A hard carbon negative electrode material and its preparation method and application

By optimizing the preparation process of phenolic resin-based hard carbon anode material and adjusting the internal pore structure, the problem of low efficiency of hard carbon material is solved, efficient electrochemical performance of lithium-ion and sodium-ion batteries is achieved, and the reversible capacity of the material is improved. Battery performance.

CN114824257BActive Publication Date: 2024-12-03湖南镕锂新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210444652.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-26
Publication Date
2024-12-03
Estimated Expiration
2042-04-26

AI Technical Summary

Technical Problem

The existing hard carbon anode materials have low Coulomb efficiency and insufficient reversible capacity, making it difficult to meet the fast charging and discharging needs of lithium-ion and sodium-ion batteries.

Method used

By adjusting the preheating, carbonization, cooling and grading process of phenolic resin materials, the internal pore structure of the hard carbon negative electrode material is optimized, the micropore volume with a pore size of 0.35-2nm is controlled, the specific surface area and particle distribution of the material are improved, thereby improving the first time Kulun Efficiency and reversible capacity.

Benefits of technology

The first coulomb efficiency of lithium-ion batteries was achieved ≥94% and the first coulomb efficiency of sodium-ion batteries was ≥91%, significantly improving the electrochemical performance and cycle life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824257B_ABST
    Figure CN114824257B_ABST
Patent Text Reader

Abstract

The present invention discloses a hard carbon negative electrode material and a preparation method and application thereof. The D50 of the hard carbon negative electrode material provided by the present invention is 8-10 μm; the specific surface area of ​​the hard carbon negative electrode material is not more than 1.3 m 2 / g; there are pores in the hard carbon negative electrode material; the pores include micropores with a pore size of 0.35-2nm; the volume of micropores accounts for ≥90% of the volume of the pores. The hard carbon material prepared by the present invention is used as a negative electrode material for lithium ion batteries by adjusting the internal pore structure of the hard carbon material. The first discharge capacity of the material is higher than 420mAh / g, and the first coulomb efficiency is not less than 94%; as a negative electrode material for sodium ion batteries, the first discharge capacity of the material is higher than 380mAh / g, and the first coulomb efficiency is not less than 91%; after 100 cycles, the capacity retention rate of lithium ion batteries and sodium ion batteries is not less than 97%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary battery negative electrode materials, and in particular to a hard carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] It is predicted that the installed capacity of power batteries will reach 1161GWh in 2025, an increase of 735% over 2020. As a key material in the battery industry, negative electrode materials cover consumer batteries, power batteries, energy storage batteries, and energy storage power stations. At present, the negative electrode materials of lithium-ion batteries are mainly artificial graphite and natural graphite. The interlayer spacing of graphite negative electrodes (about 0.335nm) is small, which cannot provide a sufficiently spacious embedding channel for lithium ions. Moreover, the diffusion mode is two-dimensional interlayer diffusion, and it is difficult to improve the rate performance and achieve fast charging and discharging. The graphite negative electrode materials sold on the market achieve fast charging by reducing the particle size of graphite particles and shortening the lithium insertion path. This method cannot fundamentally solve the problem of fast charging. Compared with graphite, hard carbon has a larger interlayer spacing (0.37-0.42nm), which provides a sufficiently spacious channel for lithium ion embedding, and can also reduce the energy barrier for lithium ion crossing, thus truly realizing fast charging of lithium-ion batteries. Sodium-ion batteries and lithium-ion batteries have the same principle, similar process, and compatible equipment. They have low cost, good rate performance, long life, and high safety. In the future, sodium-ion batteries and lithium-ion batteries will complement each other and reduce the power battery industry's dependence on overseas lithium resources. The radius of sodium ions (0.102nm) is much larger than the radius of lithium ions (0.076nm). The use of graphite materials as the negative electrode of sodium-ion batteries will cause serious volume expansion, material deformation, and a significant reduction in cycle life. Hard carbon materials with larger interlayer spacing can fully meet the requirements of sodium ion embedding and smooth passage. Therefore, whether it is for lithium-ion batteries or sodium-ion batteries, hard carbon negative electrode materials are the most promising negative electrode materials. However, the first coulomb efficiency of such materials is generally low.

[0003] In existing research, a precursor is obtained by mixing a phenolic resin solution with sulfonated polystyrene microspheres and aminosilane, and then mixed with a lithium salt and subjected to chemical vapor deposition to obtain a spherical hard carbon material; there are also studies that ultrasonically disperse TiO2, lithium salt and lithium metal powder in solvent one, dissolve allyl phenolic resin in solvent two, slowly pour solvent one into solvent two, stir evenly, heat and cure at high temperature to obtain a hard carbon negative electrode material. Although the above-mentioned pre-lithiation is an effective means to improve the first coulomb efficiency of negative electrode materials, considering the equipment cost, plant renovation cost and time cost of lithium battery manufacturing, etc., the application of pre-lithiation to improve the first coulomb efficiency of hard carbon materials is relatively rare.

[0004] Therefore, it is currently urgent to develop a hard carbon negative electrode material and its preparation method and application to solve the low coulombic efficiency and low reversible capacity in the prior art. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. The present invention provides a high reversible capacity phenolic resin-based hard carbon negative electrode material and a simple and easy preparation method thereof by changing the internal pore structure of hard carbon to improve the first coulombic efficiency. The present invention is achieved by the following scheme.

[0006] According to one aspect of the present invention, a hard carbon negative electrode material is provided, wherein the D50 of the hard carbon negative electrode material is 8-10 μm;

[0007] The specific surface area of ​​the hard carbon negative electrode material is not greater than 1.3 m 2 / g;

[0008] The hard carbon negative electrode material has pores;

[0009] The pores include micropores with a pore size of 0.35-2 nm;

[0010] The pore volume of the micropores accounts for ≥90% of the pore volume of the pores.

[0011] A hard carbon negative electrode material according to the present invention has at least the following beneficial effects:

[0012] The hard carbon negative electrode material of the present invention, as a negative electrode material for lithium ion batteries, has a reversible capacity higher than 420 mAh / g and a first coulombic efficiency ≥ 94%; as a negative electrode material for sodium ion batteries, has a reversible capacity higher than 380 mAh / g and a first efficiency not lower than 91%.

[0013] In some preferred embodiments of the present invention, the pores include micropores with a pore size of 0.35-2 nm.

[0014] In some preferred embodiments of the present invention, the micropores with a pore diameter of 0.35-2 nm account for ≥90% of the pore volume.

[0015] In some preferred embodiments of the present invention, the distribution of the hard carbon negative electrode material is controlled so that D10 is between 3-5 μm, D50 is between 8-10 μm, D90 is between 15-20 μm, and Dmax is ≤27 μm.

[0016] In some embodiments of the present invention, the raw material for preparing the hard carbon material includes phenolic resin.

[0017] In some embodiments of the present invention, the tap density of the hard carbon negative electrode material is ≥ 0.90 g / cm 3 .

[0018] The second aspect of the present invention provides a method for preparing the hard carbon negative electrode material, comprising the following steps:

[0019] S1: Pretreatment: preheating the phenolic resin,

[0020] S2: Carbonization: Carbonize the preheated phenolic resin.

[0021] S3: Cooling: Cool the carbonized phenolic resin to room temperature.

[0022] S4: Coarse crushing: Process the cooled material into particles with a size of ≤2mm.

[0023] S5: Fine crushing and classification: The coarsely crushed materials are finely crushed and classified, and the particle distribution is controlled at D10 between 3-5μm, D50 between 8-10μm, D90 between 15-20μm, and Dmax ≤ 27μm.

[0024] The method for preparing a hard carbon negative electrode material according to the present invention has at least the following beneficial effects:

[0025] 1. The phenolic resin material will produce more pores during the heat treatment process, and these pores directly affect the lithium insertion capacity and the first coulombic efficiency of the hard carbon negative electrode material. The present invention optimizes the internal pore structure of the material by adjusting the preheating, carbonization, cooling, coarse and fine crushing and classification of the phenolic resin material.

[0026] 2. The present invention not only reduces equipment costs, plant costs, labor costs, etc. by reasonably controlling the carbonization heating rate, but also has low energy consumption and short time, greatly improving production efficiency.

[0027] 3. In the implementation process of the present invention, no acid, alkali, heavy metals and their compounds and organic solvents are used, and no liquid phase system is included. Therefore, the process has the advantages of being clean, short process, easy to industrialize and low cost.

[0028] 4. The preheating step of the present invention increases the oxygen-containing functional groups on the surface of the hard carbon negative electrode material, thereby increasing the adsorption sites of lithium ions and improving the capacity of the hard carbon negative electrode material.

[0029] In some embodiments of the present invention, the step S1 further includes preparing phenolic resin.

[0030] Phenolic resin is a solid material with a particle size of ≤100μm, a residual carbon content of ≥55%, and only three elements of carbon, hydrogen and oxygen in the polymer chain.

[0031] In some embodiments of the present invention, the preheating temperature in step S1 is 150-270°C.

[0032] In some embodiments of the present invention, the preheating rate in step S1 is 1-4° C. / min.

[0033] In some embodiments of the present invention, after the preheating temperature in step S1 is reached, the temperature is maintained for 1-3 hours.

[0034] In some embodiments of the present invention, in step S2, the carbonization temperature is 1100-1400°C.

[0035] In some embodiments of the present invention, in step S2, the carbonization time is 1-3 hours.

[0036] In some embodiments of the present invention, in step S2, during the carbonization heating, the heating rate is controlled at 1-5°C / min.

[0037] In some embodiments of the present invention, in step S2, the carbonization is performed under a nitrogen or argon atmosphere.

[0038] In some preferred embodiments of the present invention, in step S2, during the carbonization heating, the heating rate in the first 3 / 4 heating stage is controlled at 1-5°C / min; and the heating rate in the last 1 / 4 heating stage is controlled at 1-2°C / min.

[0039] In the carbonization stage, the nitrogen or argon gas flow rate is kept constant, and the phenolic resin will be carbonized step by step under the control of the heating rate. According to 1 kg of the phenolic resin raw material, under the condition of the heating rate of 1-5°C, the temperature is increased to 1300°C, and the gas discharge rates are 3.98SLM, 7.97SLM, 10.96SLM, 14.94SLM and 16.93SLM respectively. As the heating rate increases, the time required to heat up to the preset temperature becomes shorter, the gas discharge rate becomes faster and faster, and the carbonization process of the phenolic resin becomes more and more intense. The present invention controls the heating temperature in the carbonization stage to make the surface dense, generate "embedded fullerene" material, reduce the loss of lithium ions on the surface of the material, and increase the first coulomb efficiency.

[0040] In some embodiments of the present invention, in step S3, the cooling rate is 5-10°C / min.

[0041] If the cooling speed is too slow, it will lead to a higher proportion of mesopores (mesopores, i.e. medium pores, refer to pores of 2-50nm) and macropores, affecting the first coulombic efficiency; if the speed is too fast, the gas in the pores will be difficult to remove in time. During the preparation of button cells and full batteries, they are seriously affected by oxygen, hydrogen and moisture. Therefore, the gas in the pores will seriously affect the electrical properties of the material, especially the first coulombic efficiency.

[0042] In some embodiments of the present invention, in step S5, the method of fine crushing and grading is to use a mechanical mill or a jet mill and a classifier to crush and grade the material after coarse crushing in step S4, and obtain 1# coarse particle material for further return, 3# ultrafine powder is treated as waste powder, and 2# material is qualified hard carbon negative electrode material.

[0043] In some preferred embodiments of the present invention, the preheating temperature in step S1 is 205-215°C.

[0044] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, the capacity retention rate of the sodium battery after 100 cycles is 97.1%.

[0045] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, the capacity retention rate of the lithium battery after 100 cycles is 97.3%.

[0046] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, in the first charge specific capacity, the specific capacity of the lithium battery is 437 mAh / g.

[0047] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, in the first charge specific capacity, the specific capacity of sodium electricity is 419 mAh / g.

[0048] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, in the first discharge specific capacity, the specific capacity of sodium electricity is 387 mAh / g.

[0049] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, in the first discharge specific capacity, the specific capacity of the lithium battery is 404 mAh / g.

[0050] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, the first coulombic efficiency of the lithium battery is 95.2%.

[0051] In some preferred embodiments of the present invention, when the preheating temperature is 205-215° C., in the charge and discharge performance test of the hard carbon material, the first coulombic efficiency of sodium battery is 92.3%.

[0052] The third aspect of the present invention proposes the use of the hard carbon negative electrode material in a secondary battery.

[0053] In some embodiments of the present invention, the secondary battery includes one of a lithium ion battery and a sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0055] Figure 1 is the micropore volume of Examples 1 to 3 and Comparative Example 1.

[0056] Figure 2 This is an electron microscope image of the negative electrode material of Example 1.

[0057] Figure 3 This is a surface electron microscope image of the negative electrode material of Example 1.

[0058] Figure 4 This is an electron microscope image of the negative electrode material of Comparative Example 1.

[0059] Figure 5 This is the surface electron microscope image of the negative electrode material prepared in Comparative Example 1. DETAILED DESCRIPTION

[0060] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0061] Embodiment 1:

[0062] This embodiment provides a high reversible capacity phenolic resin-based hard carbon negative electrode material and a preparation method thereof. The specific steps are as follows: the micropore volume of the hard carbon negative electrode material is as follows: Figure 1 As shown, the electron microscope image of the negative electrode material is as follows Figure 2 As shown, the surface electron microscope image of the negative electrode material is as follows Figure 3 shown.

[0063] A1. Material preparation: Prepare solid phenolic resin 2123#, white powder, with particle size ≤75μm, residual carbon content 55%, polymer chain containing only three elements of carbon, hydrogen and oxygen, and starting pyrolysis temperature of 210℃;

[0064] A2. Pretreatment: Preheat in a high-temperature vacuum atmosphere furnace at a heating rate of 2°C / min to 210°C and keep warm for 1h.

[0065] A3. Carbonization: nitrogen was introduced into the high temperature vacuum atmosphere furnace, and the temperature was continued to rise at a rate of 3°C / min for 223min. Then the rate of heating was reduced to 1°C / min for 221min, the temperature was raised to 1100°C, and the holding time was 1h.

[0066] A4. Cooling: Cooling rate 5℃ / min, cooling to 25℃.

[0067] A5. Coarse crushing: After cooling, the material is crushed to ≤2mm by a ceramic double-roll crusher.

[0068] A6. Fine crushing and classification: The material after crushing in step A5 is finely crushed and classified by a jet mill and a classifier. The hard carbon negative electrode material has D10=3μm, D50=8μm, D90=16μm, and Dmax=27μm.

[0069] Embodiment 2:

[0070] This embodiment provides a high reversible capacity phenolic resin-based hard carbon negative electrode material and a preparation method thereof. The specific steps are as follows: the micropore volume of the hard carbon negative electrode material is as follows: Figure 1 As shown:

[0071] A1. Preparation: solid phenolic resin 2123#, white powder, particle size ≤75μm, residual carbon content 57%, polymer chain contains only three elements of carbon, hydrogen and oxygen, and the starting pyrolysis temperature is 230℃;

[0072] A2. Pretreatment: Preheat in a high-temperature vacuum atmosphere furnace at a heating rate of 3°C / min to 230°C and keep warm for 3 hours.

[0073] A3. Carbonization: Start to introduce nitrogen into the high-temperature vacuum atmosphere furnace, continue to heat up, the heating rate is 2℃ / min, the temperature is raised to 1200℃, and the holding time is 1h.

[0074] A4. Cooling: Cooling rate 5℃ / min, cooling to 25℃.

[0075] A5. Coarse crushing: After cooling, the material is crushed to ≤2mm by a ceramic double-roll crusher.

[0076] A6. Fine crushing and classification: The material after crushing in step A5 is finely crushed and classified by a jet mill and a classifier to obtain a hard carbon negative electrode material with D10=5μm, D50=9μm, D90=18μm, and Dmax=25μm.

[0077] Example 3

[0078] This embodiment provides a high reversible capacity phenolic resin-based hard carbon negative electrode material and a preparation method thereof. The specific steps are as follows: the micropore volume of the hard carbon negative electrode material is as follows: Figure 1As shown:

[0079] A1. Preparation: solid phenolic resin 3105#, white powder, particle size ≤75μm, residual carbon content 60%, polymer chain contains only three elements of carbon, hydrogen and oxygen, starting pyrolysis temperature 270℃;

[0080] A2. Pretreatment: Preheat in a high-temperature vacuum atmosphere furnace at a heating rate of 3°C / min to 270°C and keep warm for 2h.

[0081] A3. Carbonization: Start to introduce nitrogen into the high temperature vacuum atmosphere furnace, continue to heat up, the heating rate is 4℃ / min, the heating time is 193min, then the heating rate is reduced to 2℃ / min, the heating time is 129min, the temperature is raised to 1300℃, and the holding time is 2h.

[0082] A4. Cooling: Cooling rate 5℃ / min, cooling to 25℃.

[0083] A5. Coarse crushing: After cooling, the material is crushed to ≤2mm by a ceramic double-roll crusher.

[0084] A6. Fine crushing and classification: The crushed material is finely crushed and classified by a jet mill and a classifier to obtain a hard carbon negative electrode material with D10=5μm, D50=10μm, D90=20μm, and Dmax=25μm.

[0085] Comparative Example 1

[0086] This comparative example provides a high reversible capacity phenolic resin-based hard carbon negative electrode material and a preparation method thereof. The specific steps are as follows: the micropore volume of the hard carbon negative electrode material is as follows: Figure 1 As shown, the electron microscope image of the negative electrode material is as follows Figure 4 As shown, the surface electron microscope image of the negative electrode material is as follows Figure 5 shown.

[0087] A1. Preparation: solid phenolic resin 2123#, white powder, particle size ≤75μm, residual carbon content 60%, polymer chain contains only three elements of carbon, hydrogen and oxygen, starting pyrolysis temperature 270℃;

[0088] A2. Carbonization: Start to introduce nitrogen into the high temperature vacuum atmosphere furnace, increase the temperature to 1300°C at a rate of 10°C / min, and keep the temperature for 3h.

[0089] A3. Cooling: Cooling rate 5℃ / min, cool to room temperature.

[0090] A4. Coarse crushing: After cooling, the material is crushed to ≤2mm by a ceramic double-roll crusher.

[0091] A5. Fine crushing and classification: The crushed material is finely crushed and classified by a jet mill and a classifier to obtain a hard carbon negative electrode material with D10=5μm, D50=10μm, D90=20μm, and Dmax=25μm.

[0092] Test Example 1

[0093] In this test example, button-type batteries were used to test the charge and discharge performance of Examples 1 to 3 and Comparative Example 1 at room temperature (25° C.). The test results are shown in Table 1.

[0094] Table 1 Charge and discharge performance test of hard carbon materials

[0095]

[0096] In Examples 1 to 3, the surface of the material is made dense by pre-treatment before carbonization and controlling the heating temperature in the carbonization stage, thereby generating "endogenous fullerene" materials, reducing the loss of lithium ions on the surface of the material and increasing the first coulombic efficiency. However, in Comparative Example 1, the heating rate is too high, resulting in faster and faster gas discharge and more intense carbonization of the phenolic resin. Therefore, the surface contains a large number of mesopores and macropores, resulting in the loss of lithium ions on the surface of the material, thereby affecting the first coulombic efficiency.

[0097] Test Example 2

[0098] This test example tests the pore volume distribution of Examples 1 to 3 and Comparative Example 1, and the test results are shown in Table 2. The test was performed using a Mac ASAP 2020PLUS analysis station, test method: static volumetric method; adsorbate: nitrogen; mass 5.6318 g, treatment conditions: 90°C for 1 h, 200°C for 16 h.

[0099] Table 2 Pore volume distribution of Examples 1-3 and Comparative Example 1

[0100]

[0101] Examples 1 to 3 make the material surface dense by pre-carbonization pretreatment and control the heating temperature in the carbonization stage, thereby generating "embedded fullerene" materials, while the heating rate of Comparative Example 1 is too high, resulting in an increasingly faster gas discharge rate and an increasingly intense carbonization process of the phenolic resin. Therefore, the surface of Comparative Example 1 contains a large number of holes compared to Examples 1 to 3.

[0102] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A hard carbon negative electrode material, characterized in that: The D50 of the hard carbon negative electrode material is 8-10 μm; The specific surface area of ​​the hard carbon negative electrode material is not greater than 1.3 m 2 / g; The hard carbon negative electrode material has pores; The pores include micropores with a pore size of 0.35-2 nm; The pore volume of the micropores accounts for ≥90% of the pore volume of the pores; The raw material for preparing the hard carbon negative electrode material is phenolic resin; The method for preparing the hard carbon negative electrode material comprises the following steps: S1: Pretreatment: preheat the phenolic resin, S2: Carbonization: Carbonize the preheated phenolic resin. S3: Cooling: Cool the carbonized phenolic resin to room temperature. S4: Coarse crushing: Process the cooled material into particles with a size of ≤2mm. S5: Fine crushing and classification: fine crushing and classification of the coarsely crushed materials; The preheating temperature is 150-270°C, and the preheating rate is 1-4°C / min; The carbonization temperature is 1100-1400°C, and the heating rate is controlled at 1-5°C / min during the carbonization heating. The cooling rate is 5-10℃ / min.

2. The hard carbon negative electrode material according to claim 1, characterized in that: The tap density of the hard carbon negative electrode material is ≥0.90 g / cm 3 , The raw materials for preparing the hard carbon negative electrode material include phenolic resin.

3. The hard carbon negative electrode material according to claim 1, characterized in that: The preheating temperature in step S1 is 150-270°C.

4. The hard carbon negative electrode material according to claim 1, characterized in that: The preheating rate in step S1 is 1-4°C / min.

5. The hard carbon negative electrode material according to claim 1, characterized in that: In step S2, the carbonization temperature is 1100-1400°C.

6. The hard carbon negative electrode material according to claim 1, characterized in that: In step S2, during the carbonization heating, the heating rate is controlled at 1-5°C / min.

7. The hard carbon negative electrode material according to claim 1, characterized in that: In step S3, the cooling rate is 5-10°C / min.

8. Use of the hard carbon negative electrode material as claimed in claim 1 or 2 in a secondary battery.