Electrolytic capacitor and method for manufacturing the same
By using a treatment liquid containing a surface adjuster during the manufacturing process of the electrolytic capacitor, the conductive polymer evenly covers the surface of the anode body, solving the problem of small thickness of the electrolyte layer at the corner of the anode body, and improving the stability and performance of the capacitor .
Patent Information
- Application Number
- CN202080087838.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-26
- Filing Date
- 2020-12-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-12-22
AI Technical Summary
In the prior art, the thickness of the solid electrolyte layer at the corners of the anode body is small, resulting in a problem of lowering product yield, excessive leakage current, and rising electrostatic capacitance and ESR.
The anode body is treated with a treatment liquid containing a surface adjusting agent to ensure that the conductive polymer evenly covers the entire surface, including the corners, thereby forming a solid electrolyte layer of moderate thickness and reducing thickness deviation.
It effectively suppresses the thickness of the solid electrolyte layer in the corner of the anode body, improves the stability of the electrolytic capacitor, reduces the risk of short circuit and leakage current, and maintains good electrostatic capacitance and ESR performance.
Smart Images

Figure CN114846571B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to an electrolytic capacitor including a solid electrolyte layer containing a conductive polymer and a method for manufacturing the same. Background Art
[0002] An electrolytic capacitor comprises: a capacitor element, an outer casing that seals the capacitor element, and an external electrode electrically connected to the capacitor element. The capacitor element comprises: an anode body having an anode lead-out portion including a first end and a cathode forming portion including a second end, a dielectric layer formed on the surface of at least the cathode forming portion of the anode body, and a cathode portion covering at least a portion of the dielectric layer. The cathode portion comprises: a solid electrolyte layer that covers at least a portion of the dielectric layer and includes a conductive polymer, and a cathode lead-out layer that covers at least a portion of the solid electrolyte layer. An electrolytic capacitor having a solid electrolyte layer including a conductive polymer is also called a solid electrolytic capacitor.
[0003] Patent Document 1 proposes to provide an intermediate layer between a first conductive polymer layer and a second conductive polymer layer, the intermediate layer comprising a cation agent containing a cationic group and an anion agent containing a first anionic group and a second anionic group.
[0004] Patent Document 2 proposes a solid electrolytic capacitor including a first solid electrolyte layer, a second solid electrolyte layer, and at least one continuous or discontinuous layer containing an amine compound between the first and second solid electrolyte layers.
[0005] Patent document 3 proposes a method for manufacturing a solid electrolytic capacitor, characterized in that, in the method for manufacturing a solid electrolytic capacitor, an oxide film is formed on the valve metal of the anode body, and a conductive polymer layer, a graphite layer and a silver layer are sequentially formed on the oxide film as a cathode, wherein the method for forming the conductive polymer layer containing a sulfonate compound is: a nonionic surfactant having a hydroxyl group is dissolved in a conductive polymer solution or dispersion containing a sulfonated polymer compound as a dopant, and the layer is applied onto the oxide film, and dehydration condensation is performed by heating and drying.
[0006] Patent document 4 proposes a stacked solid electrolytic capacitor, characterized in that a plurality of single-plate capacitor elements are stacked and fixed on an anode side lead frame so that their anode parts are aligned in the same direction and are stacked and fixed, and the cathode parts of the single-plate capacitor elements are stacked and fixed in a shape in which a conductive adhesive layer is formed on the cathode side lead frame and the cathode parts extend from the anode part side to the front end of the cathode part, and the anode substrates of the portions of the single-plate capacitor elements having the solid electrolyte layer are stacked basically parallel to the cathode side lead frame, wherein in the single-plate capacitor element, the end portion of the anode substrate having a dielectric oxide coating layer on the surface and formed of a flat plate-shaped valve-acting metal serves as the anode portion, and a solid electrolyte layer is sequentially formed on the dielectric oxide coating layer of the portion other than the anode portion, and a conductive layer is formed thereon as the cathode portion.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2016 / 006236
[0010] Patent Document 2: Japanese Patent Application Publication No. 2012-43958
[0011] Patent Document 3: Japanese Patent Application Publication No. 2010-245313
[0012] Patent Document 4: Japanese Patent Application Publication No. 2001-230156 Summary of the invention
[0013] In the prior art, the film thickness of the solid electrolyte layer formed at the corners tends to be smaller than that near the center of the main surface of the anode body. In addition, a portion not covered by the solid electrolyte layer may be formed at the corners of the anode body.
[0014] An electrolytic capacitor according to one aspect of the present application includes at least one capacitor element.
[0015] The capacitor element comprises:
[0016] A sheet-shaped anode body having an anode lead-out portion and a cathode forming portion;
[0017] a dielectric layer formed on a surface of at least the cathode forming portion of the anode body; and
[0018] A cathode portion covers at least a portion of the dielectric layer.
[0019] The anode body includes a first end and a second end.
[0020] The anode lead-out portion includes the first end portion, and the cathode forming portion includes the second end portion.
[0021] The cathode portion includes a solid electrolyte layer that covers at least a portion of the dielectric layer and includes a conductive polymer.
[0022] In a cross section perpendicular to the direction from the first end to the second end of the capacitor element at any position on the first end side of the cathode portion, a ratio of a thickness T1 of the solid electrolyte layer formed at a corner of the anode body to a thickness T2 of the solid electrolyte layer formed at a central portion of a main surface of the anode body is: T1 / T2 is greater than 0.8 and less than 1.7.
[0023] Another aspect of the present application relates to a method for manufacturing an electrolytic capacitor, comprising:
[0024] Step 1: prepare an anode body;
[0025] A second step of forming a dielectric layer on the surface of the anode body;
[0026] A third step of treating the anode body having the dielectric layer formed thereon with a first treatment liquid containing a first conductive polymer or a precursor thereof;
[0027] A fourth step of treating the anode body treated with the first treatment solution with a second treatment solution containing a surface conditioning agent; and
[0028] In the fifth step, the anode body treated with the second treatment solution is treated with a third treatment solution containing a second conductive polymer.
[0029] It is possible to suppress the thickness of the solid electrolyte layer formed at the corners of the anode body from being reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic cross-sectional view of an electrolytic capacitor according to one embodiment of the present application.
[0031] Figure 2 Reason Figure 1 An enlarged view of the area enclosed by the solid line α.
[0032] Figure 3 This is a schematic front view of the capacitor element as seen from one main surface side.
[0033] Figure 4 Observe in the direction of the arrow Figure 3 A schematic cross-sectional view of a capacitor element taken along line IV-IV. DETAILED DESCRIPTION
[0034] The surface tension of the treatment liquid containing conductive polymers is relatively high. Therefore, it is difficult to uniformly wet the entire surface of the cathode forming part of the anode body with the treatment liquid. As a result, it is difficult to form a solid electrolyte layer of uniform thickness on the surface of the cathode forming part. As the anode body, a sheet-shaped anode body such as a metal foil or a sintered body is usually used. If the sheet-shaped anode body is treated with a treatment liquid containing conductive polymers, a solid electrolyte layer of relatively uniform thickness is formed near the center of the main surface of the sheet. However, compared with the vicinity of the center of the main surface of the sheet, it is difficult to make the treatment liquid adhere to the corners of the sheet. Therefore, at the corners of the sheet, the thickness of the solid electrolyte layer becomes smaller, or a portion to which the conductive polymer is not attached is formed. If a portion to which the conductive polymer is not attached is formed, it is easy to cause a short circuit, resulting in a defective product and a reduced yield.
[0035] According to the present application, an electrolytic capacitor is manufactured by a manufacturing method including the following steps: a step of treating an anode body having a dielectric layer formed thereon with a first treatment liquid containing a first conductive polymer or a precursor thereof; a step of treating the anode body treated with the first treatment liquid with a second treatment liquid containing a surface conditioner; and a step of treating the anode body treated with the second treatment liquid with a third treatment liquid containing a second conductive polymer. In this way, after the anode body is treated with the second treatment liquid containing a surface conditioner, it is treated with the third treatment liquid containing the second conductive polymer, so that the second conductive polymer can be attached not only to the vicinity of the center of the main surface of the anode body but also to the corners. As a result, the thickness of the solid electrolyte layer formed at the corners of the anode body can be suppressed from becoming smaller.
[0036] The following reasons are considered to be the reason for suppressing the thickness of the solid electrolyte layer formed at the corners of the anode body from becoming smaller. First, by using a second treatment liquid containing a surface conditioner, the second treatment liquid can be spread over the entire surface of the anode body in the cathode forming portion. As a result, the components of the second treatment liquid such as the surface conditioner are attached to the entire surface of the cathode forming portion. If the anode body is treated with a third treatment liquid containing a second conductive polymer in such a state, the third treatment liquid can be spread over the entire surface of the cathode forming portion. As a result, the second conductive polymer on the surface of the cathode forming portion is suppressed from aggregating near the center of the main surface of the anode body. As a result, a solid electrolyte layer of appropriate thickness can be formed not only near the center of the main surface of the anode body, but also at the corners, thereby reducing the deviation in thickness.
[0037] As described above, according to the present application, the relative ratio of the thickness of the solid electrolyte layer formed at the corner of the anode body to the thickness of the solid electrolyte layer formed near the center of the main surface can be increased compared with the related art.
[0038] More specifically, in the electrolytic capacitor of the present application, the ratio of the thickness T1 of the solid electrolyte layer formed at the corner of the anode body to the thickness T2 of the solid electrolyte layer formed at the central portion of the main surface of the anode body: T1 / T2 is greater than 0.8 and less than 1.7. In this way, in the electrolytic capacitor, the thickness of the solid electrolyte layer formed at the corner of the anode body is suppressed from becoming smaller. In addition, a solid electrolyte layer with a more uniform thickness is formed on the entire surface of the cathode forming portion of the anode body. As a result, product defects caused by short circuits can be reduced. In addition, the leakage current is suppressed from becoming excessively large, and the reduction of electrostatic capacitance, the increase of ESR and dielectric loss tangent tanδ are also suppressed, and the quality of the electrolytic capacitor is more stabilized.
[0039] In order to suppress the deviation of the thickness of the solid electrolyte layer, it is considered important to make the third treatment liquid containing the second conductive polymer spread over the entire surface of the cathode forming part of the anode body. Therefore, in order to reduce the surface tension of the third treatment liquid, it is also considered to add a surface conditioner to the third treatment liquid. However, in fact, even if a surface conditioner is added to the third treatment liquid, the effect of suppressing the thickness of the solid electrolyte layer in the corner is small. In addition, the third treatment liquid usually contains various additives in addition to the second conductive polymer, so if a surface conditioner is added, the applicable period of the third treatment liquid is sometimes shortened. According to the present application, since the second treatment liquid containing a surface conditioner is used, it is different from adding a surface conditioner to the third treatment liquid containing a conductive polymer, and a good applicable period of the third treatment liquid can be ensured. From this point of view, the second treatment liquid preferably does not contain a conductive polymer.
[0040] It should be noted that the electrolytic capacitor has at least one capacitor element. The capacitor element comprises: an anode body having an anode lead-out portion and a cathode forming portion, a dielectric layer formed on the surface of at least the cathode forming portion of the anode body, and a cathode portion covering at least a portion of the dielectric layer. The anode lead-out portion includes a first end portion of the anode body, and the cathode forming portion includes a second end portion of the anode body. The anode body is usually in a sheet shape. The cathode portion includes a solid electrolyte layer covering at least a portion of the dielectric layer and including a conductive polymer. The above-mentioned thicknesses T1 and T2 are obtained in a cross section perpendicular to the direction from the first end side to the second end side of the capacitor element at any position of the portion on the first end side of the cathode portion. It should be noted that this cross section is sometimes referred to as cross section G. More specifically, the thickness T1 is obtained by measuring the thickness of the solid electrolyte layer formed at the four corners of the anode body in cross section G and averaging them. First, in cross section G, a straight line passing through the vertices of the corners of the anode body is drawn at an angle of 45° relative to a line segment extending outward from the main surface of the anode body. Then, the distance between the point where the straight line intersects the outer edge of the solid electrolyte layer and the vertex of the corresponding corner is taken as the thickness of the solid electrolyte layer formed at each corner. The thickness T2 is obtained by measuring the thickness of the solid electrolyte layer formed at the central part of each of the pair of main surfaces of the anode body in the cross section G and averaging them. First, in the cross section G, draw the center line of the midpoint of the line segment corresponding to the main surface of the anode body. Then, the distance between the intersection of the center line with the outer edge of the solid electrolyte layer and the corresponding above-mentioned midpoint is taken as the thickness of the solid electrolyte layer formed at the central part of each main surface.
[0041] The direction from the first end side to the second end side is set to be parallel to the direction of the straight line connecting the center of the end face of the first end and the center of the end face of the second end. This direction is sometimes referred to as the length direction of the anode body or capacitor element. Section G is: in the portion of the capacitor element where the cathode portion is formed, a section perpendicular to the length direction of the capacitor element at any position between a position of half the length of the cathode portion in a direction parallel to the length direction of the capacitor element and an end of the first end side of the cathode portion. It should be noted that the cross section of the capacitor element can be observed, for example, using an optical microscope.
[0042] The solid electrolyte layer may include: a first layer covering at least a portion of the dielectric layer and including a first conductive polymer, a second layer covering at least a portion of the first layer and including a second conductive polymer, and at least one continuous or discontinuous layer between the first layer and the second layer. Here, the continuous or discontinuous layer includes a surface conditioner. In such a solid electrolyte layer, it can be said that the surface conditioner is unevenly present between the first layer and the second layer. By sandwiching a surface conditioner between the first layer and the second layer, it is easy to cover the entire surface of the cathode forming portion of the anode body with the second layer. Therefore, the thickness of the solid electrolyte layer formed at the corner is suppressed from becoming smaller. As a result, the deviation in the thickness of the solid electrolyte layer is reduced.
[0043] It should be noted that the surface adjuster is at least between the first layer and the second layer. In the portion of the dielectric layer not covered by the first layer, the surface adjuster may be interposed between the dielectric layer and the second layer. The surface adjuster may be distributed in a manner that covers the entire surface of the cathode forming portion of the anode body. Therefore, the layer containing the surface adjuster does not necessarily have to be continuous, and may also be a discontinuous layer. It may be a state in which a portion of the layer containing the surface adjuster enters the first layer. Between the first layer and the second layer, at least one layer containing the surface adjuster may be interposed, or two or more layers may be interposed.
[0044] Hereinafter, the electrolytic capacitor and the method for manufacturing the same according to the present application will be described in more detail with reference to the drawings as needed.
[0045] [Electrolytic capacitors]
[0046] (Anode)
[0047] The anode body can include valve metal, alloy containing valve metal, and compound containing valve metal. These materials can be used alone or in combination of two or more. As the valve metal, for example, aluminum, tantalum, niobium, and titanium are preferably used.
[0048] The anode body is usually in the form of a sheet. Sheets also include foils and plates. The sheet-shaped anode body has a pair of main surfaces. There is a corner between each main surface and each end surface of the anode body.
[0049] The anode body has an anode lead-out portion and a cathode forming portion. The anode lead-out portion includes a first end portion of the anode body, and the cathode forming portion includes a second end portion of the anode body opposite to the first end portion. A cathode portion including a solid electrolyte layer is formed on the surface of the cathode forming portion of the anode body.
[0050] The anode body usually has a porous portion on the surface layer at least in the cathode forming portion. The porous portion is formed on the surface layer by roughening the surface of at least the portion of the substrate (e.g., a sheet-shaped substrate) containing the valve metal corresponding to the cathode forming portion. The porous portion can also be formed on the surface layer of the anode lead-out portion. In addition, the anode body can be a formed body or a sintered body of particles containing the valve metal. The sintered body has a porous structure, so the entire anode body can become a porous portion.
[0051] (Dielectric layer)
[0052] The dielectric layer is an insulating layer that is formed so as to cover at least a portion of the surface of the anode body and functions as a dielectric.
[0053] The dielectric layer may be formed so as to cover at least a portion of the anode body. For example, the dielectric layer may be formed on at least the surface of the cathode forming portion of the anode body. The dielectric layer may also be formed on the surface of the anode lead-out portion.
[0054] The dielectric layer is usually formed on the surface of the anode body. A porous portion is usually formed on the surface layer of the anode body. Therefore, the dielectric layer is formed along the inner wall surface of the pores and depressions (pits) on the surface of the anode body including the inner wall surface of the pores of the porous portion.
[0055] The dielectric layer includes an oxide of a valve metal. For example, when tantalum is used as the valve metal, the dielectric layer includes Ta2O5, and when aluminum is used as the valve metal, the dielectric layer includes Al2O3. It should be noted that the dielectric layer is not limited to this, as long as it functions as a dielectric.
[0056] (Cathode)
[0057] The cathode portion at least comprises a solid electrolyte layer covering at least a portion of the dielectric layer. The cathode portion is usually formed on the surface of the cathode forming portion of the anode body through the dielectric layer. The cathode portion usually comprises a solid electrolyte layer and a cathode lead layer covering at least a portion of the solid electrolyte layer. The solid electrolyte layer and the cathode lead layer are described below.
[0058] (Solid electrolyte layer)
[0059] The solid electrolyte layer is formed in a manner covering the dielectric layer. The solid electrolyte layer does not necessarily have to cover the entire dielectric layer (the entire surface), as long as it is formed in a manner covering at least a portion of the dielectric layer. The solid electrolyte layer includes, for example: a first layer including a first conductive polymer, a second layer including a second conductive polymer formed on the first layer, and a continuous or discontinuous layer including a surface conditioner between the first layer and the second layer. In the case where there is an area on the dielectric layer where the first layer is not formed, the second layer can be formed on the dielectric layer in the area, or the second layer can be formed on the dielectric layer via a layer including a surface conditioner.
[0060] (1st floor)
[0061] As the first conductive polymer, a known substance used in an electrolytic capacitor, such as a π-conjugated conductive polymer, etc. can be used. As the first conductive polymer, for example, a polymer having a basic skeleton of polypyrrole, polythiophene, polyaniline, polyfuran, polyacetylene, polyphenylene, polyphenylene vinylene, polyacene, and polythiophene vinylene can be cited. Among these, a polymer having a basic skeleton of polypyrrole, polythiophene, or polyaniline is preferred.
[0062] The polymers mentioned above also include homopolymers, copolymers of two or more monomers, and derivatives thereof (such as substituted products having substituents). For example, polythiophene includes poly(3,4-ethylenedioxythiophene) and the like.
[0063] The first conductive polymer may be used alone or in combination of two or more.
[0064] The weight average molecular weight (Mw) of the first conductive polymer is not particularly limited, and is, for example, 1,000 to 1,000,000.
[0065] In this specification, the weight average molecular weight (Mw) is a value in terms of polystyrene measured by gel permeation chromatography (GPC). In general, GPC is measured using a polystyrene gel column and water / methanol (volume ratio 8 / 2) as a fluid.
[0066] The first layer may be a single layer or may be composed of a plurality of layers. When the first layer is composed of a plurality of layers, the first conductive polymer contained in each layer may be the same or different.
[0067] The first layer may further contain a dopant. As the dopant, for example, at least one selected from anions and polyanions is used.
[0068] Examples of the anion include, but are not particularly limited to, sulfate ions, nitrate ions, phosphate ions, borate ions, organic sulfonate ions, and carboxylate ions. Examples of the dopant that generates sulfonate ions include p-toluenesulfonic acid and naphthalenesulfonic acid.
[0069] As the polyanion, for example, high molecular weight polysulfonic acid and high molecular weight polycarboxylic acid can be cited. As the high molecular weight polysulfonic acid, polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyacrylic acid sulfonic acid, and polymethacrylic acid sulfonic acid can be cited. As the high molecular weight polycarboxylic acid, polyacrylic acid, polymethacrylic acid, etc. can be cited. The polyanion also includes polyester sulfonic acid and phenol sulfonic acid phenolic resin, etc. However, the polyanion is not limited to these.
[0070] When using an anion agent described later, it is advantageous to use a dopant with a relatively high electron-withdrawing property (e.g., sulfonic acid ions, polymeric polysulfonic acid) from the viewpoint of easily suppressing dedoping. It is also preferred to use sulfonic acid ions or polymeric polysulfonic acid as a dopant from the viewpoint of easily ensuring high conductivity of the solid electrolyte layer.
[0071] The anion and the polyanion may each be contained in the first layer in the form of a salt. In the first layer, the anion and the polyanion may each form a conductive polymer complex together with the first conductive polymer. For example, the sulfonic acid group may be contained in the first layer in the form of a free form (-SO3H), an anion form (-SO3 - ), or salt form, or can be contained in a form bonded to or interacting with a conductive polymer. In this specification, all forms of sulfonic acid groups are included, and sometimes simply referred to as "sulfonic acid groups". Similarly, in the first layer, the carboxyl group can be in a free form (-COOH), an anionic form (-COO - ), or a salt form, or may be contained in a form bonded to or interacting with a conductive polymer. In this specification, the carboxyl group including all these forms may be simply referred to as a "carboxyl group".
[0072] The amount of the dopant contained in the first layer is, for example, 10 to 1000 parts by mass, or 50 to 200 parts by mass, relative to 100 parts by mass of the first conductive polymer.
[0073] The first layer may also contain a water-soluble polymer. It should be noted that polymer-type dopants are also included in water-soluble polymers. As water-soluble polymers, it is preferred to use components with lower electron-withdrawing properties than dopants. When the solid electrolyte layer contains a water-soluble polymer, the thickness of the solid electrolyte layer in the central part of the main surface of the anode body can be increased, and the deviation in the thickness of the solid electrolyte layer can be further reduced. Therefore, the quality of the electrolytic capacitor is further stabilized. In addition, by increasing the thickness of the solid electrolyte layer on the main surface of the anode body, the increase in ESR and tanδ of the electrolytic capacitor can be suppressed, the leakage current can be reduced, and the voltage resistance can be improved.
[0074] As water-soluble polymers, water-soluble polymer compounds having a hydrophilic group in the main chain or the side chain can be cited. As the hydrophilic group, polyoxyalkylene chains, hydroxyl groups, acid groups (carboxyl groups, sulfonic acid groups, etc.) can be cited. As water-soluble polymers, for example, polyalkylene glycol compounds, water-soluble polyurethanes, water-soluble polyamides, water-soluble polyimides, water-soluble acrylic resins, and polyvinyl alcohol can be cited.
[0075] Examples of the polyalkylene glycol compound include compounds having a polyoxyalkylene chain. As the polyoxyalkylene chain, preferably polyoxy C 2-4 Alkenyl chain. The polyalkylene glycol compound more preferably contains at least a polyoxyethylene chain. As the polyalkylene glycol compound, for example, polyalkylene glycol (diethylene glycol, triethylene glycol, oligoethylene glycol, polyethylene glycol, ethylene oxide-propylene oxide block copolymer, etc.), polyalkylene glycol having a substituent (halogen atom, hydroxyl group, etc.) (for example, polyalkylene glycol chlorohydrin or bromohydrin (diethylene glycol monochlorohydrin, triethylene glycol monochlorohydrin, oligoethylene glycol monochlorohydrin, polyethylene glycol monochlorohydrin, diethylene glycol monobromohydrin, triethylene glycol monobromohydrin, oligoethylene glycol monobromohydrin, etc.)) and other hydroxy compounds can be cited. The polyalkylene glycol compound also includes derivatives of these hydroxy compounds (for example, ether compounds, ester compounds, amide compounds).
[0076] Water-soluble polyurethane, water-soluble polyamide, and water-soluble polyimide each include polymers having an acid group (selected from at least one of a carboxyl group and a sulfonic acid group) in a side chain. In these water-soluble polymers, high water solubility can be obtained by introducing a plurality of acid groups into the skeleton (main chain) of each polymer.
[0077] As water-soluble acrylic resin, those having carboxyl groups in the side chains are preferred. As such water-soluble acrylic resin, polyacrylic acid, polymethacrylic acid, acrylic acid-methacrylic acid copolymer, copolymers of at least one selected from acrylic acid and methacrylic acid and other copolymerizable monomers, etc. can be cited. As other copolymerizable monomers, for example, acrylates (alkyl esters, hydroxyalkyl esters, etc.), methacrylates (alkyl esters, hydroxyalkyl esters, etc.), vinyl compounds (vinyl cyanide, olefins, aromatic vinyl compounds, etc.), polycarboxylic acids having polymerizable unsaturated bonds (maleic acid, fumaric acid, etc.) or their anhydrides can be cited. The copolymer can contain one monomer unit derived from other copolymerizable monomers, and can also contain two or more monomer units derived from other copolymerizable monomers.
[0078] The first layer may contain one type of water-soluble polymer, or may contain two or more types of water-soluble polymers.
[0079] Water-soluble polymers also include water-soluble polymers that function as dopants. When using dopants containing sulfonic acid groups and other dopants with relatively high electron-withdrawing properties (e.g., sulfonic acid ions, polymer-type polysulfonic acids) as dopants, even if water-soluble polymers with relatively low electron-withdrawing properties such as carboxyl groups coexist, most of the time, the function of the dopant as such water-soluble polymers will not be exerted. When the solid electrolyte layer contains such water-soluble polymers, the insulating properties of the polymer can be appropriately exerted, and the film thickness of the solid electrolyte layer can be increased, thereby reducing the leakage current of the electrolytic capacitor, and the withstand voltage can be improved. Therefore, as a water-soluble polymer, it is preferred to use a water-soluble polymer with lower electron-withdrawing properties than the dopant. As such a water-soluble polymer, for example, a water-soluble polymer having at least one selected from a carboxyl group, a hydroxyl group, and a polyoxyalkylene chain can be cited.
[0080] The carboxyl group and sulfonic acid group of the water-soluble polymer can be in the form of free (-COOH) or anion (-COO - ), or a salt form is contained in the first layer. In addition, a part of each of the carboxyl group and the sulfonic acid group may be contained in the first layer in a form that is bonded to or interacts with the conductive polymer. In this specification, the carboxyl group including all forms is sometimes simply referred to as a "carboxyl group", and the sulfonic acid group including all forms is sometimes simply referred to as a "sulfonic acid group".
[0081] The weight average molecular weight (Mw) of the water-soluble polymer is, for example, 100 or more, preferably 400 or more. The Mw of the water-soluble polymer having higher withstand voltage characteristics is, for example, 5 million or less, or 1 million or less. These lower limits and upper limits can be arbitrarily combined.
[0082] For the content of the water-soluble polymer in the first layer, it is preferred that the content of the water-soluble polymer in the solid electrolyte layer be adjusted in a range of, for example, more than 25% by mass and less than 70% by mass. The content of the water-soluble polymer in the solid electrolyte layer can be more than 30% by mass and less than 70% by mass (or less than 68% by mass), can be more than 40% by mass and less than 70% by mass (or less than 68% by mass), or can be more than 43% by mass and less than 70% by mass (or less than 68% by mass). When the content of the water-soluble polymer in the solid electrolyte layer is in such a range, the rise of the ESR and tanδ of the electrolytic capacitor can be suppressed to be relatively low, and the leakage current can be reduced, and a higher withstand voltage can also be ensured.
[0083] The content of the water-soluble polymer in the first layer is preferably 30% by mass or less, more preferably 20% by mass or less or 10% by mass or less. The first layer may not contain a water-soluble polymer. In this case, higher conductivity of the solid electrolyte layer can be ensured, which is preferred.
[0084] It should be noted that the content of water-soluble polymers in the solid electrolyte layer can be obtained using samples collected from the capacitor element. More specifically, first, an electrolytic capacitor is embedded in a curable resin and the curable resin is cured. The cured product is ground or cross-sectioned to expose a cross section parallel to the thickness direction of the solid electrolyte layer. Scrape the solid electrolyte layer, collect a specified amount of sample, and measure the mass. Extract water-soluble polymers from the sample with water at 20°C to 40°C. Concentrate the extract and identify the water-soluble polymer by liquid chromatography-mass spectrometry (LC-MS) or gas chromatography-mass spectrometry (GC-MS). The concentration of water-soluble polymers in the extract is obtained by the standard curve method. Based on the concentration and the mass of the sample, the content (mass) of water-soluble polymers in the solid electrolyte layer is obtained. Regarding the content of water-soluble polymers in the first layer, a sample collected by scraping the solid electrolyte layer formed in the pit of the anode body is used, and otherwise, the same steps as above are used to obtain it.
[0085] (Layer containing surface conditioning agent)
[0086] (Surface Conditioner)
[0087] The surface conditioner includes, for example, a leveling agent and a defoaming agent. From the viewpoint of allowing the second treatment liquid containing the surface conditioner to spread over the entire surface of the cathode forming portion of the anode body, the surface conditioner is preferably a surface conditioner having a leveling effect. As the surface conditioner, a surfactant can be appropriately used.
[0088] The surfactant may be any of a nonionic surfactant and an ionic surfactant. The surfactant has a hydrophilic group and a hydrophobic group. Ionic surfactants include cationic surfactants, anionic surfactants, and amphoteric surfactants. The surfactant may be used alone or in combination of two or more.
[0089] As nonionic surfactants, ether type (polyether type, etc.), ester ether type (fatty acid polyethylene glycol, fatty acid polyoxyethylene sorbitan, etc.), ester type (glycerol fatty acid ester, sorbitan fatty acid ester, sucrose fatty acid ester, etc.), or alkanolamide type (fatty acid alkanolamide, etc.) nonionic surfactants can be cited. As polyether type nonionic surfactants, nonionic surfactants having polyoxyalkylene chains such as polyoxyethylene chains (polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene polyoxypropylene glycol, etc.) can be cited. The nonionic surfactant can be a nonionic surfactant having a halogen atom. Halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. Among them, fluorine atoms are preferred.
[0090] Examples of the cationic surfactant include alkylamine salt type (monoalkylamine salt, dialkylamine salt, trialkylamine salt, etc.), quaternary ammonium salt type (alkyltrimethylammonium halide, dialkyldimethylammonium halide, alkylbenzalkonium chloride, etc.).
[0091] As anionic surfactants, for example, carboxylic acid type, sulfonic acid type, sulfate type, and phosphate type anionic surfactants can be cited. As carboxylic acid type anionic surfactants, aliphatic monocarboxylates, polyoxyethylene alkyl ether carboxylates, N-acyl sarcosinates, N-acyl glutamates, etc. can be cited. As sulfonic acid type anionic surfactants, dialkyl sulfosuccinates, alkane sulfonates, α-olefin sulfonates, alkylbenzene sulfonates, naphthalenesulfonic acid-formaldehyde condensates, alkylnaphthalenesulfonates, N-methyl-N-acyltaurates, etc. can be cited. As sulfate type anionic surfactants, alkyl sulfates, polyoxyethylene alkyl ether sulfates, oil sulfate ester salts, etc. can be cited. As phosphate type anionic surfactants, alkyl phosphates, polyoxyethylene alkyl ether phosphates, polyoxyethylene alkylphenyl ether phosphates, etc. can be cited.
[0092] Examples of the amphoteric surfactant include carboxybetaine type (alkyl betaine, fatty acid amide propyl betaine, etc.), 2-alkylimidazoline derivative type (2-alkyl-N-carboxymethyl-N-hydroxyethylimidazolium betaine, etc.), glycine type (alkyldiethylenetriaminoacetic acid, dialkyldiethylenetriaminoacetic acid, etc.), amine oxide type (alkylamine oxide, etc.) and the like.
[0093] If a nonionic surfactant is used, the pot life of the second treatment solution can be prevented from being shortened, and dedoping of the conductive polymers of the first and second layers can be prevented. From the viewpoint of further promoting the attachment of the second conductive polymer to the surface of the anode body, a cationic surfactant or an amphoteric surfactant can be used. From the viewpoint of easily suppressing the volatilization of the cationic agent described later, an anionic surfactant can be used.
[0094] The continuous or discontinuous layer containing the surface modifier can contain components other than the surface modifier. The amount of the surface modifier contained in the continuous or discontinuous layer is, for example, 0.01 to 30% by mass, and can be 0.1 to 15% by mass. When the amount of the surface modifier is in such a range, the surface modifier can be more evenly distributed over the entire surface of the cathode forming portion of the anode body, and the thickness deviation of the solid electrolyte layer can be easily reduced. In addition, the resistance of the solid electrolyte layer can be suppressed to a low level, so the increase in ESR can be suppressed.
[0095] (Other ingredients)
[0096] As the component other than the surface conditioner contained in the continuous or discontinuous layer, for example, at least one selected from a cationic agent and an anionic agent can be cited. The cationic agent and the anionic agent are different from the surface conditioner. For example, as the cationic agent and the anionic agent, substances other than surfactants are used.
[0097] The first layer and the second layer each generally contain both a conductive polymer and an anionic dopant, and the dopant is likely to be present on the surface of the first layer and the second layer. That is, the surfaces of the first layer and the second layer are likely to be negatively charged, so it is difficult to form the second layer on the surface of the first layer. When the continuous or discontinuous layer between the first layer and the second layer contains a cationic agent, the film forming property or coverage of the second layer can be improved.
[0098] When the continuous or discontinuous layer contains an anionic agent, the film repairability of the dielectric layer can be improved.
[0099] In order to fully obtain the effect of the cationic agent, it is preferred to make the cationic agent in the second treatment liquid fully dissociated. However, the cationic agent has low solubility and high volatility, so it is difficult to increase the content of the cationic agent in the continuous or discontinuous layer. From the viewpoint of promoting the dissociation of the cationic agent, it is preferred to use a second treatment liquid containing both a cationic agent and an anionic agent. The continuous or discontinuous layer obtained using such a second treatment liquid contains both a cationic agent and an anionic agent.
[0100] (Cationic Agent)
[0101] As a cationic agent having a cationic group, there is no particular limitation as long as it can generate cations in a dissociated state. As a cationic agent, for example, it can be a metal compound (inorganic bases such as metal hydroxides, etc.), preferably an organic compound (organic bases, etc.). For the cationic group of the cationic agent as an organic compound, amino groups (primary amino groups, secondary amino groups and tertiary amino groups, etc.) and quaternary ammonium groups are preferred. Such cationic groups also include salts of amino groups and salts of quaternary ammonium groups, etc. The continuous or discontinuous layer containing the surface conditioning agent can contain one cationic agent, or it can contain two or more cationic agents.
[0102] Among the cationic agents, cationic agents (amine compounds, etc.) having an amino group as a cationic group are preferred. Examples of amine compounds include amines (primary to tertiary amines) having 1 to 3 substituents on the nitrogen atom, diamines having 1 or 2 alkyl groups on the nitrogen atom, etc. The substituent is selected, for example, from an alkyl group, a cycloalkyl group, and an aryl group. The alkyl group, the cycloalkyl group, and the aryl group may each further have a substituent (for example, at least one selected from a hydroxyl group and an alkoxy group).
[0103] Examples of the above-mentioned diamines include diaminoalkanes, diaminocycloalkanes (diamino C such as diaminocyclohexane, etc.), and diaminoalkane. 5-8 Cycloalkanes, etc.), diaminoaromatics (diaminobenzene, diaminonaphthalene, etc. diamino C 6-14 Aromatic hydrocarbons, etc. As diaminoalkanes, diamino C 2-14 Alkane or diamino C 4-12 Alkanes, etc. Specific examples of diaminoalkanes include 1,4-diaminobutane, 1,6-diaminohexane, 1,8-diaminooctane, and 1,10-diaminodecane.
[0104] As the amine, at least one selected from primary amines and tertiary amines can be used. As the tertiary amine, N,N-diC 1-10 Alkyl-NC 4-16 Alkylamine, N,N-diC 4-16 Alkyl-NC 1-10 Alkylamine, tri-C 4-16 Alkylamines, etc.
[0105] The continuous or discontinuous layer (or the second treatment liquid) containing the surface conditioning agent may contain a cationic agent in any form of an amine compound, a cation corresponding to the amine compound, a quaternary ammonium compound, and a salt of a cation. For example, in the continuous or discontinuous layer (or the second treatment liquid), the cationic agent may form a salt with an anionic agent.
[0106] (Anionic agent)
[0107] As the anion agent, for example, at least one selected from the anions and polyanions exemplified as the dopant for the first layer can be used. Among them, from the viewpoint of suppressing dedoping from the first layer and the second layer, it is preferred to use a dopant different from the dopant for the first layer and the dopant for the second layer as the anion agent. From the same viewpoint, a dopant having lower electron-withdrawing property than the dopant for the first layer and the dopant for the second layer can be used as the anion agent.
[0108] From the viewpoint of suppressing the corrosion of the valve action metal constituting the anode body, an anionic agent comprising a first anionic group with high electron-withdrawing property and a second anionic group with lower electron-withdrawing property than the first anion can be used. As such anionic agent, for example, a polymer (first anionic agent) comprising a first anionic group and a second anionic group can be cited. The first anionic agent can be used alone or in combination of two or more.
[0109] As the first anionic group and the second anionic group, for example, sulfonic acid group, phosphoric acid group, phosphonic acid group, boric acid group, carboxyl group, and hydroxyl group etc. can be enumerated. From these anionic groups, the first anionic group and the second anionic group with different electron withdrawing properties can be selected. It should be noted that the anionic group is not particularly limited as long as it can generate anions in the dissociated state, and can also be salts of these groups etc.
[0110] For the first anionic agent as a polymer (polymer compound), for example, a copolymer (p1) comprising at least a monomer unit having a first anionic group and a monomer unit having a second anionic group, and a polymer (p2) comprising at least a monomer unit having a first anionic group and a second anionic group, etc. can be exemplified. These polymerizable monomer units may also include other copolymerizable monomer units. The first anionic agent may be used alone or in combination of two or more.
[0111] Examples of monomer units serving as a base of the above-mentioned monomer units include aliphatic vinyl monomer units such as ethylene and propylene, aromatic vinyl monomer units such as styrene, and diene monomer units such as butadiene and isoprene.
[0112] The weight average molecular weight (Mw) of the polymer is, for example, 5,000 to 500,000, or 10,000 to 200,000.
[0113] The first anionic agent may be used in combination with a second anionic agent which is a low molecular weight compound (monomer compound) having an anionic group, as required.
[0114] As the second anion agent, for example, a monomer compound of the anions and polyanions described as the dopant of the first layer can be used. The second anion agent can be any of an aliphatic compound, an alicyclic compound, and an aromatic compound. The second anion agent can be used alone or in combination of two or more.
[0115] As the second anion agent, for example, aliphatic sulfonic acid (C 1-6 Alkanesulfonic acid, etc.), alicyclic sulfonic acid (cyclohexanesulfonic acid, etc. 5-8 Cycloalkanesulfonic acid, etc.), aromatic sulfonic acid (benzenesulfonic acid, styrenesulfonic acid, etc. 6-14 Acidic phospho-oxyethylene glycol monoacrylate (acidic phospho-oxyethylene glycol mono(meth)acrylate (P(=O)(OH)2-(O-CH2CH2)) of carboxylic acids such as acidic phospho-oxyethyl acrylate and acidic phospho-oxyethyl methacrylate n -OC(=O)-CR=CH2) (n is an integer of 2 to 10, R is a hydrogen atom or a methyl group), aliphatic phosphonic acid (vinyl phosphonic acid, etc.), aromatic phosphonic acid (phenyl phosphonic acid, etc.), carboxylic acid [aliphatic carboxylic acid (propionic acid, butyric acid, hexanoic acid, etc. C 2-10 Alkane carboxylic acid, adipic acid, etc. 4-12 Alkanedicarboxylic acids, etc.), alicyclic carboxylic acids (carboxy cyclohexane, etc. 5-8 Cycloalkanes, cyclohexanedicarboxylic acids and other dicarboxyl groups C 5-8 Cycloalkanes, etc.), aromatic carboxylic acids (carboxyl C 6-14 Aromatic hydrocarbons, salicylic acid, and other carboxyl hydroxyl C 6-14 Aromatic hydrocarbons, phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid and other dicarboxylic acids C 6-14 aromatic hydrocarbons, etc.), phenolic compounds (phenol, hydroxytoluene, vinylphenol, hydroxyvinyltoluene, etc.), hydroxyalkyl esters of the above carboxylic acids (for example, hydroxyethyl acrylate, hydroxyethyl methacrylate, etc., hydroxy C 1-4 Alkyl esters) etc.
[0116] As the second anionic agent, an anionic agent having two or more anionic groups can be used. As such a second anionic agent, for example, a second anionic agent having a sulfonic acid group and a carboxyl group (for example, an aliphatic compound (sulfosuccinic acid, etc.), an aromatic compound (sulfobenzoic acid, sulfosalicylic acid, disulfosalicylic acid, sulfophthalic acid, sulfoisophthalic acid, sulfoterephthalic acid, naphtholsulfonic acid, etc.), a second anionic agent having a phosphate group and a carboxyl group (for example, 2-(dihydroxyphosphinyloxy)acrylic acid), a second anionic agent having a phosphonic acid group and a carboxyl group (for example, phosphonoacrylic acid, 2-methyl-3-phosphonoacrylic acid), etc. can be cited.
[0117] In the continuous or discontinuous layer (or the second treatment liquid) containing the surface conditioning agent, the anionic group of the anionic agent may be contained in any form selected from the above-mentioned anionic groups, anions corresponding to the above-mentioned anionic groups, and salts of anions.
[0118] (Layer 2)
[0119] The second layer may be formed so as to cover at least a portion of the first layer, and may be formed so as to cover the entire surface of the first layer. In at least a portion of the surface of the first layer, the second layer is formed so as to cover the first layer via a continuous or discontinuous layer containing a surface conditioner, but there may also be a region where the second layer is directly formed on the surface of the first layer without a continuous or discontinuous layer. In addition, in a region where the first layer and the continuous or discontinuous layer are not formed, the second layer may be in contact with the dielectric layer (that is, the second layer may be formed so as to cover the dielectric layer).
[0120] (Second conductive polymer)
[0121] As the second conductive polymer contained in the second layer, a known substance used in an electrolytic capacitor can be used, and specifically, it can be appropriately selected from the conductive polymers exemplified for the first conductive polymer. The weight average molecular weight (Mw) of the second conductive polymer can also be appropriately selected from the range exemplified for the first conductive polymer. The first conductive polymer and the second conductive polymer can be the same substance or different substances.
[0122] The second layer may be a single layer or may be composed of a plurality of layers. When the second layer is composed of a plurality of layers, the second conductive polymer contained in each layer may be the same or different.
[0123] The second layer may further include a dopant. As the dopant, a known dopant used in an electrolytic capacitor may be used. Specifically, it may be appropriately selected from the examples exemplified for the first layer. The dopant may be the same substance or different substances in the first and second layers.
[0124] The dopant may be contained in the second layer in the form of a salt. In the second layer, the dopant may form a conductive polymer composite together with the second conductive polymer. As in the case of the first layer, the anionic group of the dopant may be contained in the second layer in an organic form, an anionic form, or a salt form, or may be contained in a form bonded to or interacting with the conductive polymer.
[0125] The amount of the dopant contained in the second layer is, for example, 10 to 1000 parts by mass, or 50 to 200 parts by mass relative to 100 parts by mass of the second conductive polymer.
[0126] The second layer may also contain a water-soluble polymer. Regarding the water-soluble polymer, reference can be made to the description of the water-soluble polymer in the first layer. For the content (mass %) of the water-soluble polymer in the second layer, it is preferably adjusted within the range in which the content (mass %) of the water-soluble polymer in the solid electrolyte layer becomes the above-mentioned range. When the second layer contains a water-soluble polymer, it is easy to obtain the effect of increasing the thickness of the solid electrolyte layer in the central part of the anode body, which can further improve the effect of reducing leakage current and the effect of improving voltage resistance. Therefore, it is preferred that at least the second layer contains a water-soluble polymer. The content (mass %) of the water-soluble polymer in the second layer can be set to the range recorded as the content (mass %) of the water-soluble polymer in the solid electrolyte layer. It should be noted that the content of the water-soluble polymer in the second layer is obtained by the same steps as the case of obtaining the content of the water-soluble polymer in the solid electrolyte layer, except for using a sample collected by scraping the surface of the solid electrolyte layer.
[0127] (other)
[0128] In the cross section G perpendicular to the length direction of the capacitor element at any position of the part on the first end side of the cathode portion, the ratio T1 / T2 is, for example, greater than 0.8, may be greater than 0.9, or may be greater than 1 or greater than 1. When the ratio T1 / T2 is in such a range, the thickness of the solid electrolyte layer at the corner is suppressed from being reduced, so the generation of defective products caused by short circuits can be suppressed. In particular, when the ratio T1 / T2 is greater than 1 or greater than 1, the effect of reducing leakage current is improved, so the generation of defective products caused by leakage current can be suppressed. The ratio T1 / T2 is, for example, less than 1.7, may be less than 1.5, or may be less than 14. When the ratio T1 / T2 is in such a range, the reduction of electrostatic capacitance, the increase of ESR and dielectric loss tangent tan3 are suppressed, and the quality of the electrolytic capacitor is more stabilized. These upper and lower limits can be combined arbitrarily.
[0129] According to the present application, the thickness of the solid electrolyte layer formed at the corner of the anode body can also be made greater than the thickness of the solid electrolyte layer formed near the center of the main surface. The details are not clear yet, but it is speculated that it is because of the following mechanism. First, by using a second treatment liquid containing a surface treatment agent, the second treatment liquid can be spread over the entire surface of the cathode forming part of the anode body. Usually, in a droplet, the rate of volatilization of the liquid medium is faster at the edge than in the center of the droplet, so components other than the liquid medium are likely to remain at the edge. Such a phenomenon is also called the coffee ring effect or the ring stain effect. Due to such a phenomenon, in the coating film of the second treatment liquid formed on the entire surface of the cathode forming part, the liquid medium evaporates faster from the corner than near the center of the main surface of the anode body, and the components of the second treatment liquid other than the liquid medium remain in large quantities on the surface of the corner. As a result, it is believed that the components of the third treatment liquid are attached to the corner of the cathode forming part of the anode body in large quantities, so it is easy to make the second conductive polymer gather at the corner. For example, the ratio T1 / T2 can be made larger than 1 by adjusting the type and concentration of the surface conditioning agent, the type of the liquid medium used in the second treatment liquid, the drying conditions of the coating film of the second treatment liquid, and the like.
[0130] The average thickness of the solid electrolyte layer is, for example, 5 μm or more and 20 μm or less, and may be 10 μm or more and 15 μm or less.
[0131] It should be noted that the average thickness of the solid electrolyte layer is calculated as follows: in a cross section perpendicular to the length direction of the capacitor element and passing through the center of the cathode portion in a direction parallel to the length direction of the capacitor element, the thickness is measured at any number of locations (for example, 10 locations) and averaged.
[0132] Each of the first layer and the second layer may contain known additives and known conductive materials other than the conductive polymer (for example, conductive inorganic materials such as manganese dioxide and / or TCNQ complex salt, etc.) as necessary.
[0133] In addition, a layer for improving adhesion or the like may be interposed between the dielectric layer and the first layer.
[0134] Figure 1 It is a schematic cross-sectional view of an electrolytic capacitor according to one embodiment of the present application. Figure 2 To conceptually illustrate the Figure 1 An enlarged view of the area enclosed by the solid line α.
[0135] The electrolytic capacitor 1 includes a capacitor element 11, a resin outer casing 12 that seals the capacitor element 11, and an anode terminal 13 and a cathode terminal 14 that are respectively exposed to the outside of the resin outer casing 12. The capacitor element 11 includes a sheet-shaped anode body 2, a dielectric layer 3 that covers the second end side of the anode body 2, and a cathode portion 15 that covers the dielectric layer 3. The portion of the anode body 2 where the cathode portion 15 is formed is a cathode forming portion, and the portion where the cathode portion 15 is not formed is an anode lead portion. The anode terminal 13 is electrically connected to the first end of the anode lead portion of the anode body 2. The cathode terminal 14 is electrically connected to the cathode portion 15. The resin outer casing 12 has a substantially rectangular parallelepiped shape, and thus the electrolytic capacitor 1 also has a substantially rectangular parallelepiped shape.
[0136] The anode body 2 and the cathode portion 15 face each other via the dielectric layer 3. The cathode portion 15 includes a solid electrolyte layer 4 covering the dielectric layer 3, and a cathode layer 5 covering the solid electrolyte layer 4. The cathode layer 5 shown in the figure has a two-layer structure, including a carbon layer 5a in contact with the solid electrolyte layer 4, and a metal paste layer 5b covering the surface of the carbon layer 5a.
[0137] In the anode lead-out portion of the anode body 2 protruding from the cathode portion 15, an insulating separation portion 16 is formed in a region on the cathode portion 15 side in a manner that covers the surface of the anode body 2 in a strip shape, thereby limiting the contact between the cathode portion 15 and the anode body 2. The first end portion of the anode body 2 protruding from the cathode portion 15 is electrically connected to one end portion 13a of the anode terminal 13 by welding or the like. On the other hand, the cathode layer 5 formed on the outermost layer of the cathode portion 15 is electrically connected to one end portion 14a of the cathode terminal 14 by means of a conductive adhesive 17 (for example, a mixture of a thermosetting resin and metal particles). The other end portion 13b of the anode terminal 13 and the other end portion 14b of the cathode terminal 14 are respectively led out from different side surfaces of the resin outer casing 12 so as to be exposed to a main flat surface ( Figure 1 The exposed portions of the terminals on the flat surface are used for welding to a substrate (not shown) on which the electrolytic capacitor 1 is to be mounted.
[0138] The dielectric layer 3 is formed on a portion of the surface of the conductive material constituting the anode body 2. Specifically, the dielectric layer 3 can be formed by anodizing the surface of the conductive material constituting the anode body 2. Figure 2 As shown, it is formed along the surface of anode body 2 (including the holes on the inner surface and the inner wall surface of the recess).
[0139] The first layer 4a containing the first conductive polymer is formed so as to cover the dielectric layer 3, and the second layer 4b containing the second conductive polymer is formed so as to cover the first layer 4a. Moreover, a layer 4c containing a surface conditioning agent is interposed between the first layer 4a and the second layer 4b. In the example shown in the figure, the layer 4c containing the surface conditioning agent is formed so as to cover the first layer 4a, and the second layer 4b is formed so as to cover the layer 4c containing the surface conditioning agent. Figure 2 In the embodiment, the layer 4c of the surface conditioning agent is a continuous layer. However, the present invention is not limited to this case, and the layer 4c of the surface conditioning agent may be a discontinuous layer. In such a capacitor element 11, the thickness of the solid electrolyte layer 4 formed at the corner of the anode body 2 is suppressed from being reduced, and the variation in the thickness of the solid electrolyte layer 4 is reduced.
[0140] The first layer 4a does not necessarily need to cover the entirety (entire surface) of the dielectric layer 3, and may be formed to cover at least a portion of the dielectric layer 3, and is preferably formed to cover as many areas as possible. Similarly, the second layer 4b and the layer 4c containing the surface conditioning agent each do not necessarily need to cover the entirety (entire surface) of the first layer 4a, and may be formed to cover at least a portion of the first layer 4a, and is preferably formed to cover as many areas as possible.
[0141] Since dielectric layer 3 is formed along the surface of anode body 2, irregularities are formed on the surface of dielectric layer 3 in accordance with the shape of the surface of anode body 2. First layer 4a is preferably formed so as to fill in the irregularities of dielectric layer 3.
[0142] In the above configuration, anode body 2 is an anode member of capacitor element 11, and first layer 4a, second layer 4b, and cathode layer 5 are cathode members of capacitor element 11. Dielectric layer 3 is a dielectric member of capacitor element 11.
[0143] In the above embodiment, the case where the capacitor element 11 has two layers of conductive polymers, namely, the first layer 4a and the second layer 4b, has been described, but the capacitor element 11 may also have three or more layers of conductive polymers. In this case, one or more layers of conductive polymers may be formed between the first layer 4a and the second layer 4b. For example, one or more layers of conductive polymers may be formed in at least one of the first layer 4a and the layer 4c containing the surface conditioning agent, and the layer 4c containing the surface conditioning agent and the second layer 4b.
[0144] In the electrolytic capacitor of the present application, as described above, the ratio T1 / T2 of the thickness T1 of the solid electrolyte layer formed at the corner of the anode body to the thickness T2 of the solid electrolyte layer formed at the center of the main surface can be made larger than before.
[0145] Figure 3 This is a schematic front view of the capacitor element as seen from one main surface side. Figure 4 Observe in the direction of the arrow Figure 3 The thicknesses T1 and T2 of the solid electrolyte layer can be obtained, for example, by the following procedure.
[0146] The ratio T1 / T2 is obtained in a cross section G of the cathode portion 15 perpendicular to the direction from the first end E1 to the second end E2 of the capacitor element 11 (sometimes referred to as the longitudinal direction of the anode body 2 or the capacitor element 11). Here, the cross section G is formed at an arbitrary position of the portion on the first end E1 side of the cathode portion 15. The portion on the first end E1 side of the cathode portion 15 is a portion from the end on the first end E1 side of the cathode portion 15 to a position of length L / 2 when the length of the cathode portion 15 in the longitudinal direction of the capacitor element 11 is set to L. Figure 3 In FIG. 2 , the portion on the first end E1 side of the cathode portion 15 corresponds to the upper half of the cathode portion 15 .
[0147] Figure 4 The cross section G of the portion on the first end E1 side of the cathode portion 15 along the line IV-IV perpendicular to the length direction of the capacitor element 11 is shown. The line IV-IV corresponds to an arbitrarily selected position in the portion on the first end E1 side of the cathode portion 15. It should be noted that Figure 4 The shading representing the cross section is omitted.
[0148] In the above cross section G, a pair of main surfaces Ms of the sheet-like anode body 2 and a pair of end surfaces Es located at the ends of the pair of main surfaces Ms can be seen. There are corners between each main surface Ms and each end surface Es, so four corners can be confirmed in the above cross section G of the anode body 2. Extend the line corresponding to each main surface Ms outward and draw imaginary straight lines L1 and L2, and draw a straight line passing through the vertex of the corner at an angle of 45° to the straight line L1 or L2. For the point where the straight line intersects the outer edge of the solid electrolyte layer 4, the distance D11, D12, D13 and D14 between the point and the vertex of the corner are used as the thickness of the solid electrolyte layer 4 at each corner. Then, the values of the four distances (D11, D12, D13, D14) are averaged to obtain T1.
[0149] In the cross section G, when the width of the anode body 2 corresponding to the length of the line segment corresponding to the main surface Ms is set to W, a center line CL is drawn from each end surface Es at a position of W / 2. The center line CL passes through the midpoint of the line segment corresponding to each main surface Ms of the anode body 2. The distances D21 and D22 between the intersection of the center line CL and the outer edge of the solid electrolyte layer 4 and the midpoint of the above line segment are respectively taken as the thickness of the solid electrolyte layer at the center of the main surface Ms. The values of the two distances (D21, D22) are averaged to obtain T2.
[0150] [Method for manufacturing electrolytic capacitor]
[0151] A method for manufacturing an electrolytic capacitor according to one embodiment of the present application includes: a first step of preparing an anode body; a second step of forming a dielectric layer on the surface of the anode body; a third step of treating the anode body having the dielectric layer formed thereon with a first treatment liquid containing a first conductive polymer or a precursor thereof; a fourth step of treating the anode body treated with the first treatment liquid with a second treatment liquid containing a surface conditioner; and a fifth step of treating the anode body treated with the second treatment liquid with a third treatment liquid containing a second conductive polymer.
[0152] Hereinafter, each step will be described in more detail.
[0153] (1st step)
[0154] In the first step, the anode body is formed by a known method depending on the type of the anode body.
[0155] The anode body is prepared, for example, by forming a porous portion at least on the surface of a portion corresponding to at least the cathode forming portion. The porous portion may be formed on the entire surface of the anode body or on the entire anode body.
[0156] The porous portion can be formed, for example, by roughening the surface of a sheet-shaped substrate formed of a conductive material containing a valve-acting metal. Roughening is sufficient as long as it can form bumps and depressions on the substrate surface. Roughening can be performed, for example, by etching the substrate surface, or by depositing particles of a conductive material containing a valve-acting metal on the substrate surface using a vapor phase method such as evaporation. As etching, a known method can be used, for example, electrolytic etching can be cited. For example, if a prescribed shielding member is arranged on the surface of the anode lead-out portion and then roughened, a porous portion can be formed on the surface layer of the cathode forming portion. The shielding member is not particularly limited, and can be an insulator such as a resin, or a conductor containing a conductive material.
[0157] In addition, a sintered body obtained by sintering particles containing a valve action metal may be used as the anode body.
[0158] (Second step)
[0159] In the second step, a dielectric layer is formed on the anode body. The dielectric layer is formed by anodizing the surface of the anode body. By anodizing, at least the valve action metal present on the surface of the anode body is oxidized to generate an oxide.
[0160] Anodic oxidation can be performed by a known method, for example, chemical conversion treatment, etc. However, in the anodization, any method is sufficient as long as an oxide of a valve action metal can be formed, and the method is not limited to chemical conversion treatment.
[0161] The chemical conversion treatment can be performed, for example, by immersing the anode body in a chemical conversion solution so that the chemical conversion solution is impregnated into the surface of the anode body (pores on the inner surface, inner wall surfaces of the depressions), using the anode body as an anode, and applying a voltage between the anode body and a cathode immersed in the chemical conversion solution. As the chemical conversion solution, for example, a phosphoric acid aqueous solution, an ammonium phosphate aqueous solution, or an ammonium adipate aqueous solution is preferably used.
[0162] (Step 3)
[0163] In the third step, it is sufficient as long as the first treatment liquid can at least contact the dielectric layer. For example, the first treatment liquid can be at least contacted with the dielectric layer by immersing the anode body formed with the dielectric layer in the first treatment liquid, or by injecting the first treatment liquid into the anode body formed with the dielectric layer. The first treatment liquid can be impregnated into the surface of the anode body formed with the dielectric layer (the inner wall surface of the hole or depression on the inner side of the surface formed with the dielectric layer) by immersion or injection. In addition, it is not limited to impregnation or injection, and a known coating method (for example, a spray coating method) or a printing method can also be used. These methods can be combined as needed.
[0164] When using the first treatment liquid containing the precursor of the first conductive polymer, it is preferred to immerse the anode body and polymerize the precursor by chemical polymerization or electrolytic polymerization to generate the first conductive polymer. The anode body is usually dried after being taken out from the first treatment liquid. During drying, the anode body can be heated as needed. The anode body taken out from the first treatment liquid can be cleaned as needed before drying. In this way, the first layer containing the first conductive polymer is formed.
[0165] When the first treatment liquid containing the first conductive polymer is used, for example, the first treatment liquid is brought into contact with at least the dielectric layer of the anode body and dried. In this way, the first layer containing the first conductive polymer is formed. The anode body may be heated as needed during drying.
[0166] The first treatment liquid is prepared by dissolving or dispersing the constituent components of the first treatment liquid in a liquid medium. As constituent components, for example, the first conductive polymer or its precursor, a dopant, a water-soluble polymer, and an additive can be cited. For the first conductive polymer, the dopant, and the water-soluble polymer, reference can be made to the description of the first layer.
[0167] Examples of the precursor of the first conductive polymer include monomers, oligomers, and prepolymers of the first conductive polymer. The first treatment liquid may contain one type of precursor or two or more types of precursors.
[0168] The first treatment liquid may contain one first conductive polymer, or two or more first conductive polymers. The first treatment liquid may contain one dopant, or two or more dopant. The first treatment liquid may contain one water-soluble polymer, or two or more water-soluble polymers.
[0169] As the liquid medium contained in the first treatment liquid, water, an organic medium, and a mixture thereof can be exemplified. As the organic medium, for example, aliphatic alcohols, aliphatic ketones (acetone, etc.), nitriles (acetonitrile, benzonitrile, etc.), amides (N, N-dimethylformamide, etc.), and sulfoxides (dimethyl sulfoxide, etc.) can be cited. As aliphatic alcohols, aliphatic alcohols having 1 to 5 carbon atoms are preferred. The aliphatic alcohol can be any of a monohydric alcohol and a polyhydric alcohol. As aliphatic monohydric alcohols, for example, methanol, ethanol, propanol, butanol can be cited. As aliphatic polyhydric alcohols, ethylene glycol, glycerol, etc. can be cited.
[0170] The first treatment liquid may contain a known additive used when forming a solid electrolyte layer. As the additive, a silane compound may be used.
[0171] When the first treatment liquid containing the precursor of the first conductive polymer is used, an oxidant is used to polymerize the precursor. The oxidant may be contained in the first treatment liquid as an additive. In addition, the oxidant may be applied to the anode body before or after the first treatment liquid is brought into contact with the anode body having the dielectric layer formed thereon. As such an oxidant, sulfates, sulfonic acids or salts thereof may be exemplified. The oxidant may be used alone or in combination of two or more.
[0172] Examples of sulfates include salts of sulfuric acid such as iron sulfate and sodium persulfate, and salts of sulfuric acid such as persulfate and metals. Examples of metals constituting the salts include alkali metals such as sodium and potassium; iron, copper, chromium, zinc, and the like. Sulfonic acid or its salt has a function as a dopant in addition to its function as an oxidant. As sulfonic acid or its salt, the low molecular weight sulfonic acid or its salt exemplified as a dopant can be used.
[0173] The process of forming the first layer by immersion in the first treatment liquid and polymerization (or drying) can be performed once or repeatedly. In each case, the composition and viscosity of the first treatment liquid can be the same, or at least one of the conditions can be changed.
[0174] (Step 4)
[0175] The fourth step can be performed, for example, by bringing the second treatment liquid containing the surface conditioning agent into contact with the anode body treated with the first treatment liquid. After contacting with the second treatment liquid, the anode body can be dried as needed. During drying, the anode body can be heated as needed.
[0176] In the fourth step, the second treatment liquid may be attached so as to cover the first conductive polymer attached to the surface of the dielectric layer. From the viewpoint of forming the second layer more uniformly over the entire surface of at least the cathode forming portion of the anode body, it is preferred that the second treatment liquid be attached so as to distribute the surface conditioning agent over at least the entire surface of the cathode forming portion.
[0177] The second treatment liquid is applied to the surface of the anode body by at least one method selected from, for example, immersion, injection, coating, and printing, depending on the condition of the first treatment liquid.
[0178] The second processing liquid may contain a liquid medium. Examples of the liquid medium include the liquid medium exemplified in relation to the first processing liquid.
[0179] The second treatment liquid may contain at least one selected from a cationic agent and an anionic agent.
[0180] As the components contained in the second treatment liquid, reference can be made to the description regarding the continuous or discontinuous layer containing the surface conditioner.
[0181] The amount of the surface conditioning agent in the second treatment liquid is, for example, 0.01 mass % or more and 5 mass % or less, and may be 0.05 mass % or more and 2.5 mass % or less. When the amount of the surface conditioning agent is within such a range, the surface conditioning agent can be more evenly distributed over the entire surface of the cathode forming portion of the anode body, and the thickness deviation of the solid electrolyte layer can be easily reduced. Moreover, the resistance of the solid electrolyte layer can be suppressed to a lower level, thereby suppressing the increase in ESR. The amount of the surface conditioning agent in the second treatment liquid is the concentration of the surface conditioning agent in the second treatment liquid.
[0182] The amount of the surface conditioner in the dry solid content of the second treatment liquid is selected from the range described for the amount of the surface conditioner contained in the continuous or discontinuous layer containing the surface conditioner.
[0183] In this specification, the amount of the surface conditioning agent in the dry solid content of the second treatment liquid is used synonymously with the amount of the surface conditioning agent in the components other than the liquid medium in the second treatment liquid.
[0184] As described above, the second treatment liquid preferably does not contain a conductive polymer.
[0185] (5th step)
[0186] For the fifth step, an anode body treated with a second treatment liquid is used, and a third treatment liquid containing a second conductive polymer (a dopant, a water-soluble polymer as needed) is used instead of the first treatment liquid. Otherwise, it can be carried out according to the situation of the third step. As the third treatment liquid, the second conductive polymer is contained instead of the first conductive polymer. Otherwise, the treatment liquid described in the first treatment liquid can be used. Through the fifth step, the second layer containing the second conductive polymer is formed. Through the fourth step, the components contained in the second treatment liquid such as the surface conditioning agent are distributed on the entire surface of at least the cathode forming part of the anode body. In such a state, the surface of the cathode forming part is treated with the third treatment liquid, thereby enabling the second conductive polymer to be attached to the entire surface of the cathode forming part including the corner. In addition, when the third treatment liquid contains a water-soluble polymer, the effect of reducing the thickness deviation of the solid electrolyte layer is improved, the leakage current of the electrolytic capacitor can be suppressed to a lower level, and high voltage resistance can be obtained.
[0187] (Step of forming cathode layer)
[0188] The method for manufacturing an electrolytic capacitor may further include a step of forming a cathode layer (sixth step).
[0189] In the sixth step, for example, a carbon layer and a metal paste layer are sequentially laminated on the surface of the anode body obtained in the fifth step to form a cathode layer.
[0190] The carbon layer can be formed by immersing the anode body having the dielectric layer formed with the second layer in a dispersion containing conductive carbon, or applying a paste containing conductive carbon to the surface of the second layer. As conductive carbon, for example, graphites such as artificial graphite and natural graphite can be used. As the dispersion and paste, for example, conductive carbon can be dispersed in an aqueous liquid medium.
[0191] The metal paste layer can be formed, for example, by laminating a composition containing metal particles on the surface of the carbon layer. As the metal paste layer, for example, a silver paste layer formed using a composition containing silver particles and a resin (binder resin) can be used. As the resin, a thermoplastic resin can also be used, and a thermosetting resin such as an imide resin or an epoxy resin is preferably used.
[0192] It should be noted that the structure of the cathode layer is not limited to this, and any structure may be used as long as it has a current collecting function.
[0193] The cathode terminal is connected to the cathode layer. For example, a conductive adhesive is applied to the cathode layer and the cathode terminal is bonded to the cathode layer via the conductive adhesive.
[0194] (Process of sealing capacitor element)
[0195] The capacitor element thus formed is sealed with an outer body. Specifically, the material resin of the capacitor element and the outer body (for example, uncured thermosetting resin and filler) is placed in a mold, and the capacitor element is sealed with an outer body by transfer molding, compression molding, etc. At this time, a portion of the anode terminal and cathode terminal connected to the anode lead drawn from the capacitor element are exposed from the mold respectively. The molding conditions are not particularly limited, and the time and temperature conditions can be appropriately set considering the curing temperature of the thermosetting resin used.
[0196] [Example]
[0197] Hereinafter, the present application will be specifically described based on Examples and Comparative Examples, but the present application is not limited to the following Examples.
[0198] 《Electrolytic Capacitor A1》
[0199] Follow the steps below to make Figure 1 The electrolytic capacitor 1 shown was used and its characteristics were evaluated.
[0200] (1) Step of Preparing Anode Body 2 (First Step)
[0201] Anode body 2 was produced by roughening both surfaces of an aluminum foil (thickness: 100 μm) as a base material by etching.
[0202] (2) Step of forming dielectric layer 3 (second step)
[0203] The second end portion of anode body 2 was immersed in a chemical conversion solution, and a DC voltage of 70 V was applied for 20 minutes to form dielectric layer 3 containing aluminum oxide.
[0204] (3) Step of forming the first layer 4a (third step)
[0205] Under stirring, 3,4-ethylenedioxythiophene monomer is added to an aqueous solution of polystyrene sulfonic acid (Mw: 75,000), and then an oxidant (iron (III) sulfate and sodium persulfate) is added to perform chemical oxidative polymerization. The obtained polymerization solution is filtered using an ion exchange device to remove impurities, thereby obtaining a solution containing poly (3,4-ethylenedioxythiophene) (PEDOT) as a first conductive polymer and polystyrene sulfonic acid (PSS) as a dopant.
[0206] Pure water was added to the obtained solution, and the mixture was homogenized using a high-pressure homogenizer, and then filtered using a filter, thereby preparing a first treatment liquid in a dispersed liquid state.
[0207] The anode body 2 having the dielectric layer 3 formed thereon obtained in (2) above is immersed in the first treatment liquid, taken out from the first treatment liquid, and then dried at 120° C. for 10 to 30 minutes. The immersion in the first treatment liquid and the drying are repeated once each, thereby forming the first layer 4 a including the first conductive polymer so as to cover the surface of the dielectric layer 3.
[0208] (4) Step of forming layer 4c containing surface conditioning agent (fourth step)
[0209] The ester-type nonionic surfactant (surface conditioner), N,N-dimethyloctylamine (cationic agent), and a copolymer of styrenesulfonic acid and acid phosphoethyl acrylate (P(=O)(OH)2-O-CH2CH2-OC(=O)-CH=CH2) (anionic agent) are dissolved in pure water to prepare the second treatment liquid. The amount of the surface conditioner in the second treatment liquid is set to 0.5 mass %. The concentration of the cationic agent in the second treatment liquid is set to 0.05 mol / L, and the concentration of the anionic agent is set to 0.03 mol / L. It should be noted that the amount of the surface conditioner in the total amount of the components contained in the second treatment liquid other than water as a liquid medium is 12.5 mass %.
[0210] Anode body 2 treated in (3) above was immersed in the second treatment liquid, taken out, and dried at 100° C. for 3 minutes, thereby forming layer 4 c containing a surface conditioning agent so as to cover the surface of first layer 4 a .
[0211] In addition, the said anion agent used for the 2nd process liquid was manufactured as follows.
[0212] Sodium styrene sulfonate and acid phosphoethyl acrylate are added to a specified amount of pure water and mixed to prepare a monomer solution. At this time, sodium styrene sulfonate and acid phosphoethyl acrylate are used in a ratio of 75:25 between the copolymerization ratio (molar ratio) of styrene sulfonic acid and acid phosphoethyl acrylate in the copolymer. Under stirring, a specified amount of ammonium persulfate (oxidant) is added to the monomer solution, and a polymerization reaction is carried out for 8 hours. Pure water and an ion exchange resin are added to the obtained polymerization solution, and the mixture is stirred and filtered to perform a purification treatment. The purification treatment is repeated several times to finally obtain the above copolymer. The molecular weight of the copolymer is measured by GPC, and the result is Mw of 83,000.
[0213] (5) Step of forming the second layer 4b (fifth step)
[0214] A third treatment liquid having the same composition as the first treatment liquid used in (3) above is used. The anode body 2 treated in (4) above is immersed in the third treatment liquid, taken out, and then dried at 120° C. for 10 to 30 minutes. The immersion in the third treatment liquid and the drying are further repeated twice alternately, thereby forming the second layer 4b containing the second conductive polymer in a manner covering the surface of the layer 4c containing the surface conditioning agent.
[0215] In this way, the solid electrolyte layer 4 including the first layer 4 a , the layer 4 c including the surface conditioning agent, and the second layer 4 b is formed so as to cover the surface of the dielectric layer 3 .
[0216] (6) Step of forming cathode layer 5 (sixth step)
[0217] Anode body 2 obtained in (5) above is immersed in a dispersion of graphite particles dispersed in water, taken out of the dispersion and then dried, thereby forming carbon layer 5a at least on the surface of second layer 4b. Drying is performed at 130 to 180°C for 10 to 30 minutes.
[0218] Next, a silver paste containing silver particles and a binder resin (epoxy resin) is applied to the surface of the carbon layer 5a, and heated at 150 to 200°C for 10 to 60 minutes to cure the binder resin and form a metal paste layer 5b. In this way, a cathode layer 5 composed of the carbon layer 5a and the metal paste layer 5b is formed.
[0219] As described above, capacitor element 11 is manufactured.
[0220] (7) Assembly of electrolytic capacitors
[0221] Cathode layer 5 of capacitor element 11 obtained in (6) above and one end 14a of cathode terminal 14 are bonded with conductive adhesive 17. A first end of anode body 2 protruding from capacitor element 11 and one end 13a of anode terminal 13 are bonded by laser welding.
[0222] Next, resin outer package 12 made of insulating resin is formed around capacitor element 11 by transfer molding. At this time, the other end 13b of anode terminal 13 and the other end 14b of cathode terminal 14 are drawn out from resin outer package 12.
[0223] Thus, the electrolytic capacitor 1 (A1) is completed. A total of 20 electrolytic capacitors 1 are manufactured in the same manner as above.
[0224] (8) Evaluation
[0225] The following evaluation was performed using an electrolytic capacitor.
[0226] (a) Thickness ratio T1 / T2 of the solid electrolyte layer 4
[0227] The thickness ratio T1 / T2 of the solid electrolyte layer 4 in each electrolytic capacitor was obtained by the above-described procedure. Then, the average value of the ratios T1 / T2 of 20 electrolytic capacitors was obtained.
[0228] (b) Initial electrostatic capacitance, tan3, and ESR
[0229] In an environment of 20°C, using a 4-terminal LCR meter, the initial electrostatic capacitance (μF) and initial tan3 of each electrolytic capacitor at a frequency of 120kHz were measured, and the initial ESR (mΩ) at a frequency of 100kHz was measured. Then, the average value of 20 electrolytic capacitors was calculated.
[0230] (c) Leakage current (LC)
[0231] A resistor of 1 kΩ was connected in series to the electrolytic capacitor, and a leakage current (μA) was measured after a rated voltage of 25 V was applied for 1 minute using a DC power supply. The average value of 20 electrolytic capacitors was calculated.
[0232] 《Electrolytic capacitor B1》
[0233] In the fourth step, no surface conditioner was used when preparing the second treatment liquid. Except for this, the electrolytic capacitor B1 was produced and evaluated in the same manner as the electrolytic capacitor A1.
[0234] 《Electrolytic capacitor B2》
[0235] In the fifth step, an ester-type nonionic surfactant (surface conditioner) which is the same as the surfactant used in the second treatment liquid of the electrolytic capacitor A1 is added to the third treatment liquid. The amount of the surface conditioner in the third treatment liquid is set to 0.5% by mass. In addition, in the fourth step, when preparing the second treatment liquid, no surface conditioner is used. Except for this, the electrolytic capacitor B2 is manufactured and evaluated in the same manner as the electrolytic capacitor A1.
[0236] 《Electrolytic capacitors A2 and A3》
[0237] In the fourth step, a commercially available nonionic surfactant different from the surfactant used in the electrolytic capacitor A1 was used as a surface conditioner. Electrolytic capacitors A2 and A3 were produced and evaluated in the same manner as the electrolytic capacitor A1. It should be noted that different nonionic surfactants were used in the electrolytic capacitors A2 and A3. The nonionic surfactant used in the electrolytic capacitor A2 was an ester type, and the nonionic surfactant used in the electrolytic capacitor A3 was a linear alkyl polyether type.
[0238] The results of electrolytic capacitors A1 to A3 and B1 to B2 are shown in Table 1. Each evaluation is expressed as a ratio (%) when the measured value of electrolytic capacitor A1 is 100%. Electrolytic capacitors A1 to A3 are examples, and electrolytic capacitors B1 to B2 are comparative examples.
[0239] [Table 1]
[0240]
[0241] As shown in Table 1, for the electrolytic capacitor B1 that does not use a surface conditioner and the electrolytic capacitor B2 that uses the third treatment solution containing a surface conditioner, the ratio T1 / T2 becomes lower, which is 0.552 to 0.769. In contrast, for the electrolytic capacitors A1 to A3 that use the second treatment solution containing a surface conditioner, the ratio T1 / T2 is 0.932 to 1.280, which is significantly improved compared to the electrolytic capacitors B1 and B2. The value of T2 of the electrolytic capacitors A1 to A3 is not much different from the value of T2 of the electrolytic capacitors B1 and B2. Therefore, for the electrolytic capacitors A1 to A3, compared with the electrolytic capacitors B1 to B2, it can be said that the thickness of the solid electrolyte layer formed at the corner of the anode body is suppressed, and the deviation of the thickness of the solid electrolyte layer is reduced.
[0242] In particular, in the electrolytic capacitor A1, the thickness of the solid electrolyte layer at the corner portion is increased, and the electrostatic capacitance, tan δ, and ESR are maintained at good levels, and the leakage current can be significantly reduced.
[0243] The electrolytic capacitors A2 and A3 were able to suppress the leakage current from becoming excessively large, and excellent results were obtained with respect to electrostatic capacitance, tan δ, and ESR.
[0244] It should be noted that when T1 / T2 is large, the risk of product failure due to short circuit occurrence is reduced. Therefore, for electrolytic capacitors A1 to A3, the occurrence of product failure due to short circuit occurrence can be reduced compared to electrolytic capacitors B1 and B2.
[0245] 《Electrolytic capacitors A4~A8》
[0246] As the third treatment liquid, a treatment liquid prepared by further adding a water-soluble polymer to a dispersion liquid having the same composition as the first treatment liquid was used. Electrolytic capacitors A4 to A8 were prepared and evaluated in the same manner as electrolytic capacitor A1. In the third treatment liquid, the amount of water-soluble polymer added was adjusted so that the content (mass %) of the water-soluble polymer in the solid electrolyte layer became the value shown in Table 2. As the water-soluble polymer, a copolymer of acrylic acid and methacrylic acid (Mw: about 100,000) was used.
[0247] The withstand voltage of the electrolytic capacitors A4 to A8, A1, and B1 was evaluated according to the following procedure.
[0248] (Pressure resistance)
[0249] The electrolytic capacitor was boosted at a rate of 1.0 V / sec while applying voltage, and the breakdown withstand voltage of 0.5 A overcurrent was measured. The breakdown withstand voltage is expressed as an index (withstand voltage index V) when the breakdown withstand voltage of electrolytic capacitor A1 is set to 100 (%). The withstand voltage is evaluated based on the withstand voltage index. The larger the withstand voltage index, the higher the withstand voltage.
[0250] The results are shown in Table 2. Electrolytic capacitors A4 to A8 are examples.
[0251] [Table 2]
[0252]
[0253] As shown in Table 2, by making the solid electrolyte layer contain a water-soluble polymer, a high voltage resistance is obtained (electrolytic capacitors A4 to A8). For electrolytic capacitors A4 to A8, the increase in tanδ and ESR is suppressed, and LC can also be greatly reduced. For electrolytic capacitors A4 to A8, the ratio T1 / T2 is improved compared to electrolytic capacitor B1 (and B2 in Table 1). The value of T1 of electrolytic capacitors A4 to A8 is not much different from the value of T1 of electrolytic capacitor A1. Therefore, for electrolytic capacitors A4 to A8, compared with electrolytic capacitor A1, it can be said that the thickness T2 of the solid electrolyte layer formed in the central part of the main surface of the anode body becomes larger, thereby reducing the deviation in the thickness of the solid electrolyte layer. Therefore, it is believed that the LC of electrolytic capacitors A4 to A8 is greatly reduced, and a high voltage resistance is obtained.
[0254] Industrial Applicability
[0255] According to the present application, the variation in thickness of the solid electrolyte layer can be reduced, so short-circuit failures can be reduced and a high-quality electrolytic capacitor can be provided. Therefore, the electrolytic capacitor can be used for various purposes.
[0256] Description of Reference Numerals
[0257] 1: electrolytic capacitor, 2: anode body, 3: dielectric layer, 4: solid electrolyte layer, 4a: first layer, 4b: second layer, 4c: layer containing surface conditioning agent, 5: cathode layer, 5a: carbon layer, 5b: metal paste layer, 11: capacitor element, 12: resin outer casing, 13: anode terminal, 13a: one end of the anode terminal, 13b: the other end of the anode terminal, 14: cathode terminal, 14a: one end of the cathode terminal, 14b: the other end of the cathode terminal, 15: cathode part, 16: separation part, 17: conductive adhesive, E1: first end of the anode body, E2: second end of the anode body, Ms: main surface of the anode body, Es: end surface of the anode body, L1, L2: straight lines formed by extending line segments corresponding to a pair of main surfaces of the anode body, CL: center line of each main surface of the anode body
Claims
1. An electrolytic capacitor comprising at least one capacitor element, The capacitor element comprises: A sheet-shaped anode body having an anode lead-out portion and a cathode forming portion, a dielectric layer formed on at least a surface of the cathode forming portion of the anode body, and a cathode portion covering at least a portion of the dielectric layer, The anode body includes a first end and a second end, The anode lead-out portion includes the first end portion, and the cathode forming portion includes the second end portion. The cathode portion includes a solid electrolyte layer covering at least a portion of the dielectric layer and containing a conductive polymer. In a cross section perpendicular to a direction from the first end toward the second end of the capacitor element at any position of a portion on the first end side of the cathode portion, a ratio of a thickness T1 of the solid electrolyte layer formed at a corner of the anode body to a thickness T2 of the solid electrolyte layer formed at a center portion of a main surface of the anode body: T1 / T2 is greater than or equal to 0.8 and less than or equal to 1.7, The solid electrolyte layer comprises: a first layer covering at least a portion of the dielectric layer and comprising a first conductive polymer, a second layer covering at least a portion of the first layer and comprising a second conductive polymer, and at least one continuous or discontinuous layer interposed between the first layer and the second layer, The continuous or discontinuous layer comprises a surface conditioning agent, The continuous or discontinuous layer further comprises at least one selected from a cationic agent comprising a cationic group and an anionic agent comprising an anionic group, The cationic agent and the anionic agent are different from the surface conditioning agent.
2. The electrolytic capacitor according to claim 1, in, The ratio T1 / T2 is greater than or equal to 0.9 and less than or equal to 1.
5.
3. The electrolytic capacitor according to claim 1 or 2, in, The ratio T1 / T2 is greater than 1.
4. The electrolytic capacitor according to claim 1 or 2, in, The solid electrolyte layer further includes a water-soluble polymer.
5. The electrolytic capacitor according to claim 4, in, At least the second layer contains the water-soluble polymer.
6. The electrolytic capacitor according to claim 4, in, The content of the water-soluble polymer in the solid electrolyte layer is 25 mass % or more and 70 mass % or less.
7. The electrolytic capacitor according to claim 1 or 2, in, The surface conditioner includes at least one surfactant selected from the group consisting of a nonionic surfactant, a cationic surfactant, an anionic surfactant, and an amphoteric surfactant.
8. The electrolytic capacitor according to claim 1 or 2, in, The amount of the surface conditioner contained in the continuous or discontinuous layer is 0.01 mass % or more and 30 mass % or less.
9. A method for manufacturing an electrolytic capacitor, wherein include: The first step is to prepare an anode body; A second step of forming a dielectric layer on the surface of the anode body; A third step of treating the anode body having the dielectric layer formed thereon with a first treatment liquid containing a first conductive polymer or a precursor thereof; A fourth step of treating the anode body treated with the first treatment solution with a second treatment solution containing a surface conditioning agent; and In a fifth step, the anode body treated with the second treatment solution is treated with a third treatment solution containing a second conductive polymer. The second treatment liquid further comprises at least one selected from a cationic agent containing a cationic group and an anionic agent containing an anionic group. The cationic agent and the anionic agent are different from the surface conditioning agent.
10. The method for manufacturing an electrolytic capacitor according to claim 9, in, The surface conditioner includes at least one surfactant selected from the group consisting of a nonionic surfactant, a cationic surfactant, an anionic surfactant, and an amphoteric surfactant.
11. The method for manufacturing an electrolytic capacitor according to claim 9 or 10, in, The amount of the surface conditioner in the second treatment liquid is 0.01 mass % or more and 5 mass % or less.
12. The method for manufacturing an electrolytic capacitor according to claim 9 or 10, in, The third treatment liquid further contains a water-soluble polymer.