Lithium ion battery and preparation method thereof

By using aluminum foam and aluminum coated carbon foam as current collectors in lithium-ion batteries, the positive electrode and negative electrode materials are embedded in a three-dimensional grid, which solves the polarization problem of lithium-ion batteries when increasing energy density, and achieves high energy density. Long life and safety improvements.

CN114883575BActive Publication Date: 2024-11-08TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210496395.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-09
Publication Date
2024-11-08
Estimated Expiration
2042-05-09

AI Technical Summary

Technical Problem

In the process of increasing the energy density of lithium-ion batteries, they lead to problems of electron polarization and ion polarization. The electrode sheets are insufficient in thermal conductivity, making it easy to cause accidents such as heating, fire, combustion or explosion.

Method used

Using aluminum foam as the current collector of the positive electrode material, the positive electrode material is embedded in a three-dimensional grid, and using aluminum coated carbon foam as the current collector of the negative electrode material, the negative electrode material is embedded in a three-dimensional grid of aluminum coated carbon foam, through extrusion and rolling Technology prepares electrode sheets, combining diaphragm separation and multi-sheet assembly processes.

Benefits of technology

Lithium-ion batteries with high energy density, light weight and avoid lithium corrosion are achieved, which improves the service life and safety of the device, increases the energy density by 8% to 38%, extends the service life by 30% to 300%, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a lithium-ion battery and a preparation method thereof. The lithium-ion battery comprises a positive electrode plate and a negative electrode plate; the positive electrode plate comprises a positive electrode material and a positive electrode material current collector, the positive electrode material current collector is foamed aluminum, and the positive electrode material is embedded in the three-dimensional grid of the positive electrode material current collector; the negative electrode plate comprises a negative electrode material and a negative electrode material current collector, the negative electrode material current collector is carbon-coated foamed aluminum, and the negative electrode material is embedded in the three-dimensional grid of the negative electrode material current collector. The present invention adopts foamed aluminum as the positive electrode material current collector and carbon-coated foamed aluminum as the negative electrode material current collector. By matching the positive and negative electrodes, the lithium-ion battery has the advantages of high energy density, light weight, and can avoid lithium corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery preparation, and in particular relates to a high-performance lithium ion battery with a novel structure and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the advantage of high energy density and are widely used in automotive power batteries and mobile electronic consumer products. They are an important component of new energy. After years of development, lithium-ion batteries have formed mature positive electrode materials containing lithium compounds and negative electrode materials using various types of graphite carbon. In addition, relatively mature processing methods have been formed.

[0003] Currently, the more commonly used processing method is: mix the positive electrode material with a conductive agent, an adhesive, etc. to form a slurry, and apply it on an aluminum foil; mix the negative electrode material with an adhesive to form a slurry, and apply it on a copper foil; then weld the electrode ears, separate the diaphragms, and inject the electrolyte to form a finished battery.

[0004] At present, the development trend of lithium-ion batteries is to increase energy density as much as possible without losing its power density. However, for foil pole pieces, this means increasing the thickness of both the positive and negative electrodes, which brings serious problems of electronic polarization and ion polarization. At the same time, the thermal conductivity of the pole piece is not high, which often leads to heating, temperature runaway, electrolyte decomposition, fire, combustion or explosion when charging at high power or high current. Summary of the invention

[0005] In order to solve the above problems, the present invention aims to provide a lithium ion battery and a method for preparing the same. The above objects of the present invention can be achieved by the following technical solutions:

[0006] According to one aspect of the present invention, a lithium-ion battery provided by the present invention comprises: a positive electrode plate and a negative electrode plate, wherein the positive electrode plate comprises a positive electrode material and a positive electrode material current collector, the positive electrode material current collector is foamed aluminum, and the positive electrode material is embedded in a three-dimensional grid of the positive electrode material current collector; the negative electrode plate comprises a negative electrode material and a negative electrode material current collector, the negative electrode material current collector is carbon-coated foamed aluminum, and the negative electrode material is embedded in the three-dimensional grid of the negative electrode material current collector.

[0007] Optionally, the porosity of the foamed aluminum of the positive electrode material current collector is 85% to 96%; the porosity of the foamed aluminum used for the carbon-coated foamed aluminum of the negative electrode material current collector is 85% to 95%.

[0008] Optionally, the negative electrode sheet has the same length and width as the positive electrode sheet. Optionally, the positive electrode sheet has a thickness of 100 μm to 400 μm and a surface density of 50 mg / cm 2 ~200mg / cm2 Optionally, the thickness of the negative electrode plate is determined according to the thickness of the positive electrode plate and the positive and negative electrode energy matching principle. Optionally, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.01 to 1.15:1.

[0009] According to another aspect of the present invention, a method for preparing a lithium-ion battery provided by the present invention comprises: step S10, preparing a positive electrode slurry from a positive electrode material, using foamed aluminum as a positive electrode material current collector, filling the positive electrode slurry into a three-dimensional grid of the positive electrode material current collector, and preparing a positive electrode sheet; step S20, preparing a negative electrode slurry from a negative electrode material, using carbon-coated foamed aluminum as a negative electrode material current collector, filling the negative electrode slurry into a three-dimensional grid of the negative electrode material current collector, and preparing a negative electrode sheet.

[0010] Optionally, in step S10, the positive electrode slurry is filled into the three-dimensional grid of the positive electrode material collector by extrusion, rolled, and dried at 100° C. to 150° C. for 1 h to 20 h to prepare a positive electrode sheet. Optionally, the viscosity of the positive electrode slurry is 1000 to 10000 centipoise.

[0011] Optionally, in step S20, the negative electrode slurry is filled into the three-dimensional grid of the negative electrode material collector by extrusion, rolled, and dried at 100° C. to 150° C. for 1 h to 20 h to prepare a negative electrode sheet. Optionally, the viscosity of the negative electrode slurry is 1000 to 10000 centipoise.

[0012] Optionally, the step of preparing positive electrode material to obtain positive electrode slurry includes: weighing raw materials; mixing the raw materials to prepare positive electrode slurry; the raw materials, in terms of mass percentage, include: 90% to 97% positive electrode material, 1% to 5% conductive agent, and 2% to 8% binder.

[0013] Optionally, the particle size of the positive electrode material is 0.01 μm to 10 μm.

[0014] Optionally, the positive electrode material is one or more selected from lithium-containing compounds, and / or one or more selected from carbon-doped lithium-containing compounds.

[0015] Optionally, the step of preparing negative electrode material to obtain negative electrode slurry includes: weighing raw materials; mixing the raw materials to prepare negative electrode slurry; the raw materials, in terms of mass percentage, include: 90% to 97% negative electrode material, 1% to 5% conductive agent, and 2% to 7% binder.

[0016] Optionally, the particle size of the negative electrode material is 0.01 μm to 10 μm.

[0017] Optionally, the negative electrode material is one or more of graphite, graphite-like carbon, mesophase carbon microbeads, silicon, tin, silicon-carbon material, silicon-oxygen-carbon material, lithium titanate, and metallic lithium material.

[0018] Optionally, the method for preparing the lithium-ion battery further includes: step S30, welding the positive electrode tab and the negative electrode tab of the positive electrode sheet and the negative electrode sheet respectively, separating them with a diaphragm, assembling multiple sheets, encapsulating them in a shell, and injecting electrolyte after dehydration and degassing to prepare a lithium-ion battery.

[0019] Optionally, before the step of welding the negative electrode tab to the negative electrode sheet, the method further includes: cutting the negative electrode sheet according to the size of the positive electrode sheet, applying glue to the cut surface, and heating and curing.

[0020] Optionally, the step of welding the positive electrode sheet and the negative electrode sheet to the positive electrode tab and the negative electrode tab respectively includes: directly reserving a sufficient area on the positive electrode sheet, pressing, and welding it to the positive electrode tab; directly reserving a sufficient area of ​​foam aluminum on the negative electrode sheet, pressing, and welding it to the negative electrode tab.

[0021] Beneficial effects: The present invention uses aluminum foam as the current collector of the positive electrode material, and embeds the positive electrode material in the three-dimensional grid of the aluminum foam current collector to form a high-power, high-energy positive electrode plate; at the same time, carbon-coated aluminum foam made of carbon-coated aluminum foam is used as the current collector of the negative electrode material, and the negative electrode material is embedded in the three-dimensional grid of the carbon-coated aluminum foam. The strict carbon layer protects the aluminum foam from being corroded by lithium, and at the same time significantly reduces the weight of the negative electrode and the overall device, and cooperates with the high-performance positive electrode to realize a high-energy-density lithium-ion battery. The lithium-ion battery has the advantages of high energy density, light weight, and avoidance of lithium corrosion. DETAILED DESCRIPTION

[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The present invention provides a lithium-ion battery, wherein foamed aluminum is used as the positive electrode material collector in the positive electrode plate, and carbon-coated foamed aluminum is used as the negative electrode material collector in the negative electrode plate; thereby the energy density of the lithium-ion battery is increased and the service life of the device is prolonged. It is mainly used for energy-type batteries, and the energy density of the device is 8% to 38% higher than that of the device with the negative electrode currently processed with copper foil, and the service life is prolonged by 30% to 300%.

[0024] The present invention is a lithium-ion battery with a new structure and high performance, wherein the positive electrode plate is formed by embedding the positive electrode material into a three-dimensional grid of aluminum foam to form a fixed composite structure. The negative electrode plate is formed by embedding the negative electrode material into a three-dimensional grid of carbon-coated aluminum foam to form a fixed composite structure. Aluminum foam is used as a current collector for positive electrode material, and the positive electrode material is embedded into the three-dimensional grid of aluminum foam to form a thicker positive electrode plate, thereby increasing the energy density of the positive electrode side and maintaining the power density; carbon-coated aluminum foam is used as a current collector for negative electrode material, and the negative electrode material is embedded into the three-dimensional grid of carbon-coated aluminum foam. The tight carbon layer protects the aluminum foam from corrosion, and at the same time significantly reduces the weight of the negative electrode and the overall device. By cooperating with a high-performance positive electrode, a lithium-ion battery with high energy density is achieved.

[0025] The present invention provides a method for preparing a lithium-ion battery, comprising: preparing a positive electrode material to obtain a positive electrode slurry, using aluminum foam as a positive electrode material current collector, filling the positive electrode slurry into the three-dimensional grid of the positive electrode material current collector, and preparing a positive electrode sheet; preparing a negative electrode material to obtain a negative electrode slurry, using carbon-coated aluminum foam as a negative electrode material current collector, and filling the negative electrode slurry into the three-dimensional grid of the negative electrode material current collector, and preparing a negative electrode sheet. The method can be applied to the processing of a variety of positive and negative electrode materials with different particle sizes, and has the advantages of flexible structure, convenient processing, etc.; the device has the advantages of high energy density, long service life, and low cost.

[0026] In an optional embodiment, a method for preparing a lithium-ion battery includes:

[0027] Step S10, weighing raw materials, mixing, preparing positive electrode slurry, controlling the viscosity to be 1000-10000 centipoise; filling the positive electrode slurry into the three-dimensional grid of the positive electrode material collector by extrusion, and making the two in close contact by rolling; drying at 100°C-150°C for 1h-20h to form a positive electrode sheet.

[0028] The thickness of the positive electrode sheet is 100 μm to 400 μm, and the surface density is 50 mg / cm 2 ~200mg / cm 2 The thickness of the negative electrode sheet is made by filling the negative electrode material in carbon-coated aluminum foam according to the principle of energy matching between the positive and negative electrodes; and the energy ratio of the single negative electrode to the single positive electrode is controlled to be 1.01:1 to 1.15:1. The positive electrode material current collector is aluminum foam, and its porosity is 85% to 96%.

[0029] The raw materials, in terms of mass percentage, include: 90% to 97% positive electrode material, 1% to 5% conductive agent, and 2% to 8% binder. The particle size of the positive electrode material is 0.01 μm to 10 μm. The positive electrode material is one or more selected from lithium-containing compounds, and / or one or more selected from carbon-doped lithium-containing compounds. Further, the positive electrode material includes lithium-containing compounds that can be subjected to bulk redox charging and lithium-containing compounds doped with carbon materials; for example, one or more of lithium iron phosphate and its doped materials, lithium manganate and its doped materials, lithium nickel cobalt manganate, lithium nickel cobalt aluminum oxide, lithium-rich solid solution materials, polyanion materials (such as lithium orthosilicate ion type, lithium titanium phosphate type, etc.), and necessary carbon-coated compounds). The conductive agent is a carbon material. The binder can be, for example, a common glue.

[0030] Step S20, weighing the raw materials, mixing them, preparing the negative electrode slurry, and controlling the viscosity to be 1000-10000 centipoise; determining the amount of the negative electrode material according to the capacity of the positive electrode plate, filling it into the three-dimensional grid of the carbon-coated foam aluminum current collector by extrusion, and making the two in close contact by rolling, and drying at 100°C-150°C for 1h-20h to form a negative electrode plate with controllable thickness.

[0031] The negative electrode sheet has the same length and width as the positive electrode sheet, and the capacity ratio of the negative electrode sheet to the positive electrode sheet is 1.01 to 1.15: 1. The negative electrode material current collector is carbon-coated foamed aluminum, which is obtained by coating a carbon layer on the surface of the foamed aluminum, wherein the porosity of the foamed aluminum is 85% to 95%.

[0032] The raw materials, by mass percentage, include: 90% to 97% of negative electrode material, 1% to 5% of conductive agent, and 2% to 7% of binder. The negative electrode material is one or more of graphite, graphite-like carbon, mesophase carbon microspheres, silicon, tin, silicon-carbon material, silicon-oxygen-carbon material, lithium titanate, and metallic lithium material. The particle size of the negative electrode material is 0.01 μm to 10 μm. The conductive agent is a carbon material.

[0033] Step S30, for the side of the cut negative electrode plate, apply glue to cover the exposed aluminum, heat and cure for protection. The positive electrode plate and the negative electrode plate are welded to the positive electrode tab and the negative electrode tab respectively, separated by a diaphragm, and assembled in multiple pieces. The aluminum-plastic film or metal shell is stamped to form a shell, and the assembled electrode plate is encapsulated in the shell. After dehydration and degassing steps, a commercially available electrolyte, such as lithium hexafluorophosphate electrolyte, is injected for aging and packaging to form a lithium-ion battery product. Among them, when welding the tabs, the positive electrode plate is directly reserved for a part of the sufficient area, pressed, and welded with the positive electrode tab. The positive electrode tab is a metal tab, such as aluminum, steel, nickel and other materials. The negative electrode plate is directly reserved for a part of the sufficient foam aluminum area, pressed, and welded with the negative electrode tab. The negative electrode tab is a metal tab, such as copper, steel, nickel and other materials.

[0034] In the above optional embodiments, the performance of the lithium-ion battery is optimized by optimizing each step and its parameters. Among them, the positive electrode material collector uses foamed aluminum, and its porosity is controlled to be 85% to 96%, and the negative electrode material collector uses carbon-coated foamed aluminum, and the porosity of the foamed aluminum used is controlled to be 85% to 95%, which can not only obtain a higher surface density of active materials, but also increase the conductivity of the electrolyte; by controlling the capacity ratio of the negative electrode plate to the positive electrode plate to 1.01:1 to 1.15, the device performance can be optimized; by controlling the particle size of the positive electrode material and the negative electrode material to 0.01μm to 10μm, the rate performance is improved.

[0035] The technical solution of the present invention is further described below in conjunction with specific embodiments:

[0036] Example 1

[0037] 93% positive electrode material (lithium manganate, average particle size 0.5-10 microns), 3% conductive agent (carbon nanotubes) and 4% glue are made into positive electrode slurry (viscosity 10000 centipoise). It is filled into the three-dimensional grid of the foam aluminum current collector (porosity 95%) by extrusion, and the two are closely contacted by rolling. Dry at 100°C for 20 hours to form a positive electrode sheet. The thickness is 100 microns and the surface density is 90 mg / cm 2 .

[0038] 94% negative electrode material (graphite, particle size 5-10 microns), 3% conductive agent (carbon black) and 3% glue are made into negative electrode slurry (viscosity 10000 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 95%), and the two are closely contacted by rolling, and dried at 100°C for 20 hours to form a negative electrode plate with controllable thickness. Among them, for the side of the cut negative electrode plate (which may expose aluminum), it is coated with glue, heated and cured, and protected. Make the length and width of the negative electrode plate consistent with the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.01:1.

[0039] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode tab (aluminum) and the negative electrode tab (copper) respectively, separated by a diaphragm, and assembled in multiple pieces; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell, and after dehydration and degassing steps, an electrolyte is injected, and the electrolyte is a lithium hexafluorophosphate type electrolyte, and aging and packaging are performed to form a lithium-ion battery product.

[0040] According to tests, compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density of the lithium ion battery of this embodiment is increased by 20% and the device life is increased by 30%.

[0041] Example 2

[0042] 94.5% positive electrode material (carbon-coated lithium iron phosphate, average particle size 5-6 microns), 2.5% conductive agent (carbon black) and 3% glue are made into positive electrode slurry (viscosity 10,000 centipoise); it is filled into the three-dimensional grid of the foam aluminum current collector (porosity 95%) by extrusion, and the two are closely contacted by rolling. Dry at 105°C for 8 hours to form a positive electrode sheet. The thickness is 100 microns and the surface density is 180 mg / cm 2 .

[0043] 96.5% negative electrode material (30% graphite, 60% mesophase carbon microspheres and 10% silicon carbon material, particle size 5-10 microns), 1.5% conductive agent (carbon nanotubes) and 2% glue are made into negative electrode slurry (viscosity 5000 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 95%), and the two are closely contacted by rolling, and dried at 115°C for 8 hours to form a negative electrode plate with controllable thickness. For the side of the cut negative electrode plate (which may expose aluminum), it is coated with glue, heated and cured, and protected. The length and width of the negative electrode plate are consistent with the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.15:1.

[0044] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode tab (aluminum) and the negative electrode tab (copper) respectively, separated by a diaphragm, and multiple sheets are assembled; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell. After dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0045] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 8% and the device life is increased by 55%.

[0046] Example 3

[0047] 97% positive electrode material (nickel cobalt manganese oxide material, average particle size 2-6 microns), 1% conductive agent (10% graphene and 70% carbon nanotubes, 20% carbon black) and 2% glue are made into positive electrode slurry (viscosity 4000 centipoise); it is filled into the three-dimensional grid of foam aluminum current collector (porosity 95%) by extrusion, and the two are closely contacted by rolling. Dry at 110°C for 16 hours to form a positive electrode sheet. The thickness is 200 microns and the surface density is 100 mg / cm 2 .

[0048] 97% negative electrode material (90% graphite and 10% silicon oxygen carbon material, particle size 5-10 microns), 1% conductive agent (carbon nanotubes) and 2% glue are made into negative electrode slurry (viscosity 5000 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 95%), and the two are closely contacted by rolling, and dried at 108°C for 5 hours to form a negative electrode plate with controllable thickness. Among them, the side of the cut negative electrode plate (which may expose aluminum) is coated with glue, heated and cured, and protected. The length and width of the negative electrode plate are consistent with those of the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.05:1.

[0049] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode ear (steel) and the negative electrode ear (copper) respectively, separated by a diaphragm, and multiple sheets are assembled; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell. After dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0050] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 12% and the device life is increased by 120%.

[0051] Example 4

[0052] 95% positive electrode material (nickel cobalt aluminum lithium material, average particle size 2-4 microns), 3% conductive agent (50% carbon nanotubes, 50% carbon black) and 2% glue are made into positive electrode slurry (viscosity 4000 centipoise); it is filled into the three-dimensional grid of foam aluminum current collector (porosity 95%) by extrusion, and the two are closely contacted by rolling. Dry at 100°C for 6 hours to form a positive electrode sheet. The thickness is 400 microns and the surface density is 50mg / cm 2 .

[0053] 96% negative electrode material (90% graphite and 10% silicon oxygen carbon material, particle size 5-10 microns), 2% conductive agent (carbon nanotubes) and 2% glue are made into negative electrode slurry (viscosity 5000 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 85%), and the two are closely contacted by rolling, and dried at 120°C for 1 hour to form a negative electrode plate with controllable thickness. For the side of the cut negative electrode plate (which may expose aluminum), it is coated with glue, heated and cured, and protected. The length and width of the negative electrode plate are consistent with the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.04:1.

[0054] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode ear (steel) and the negative electrode ear (nickel) respectively, separated by a diaphragm, and multiple sheets are assembled; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell. After dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0055] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 20% and the device life is increased by 105%.

[0056] Example 5

[0057] 93% positive electrode material (lithium-rich manganese-based solid solution, average particle size 0.5-2 microns), 4% conductive agent (50% carbon nanotubes, 50% graphene) and 3% glue are made into positive electrode slurry (viscosity 2000 centipoise); it is filled into the three-dimensional grid of foam aluminum current collector (porosity 85%) by extrusion, and the two are closely contacted by rolling. Dry at 110°C for 15 hours to form a positive electrode sheet. The thickness is 200 microns and the surface density is 80 mg / cm2.

[0058] 94% negative electrode material (metal lithium particles, particle size 0.5-1 micron), 3% conductive agent (carbon nanotubes) and 3% glue are made into negative electrode slurry (viscosity 6000 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 95%), and the two are closely contacted by rolling, and dried at 100°C for 15 hours to form a negative electrode plate with controllable thickness. The side of the cut negative electrode plate is coated with glue, heated and cured, and protected. The length and width of the negative electrode plate are consistent with the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.1:1.

[0059] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode ear (steel) and the negative electrode ear (steel) respectively, separated by a diaphragm, and assembled in multiple pieces; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell, and after dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0060] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 30% and the device life is increased by 150%.

[0061] Example 6

[0062] 95% positive electrode material (polyanion material, such as lithium titanium phosphate, average particle size 0.1-6.5 microns), 1% conductive agent (50% carbon nanotubes, 50% graphene) and 4% glue are made into positive electrode slurry (viscosity 2000 centipoise); it is filled into the three-dimensional grid of the foam aluminum current collector (porosity 92%) by extrusion, and the two are closely contacted by rolling. Dry at 120°C for 3 hours to form a positive electrode sheet. The thickness is 300 microns and the surface density is 200 mg / cm 2 .

[0063] 95% negative electrode material (80% graphite-like carbon and 20% tin, particle size 0.2-0.8 microns), 1% conductive agent (carbon black) and 4% glue are made into negative electrode slurry (viscosity 6000 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 92%), and the two are closely contacted by rolling, and dried at 100°C for 20 hours to form a negative electrode plate with controllable thickness. The side of the cut negative electrode plate is coated with glue, heated and cured, and protected. The length and width of the negative electrode plate are consistent with the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.05:1.

[0064] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode tab (aluminum) and the negative electrode tab (copper) respectively, separated by a diaphragm, and multiple sheets are assembled; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell. After dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0065] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 35% and the device life is increased by 250%.

[0066] Example 7

[0067] 92% of the positive electrode material (LiNi 0.5 Mn 1.5 O4, particle size 2-5 microns), 3% conductive agent (50% carbon nanotubes, 50% graphene) and 5% glue are used to make positive electrode slurry (viscosity 5600 centipoise); it is filled into the three-dimensional grid of the foam aluminum current collector (porosity 96%) by extrusion, and the two are closely contacted by rolling. Dry at 140°C for 8 hours to form a positive electrode sheet. The thickness is 150 microns and the surface density is 150 mg / cm 2 .

[0068] 90% negative electrode material (silicon material, particle size 0.2-2 microns), 3% conductive agent (carbon black) and 7% glue are made into negative electrode slurry (viscosity 8200 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 92%), and the two are closely contacted by rolling, and dried at 128°C for 10 hours to form a negative electrode plate with controllable thickness. The side of the cut negative electrode plate is coated with glue, heated and cured, and protected. The length and width of the negative electrode plate are consistent with the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.08:1.

[0069] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode tab (aluminum) and the negative electrode tab (copper) respectively, separated by a diaphragm, and multiple sheets are assembled; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell. After dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0070] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 10% and the device life is increased by 300%.

[0071] Example 8

[0072] 90% positive electrode material (polyanion material (Li2MnSiO4), particle size 1-5 microns), 2% conductive agent (90% carbon black, 10% graphene) and 8% glue are made into positive electrode slurry (viscosity 3600 centipoise); it is filled into the three-dimensional grid of foam aluminum current collector (porosity 92%) by extrusion, and the two are closely contacted by rolling. Dry at 120℃ for 10 hours to form a positive electrode sheet. The thickness is 300 microns and the surface density is 120mg / cm 2 .

[0073] 90% negative electrode material (lithium titanate material, particle size 2-10 microns), 3% conductive agent (carbon black) and 7% glue are made into negative electrode slurry (viscosity 4800 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 92%), and the two are closely contacted by rolling, and dried at 130°C for 10 hours to form a negative electrode plate with controllable thickness. The side of the cut negative electrode plate is coated with glue, heated and cured, and protected. The length and width of the negative electrode plate are consistent with the positive electrode plate; in terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.02:1.

[0074] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode tab (aluminum) and the negative electrode tab (copper) respectively, separated by a diaphragm, and multiple sheets are assembled; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell. After dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0075] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 28% and the device life is increased by 100%.

[0076] Example 9

[0077] 89% positive electrode material (polyanion material, Li2FeSiO4, particle size 0.5-5 microns), 5% conductive agent (50% carbon nanotubes, 50% graphene) and 6% glue are made into positive electrode slurry (viscosity 3600 centipoise); it is filled into the three-dimensional grid of foam aluminum current collector (porosity 92%) by extrusion, and the two are closely contacted by rolling. Dry at 150°C for 1 hour to form a positive electrode sheet. The thickness is 170 microns and the surface density is 90 mg / cm 2 .

[0078] 85% negative electrode material (silicon carbon material, particle size 2-7 microns), 5% conductive agent (carbon black) and 10% glue are made into negative electrode slurry (viscosity 6800 centipoise). According to the capacity of the positive electrode plate, the amount of negative electrode material is determined, and it is filled into the three-dimensional grid of the carbon-coated foam aluminum current collector (porosity 92%), and the two are closely contacted by rolling, and dried at 150°C for 1 hour to form a negative electrode plate with controllable thickness. The side of the cut negative electrode plate is coated with glue, heated and cured, and protected. Make the negative electrode plate consistent with the positive electrode plate in length and width. In terms of capacity, the capacity ratio of the negative electrode plate to the positive electrode plate is 1.08:1.

[0079] The positive electrode sheet and the negative electrode sheet are welded to the positive electrode ear (aluminum) and the negative electrode ear (steel) respectively, separated by a diaphragm, and multiple sheets are assembled; an aluminum-plastic film or a metal shell is stamped to form a shell, and the assembled electrode sheets are packaged in the shell. After dehydration and degassing steps, an electrolyte (lithium hexafluorophosphate type electrolyte) is injected, and aging and packaging are performed to form a lithium-ion battery product.

[0080] Compared with batteries of the same weight (same positive electrode) using copper foil current collectors, the energy density is increased by 38% and the device life is increased by 200%.

[0081] The above embodiments of the present invention also have the following advantages and beneficial effects:

[0082] 1) The present invention uses aluminum foam as the current collector on the positive electrode side to form a thicker pole piece, improve the energy density of the positive electrode side, and maintain the power density; the carbon-coated aluminum foam current collector is used on the negative electrode side, which can not only match well with the positive electrode using aluminum foam, but also significantly reduce the weight of the negative electrode and the overall device because it is less dense than copper foil or copper foam, so that the energy density of the device is increased by 8% to 38%; and a large amount of copper resources are saved. Thus, the problem of poor negative electrode performance existing in the existing use of copper foil as the negative electrode current collector is overcome; the problem of heavy device weight existing in the existing use of copper foam as the negative electrode current collector is overcome; and the problem of aluminum being unstable and unusable on the negative electrode side is solved.

[0083] 2) The present invention uses a carbon-coated aluminum foam current collector on the negative electrode side. The three-dimensional carbon-coated aluminum foam current collector provides a three-dimensional electrical and thermal conductivity, making the internal temperature of the device more uniform during rapid charging and discharging; at the same time, the strict carbon layer protects the aluminum foam to avoid corrosion by the electrolyte, thereby increasing the life of the device by 50% to 100%.

[0084] 3) The present invention adopts carbon-coated aluminum foam current collector on the negative electrode side. Carbon-coated aluminum foam has both chemical stability and processing rigidity. Compared with the full carbon current collector, the present invention is easier to implement industrially; the product consistency is high, and the manufacturing cost is reduced by about 80%. It solves the problems of poor welding polarity, poor repeatability of the preparation process, easy deformation of the structure in the electrolyte, inability to withstand rolling, and lack of consistency for large-scale industrial sheeting in the full carbon current collector.

[0085] 4) The three-dimensional carbon-coated aluminum foam on the negative electrode side of the present invention has a large number of pores in its structure, which allows the volume expansion of the negative electrode material when embedded with lithium, protects the overall structure of the device from deformation, and extends the service life by 200% to 300%.

[0086] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.

Claims

1. A lithium-ion battery, It is characterized in that include: Positive electrode sheet and negative electrode sheet, wherein, The positive electrode sheet comprises a positive electrode material and a positive electrode material current collector, the particle size of the positive electrode material is 0.01 μm to 10 μm, the positive electrode material current collector is foamed aluminum, the positive electrode material is embedded in the three-dimensional grid of the positive electrode material current collector, and the porosity of the foamed aluminum is 85% to 96%; The negative electrode plate comprises a negative electrode material and a negative electrode material current collector, wherein the particle size of the negative electrode material is 0.01 μm to 10 μm, the negative electrode material current collector is carbon-coated foamed aluminum, which is obtained by coating a carbon layer on the surface of the foamed aluminum, and the porosity of the foamed aluminum used is 85% to 95%, and the negative electrode material is embedded in the three-dimensional grid of the negative electrode material current collector; the capacity ratio of the negative electrode plate to the positive electrode plate is 1.01 to 1.15:1; The thickness of the positive electrode sheet is 100 μm to 400 μm, and the surface density is 50 mg / cm 2 ~200mg / cm 2 ; The thickness of the negative electrode plate is determined according to the thickness of the positive electrode plate and the positive and negative electrode energy matching principle; The negative electrode sheet has the same length and width as the positive electrode sheet and is cut according to the size of the positive electrode sheet, and the cut surface of the negative electrode sheet has a heat-cured glue layer.

2. A method for preparing a lithium ion battery according to claim 1, It is characterized in that include: Step S10, preparing a positive electrode slurry from a positive electrode material, using foamed aluminum as a positive electrode material current collector, and filling the positive electrode slurry into a three-dimensional grid of the positive electrode material current collector to prepare a positive electrode sheet; Step S20, preparing a negative electrode slurry from a negative electrode material, using carbon-coated aluminum foam as a negative electrode material current collector, and filling the negative electrode slurry into a three-dimensional grid of the negative electrode material current collector to prepare a negative electrode sheet; Step S30, welding the positive electrode tab and the negative electrode tab of the positive electrode sheet and the negative electrode sheet respectively, separating them with a diaphragm, assembling multiple sheets, packaging them in a shell, and injecting electrolyte after dehydration and degassing to prepare a lithium-ion battery; Before the step of welding the negative electrode tab to the negative electrode sheet, the method further includes: cutting the negative electrode sheet according to the size of the positive electrode sheet, applying glue to the cut surface, and heating and curing the cut surface.

3. The method for preparing a lithium ion battery according to claim 2, It is characterized in that In step S10, the positive electrode slurry is filled into the three-dimensional grid of the positive electrode material collector by extrusion, and then rolled and dried at 100° C. to 150° C. for 1 h to 20 h to prepare a positive electrode sheet; wherein the viscosity of the positive electrode slurry is 1000 to 10000 centipoise; In step S20, the negative electrode slurry is filled into the three-dimensional grid of the negative electrode material collector by extrusion, rolled, and dried at 100° C. to 150° C. for 1 h to 20 h to prepare a negative electrode sheet; wherein the viscosity of the negative electrode slurry is 1000 to 10000 centipoise.

4. The method for preparing a lithium ion battery according to claim 2, It is characterized in that The step of preparing the positive electrode material to obtain the positive electrode slurry comprises: weighing raw materials; mixing the raw materials to prepare the positive electrode slurry; the raw materials, in terms of mass percentage, comprise: 90% to 97% of the positive electrode material, 1% to 5% of the conductive agent, and 2% to 8% of the binder; The positive electrode material is one or more selected from lithium-containing compounds, and / or one or more selected from carbon-doped lithium-containing compounds.

5. The method for preparing a lithium ion battery according to claim 2, It is characterized in that The step of preparing the negative electrode material to obtain the negative electrode slurry comprises: weighing raw materials; mixing the raw materials to prepare the negative electrode slurry; the raw materials, in terms of mass percentage, comprise: 90% to 97% of the negative electrode material, 1% to 5% of the conductive agent, and 2% to 7% of the binder; The negative electrode material is one or more of graphite, graphite-like carbon, mesophase carbon microspheres, silicon, tin, silicon-carbon material, silicon-oxygen-carbon material, lithium titanate, and metallic lithium material.

6. The method for preparing a lithium ion battery according to claim 2, It is characterized in that The steps of welding the positive electrode sheet and the negative electrode sheet to the positive electrode tab and the negative electrode tab respectively include: directly reserving a sufficient area on the positive electrode sheet, pressing, and welding it to the positive electrode tab; directly reserving a sufficient area of ​​the foam aluminum on the negative electrode sheet, pressing, and welding it to the negative electrode tab.