, the ratio B / A (i.e., density increase ratio) of the overall density B of the negative electrode layer to the density A of the negative electrode layer precursor can be more reliably set within the above range, thereby improving the effect of the above skeleton forming agent. The overall density A of the negative electrode layer precursor is more preferably in the range of 0.6 to 1.5 g / cm 3 By setting the overall density A of the negative electrode layer precursor to 0.6 g / cm 3 The above can suppress the decrease in energy density caused by the decrease in electrode density. 3 Hereinafter, a decrease in capacity can be suppressed.

[0135] [Effect]

[0136] According to this embodiment, the following effects are achieved.

[0137] In this embodiment, at least one of a pair of current collectors formed of a porous metal body has a region 18 with a higher filling density of the negative electrode material and a region not filled with the negative electrode material 13 or a region 19 with a lower filling density of the negative electrode material 13 and arranged in contact with the current collector foil 11.

[0138] In the present embodiment, by providing a region 18 with a relatively high filling density of the negative electrode material and a region 19 which is not filled with the negative electrode material 13 and is arranged in contact with the collector foil 11 or has a filling density of the negative electrode material lower than that of other regions in at least one of a pair of collectors formed by a porous metal body, even if the negative electrode is peeled off, cracked, or broken, the collector foil 11 can be used to more reliably ensure conduction (conductive path), thereby further suppressing performance degradation and further improving cycle life.

[0139] Therefore, by using a pair of collectors 12 as described above to clamp the two sides of the collector foil 11, even if the negative electrode is peeled, cracked, or broken, the collector foil 11 can be used to more fully ensure conduction (conductive path), so that even in the case of a full charge and discharge cycle with an SOC of 0 to 100, the strength of the electrode mixture boundary area is further improved, so the negative electrode structure can be maintained. Furthermore, the shedding and the breakage of the conductive path caused by the thickening of the negative electrode at high capacity or high unit area weight can be further suppressed, and higher cyclability can be achieved, and more overwhelmingly high energy density can be achieved.

[0140] In addition, the present invention is not limited to the above-mentioned embodiments, and deformation and improvement within the scope of the purpose of the present invention are included in the present invention. For example, a non-aqueous electrolyte secondary battery is a secondary battery (power storage device) in which a non-aqueous electrolyte such as an organic solvent is used as an electrolyte, including not only a lithium ion secondary battery, but also a sodium ion secondary battery or a potassium ion secondary battery, a magnesium ion secondary battery, a calcium ion secondary battery, etc. In addition, a lithium ion secondary battery refers to a battery as follows: a secondary battery with a non-aqueous electrolyte that is not mainly composed of water, and lithium ions are contained in the carrier that bears the conductive function. For example, lithium ion secondary batteries, metal lithium batteries, lithium polymer batteries, all-solid-state lithium batteries, air lithium ion batteries, etc. meet the conditions. And other secondary batteries are also the same. Here, a non-aqueous electrolyte that is not mainly composed of water refers to an electrolyte in which the main component is not water. That is, it is a well-known electrolyte used in a non-aqueous electrolyte secondary battery. Although the electrolyte can function as a secondary battery even if it contains a small amount of water, it will have an adverse effect on the cycle characteristics or storage characteristics and input-output characteristics of the secondary battery. Therefore, it is more desirable to have an electrolyte that does not contain water as much as possible. In fact, the water in the electrolyte is preferably less than 5000ppm.

[0141] [Example]

[0142] Next, examples of the present invention will be described, but the present invention is not limited to these examples.

[0143] <Example 1>

[0144] [Production of negative electrode]

[0145] A slurry containing silicon (particle size 1-10 μm) as a negative electrode active material, acetylene black as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder was prepared. 2 The nickel was filled into "Nickel Celmet" (registered trademark) manufactured by Sumitomo Electric Industries, Ltd., which is a current collector. Thereafter, drying and pressure adjustment treatment were performed to obtain a negative electrode layer precursor.

[0146] At the same time, a 10 mass % aqueous solution of Na2O·3SiO2 is prepared as a skeleton forming agent liquid including a skeleton forming agent and water. The negative electrode layer precursor obtained above is immersed in the prepared skeleton forming agent liquid. And after the immersion, the negative electrode precursor is heated and dried at 160°C to obtain a single-layer negative electrode with a negative electrode layer formed thereon.

[0147] Next, the negative electrode was used to sandwich a current collector foil, which was a copper foil, at the center, and these were sandwiched and pressed using a roll press at a pressure of 1 ton to obtain the negative electrode of the first embodiment.

[0148] [Production of positive electrode]

[0149] Preparation of LiNi 0.5 Co 0.2 Mn 0.3 O2 (particle size 5-15 μm) is used as the positive electrode active material. 94% by mass of the positive electrode active material, 4% by mass of carbon black as a conductive aid, and 2% by mass of polyvinylidene fluoride (PVdF) as a binder are mixed, and the obtained mixture is dispersed in an appropriate amount of N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode mixture slurry. Prepare a slurry with a thickness of 1.0 mm, a porosity of 95%, a number of grooves of 46-50 / inch, a pore diameter of 0.5 mm, and a specific surface area of ​​5000 m 2 / m 3 The foamed aluminum was used as the current collector. The coating amount was 45 mg / cm 2 The prepared positive electrode mixture slurry was applied to the current collector in a manner of . Drying was performed at 120° C. for 12 hours in a vacuum, and then roll pressing was performed at a pressure of 15 tons, thereby preparing a positive electrode for a lithium ion secondary battery in which the pores of the foamed aluminum were filled with the electrode mixture.

[0150] [Manufacturing of lithium-ion secondary batteries]

[0151] A microporous film having a thickness of 15 μm and being a three-layer laminate of polypropylene / polyethylene / polypropylene was prepared as a separator and punched into a size of 100 mm in length and 90 mm in width. The positive electrode for lithium ion secondary battery and the negative electrode for lithium ion secondary battery obtained above were stacked in the order of positive electrode / separator / negative electrode / separator / positive electrode / negative electrode to prepare an electrode laminate.

[0152] After that, the tab leads are joined to the current collecting areas of each electrode by ultrasonic welding. The electrode laminate to which the tab leads are joined by welding is inserted into a product obtained by heat-sealing and processing the aluminum laminate for secondary batteries into a bag shape to produce a laminated battery. A solution of 1.2 moles of LiPF6 dissolved in a solvent of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 3:4:3 is prepared as an electrolyte and injected into the above-mentioned laminated battery to produce a lithium-ion secondary battery.

[0153] <Example 2>

[0154] [Production of negative electrode]

[0155] A slurry containing silicon (particle size 1-10 μm) as a negative electrode active material, acetylene black as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder was prepared. 2 The nickel was filled into "Nickel Celmet" (registered trademark) manufactured by Sumitomo Electric Industries, Ltd., which is a current collector. Thereafter, drying and pressure adjustment treatment were performed to obtain a negative electrode layer precursor.

[0156] At the same time, a 10 mass % aqueous solution of Na2O·3SiO2 is prepared as a skeleton forming agent liquid including a skeleton forming agent and water. The negative electrode layer precursor obtained above is immersed in the prepared skeleton forming agent liquid. And after the immersion, the negative electrode precursor is heated and dried at 160°C to obtain a single-layer negative electrode with a negative electrode layer formed thereon.

[0157] Next, a nickel foam metal having a thickness of 1000 μm and a void content of 97% was pressurized at a pressure of 15 tons using a roll press to a thickness of 50 μm.

[0158] Next, a current collector foil of copper foil is placed in the center, a pressure-adjusted foam metal is placed inside, and a negative electrode is placed outside, and they are sandwiched and pressed at a pressure of 1 ton using a roller press to obtain a negative electrode of the second embodiment.

[0159] [Production of positive electrode]

[0160] The production was carried out in the same manner as in Example 1.

[0161] [Manufacturing of lithium-ion secondary batteries]

[0162] The production was carried out in the same manner as in Example 1.

[0163] <Example 3>

[0164] [Production of negative electrode]

[0165] A slurry containing silicon (particle size 1-10 μm) as a negative electrode active material, acetylene black as a conductive aid, and polyvinylidene fluoride (PVdF) as a binder was prepared. A plunger-type die coater was used to coat the slurry at a coating amount of 4 mg / cm 2 The prepared mixture slurry was applied from one side onto "Nickel Celmet" (registered trademark) manufactured by Sumitomo Electric Industries, Ltd., which served as a current collector.

[0166] Next, the prepared slurry was diluted with N-methyl-2-pyrrolidone (NMP). A plunger-type die coater was used to coat the slurry at a total amount of 5 mg / cm 2 The diluted slurry is filled into the collector from the side opposite to the coated side in a manner. Thereafter, drying and pressure adjustment treatment are performed to obtain a negative electrode layer precursor.

[0167] Thereafter, the production was performed in the same manner as in Example 1 to obtain the negative electrode of the third embodiment.

[0168] [Production of positive electrode]

[0169] The production was carried out in the same manner as in Example 1.

[0170] [Manufacturing of lithium-ion secondary batteries]

[0171] The production was carried out in the same manner as in Example 1.

[0172] <Comparative Example 1>

[0173] [Production of negative electrode]

[0174] A slurry containing silicon (particle size 1 to 10 μm) as a negative electrode active material, acetylene black as a conductive aid, and polyvinylidene fluoride (PVdF) as a binder was prepared. 2 The prepared slurry was filled into "Nickel Celmet" (registered trademark) manufactured by Sumitomo Electric Industries, Ltd. as a current collector in a manner of . Thereafter, drying and voltage adjustment treatment were performed to obtain a negative electrode layer precursor.

[0175] At the same time, a 10 mass % aqueous solution of Na2O·3SiO2 is prepared as a skeleton forming agent liquid including a skeleton forming agent and water. The negative electrode layer precursor obtained above is immersed in the prepared skeleton forming agent liquid. And after the immersion, the negative electrode precursor is heated and dried at 160°C to obtain a single-layer negative electrode with a negative electrode layer formed thereon.

[0176] [Production of positive electrode]

[0177] The production was carried out in the same manner as in Example 1.

[0178] [Manufacturing of lithium-ion secondary batteries]

[0179] The production was carried out in the same manner as in Example 1.

[0180] [Durability test]

[0181] A cycle life test was conducted on each of the examples and comparative examples. The cycle life test was conducted at a test environment temperature of 25° C., a current density of 0.2 C-rate, and a cutoff potential of 2.5 to 4.2 V.

[0182] Figure 4 It is a graph showing the relationship between the number of cycles and the discharge capacity of the embodiments and comparative examples. It was confirmed that according to the present embodiments 1 to 3, the following negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery including the negative electrode for a non-aqueous electrolyte secondary battery can be obtained: even if the number of cycles increases, the capacity retention rate can be maintained, so there is cycle durability, and durable degradation can be suppressed, and the energy density can be increased.

[0183] Reference numerals

[0184] 1 Negative electrode for non-aqueous electrolyte secondary battery

[0185] 11 Collector foil

[0186] 12 Current Collector

[0187] 13. Anode Materials

[0188] 14 Negative electrode active material

[0189] 15. Scaffolding agent

[0190] 16 Conductive additive

[0191] 17 Adhesive

[0192] 18 Areas with high packing density of negative electrode materials

[0193] 19 Areas that are not filled with negative electrode material or areas where the filling density of negative electrode material is lower than other areas

Claims

1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising: Collector foil; A pair of current collectors, arranged on both sides of the current collector foil in contact with each other, and composed of a porous metal body; and, A negative electrode material is disposed in the pores of the porous metal body; Furthermore, the negative electrode material comprises: a negative electrode active material composed of a silicon-based material, a skeleton forming agent containing a silicate having a siloxane bond, a conductive auxiliary agent, and a binder. At least one of the pair of current collectors has a region that is in contact with the current collector foil and is not filled with the negative electrode material, or a region in which the amount of the negative electrode material filled in each pore is smaller than that in other regions.

2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The thickness of the region not filled with the negative electrode material or the region in which the amount of the negative electrode material filled per pore is smaller than that of other regions is 50 μm or less.

3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The aforementioned skeleton forming agent includes a silicate represented by the following general formula (1): A2O·nSiO2 formula (1) In the above general formula (1), A represents an alkali metal.

4. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The aforementioned porous metal body is a foamed metal body. 5 . A non-aqueous electrolyte secondary battery comprising the negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 .

Citation Information

Patent Citations

  • Control method of idle speed

    JP1986049147A

  • Resin composition

    JP1988069818A

  • Skeleton-forming agent and negative electrode using same

    CN108475787A

  • Non-aqueous electrolytic secondary battery and its manufacture

    JP1997265976A

  • Nonaqueous electrolyte secondary battery

    US20040170895A1