Multilayer structure, stand-up bag and method thereof

By curing ultraviolet or electron beam curable ink or varnish on the polyethylene-based polymer film of the self-standing bag, a multi-layer structure is formed, which solves the problems of self-standing bag stability and recycling, and achieves higher heat resistance and resistance Mechanical and chemical resistance improve the recyclability of polymer substrates.

CN114929476BInactive Publication Date: 2024-12-03BRASKEM SA +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080088936.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-22
Filing Date
2020-10-22
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing stand-up bags have shortcomings in stability and recycling, making it difficult to maintain the upright posture of the product on the shelves, and due to the differences in materials, it is difficult to effectively recycle.

Method used

Using a multi-layer structure, including a polyethylene-based polymer film, a sealing layer, an intermediate layer and a printing layer, and curing UV or electron beam curable ink or varnish on the printing layer of the polyethylene-based polymer film, providing a heat-resistant surface and chemical resistance, improving the heat resistance, mechanical resistance and chemical resistance of polymer substrates.

Benefits of technology

Achieves the stability of the stand-up bag, which can keep the sealing rod free of polymer in a sealing cycle of no more than 2 seconds, and exhibits higher durability during cold friction tests and chemical contacts, and improves polymer Recyclability of the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114929476B_ABST
    Figure CN114929476B_ABST
Patent Text Reader

Abstract

The multilayer structure may include: a polyethylene polymer film, the polyethylene polymer film including: a sealing layer; at least one intermediate layer; and a printing layer; and an outer layer of UV or electron beam curable ink or varnish cured on the printing layer of the polyethylene polymer substrate, wherein the multilayer structure has a heat-resistant surface so that when a sealing bar is applied to the polyethylene polymer film in a sealing cycle of no more than 2 seconds and at a temperature corresponding to the melting temperature of polyethylene, the sealing bar remains free of polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] In recent years, the use of flexible packaging for products such as consumer goods has increased due to the unique market benefits and resource efficiencies provided by such packaging. For example, compared to conventional bottles, cans, boxes, etc., flexible packaging provides a unique appeal to consumers, who may be more inclined to choose products contained therein over products in boxes or other packaging. In addition, flexible packaging is more resource efficient than its traditional packaging counterparts.

[0002] An example of such a flexible package is a stand-up pouch, which is increasingly used in commercial applications as packaging for consumer goods. These pouches are attractive to consumers and, when properly designed, allow a minimum amount of polymer material to be used very efficiently to prepare the package.

[0003] For example, stand-up pouches have a much higher product-to-packaging ratio than traditional packaging methods. As a result, manufacturers can reduce the resources and costs associated with packaging retail products (e.g., consumer goods) while promoting their packaging as "green" to attract eco-conscious consumers. However, conventional stand-up pouches use a laminate of polyethylene terephthalate (PET) layers and polyethylene (PE) layers, which makes the pouches difficult to recycle due to the different materials of construction.

[0004] Conventional stand-up pouches also have some disadvantages relative to traditional packaging methods and materials. One such disadvantage is the reduced stability exhibited by the stand-up pouch relative to its bottle, can or box counterpart. For example, particularly in the case of solid narrow products, the stand-up pouch may not exhibit adequate stability to maintain the product in an upright position on the shelf. Thus, if a stand-up pouch is used for such a product, the product may not sit upright on the shelf, or worse, may completely tip over, resulting in reduced visibility of the package and / or product to the consumer.

[0005] Thus, there continues to be a need for a stand-up pouch that exhibits the market and eco-friendly benefits of a stand-up pouch while also exhibiting improved stability. Summary of the invention

[0006] This Summary is provided to introduce a selection of concepts that are further described below in the Detailed Description. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.

[0007] In one aspect, embodiments disclosed herein relate to a multilayer structure (also referred to as a multilayer structure) comprising: a polyethylene polymer film, the polyethylene polymer film comprising: a sealing layer; at least one intermediate layer; and a print layer; and an outer layer of UV or electron beam curable ink or varnish cured on the print layer of the polyethylene polymer film, wherein the multilayer structure has a heat-resistant surface so that when a sealing bar is applied to the polyethylene polymer film in a sealing cycle of no more than 2 seconds and at a temperature corresponding to the melting temperature of the polyethylene polymer film, the sealing bar remains free of polymer.

[0008] In another aspect, embodiments disclosed herein relate to a stand-up bag comprising a multilayer structure comprising: a polyethylene polymer film comprising: a sealing layer; at least one intermediate layer; and a print layer; and an outer layer of UV or electron beam curable ink or varnish cured on the print layer of the polyethylene polymer film, wherein the multilayer structure has a heat-resistant surface so that when a sealing bar is applied to the polyethylene polymer film in a sealing cycle of no more than 2 seconds and at a temperature corresponding to the melting temperature of the polyethylene polymer film, the sealing bar remains free of polymer.

[0009] In another aspect, embodiments disclosed herein relate to a stand-up pouch comprising a plurality of panels, each panel being sealed to another panel and comprising: a polymer substrate; and an outer layer of UV or electron beam curable ink or varnish cured on a surface of the polymer substrate, wherein the polymer substrate having the UV or electron beam curable ink or varnish cured thereon meets at least one of the following criteria:

[0010] - a heat-resistant surface such that, when a sealing bar is applied to the plurality of panels in a sealing cycle not exceeding 2 seconds and at a temperature corresponding to the melting temperature of the polyethylene substrate, the sealing bar remains free of polymer;

[0011] - at least 30% more cold rub test cycles measured according to ASTM D5264 when subjected to the printed surface rub test as compared to a polymeric substrate having no UV or e-beam curable ink or varnish cured thereon; or

[0012] - Chemical resistance in an immersion test subjected to direct contact with one or more of soybean oil, 50% concentration of ethanol in water or polyoxyethylene (9) nonylphenyl ether for 24 hours.

[0013] In another aspect, the embodiments disclosed herein relate to a method for forming a multilayer structure, the method comprising: forming a polyethylene polymer film, the polyethylene polymer film comprising: a sealing layer; at least one intermediate layer; and a printing layer; applying a UV or electron beam curable ink or varnish to the printing layer; and irradiating the UV or electron beam curable ink or varnish with UV or electron beam radiation to form a multilayer structure, the multilayer structure comprising: a polyethylene polymer film, the polyethylene polymer film comprising: a sealing layer; at least one intermediate layer; and a printing layer; and an outer layer of UV or electron beam curable ink or varnish cured on the printing layer of the polyethylene polymer film, wherein the multilayer structure has a heat-resistant surface so that when a sealing bar is applied to the polyethylene polymer film in a sealing cycle of no more than 2 seconds and at a temperature corresponding to the melting temperature of the polyethylene polymer film, the sealing bar remains free of polymer.

[0014] In yet another aspect, embodiments disclosed herein relate to a method of forming a stand-up bag, the method comprising: applying a UV or electron beam curable ink or varnish onto a polymer substrate; irradiating the UV or electron beam curable ink or varnish with UV or electron beam radiation to form a multilayer structure; and sealing the multilayer structure to at least one other multilayer structure to form a stand-up bag, the stand-up bag comprising a plurality of panels, each panel being sealed to another panel and comprising: a polymer substrate; and an outer layer of UV or electron beam curable ink or varnish cured on a surface of the polymer substrate, wherein the polymer substrate having the UV or electron beam curable ink or varnish cured thereon meets at least one of the following criteria:

[0015] - a heat-resistant surface such that when a sealing bar is applied to the multilayer structure in a sealing cycle not exceeding 2 seconds and at a temperature corresponding to the melting temperature of the polyethylene substrate, the sealing bar remains free of polymer;

[0016] - at least 30% more cold rub test cycles measured according to ASTM D5264 when subjected to the printed surface rub test as compared to a polymeric substrate having no UV or e-beam curable ink or varnish cured thereon; or

[0017] - Chemical resistance in an immersion test subjected to direct contact with one or more of soybean oil, 50% concentration of ethanol in water or polyoxyethylene (9) nonylphenyl ether for 24 hours.

[0018] Other aspects and advantages of the claimed subject matter will be apparent from the following description and appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1-3 Various views of a stand-up pouch according to one or more embodiments of the present disclosure are shown.

[0020] Figure 4 The effect of different electron beam doses on the tensile strength of low density polyethylene is shown.

[0021] Figure 5 The effect of different electron beam doses on the elongation at break of low density polyethylene is shown.

[0022] Figure 6 The effect of different electron beam doses on the thermal deformation of low-density polyethylene is shown.

[0023] Figure 7 Electron absorption according to one or more embodiments of the present disclosure is shown.

[0024] Figure 8 Heat absorption according to one or more embodiments of the present disclosure is shown. DETAILED DESCRIPTION

[0025] In one aspect, embodiments disclosed herein relate to films including multilayer structures for use in packaging such as stand-up pouches. In particular, films and multilayer structures can have UV and / or electron beam curable inks or varnishes cured on their surfaces, which can not only provide graphics or finishes to the outer surface of the material, but can also result in improved heat resistance, mechanical resistance, and chemical resistance of the structure, thereby providing a material with properties that enable it to be used as, for example, a stand-up pouch.

[0026] Stand Up Pouch

[0027] The stand-up pouch can have various configurations, but a representative example of the configuration is shown in Figure 1-3 It is shown in Figure 1-3 The side view, top view and bottom view of an example stand-up bag are shown respectively. The stand-up bag 100 can be formed by a plurality of multilayer structures, which can include a front panel 110, a back panel 120 and a bottom gusset 130 disposed between the front panel 110 and the back panel 120. The front panel 110 and the back panel 120 can be sealed together along sealing areas A and C, and each of the front panel 110 and the back panel 120 can be sealed to the bottom gusset 130 at a sealing area B.

[0028] As will be appreciated by those skilled in the art, the stand-up pouch 100 is configured to be Figure 1The stand-up pouch 100 can be moved between a substantially flat state (i.e., when the stand-up pouch 100 does not contain a product) and a self-standing state (when the stand-up pouch contains a product). In the substantially flat state, the bottom gusset 130 can be folded along its center and sandwiched between the front panel 110 and the back panel 120.

[0029] The front panel 110, the back panel 120, and the bottom gusset 130 are sealed to each other along the periphery of the self-supporting bag 100 to form a closed interior with an opening. Therefore, the self-supporting bag 100 is configured to move between a flat substrate state and a self-supporting state, wherein when in the self-supporting state, it can contain a product in the closed interior with an opening. Specifically, the self-supporting bag 100 includes sealed portions A, B, C, and an unsealed portion (in Figure 1 indicated by white space in the figure).

[0030] The seals A, B, C may have sufficient thickness to create a strong, airtight and / or liquid-tight seal between the closed, open interior and exterior of the stand-up pouch 100. It is contemplated that the seals A, B, C may have the same dimensions, or may have different dimensions.

[0031] For example, in one or more embodiments, after placing a product (e.g., a consumer product) into the closed interior with an opening, the top sides of the front panel 110 and the back panel 120 can be sealed to each other. In such an embodiment, the user (e.g., a consumer) can eventually tear open this top seal to obtain the product therein. A cut (such as, for example, a "V" shaped tear cut) or other tear guides can be provided on either or both sides to assist the user in tearing open the bag.

[0032] In addition, in one or more embodiments, the stand-up bag can include a resealable zipper or the like and a seal at the top side of the stand-up bag 100. For example, the stand-up bag 100 can be sealed along the top side so that, for example, the consumer must tear the top seal to enter the closed interior with an opening in question. However, the stand-up bag 100 can also include a resealable zipper (for example, closer to the bottom side than the top seal) disposed below the top seal so that after the consumer enters the closed interior with an opening for the first time by removing the top seal, the consumer can repeatedly open and close the stand-up bag 100 using the resealable zipper. In view of the benefits of the present disclosure, without departing from the scope of the present disclosure, those skilled in the art will recognize a variety of other configurations suitable for sealing or removably sealing the top side of the stand-up bag. It is contemplated that the stand-up bag can include other features arranged at the top of the bag or on the front panel or rear panel, such as a rigid nozzle, by which the contents of the bag can be emptied. Additionally, while the foregoing figures show different panels sealed together, it is contemplated that more than two portions of a single panel may alternatively be sealed together to form a flexible packaging structure.

[0033] Films and multilayer structures

[0034] The panel of a stand-up bag or other flexible packaging can be formed by a film or multilayer structure, which includes a polymer substrate and a cured layer of ink or varnish applied to at least a portion of the polymer substrate. In particular, the ink or varnish of the present disclosure can be an outer layer on the surface opposite to the surface to be sealed together (with another panel) to form a packaging material. In particular, the ink or varnish can be an external printing in the case of a protective layer such as a conventional protective polyester layer without applying (or laminating) thereon. In one or more embodiments, the ink or varnish described herein can be applied to at least the part (region) to be sealed together of the polymer substrate, such as those described above for the example stand-up bag, but on the surface opposite to the surface to be sealed of the substrate. In one or more embodiments, the ink or varnish can be applied to the entire exposed surface of the polymer substrate. Such ink or varnish can optionally provide graphics or facings for packaging, so it can ideally make all, substantially all or most of one or more panels coated with external printing of ink or varnish. Advantageously, these inks or varnishes can also provide thermal, mechanical or chemical resistance to the underlying polymer substrate, which enables the polymer substrate to be suitable for packaging without the need to laminate two materials with different melting points to accommodate thermal resistance and seal strength, such as is conventionally achieved using a high temperature resistant outer polyester film.

[0035] UV or electron beam curable ink or varnish

[0036] Embodiments of the present disclosure may utilize UV ​​or electron beam curable inks or varnishes that are coated and cured on at least a portion of a polymer substrate (at least areas that may be subject to mechanical and thermal stresses, such as seals).

[0037] In one or more embodiments, the UV or electron beam curable ink or varnish can be a thermosetting material with high heat resistance, which can be used to protect the lower melting temperature polymer substrate coated with the ink or varnish from the mechanical and thermal stresses that may be experienced during the construction and sealing of the material into the package. The UV or electron beam curable ink or varnish can behave as a non-elastic filler, which does not impair the recyclability of the material (unlike laminating adhesives), and does not require a high heat and mechanical resistance film for structural protection or protection of the printed ink (which is usually performed by laminating a higher resistance film on the printed ink).

[0038] Examples of oligomers that can be used in the inks or varnishes described herein can include, but are not limited to, bisphenol A [4EO] diacrylate, polyethylene glycol 200 diacrylate (PEG200DA), polyethylene glycol 400 diacrylate (PEG400DA), polyethylene glycol 600 diacrylate (PEG600DA), tripropylene glycol diacrylate (TPGDA), bisphenol A [4EO] diacrylate, neopentyl glycol [2PO] diacrylate (NPGPODA), dipropylene glycol diacrylate (DPGDA), hexanediol [2EO] diacrylate (HD2EODA, hexanediol [2PO] diacrylate) Ester (HD2PODA), trimethylolpropane triacrylate (TMPTA), trimethylolpropane [3PO] triacrylate (TMP3POTA), trimethylolpropane [3EO] triacrylate (TMP3EOTA), trimethylolpropane [6EO] triacrylate (TMP9EOTA), trimethylolpropane [9EO] triacrylate (TMP9EOTA), pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol [5EO] tetraacrylate (PPTTA), pentaerythritol [5EO] tetraacrylate (PPTTA) and dipentaerythritol hexaacrylate (DPPA).

[0039] Other oligomer examples include, but are not limited to, acrylated epoxidized soybean oil (ESBOA), bisphenol A epoxy diacrylate, amine-modified epoxy acrylates, polyester diacrylates, polyester triacrylates, polyester tetraacrylates, fatty acid-modified polyester acrylates, amine-modified polyether acrylates, aliphatic polyurethane diacrylates, aliphatic polyurethane triacrylates, aliphatic polyurethane tetraacrylates, aromatic polyurethane diacrylates, aromatic polyurethane triacrylates, and aromatic polyurethane tetraacrylates.

[0040] In embodiments using UV-curable inks or varnishes, a photoinitiator may be present, such as 2-hydroxy-2-methyl-1-phenylpropanone, bis-acylphosphine oxide (BAPO), 1-hydroxycyclohexyl-phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-(dimethylamino)-4′-morpholinobutyrophenone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), ethyl (2,4,6-trimethylbenzoyl)-phenylphosphinate (TPO liquid), 2-isopropylthioxanthone, 2,4-diethylthioxanthone, 4,4′-bis(diethylamino)benzophenone, piperazine based aminoalkylphenone, polymerized methyl benzoylformate, poly(ethylene glycol)bis(p-dimethylaminobenzoate), or ethyl 4-(dimethylamino)benzoate.

[0041] In one or more embodiments, additives such as wetting agents, acrylated silicon, fillers such as precipitated silica, fumed silica, calcium carbonate, kaolinite can be used. In addition, waxes added to increase the coefficient of friction, such as polyethylene wax, paraffin wax, carnauba wax, etc. can also be used.

[0042] In addition, for embodiments involving inks, pigments may be present to provide color properties to the inks. For example, the inks may include components such as organic pigments such as CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 110, CI Pigment Yellow 150, CI Pigment Yellow 151, CI Pigment Yellow 155, CI Pigment Red 48, CI Pigment Red 48.1, CI Pigment Red 48.2, CI Pigment Red 48.3, CI Pigment Red 48.4, CI Pigment Red 57.1, CI Pigment Red 122, CI Pigment Red 168, CI Pigment Red 184, CI Pigment Blue 15.3, CI Pigment Blue 15.4, CI Pigment Black 7, CI Pigment Black 32, CI Pigment Green 7, CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 34, CI Pigment Orange 36, CI Pigment Violet 23, titanium dioxide, etc. In addition, in one or more embodiments, dispersants, pigment synergists, etc. are other additives that may be present in the ink formulations.

[0043] In specific embodiments where high stiffness in the package is desired, stiffness or rigidity in the ink may be desirable. In such embodiments, a rigid thermosetting ink or varnish may be used that may have visible cracks or fissures when the structure is subjected to a maximum elongation of 10% (the elongation being in any direction). Examples of such inks or varnishes may include high Tg low flexibility epoxy oligomers such as acrylated epoxidized soybean oil (ESBOA), bisphenol A epoxy diacrylate, or monomers such as TMPTA (trimethylolpropane triacrylate), TPGDA (tripropylene glycol diacrylate). In one or more embodiments, the ink or varnish may have a Tg of at least 30°C.

[0044] On the other hand, one or more embodiments of packaging may require greater flexibility (and the ability to withstand greater elongation), but do not cause unacceptable defects from an aesthetic point of view. In addition, in packaging including features such as nozzles or zippers, there may be irregularities in the panels sealed around these features, and when sealing the panels, these features may cause greater elongation and contraction in the sealed area. Therefore, in one or more embodiments, curable ink or varnish may include flexible thermosetting ink or varnish, which only shows visible cracks when the elongation of the structure (this elongation is in any direction) is not less than 10%. Such flexible ink may be able to withstand up to 20%, 40% or 60% elongation without tearing, cracks or cracks. Examples of such inks or varnishes include polyester-based oligomers, polyurethane-based oligomers, such as aliphatic polyurethane diacrylates or aliphatic polyurethane triacrylates, and / or ethoxylated or propoxylated monomers, such as TMP3EOTA (trimethylolpropane [3EO] triacrylate), TMP9EOTA (trimethylolpropane [9EO] triacrylate), TMP3POTA (trimethylolpropane [3PO] triacrylate). In one or more embodiments, the ink or varnish may have a Tg below 30°C.

[0045] Other exemplary formulations of ink or varnish compositions include those described in, for example, US Pat. Nos. 9,238,740, 9,404,000, and 8,729,147, each of which is incorporated by reference in its entirety.

[0046] In one or more embodiments, a water-based or solvent-based ink (non-UV or e-beam curable) can be applied to a polymer substrate, and then a UV or e-beam curable varnish layer can be applied over the ink and subsequently cured. In this embodiment, as well as other embodiments using a single print layer, it is contemplated that the varnish applied may include a glossy, matte, textured, or soft-touch varnish.

[0047] In one or more embodiments, the flexographic printing process, offset printing process or rotogravure printing process can be compatible with UV or electron beam drying systems for coating and then curing the ink or varnish. In a specific embodiment, rotogravure printing can be used when printing with water-based or solvent-based inks followed by varnish coating with electron beam curable varnishes.

[0048] In order to trigger the curing of curable ink or varnish, an electron beam intensity in the range of 20 kGv to 100 kGv, or ultraviolet radiation in the range of 25 mJ to 400 mJ can be used. In one or more embodiments, the electron beam intensity can have a lower limit of any one of 20, 30, 40, 50 or 60 kGv, and an upper limit of any one of 40, 50, 60, 70, 80, 90 or 100 kGv, wherein any lower limit can be used in combination with any upper limit. In one or more embodiments, ultraviolet radiation can have a lower limit of any one of 25, 50, 75, 100, 150 or 200 mJ, and an upper limit of any one of 200, 250, 300, 350 or 400 mJ, wherein any lower limit can be used in combination with any upper limit.

[0049] Polymer substrate

[0050] As mentioned above, conventional packaging may use multiple types of materials, resulting in a lack of recyclability of the materials. However, in one or more embodiments of the present disclosure, the polymer substrate can be at least substantially formed by a single material (or a combination of different types of single materials with different physical, chemical or optical properties, i.e., one or more polyethylenes, etc.) coated with ink or varnish thereon, thereby improving the recyclability of the structure without sacrificing performance. In one or more embodiments, the polymer substrate can be selected from polyethylene, polypropylene, polyester (such as but not limited to polylactic acid), polyamide or ethylene vinyl alcohol copolymer.

[0051] However, it is contemplated that the polymer substrate may comprise a blend of polyolefins, such as at least 70% by weight of at least one polyethylene blended with up to 30% by weight of at least one polypropylene, or at least 70% by weight of at least one polypropylene blended with up to 30% by weight of at least one polyethylene. It is contemplated that a multilayer film having one or more polyethylene layers and one or more polypropylene layers may be used, wherein there is a weight ratio such as 70 / 30 or 30 / 70. In another embodiment, such a multilayer film may be used: a multilayer film in which at least one ethylene vinyl alcohol accounting for up to 10% by weight or up to 5% by weight of the multilayer film is combined with at least one polyethylene accounting for at least 90% by weight or at least 95% by weight of the multilayer film. This multilayer film may be recyclable while also having high oxygen barrier properties (preventing oxidation of oxygen-sensitive foods such as oils). For example, in such an embodiment, an ethylene vinyl alcohol barrier layer may be used in combination with one or more polyethylene layers while maintaining recyclability. It is contemplated that in one embodiment, a polyamide barrier layer may be used in combination with one or more layers of at least one polyethylene.

[0052] In one or more embodiments, the at least one polyethylene used in the present disclosure may include at least one selected from the group consisting of high density polyethylene (HDPE), low density polyethylene (LDPE) and / or linear low density polyethylene (LLDPE), or combinations thereof.

[0053] While one or more embodiments may utilize petrochemical HDPE, LDPE, and / or LLDPE resins in the polymer substrate, in one or more specific embodiments, the polyethylene virgin resin may be bio-based.

[0054] Bio-based ethylene polymers (HDPE, LDPE and / or LLDPE) according to the present disclosure may include polyolefins containing a certain weight percentage of biologically derived monomers. Bio-based ethylene polymers and monomers derived from natural products can be distinguished from polymers and monomers obtained from fossil fuel sources (also known as petroleum-based polymers). Because bio-based materials are produced by actively reducing CO in the atmosphere, 2 sources that obtain or otherwise require less CO during production 2 Emissions, so such materials are generally considered to be "green" or renewable. Unlike those products obtained from fossil sources, the use of products derived from natural sources has become increasingly popular as an effective means to suppress the increase in atmospheric carbon dioxide concentrations, thereby effectively limiting the expansion of the greenhouse effect. Products thus obtained from natural raw materials differ from products from fossil sources in their renewable carbon content. This renewable carbon content can be confirmed by the method described in ASTM D 6866-18 technical specification, "Standard Test Methods for Determining the Biobased Content of Solid, Liquid, and Gaseous Samples Using Radiocarbon Analysis". Products obtained from renewable natural raw materials have the additional ability to be incinerated at the end of their life cycle and produce only non-fossil-derived CO. 2 nature.

[0055] Examples of bio-based ethylene-based polymers can include polymers generated from ethylene derived from natural sources, such as sugar cane and sugar beets, maple trees, date palms, sugar palms, sorghum, agave, starch, corn, wheat, barley, sorghum, rice, potatoes, cassava, sweet potatoes, algae, fruits, citrus fruits, cellulose-containing materials, wine, hemicellulose-containing materials, lignin-containing materials, cellulosic products, lignocellulosic products, wood, woody plants, straw, bagasse, sugar cane leaves, corn stover, wood waste, paper, polysaccharides (such as pectin, chitin, fructan, pullulan, etc.), and any combination thereof.

[0056] Bio-based materials can be processed by any suitable method to produce ethylene, such as producing ethanol from sugar cane, and then ethanol is dehydrated to ethylene. In addition, it should also be understood that, in addition to ethanol, fermentation also produces higher alcohol by-products. If there are higher alcohol by-products during dehydration, higher olefin impurities may be formed together with ethanol. Therefore, in one or more embodiments, ethanol can be purified to remove higher alcohol by-products before dehydration, and in other embodiments, ethylene can be purified to remove higher olefin impurities after dehydration.

[0057] Biologically derived ethanol (referred to as bioethanol) for the production of ethylene can be obtained by fermenting sugars derived from cultures such as cultures of sugar cane and sugar beets or from hydrolyzed starch, which in turn is associated with other materials such as corn. It is envisioned that bio-based ethylene can be obtained from hydrolysis-based products from cellulose and hemicellulose, which are found in a variety of agricultural byproducts such as straw and sugar cane husks. This fermentation is carried out in the presence of various microorganisms, the most important of which is the presence of Saccharomyces cerevisiae. The ethanol thus obtained can be converted into ethylene by a catalytic reaction at temperatures generally above 300° C. Various catalysts can be used for this purpose, such as high specific surface area γ-alumina. Other examples include the teachings described in U.S. Patent Nos. 9,181,143 and 4,396,789, which are incorporated herein by reference in their entirety.

[0058] In one or more embodiments, the renewable carbon content of biobased products derived from natural materials can be certified according to the methods described in the technical standard ASTM D 6866-18, "Standard Test Methods for Determining the Biobased Content of Solid, Liquid, and Gaseous Samples Using Radiocarbon Analysis."

[0059] Bio-based resins according to the present disclosure, including bio-based HDPE, bio-based LDPE, and bio-based LLDPE, may include ethylene-containing resins having a bio-based carbon content (as determined by ASTM D6866-18 Method B) of at least 5% or having a lower limit of any one of 5%, 10%, 15%, 25%, 40%, and 50% and an upper limit selected from any one of 60%, 75%, 90%, 98%, and 100%, wherein any lower limit may be combined with any upper limit. In addition, it should also be noted that another polymer derived from a renewable source that can be used in one or more embodiments is polylactic acid, which, in addition to being formed from a renewable source, is also compostable.

[0060] In one or more embodiments, one or more of the ethylene polymer compositions comprises HDPE and / or LDPE and / or LLDPE (each of which may optionally be bio-based) having a melt index (measured according to ASTM D1238 at 190°C / 2.16kg) in the range of 0.5 to 2 g / 10min. In particular, the melt index may have a lower limit of any one of 0.25, 0.5, or 0.75 g / 10min to an upper limit of any one of 0.4, 0.5, 1, or 2 g / 10min, wherein any lower limit may be used in combination with any upper limit.

[0061] In one or more embodiments, one or more of the ethylene polymer compositions comprises a density (measured according to ASTM D 792) of 0.950 to 0.965 g / cm 3 HDPE (which may optionally be bio-based) in the range of 0.940, 0.950 and 0.955 g / cm 3 The lower limit of any one of them is 0.955, 0.960, 0.965 and 0.970 g / cm 3 Any lower limit may be used in combination with any upper limit.

[0062] In one or more embodiments, one or more of the ethylene polymer compositions comprises a density (measured according to ASTM D 792) of 0.910 to 0.930 g / cm 3 In particular, the density can be from 0.910, 0.916 and 0.920 g / cm 3 The lower limit of any one of them is 0.920, 0.925, 0.930, 0.935 and 0.940 g / cm 3 Any lower limit may be used in combination with any upper limit.

[0063] Although one or more embodiments can use a single layer polymer substrate, it is also contemplated that multiple layers, such as 2, 3, 5 or 7 layers, can be used. When using a multilayer polymer substrate, one or more embodiments can use a coextruded multilayer substrate, while other embodiments can use a laminated multilayer substrate, which can be laminated using a water-based, solvent-based or even solvent-free adhesive. In one or more embodiments, although the polymer substrate can be laminated, the ink or varnish coated and cured on the polymer substrate is the outer layer, and no additional lamination or film is applied thereto. In an embodiment with a thickness of less than 80 microns, a laminated structure can be particularly ideal, wherein one or more first layers can be laminated to one or more second layers having ultraviolet or electron beam curable ink or varnish already cured thereon. In such an embodiment, one or more first layers at least form a sealing layer, and one or more second layers at least form a printing layer.

[0064] In a specific embodiment, the polymer substrate may include a multilayer film having at least three layers: a sealing layer (for sealing to another film), an intermediate layer, and a printing layer (on which ink or varnish is applied and cured). For example, in one or more embodiments, the sealing layer may be formed to be 10% to 30% of the total thickness of the polymer substrate, and may be formed of 60% to 95% by weight of LLDPE (specifically, for example, metallocene LLDPE) and 5% to 40% by weight of LDPE. The intermediate layer may be formed to be 40% to 80% of the total thickness of the polymer substrate, and may be formed of 50% to 100% by weight of HDPE and up to 50% by weight of LLDPE (specifically, for example, metallocene LLDPE). The printing layer may be formed to be 10% to 30% of the total thickness of the polymer substrate, and may be formed of 50% to 100% by weight of HDPE and up to 50% by weight of LLDPE (specifically, for example, metallocene LLDPE). The weight % presented in this paragraph is based on the total weight of each layer in the multilayer film structure.

[0065] In one or more embodiments, the polymer substrate may include a multilayer film having at least five layers: a sealing layer (for sealing to another film), a first intermediate layer, a barrier layer, a second intermediate layer, and a printing layer (on which ink or varnish is applied and cured). For example, in one or more embodiments, the sealing layer may be formed to be 10% to 20% of the total thickness of the polymer substrate, and may be formed of 60% to 95% by weight of LLDPE (specifically, for example, metallocene LLDPE) and 5% to 40% by weight of LDPE. The first intermediate layer may be formed to be 15% to 30% of the total thickness of the polymer substrate, and may be formed of 50% to 100% by weight of HDPE and up to 50% by weight of LLDPE (specifically, for example, metallocene LLDPE). The barrier layer may be formed to be 5% to 20% of the total thickness of the polymer substrate, and may be formed of ethylene vinyl alcohol, or in a more specific embodiment, of 5% to 10% by weight of ethylene vinyl alcohol. The second intermediate layer may be formed to be 15% to 30% of the total thickness of the polymer substrate, and may be formed of 50% to 100% by weight of HDPE and up to 50% by weight of LLDPE (specifically, for example, metallocene LLDPE). The printing layer may be formed to be 10% to 20% of the total thickness of the polymer substrate, and may be formed of 50% to 100% by weight of HDPE and up to 50% by weight of LLDPE (specifically, for example, metallocene LLDPE). The weight % presented in this paragraph is based on the total weight of each layer in the multilayer film structure.

[0066] In addition, the polymer substrate can be formed from a polymer composition that can contain fillers and additives that change various physical and chemical properties when added to the polymer composition during blending, including one or more polymer additives such as processing aids, lubricants, antistatic agents, clarifiers, nucleating agents, β-nucleating agents, slip agents, antioxidants, compatibilizers, antacids, light stabilizers such as HALS, IR absorbers, brighteners, inorganic fillers, organic and / or inorganic dyes, anti-caking agents, processing aids, flame retardants, plasticizers, biocides, adhesion promoters, metal oxides, mineral fillers, flow aids, oils, antioxidants, antiozonants, accelerators and vulcanizing agents.

[0067] Multilayer structure performance

[0068] In one or more embodiments, the multilayer structure can have a thickness in the range of 50 to 250 microns, such as a lower limit of any one of 50, 60, 70, 80 or 100 microns, and an upper limit of any one of 120, 150, 200 or 250 microns, wherein any lower limit can be used in combination with any upper limit. In a specific embodiment, the stand-up bag can be constructed from a panel of a multilayer structure having a thickness in the range of 70 to 250 microns. In addition, in an embodiment using a laminated structure, the laminated film can have a thickness in the range of 50 to 100 microns.

[0069] As described above, the coating and curing of UV or electron beam curable ink or varnish on the surface of a polymer substrate can provide improved heat resistance, mechanical resistance and / or chemical resistance of the surface compared to a polymer substrate without cured ink or varnish. In one or more embodiments, the ink or varnish cured on the polymer substrate can result in performance differences across the thickness of the polymer substrate, so that the printed surface of the polymer substrate can exhibit improved performance, particularly relative to the sealing surface.

[0070] For example, the heat resistance of improvement can be confirmed during the sealing to each other of the panel of multilayer substrate or film.During such sealing operation, sealing bar can be used that panel is heated and sealed together.Although sealing bar can heat polymer substrate to the temperature that polymer substrate begins to melt (and is sealed together), the outer printing layer of thermosetting ink or varnish (at least in the region corresponding to the position of sealing bar) can change the thermal property of the printing surface of film, so that ink or varnish can prevent sealing bar from being polluted by molten polymer.In one or more embodiments, compared with the polymer substrate of UV or EB that do not solidify thereon, the heat resistance provided by UV or EB curable ink or varnish (once solidified on polymer substrate) can be increased to enough degree by the heat resistance of polymer substrate or protection, so that sealing bar can keep contacting with polymer substrate and carry out the sealing cycle of up to 2min, and there is no polymer melt on sealing bar (namely sealing bar keeps not containing polymer).

[0071] In one or more embodiments, thermal stability can be an increased heat resistance of the polymer substrate during the process of forming the stand-up pouch, enabling the processing temperature to be increased by at least 20°C, at least 40°C, or at least 60°C relative to the melt temperature of the polymer substrate without cured ink or varnish thereon.

[0072] Similarly, the presence of thermosetting ink or varnish can also be used to protect the multilayer structure or film from scratches by improving scratch resistance. In one or more embodiments, the cured ink or varnish can improve the surface resistance so that when the multilayer structure or film is subjected to a friction test, the cold friction test cycle measured according to ASTM D5264 is at least 30% more than the polymer substrate without the cured ink or varnish thereon. In a more specific embodiment, the film of the present invention having the cured ink or varnish thereon can be able to withstand a cycle of the lower limit of any one of 30%, 50%, 70% or 100%, or a cycle of the upper limit of any one of 100%, 125%, 150%, 175% or 200%, wherein any lower limit can be used in combination with any upper limit.

[0073] EB solidification causes polymerization or 3D reticulation or fracture on polymer molecules. In one or more embodiments, polymers can be reticulated with the increase of molecular size and the improvement of some properties thereof, which may lead to the increase of melting point, sealing temperature, tensile strength, while leading to the reduction of elongation, elongation at break and flexibility. This effect can be particularly present when polyethylene is used. Compared with heating itself, polyethylene may require more energy to change physical state. The heat of these two different states is recognized as sensible heat (heat perceived by generating temperature rise) and latent heat (heat consumed by promoting physical state change without temperature change). As an example, the sensible heat of polyethylene is 1.55 J / g℃, and the latent heat is 164 J / g. Therefore, about 162.75 J is consumed in order to heat each gram of PE from 25℃ to the average melting temperature of about 130℃ of medium-density PE. However, in addition to this, if heat is still supplied to up to 164 J / g in an adiabatic environment, no temperature change will be observed, but the physical state will change from solid to liquid (viscous).

[0074] Now refer to Figure 4-6 , Figure 4-6 The effect of electron beam radiation on the mechanical properties of low density polyethylene samples, particularly tensile strength and elongation at break (both measured according to ASTM D638), is illustrated. Figure 4 As shown, Figure 4 The correlation between electron beam dose and tensile strength increase is shown to be approximately 0.4 kgf / cm per kGV between 0 kGV and 100 kGV. 2 This improvement in the mechanical resistance of polyethylene caused by 3D polymerization due to EB radiation on the film can also provide benefits regarding the stability of the overall package during the stand-up pouch cycle formation.

[0075] Now refer to Figure 5 , Figure 5It is shown that the elongation at break of LDPE decreases from 570% to 437% at a rate of nearly 1.33% per kGy dose in the interval between 0 kGy and 100 kGy, with a total change in total elongation of 23%. Elongation at break is a property related to the elasticity of polyethylene. Elasticity is even more pronounced at higher temperatures, and the tendency of EB radiation to reduce the elasticity of PE is very beneficial to the production process of self-supporting bags, because the lower elasticity maintains the dimensional stability of the self-supporting bags during production.

[0076] Now refer to Figure 6 , Figure 6 The heat deformation of LDPE with EB dose is shown. In the heat deformation test, LDPE samples with a thickness of 3.0×1.5 cm×2 mm were subjected to a pulling force of 1 kg in an oven at 120°C, preheated for a total of 30 minutes before weight gain, and preheated for another 30 minutes after weight gain. The thickness change in % is considered as the heat deformation. The value of the non-irradiated LDPE is the standard value of 100%, and the thickness reduction decreases very significantly with increasing dose. Therefore, the inventors have found that irradiation with electron beams can significantly improve the properties of polymer substrates such as Figure 4-6 The heat resistance of low density polyethylene is shown in.

[0077] like Figure 7 As shown, during electron beam curing of ink or varnish, electrons are absorbed into the polymer substrate, and the absorption decreases as they travel deeper into the polymer substrate. This electron beam radiation can increase the melting temperature, sealing temperature and tensile strength of polymer substrates such as polyethylene. Although electron beam radiation is very capable of increasing the melting point of polyethylene through polymerization and crosslinking of molecules, the total amount of heat required to reach the melting point of polyethylene from room temperature and the total amount of heat required to melt the polyethylene at the melting temperature are very close. The inventors have found that when polyethylene is treated with an electron beam, the sum of these two characteristics produces a unique performance: the melting temperature of the film at the front several microns at the printing surface is increased, so that the consumption of incoming heat is reduced in the frontmost part of the film, and heat is saved for the deeper part of the film, where the sealing process will be carried out. Specifically, although the electron absorption is highest at the surface, as shown in FIG. Figure 8 As shown, the rate of heat absorption increases with depth. This result is due to the increased melting temperature in the upper portion of the substrate, thereby absorbing heat at a deeper location in the substrate where structural sealing will occur.

[0078] Therefore, not only does the UV or electron beam cure the ink and result in increased heat resistance of the polymer substrate, but the polymer substrate irradiated with EB can also have greater mechanical stability, which not only comes from increased tensile strength and reduced elongation at break, but also because energy concentration occurs at deeper locations in the polymer substrate adjacent to the seal, which also helps avoid cracks in the printed side of the structure.

[0079] Thus, in one or more embodiments, the ink or varnish, after curing, can provide the polymer substrate surface with mechanical strength to withstand the printed side x printed side rub test, at least 30% more cycles in the cold rub test according to ASTM D5264 compared to the same polymer surface without the ink or varnish discussed herein. In one or more embodiments, the film can withstand at least 50%, 100% and 200% more cycles in the cold rub test compared to the same polymer without the ink and varnish protection.

[0080] Thus, in one or more embodiments, the tensile strength of the currently described film can be increased by at least 10% after EB irradiation compared to the same structure before EB irradiation. In one or more embodiments, the tensile strength of the structure can be increased by 15%, 20%, 25% and 30%.

[0081] Thus, in one or more embodiments, the elongation at break of the currently described films can be reduced by at least 5% after EB irradiation compared to the same structure before EB irradiation. In one or more embodiments, the tensile strength of the structure can be reduced by 10%, 15%, 15%, 20%, and 25% compared to the same structure before EB irradiation.

[0082] Additionally, since the structure is envisioned for packaging, the structure must also be resistant to the product to be packaged therein. In one or more embodiments, the ink or varnish, after curing, can provide chemical resistance to the polymer substrate such that it can withstand direct contact with the product to be packaged in a cold 24h product immersion test without exhibiting mechanical displating, flaking, discoloration, or embrittlement. Although such tests are conventionally performed on the final product to be carried by the self-supporting bag, in accordance with the present disclosure, an immersion test can be performed on an example product. Specifically, such an immersion test can include immersing a sample of UV or EB-cured ink or varnish on a polymer substrate in an immersion bath at 25°C for 24 hours. The sample can be immersed in soybean oil, 50% concentration of ethanol in water, or a detergent (specifically polyoxyethylene (9) nonylphenyl ether (trade name CO-630 (sold)). After 24 hours, the samples were visually inspected. If the sample did not show mechanical delamination, flaking, discoloration or embrittlement in any of the three baths, it was considered "passed". In one or more embodiments, a sample of the membrane described herein can "pass" the immersion test in each of the three baths (one sample for each bath).

[0083] In one or more embodiments, the film may have a 45° angle gloss (measured according to ASTM D2457) ranging from greater than 5 points (matte) to 100 points (glossy).

[0084] In one or more embodiments, the film may have an Elmendorf tear strength (measured according to ASTM D 1922) greater than 30 gF in the machine direction (MD) and greater than 100 gF in the transverse direction (TD).

[0085] In one or more embodiments, the film may have a 1% secant tensile modulus (measured according to ASTM D882) greater than 350 MPa in the machine direction (MD) and greater than 400 MPa in the transverse direction (TD).

[0086] In one or more embodiments, the film may have a tensile strength at yield greater than 8 MPa in the machine direction and greater than 8 MPa in the cross direction (measured according to ASTM D 882).

[0087] In one or more embodiments, the film may have a tensile strength at break greater than 40 MPa in the machine direction (MD) and greater than 30 MPa in the transverse direction (TD) (measured according to ASTM D 882).

[0088] In one or more embodiments, the film may have a Plastic Film Impact Resistance by Free Falling Dart Method (measured according to ASTM D1709-01) of greater than 80 gf.

[0089] Although only some exemplary embodiments are described in detail above, it will be readily understood by those skilled in the art that a variety of changes are feasible in the exemplary embodiments without substantially departing from the present invention. Therefore, all such changes are intended to be included within the scope of the present disclosure as defined in the appended claims. In the claims, functionally defined statements are intended to cover structures described herein as performing the functions described, and not only structural equivalents, but also equivalent structures. Therefore, although nails and bolts may not be structural equivalents because nails use cylindrical surfaces to fasten wood parts together, while bolts use helical surfaces, nails and bolts may be equivalent structures in the context of fixing wood parts. It is the clear intention of the applicant not to invoke 35 U.S.C. § 112 (f) to impose any limitation on any of the claims herein, except for those in which the claims explicitly use the term "device for..." in conjunction with the relevant functions.

Claims

1. A recyclable multilayer structure for a stand-up pouch, the recyclable multilayer structure comprising a polymer substrate comprising a polyethylene layer, the polymer substrate being a multilayer polyethylene polymer film, the multilayer polyethylene polymer film comprising: a sealing layer comprising 5 to 40 wt % of a low density polyethylene and 50 to 95 wt % of a linear low density polyethylene; at least one intermediate layer comprising no more than 50 wt % linear low density polyethylene and 50 wt % to 100 wt % high density polyethylene; and a polyethylene-based printing layer comprising no more than 50% by weight of linear low-density polyethylene and 50% to 100% of high-density polyethylene; and an outer layer of UV or electron beam curable ink or varnish cured on said printed layer of said polyethylene based polymer film, wherein the multilayer structure has a heat resistant surface such that when a sealing bar is applied to the polyethylene-based polymer film in a sealing cycle of no more than 2 seconds and at a temperature corresponding to the melting temperature of the polyethylene-based polymer film, the sealing bar remains free of polymer, and wherein the polymer substrate comprises at least 70 wt% polyethylene.

2. The multilayer structure of claim 1, wherein the polyethylene-based polymer film further comprises a barrier layer between at least two intermediate layers.

3. The multilayer structure of claim 2, wherein the barrier layer comprises ethylene vinyl alcohol or polyamide.

4. The multilayer structure of any one of claims 1-3, wherein at least a portion of the polyethylene-based polymer film exhibits a bio-based carbon content of at least 50% as determined by ASTM D6866-18 Method B.

5. The multilayer structure of any one of claims 1-3, wherein the sealing layer, the at least one intermediate layer and the printing layer are coextruded together.

6. The multilayer structure of any one of claims 1 to 3, wherein the sealing layer, the at least one intermediate layer and the printing layer are laminated together.

7. The multilayer structure of any one of claims 1 to 3, wherein the polymer substrate having a UV or electron beam curable ink or varnish cured thereon meets at least one of the following criteria: - when subjected to the printed surface rub test, at least 30% more cold rub test cycles measured in accordance with ASTM D5264 than a polyethylene film having no UV or e-beam curable ink or varnish cured thereon; or - Chemical resistance in an immersion test subjected to direct contact with one or more of soybean oil, 50% ethanol in water or polyoxyethylene (9) nonylphenyl ether for 24 hours.

8. A stand-up bag comprising the multilayer structure according to any one of the preceding claims.

9. A recyclable stand-up bag, comprising: A plurality of panels, each panel being sealed to another panel, each panel comprising a multilayer structure and comprising: A polymer substrate, wherein the polymer substrate is a multilayer polyethylene-based polymer film, the multilayer polyethylene-based polymer film comprising a sealant layer, at least one intermediate layer, and a polyethylene-based print layer, wherein the sealant layer comprises 5 wt% to 40 wt% low density polyethylene and 50 wt% to 95 wt% linear low density polyethylene, the at least one intermediate layer comprises no more than 50 wt% linear low density polyethylene and 50 wt% to 100 wt% high density polyethylene, and the polyethylene-based print layer comprises no more than 50 wt% linear low density polyethylene and 50% to 100% high density polyethylene, wherein the polymer substrate comprises at least 70 wt% polyethylene; and an outer layer of UV or electron beam curable ink or varnish cured on the surface of the polymer substrate, Wherein the polymeric substrate having a UV or electron beam curable ink or varnish cured thereon meets at least one of the following criteria: - a heat-resistant surface such that when a sealing bar is applied to the plurality of panels in a sealing cycle not exceeding 2 seconds and at a temperature corresponding to the melting temperature of the polymer substrate, the sealing bar remains free of polymer; - when subjected to the Printed Side Rub Test, at least 30% more cold rub test cycles measured according to ASTM D5264 than a polymeric substrate having no UV or e-beam curable ink or varnish cured thereon; or - Chemical resistance in an immersion test subjected to direct contact with one or more of soybean oil, 50% ethanol in water or polyoxyethylene (9) nonylphenyl ether for 24 hours.

10. The stand-up pouch of claim 9, wherein the cured UV or electron beam curable varnish is coated on the water-based or solvent-based ink.

11. The stand-up pouch according to any one of claims 9 to 10, wherein the UV or electron beam curable ink or varnish is applied to at least a sealing area of ​​the multi-layer polyethylene-based polymer film.

12. The stand-up pouch of any one of claims 8-10, wherein the stand-up pouch comprises at least 70% by weight of at least one polyethylene and no more than 30% by weight of at least one polypropylene.

13. The stand-up pouch of claim 12, wherein the at least one polyethylene and at least one polypropylene are blended together in one layer.

14. The stand-up pouch of claim 12, wherein the at least one polyethylene and the at least one polypropylene are in different layers.

15. The stand-up pouch of any one of claims 8-10, wherein the stand-up pouch comprises at least 90% by weight of at least one polyethylene, and no more than 10% by weight of at least one ethylene vinyl alcohol in a different barrier layer.

16. The stand-up pouch of any one of claims 9-10, wherein the polymer substrate comprises at least two layers that are coextruded together.

17. The stand-up pouch of any one of claims 9-10, wherein the polymer substrate comprises at least two layers laminated together.

18. The stand-up pouch of claim 9, wherein the polyethylene-based polymer film further comprises a barrier layer between the at least two intermediate layers.

19. The stand-up pouch of claim 18, wherein the barrier layer comprises ethylene vinyl alcohol or polyamide.

20. The stand-up pouch of any of claims 9-10, wherein at least a portion of the polyethylene-based polymer film exhibits a bio-based carbon content of at least 50% as determined by ASTM D6866-18 Method B.

21. The stand-up pouch of any one of claims 8-10, wherein the multilayer structure has at least a 10% increase in tensile strength compared to the same multilayer structure that has not been exposed to an electron beam of at least 20 kGv.

22. The stand-up pouch of any one of claims 8-10, wherein the multilayer structure has at least a 5% reduction in elongation at break compared to the same multilayer structure that has not been subjected to electron beam irradiation of at least 20 kGy.

23. The stand-up pouch of any one of claims 8 to 10, wherein the multilayer structure has a melting temperature in the range of 90-135°C as measured according to ASTM D3418.

24. The stand-up pouch of any one of claims 8 to 10, wherein the sealing temperature of the multilayer structure measured according to ASTM D3418 is in the range of 90-135°C.

25. The stand-up pouch of any one of claims 8-10, wherein the multilayer structure has an impact resistance of greater than 80 gf as measured by the free-falling dart method according to ASTM D1709-01.

26. A method of forming a multilayer structure, the method comprising: A polyethylene-based polymer film is formed, the polyethylene-based polymer film comprising: Sealing layer; at least one intermediate layer; and Polyethylene based printing layer; applying a UV or electron beam curable ink or varnish onto the printed layer; and The UV or electron beam curable ink or varnish is irradiated with UV or electron beam radiation to form the multilayer structure of any one of claims 1-7.

27. The method of claim 26, further comprising: A portion of the sealing layer of the polyethylene-based polymer film is sealed to a sealing layer of another polyethylene-based polymer film to form a stand-up pouch.

28. A method of forming a stand-up pouch, the method comprising: applying a UV or electron beam curable ink or varnish to a polymer substrate; irradiating the UV or electron beam curable ink or varnish with UV or electron beam radiation to form a multilayer structure; and The multilayer structure is sealed to at least one other multilayer structure to form the stand-up pouch of any one of claims 8-25.

29. The method of any one of claims 26-28, wherein the irradiating comprises irradiating with electron beam radiation having an intensity of 20 kGv to 100 kGv.