Chlorinated polyolefin resin, primer, adhesive, bonding agent, laminate, food packaging material using the same, and method for producing the same

By chlorinating polyolefins A and B under chlorine-free solvent conditions, a chlorinated polyolefin resin with moderate chlorine content is formed, which solves the problem of residual chlorine-based low molecular compounds and achieves excellent adhesion and compatibility with chemical substance restrictions. sex.

CN114945603BActive Publication Date: 2024-10-18NIPPON PAPER IND CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180009355.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-06
Publication Date
2024-10-18
Estimated Expiration
2041-01-06

AI Technical Summary

Technical Problem

It is difficult to completely remove chlorine-based low molecular compounds in the existing chlorinated polyolefin manufacturing process. Especially when restrictions on chemical substances are tightened, how to develop chlorinated polyolefin resins with excellent adhesion without using chlorine-based solvents.

Method used

In the presence of an inorganic solvent, polyolefin A or its acid-modified product with excellent fluidity is chlorinated with polyolefin B or its acid-modified product with a high melting point to form a chlorinated polyethylene with a chlorine content of 1 to 45%. Olefin resin, and using specific gas chromatography analysis conditions to ensure that no chlorine-based low molecular compounds are detected.

Benefits of technology

The chlorinated polyolefin resin produced under chlorine-free solvent conditions has excellent adhesion and low chlorine residue, and is suitable for food packaging materials and other industrial uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DEST_PATH_IMAGE002
    Figure DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The object of the present invention is to provide a chlorinated polyolefin resin having excellent adhesion, wherein no chlorine-based low molecular weight compounds are detected by gas chromatography analysis under specified conditions. The present invention is a chlorinated polyolefin resin characterized in that the chlorinated polyolefin resin comprises a resin formed by chlorinating a polyolefin A having fluidity at 40°C or less or its acid-modified product, and a resin formed by chlorinating a polyolefin B having a melting point of more than 40°C and less than 150°C or its acid-modified product, and has a chlorine content of 1 to 45% by weight, and no peak derived from chlorine-based low molecular weight compounds is detected in a retention time range of 4 minutes to 7 minutes when subjected to gas chromatography analysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a chlorinated polyolefin resin, a primer, an adhesive, an adhesive, a laminate, a food packaging material using the same, and a method for producing the same. Background Art

[0002] In recent years, restrictions on chemical substances in inks used to print food packaging films have been strengthened. For example, in Japan, a negative list of chemical substances contained in inks has been drawn up. In addition, in the EU region, restrictions have been introduced to make a positive list of chemical substances that can be used in inks for food packaging. It is believed that restrictions on chemical substances in this field will be further strengthened in the future. In particular, it is believed that restrictions on halogen-based solvents that have a great impact on the human body will become stricter.

[0003] Chlorinated polyolefins are generally produced by dissolving polyolefins in organic solvents and then subjecting them to chlorine addition reaction (see, for example, Patent Document 1). In the chlorine addition reaction, chlorination of the organic solvent also occurs, generating a large amount of by-products. Therefore, in this process, chlorine-based solvents (chlorine-based low molecular weight compounds) such as chloroform are used, which are particularly difficult to undergo chlorine addition reaction even in organic solvents. The chlorine-based solvents used in the chlorine addition reaction process are effectively removed and recovered from the chlorinated polyolefin by vacuum distillation or the like. Therefore, the chlorinated polyolefin as a product contains almost no chlorine-based solvents.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-209450. Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, it is undeniable that chlorine-based solvents (chlorine-based low molecular weight compounds) are used in the chlorine addition reaction process. In view of the tightening of chemical substance regulations in recent years, it is required to develop chlorinated polyolefins that are produced without using chlorine-based solvents in the production process of chlorinated polyolefins and in which no chlorine-based low molecular weight compounds are detected.

[0009] As described above, even if a non-halogen organic solvent is used instead of a chlorine-based solvent, a chlorine addition reaction occurs in the chlorination step, and there is a problem that a chlorine-based solvent, which is a halogen-based solvent, is produced as a by-product.

[0010] An object of the present invention is to provide a chlorinated polyolefin resin having excellent adhesiveness and in which no chlorine-based low-molecular compound is detected by gas chromatography analysis under predetermined conditions.

[0011] Means for solving problems

[0012] The present inventors have conducted intensive studies on the above-mentioned problems and have found that the above-mentioned problems can be solved by chlorinating a combination of two or more polyolefins, namely, a polyolefin A or its acid-modified product having excellent fluidity and a polyolefin B or its acid-modified product having a high molecular weight and capable of exerting cohesive force, in the absence of an organic solvent, thereby completing the present invention.

[0013] That is, the present inventors provide the following [1] to

[13] .

[0014] [1] A chlorinated polyolefin resin characterized in that it is a chlorinated polyolefin resin comprising a resin obtained by chlorinating a polyolefin A having fluidity at 40°C or less or its acid-modified product and a resin obtained by chlorinating a polyolefin B having a melting point of more than 40°C and less than 150°C or its acid-modified product, and having a chlorine content of 1 to 45% by weight,

[0015] When gas chromatography analysis was performed under the following conditions, no peaks derived from chlorine-based low molecular weight compounds were detected in the retention time range of 4 minutes to 7 minutes.

[0016] <Gas chromatography analysis conditions>

[0017] A gas chromatograph GC-2010 plus Tracera manufactured by Shimadzu Corporation (using a BID detector) was used, with a carrier gas of helium (linear flow rate: 40 cm / sec), a capillary column (Rtx-624 manufactured by Restek (inner diameter: 0.32 mm, film thickness: 1.8 μm, length: 30 m), a sample introduction temperature (injection (injection) temperature): 160°C, a column temperature: 60°C), and a chlorinated polyolefin resin was adjusted in a p-xylene solvent to a concentration of 5 wt% and introduced into the apparatus for analysis.

[0018] [2] A chlorinated polyolefin resin characterized in that it is a chlorinated polyolefin resin having a chlorine content of 1 to 45% by weight, obtained by chlorinating a raw material composition comprising at least a polyolefin A having fluidity at 40°C or less or an acid-modified product thereof and a polyolefin B having a melting point of more than 40°C and less than 150°C or an acid-modified product thereof in the absence of an organic solvent,

[0019] When gas chromatography analysis was performed under the following conditions, no peaks derived from chlorine-based low molecular weight compounds were detected in the retention time range of 4 minutes to 7 minutes.

[0020] <Gas chromatography analysis conditions>

[0021] A gas chromatograph GC-2010 plus Tracera manufactured by Shimadzu Corporation (using a BID detector), carrier gas: helium (linear flow rate: 40 cm / sec), capillary column (Rtx-624 manufactured by Restek (inner diameter: 0.32 mm, film thickness: 1.8 μm, length: 30 m), sample introduction temperature (injection temperature): 160°C, column temperature: 60°C) was used. The chlorinated polyolefin resin was adjusted in p-xylene solvent to a concentration of 5 wt% and then introduced into the apparatus for analysis.

[0022] [3] The chlorinated polyolefin resin described in [2], wherein the raw material composition contains at least the polyolefin A and the acid-modified product of the polyolefin B, or contains at least the acid-modified product of the polyolefin A and the acid-modified product of the polyolefin B.

[0023] [4] The chlorinated polyolefin resin according to any one of [1] to [3], wherein the melt viscosity of the chlorinated polyolefin resin at 80°C is less than 100,000 mPa·s.

[0024] [5] The chlorinated polyolefin resin according to any one of [1] to [4], wherein the weight average molecular weight of the polyolefin B is less than 250,000.

[0025] [6] A resin composition comprising the chlorinated polyolefin resin according to any one of [1] to [5] and an organic solvent.

[0026] [7] A primer comprising the chlorinated polyolefin resin according to any one of [1] to [5].

[0027] [8] A coating binder comprising the chlorinated polyolefin resin according to any one of [1] to [5].

[0028] [9] An ink binder comprising the chlorinated polyolefin resin according to any one of [1] to [5].

[0029]

[10] An adhesive comprising the chlorinated polyolefin resin according to any one of [1] to [5].

[0030]

[11] A laminate having an adhesive layer comprising the chlorinated polyolefin resin according to any one of [1] to [5].

[0031]

[12] A food packaging material comprising the chlorinated polyolefin resin according to any one of [1] to [5].

[0032]

[13] A method for producing a chlorinated polyolefin resin according to any one of [1] to [5], the method comprising: chlorinating a raw material composition in the absence of an organic solvent, the raw material composition comprising at least the above-mentioned polyolefin A or its acid-modified product and the above-mentioned polyolefin B or its acid-modified product.

[0033] Effects of the Invention

[0034] According to the present invention, there can be provided a chlorinated polyolefin resin having excellent adhesiveness and in which no chlorine-based low-molecular compound is detected by gas chromatography analysis under predetermined conditions. DETAILED DESCRIPTION

[0035] Hereinafter, it will be described in detail according to a suitable embodiment of the present invention. It should be noted that, in this specification, "having fluidity below 40°C" means that the viscosity at 40°C measured using a cylindrical rotational viscometer or a lamina viscometer is 100,000 mPa or less. In addition, the expression "AA to BB%" means AA% or more and BB% or less.

[0036] [1. Chlorinated polyolefin resin]

[0037] In one embodiment, the chlorinated polyolefin resin of the present invention comprises a resin formed by chlorinating a polyolefin A having fluidity at 40° C. or less or its acid-modified product, and a resin formed by chlorinating a polyolefin B having a melting point of more than 40° C. and less than 150° C. or its acid-modified product. The chlorine content is 1 to 45% by weight.

[0038] In one embodiment, the chlorinated polyolefin resin of the present invention is obtained by chlorinating a raw material composition containing at least a polyolefin A or an acid-modified product thereof having fluidity at 40° C. or lower, and a polyolefin B or an acid-modified product thereof having a melting point of more than 40° C. and less than 150° C. in the absence of an organic solvent. The chlorine content is 1 to 45% by weight.

[0039] The chlorinated polyolefin resin of the present invention can be chlorinated in the absence of an organic solvent because the raw material composition before chlorination contains polyolefin A or its acid-modified product. In addition, the chlorinated polyolefin resin of the present invention can be a chlorinated polyolefin resin that can be used for ink applications, etc. because the raw material composition before chlorination contains polyolefin B or its acid-modified product.

[0040] The chlorinated polyolefin resin of the present invention may be a chlorinated polyolefin resin obtained by acid modification (hereinafter, referred to as "acid-modified chlorinated polyolefin resin" for convenience). In the case of an acid-modified chlorinated polyolefin resin, the polarity of the obtained chlorinated polyolefin resin can be adjusted by the acid modification amount (hereinafter, also referred to as "graft weight"). Therefore, the chlorinated polyolefin resin of the present invention can be applied to various polar adherends.

[0041] The acid modification treatment may be (1) performed on polyolefin A and / or polyolefin B alone, (2) performed on a mixture of polyolefin A and polyolefin B before chlorination treatment (hereinafter, referred to as "polyolefin mixture" for convenience), or (3) performed on a chlorinated polyolefin resin after chlorination treatment. It should be noted that the acid modification treatment may be any one of (1) to (3), or a combination of (1) and (2) or a combination of (1) and (3). Among them, the acid modification treatment is preferably the treatment of (1) or (2), especially the treatment performed on polyolefin B alone or on a polyolefin mixture.

[0042] In addition, in this specification, the raw material composition containing the polyolefin mixture subjected to acid modification or the polyolefin B subjected to acid modification is also referred to as "acid-modified raw material composition".

[0043] Next, the acid modification treatment will be described.

[0044] The method of acid modification treatment is not particularly limited and can be carried out by a known method. For example, the following method can be mentioned: polyolefin B or a polyolefin mixture, α , β - Unsaturated carboxylic acid or its derivative is heated and dissolved in a solvent such as toluene, and a free radical generator is added; using a Banbury mixer, a kneader, an extruder, etc., polyolefin B or a polyolefin mixture, α , β - A melt-kneading method in which an unsaturated carboxylic acid or a derivative thereof and a radical generator are kneaded.

[0045] As α , β - Unsaturated carboxylic acids or derivatives thereof, for example, maleic acid, maleic anhydride, fumaric acid, citraconic acid, citraconic anhydride, mesaconic acid, itaconic acid, itaconic anhydride, aconitic acid, aconitic anhydride, nadic anhydride (himicanhydride), (meth)acrylic acid, (meth)acrylic acid esters. Among them, maleic anhydride is preferred.

[0046] It should be noted that α , β - unsaturated carboxylic acid or its derivatives as long as they are selected from α , β- one or more compounds of unsaturated carboxylic acids and their derivatives, which may be one or more α , β - a combination of an unsaturated carboxylic acid and one or more of its derivatives, a combination of two or more α,β-unsaturated carboxylic acids, α , β - Combinations of derivatives of unsaturated carboxylic acids.

[0047] When the acid-modified raw material composition is 100 wt %, α , β The amount of the unsaturated carboxylic acid or its derivative introduced (graft weight) is preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight. By making the graft weight 0.1% or more by weight, the adhesion of the obtained acid-modified chlorinated polyolefin resin to materials such as metal adherends can be maintained. By making the graft weight 10% or less by weight, the generation of graft unreacted products can be prevented, and sufficient adhesion to the resin adherend can be obtained.

[0048] It should be noted that α , β - The amount of the unsaturated carboxylic acid or its derivative introduced (graft weight) is a value measured by an alkali titration method.

[0049] The free radical generator can be appropriately selected from known free radical generators. Among them, organic peroxide compounds are preferred. For example, di-tert-butyl peroxide, dicumyl peroxide, tert-butyl cumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, 1,1-bis (tert-butyl peroxy) -3,5,5-trimethylcyclohexane, 1,1-bis (tert-butyl peroxy) -cyclohexane, cyclohexanone peroxide, tert-butyl peroxybenzoate, tert-butyl peroxyisobutyrate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisopropyl carbonate, cumyl peroxyoctanoate, 2,5-dimethyl-2,5-di (tert-butyl peroxy) hexane. Among them, dicumyl peroxide, di-tert-butyl peroxide, dilauryl peroxide, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane are preferred.

[0050] Relative to α , β The total amount (weight) of the added amount of the unsaturated carboxylic acid or its derivative and the added amount of the (meth)acrylate, the added amount of the free radical generator is preferably 1 to 100 weight %, more preferably 10 to 50 weight %. By being 1 weight % or more, sufficient grafting efficiency can be maintained. By being 100 weight % or less, a decrease in the weight average molecular weight of the acid-modified raw material composition can be prevented.

[0051] The chlorinated polyolefin resin of the present invention is obtained by chlorinating a raw material composition containing at least a polyolefin A or an acid-modified product thereof having fluidity at 40°C or less, and a polyolefin B or an acid-modified product thereof having a melting point of more than 40°C and less than 150°C. Therefore, the chlorinated polyolefin resin of the present invention includes a resin formed by chlorinating a polyolefin A or an acid-modified product thereof having fluidity at 40°C or less, and a resin formed by chlorinating a polyolefin B or an acid-modified product thereof having a melting point of more than 40°C and less than 150°C. This can improve adhesion to a non-polar resin substrate or compatibility with other components.

[0052] As a method for chlorination, for example, the following method can be mentioned: chlorine gas is blown into the raw material composition to introduce chlorine atoms into polyolefin A or its acid-modified product having fluidity below 40°C and polyolefin B or its acid-modified product having a melting point of more than 40°C and below 150°C contained in the raw material composition.

[0053] It should be noted that in the present invention, it is not necessary to use a chlorinated solvent such as chloroform or dichloromethane or other organic solvent when blowing in chlorine gas. This is because: since the raw material composition contains polyolefin A or its acid-modified product having fluidity below 40°C, polyolefin A or its acid-modified product can dissolve chlorine gas, and polyolefin B or its acid-modified product can react with chlorine gas.

[0054] The blowing of chlorine gas can be carried out under the irradiation of ultraviolet rays, or in the presence or absence of a free radical reaction initiator. The pressure when blowing chlorine gas is not particularly limited, and it can be normal pressure or pressurized. The temperature when blowing chlorine gas is not particularly limited, and it is usually 50 to 140°C.

[0055] As the radical reaction initiator, an organic peroxide compound or an azonitrile such as 2,2-azobisisobutyronitrile can be used. The details of the organic peroxide compound will be described later.

[0056] The chlorinated polyolefin resin of the present invention can be obtained by introducing chlorine atoms into a polyolefin mixture or an acid-modified product thereof, a mixture of polyolefin A and an acid-modified product of polyolefin B, or a mixture of an acid-modified product of polyolefin A and polyolefin B.

[0057] The chlorine content of the chlorinated polyolefin resin of the present invention is 1 to 45% by weight, preferably 10 to 45% by weight, and more preferably 20 to 45% by weight. By setting the chlorine content within the above range, the polarity of the chlorinated polyolefin resin can be adjusted to a certain range. Therefore, the compatibility with other resins in the coating becomes good, and sufficient adhesion to non-polar substrates such as polyolefin substrates can be obtained.

[0058] In addition, the chlorine content of a chlorinated polyolefin resin is a value measured according to JIS-K7229.

[0059] The chlorine content varies depending on the type of polyolefin resin, reaction scale, reaction apparatus, etc. Therefore, the chlorine content can be adjusted while monitoring the amount or time of chlorine injection.

[0060] Examples of organic peroxide compounds include di-tert-butyl peroxide, dicumyl peroxide, tert-butyl cumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, 1,4-bis[(tert-butylperoxy)isopropyl]benzene, 1,1-bis(tert-butylperoxy)-3,5,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)-cyclohexane, cyclohexanone peroxide, tert-butyl peroxybenzoate, tert-butyl peroxyisobutyrate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisopropyl carbonate, and cumyl peroxyoctanoate. Among these, di-tert-butyl peroxide, dicumyl peroxide, and dilauryl peroxide are preferred.

[0061] The free radical generator may be a single free radical generator or a combination of a plurality of free radical generators.

[0062] The lower limit of the weight average molecular weight of the chlorinated polyolefin resin is preferably 5,000 or more, more preferably 7,000 or more, and further preferably 8,000 or more. If it is 5,000 or more, it has the cohesive force of the resin and can exhibit adhesion to the adherend. On the other hand, the upper limit is preferably 100,000 or less, more preferably 60,000 or less, and further preferably 40,000 or less. If it is 100,000 or less, it has compatibility with other resins or solubility in solvents, and can be applied to coatings, inks, etc.

[0063] The weight average molecular weight of the chlorinated polyolefin resin is preferably 5,000 to 100,000, more preferably 7,000 to 60,000, further preferably 8,000 to 40,000.

[0064] In addition, the weight average molecular weight is a value calculated|required from the standard polystyrene calibration curve by the gel permeation chromatography (GPC) method.

[0065] It is important that the chlorinated polyolefin resin of the present invention does not detect a peak derived from a chlorine-based low molecular weight compound in the retention time range of 4 to 7 minutes when subjected to gas chromatography analysis under the following conditions. Examples of chlorine-based low molecular weight compounds detectable under such conditions include chloroform and dichloromethane.

[0066] <Gas chromatography analysis>

[0067] A gas chromatograph GC-2010 plus Tracera manufactured by Shimadzu Corporation (using a BID detector), carrier gas: helium (linear flow rate: 40 cm / sec), capillary column (Rtx-624 manufactured by Restek (inner diameter: 0.32 mm, film thickness: 1.8 μm, length: 30 m), sample introduction temperature (injection temperature): 160°C, column temperature: 60°C) was used. The chlorinated polyolefin resin was adjusted in p-xylene solvent to a concentration of 5 wt% and then introduced into the apparatus for analysis.

[0068] As described above, when chlorination is performed using a chlorine-based solvent such as chloroform in the chlorine addition reaction step, there is a concern that some byproducts or chloroform etc. may remain even if vacuum distillation is performed. If such a residue exists, a peak derived from a chlorine-based low molecular weight compound will appear within a retention time of 4 to 7 minutes under the above-mentioned gas chromatography analysis conditions, so it can be judged.

[0069] The chlorinated polyolefin resin of the present invention does not have a peak derived from a chlorine-based low molecular weight compound that appears in the retention time range of 4 to 7 minutes, and can therefore be distinguished from such conventional chlorinated polyolefin resins and can be suitably used as a chlorinated polyolefin resin with very little chlorine-based solvent residue or chlorination by-products.

[0070] [1-1. Polyolefin A]

[0071] The polyolefin A is a polyolefin having fluidity at 40° C. or lower. By including the polyolefin A, the melt viscosity in the chlorination reaction can be reduced, and chlorination can be performed without using an organic solvent.

[0072] More specifically, polyolefin A preferably has a viscosity of 100,000 mPa·s or less at 40° C., and more preferably 60,000 mPa·s or less. The lower limit of the viscosity is not particularly limited, but is usually 100 mPa·s or more.

[0073] In addition, the viscosity at 40° C. is a value measured using a cone-type viscometer (manufactured by Brookfield, model: CAP200H).

[0074] The polyolefin A may be any polyolefin satisfying the above-mentioned physical properties. Examples thereof include ethylene-propylene copolymers, hydrogenated polybutadiene, ethylene-butene copolymers, ethylene-octene copolymers, propylene-butene copolymers, α -Olefin derivatives.

[0075] In addition, these may be commercially available items. In addition, the polyolefin A may be used alone or in combination of two or more.

[0076] [1-2. Polyolefin B]

[0077] The polyolefin B is a polyolefin having a melting point of more than 40° C. and not more than 150° C. By including the polyolefin B, a chlorinated polyolefin resin that can be used for ink applications and the like can be obtained.

[0078] It should be noted that the melting point is a value measured according to JIS K7121 (1987) using a DSC measuring device (e.g., "DISCOVERYDSC2500", manufactured by TA Instruments Japan). More specifically, about 5 mg of a sample is kept in a heated melting state at 200°C for 10 minutes. The temperature is lowered to -50°C at a rate of 10°C / min, and then kept stable for 5 minutes. Thereafter, the temperature is raised to 200°C at 10°C / min and the melting peak temperature is obtained when the sample is melted.

[0079] More specifically, the polyolefin B is preferably a polyolefin having a weight average molecular weight of 8,000 or more and less than 250,000, more preferably a polyolefin having a weight average molecular weight of 8,000 or more and less than 200,000, and further preferably a polyolefin having a weight average molecular weight of 10,000 or more and less than 100,000.

[0080] In addition, the weight average molecular weight is a value calculated|required from the standard polystyrene calibration curve by the gel permeation chromatography (GPC) method.

[0081] The polyolefin B may be any polyolefin satisfying the above-mentioned physical properties. Among them, polyolefins using a Ziegler-Natta catalyst or a metallocene catalyst as a polymerization catalyst are preferred, and polypropylene resins using a Ziegler-Natta catalyst or a metallocene catalyst as a polymerization catalyst, or polypropylene and α The present invention relates to a polyolefin obtained by copolymerizing olefins (e.g., ethylene, butene, 3-methyl-1-butene, 3-methyl-1-heptene), preferably a propylene-based random copolymer using a metallocene catalyst as a polymerization catalyst, and more preferably polypropylene, ethylene-propylene copolymer, propylene-butene copolymer, or ethylene-propylene-butene copolymer using a metallocene catalyst as a polymerization catalyst. It should be noted that if a metallocene catalyst is used, the obtained polyolefin has the following characteristics: narrow molecular weight distribution, excellent random copolymerizability, narrow composition distribution, and a wide range of copolymerizable comonomers. It should be noted that these can be commercially available products.

[0082] Here, the propylene-based random copolymer refers to polypropylene or a mixture of propylene and α Examples of the polyolefin obtained by random copolymerization of olefins include polypropylene, ethylene-propylene copolymer, propylene-butene copolymer, ethylene-propylene-diene copolymer, and ethylene-propylene-butene copolymer.

[0083] It should be noted that the (co)polymer constituting the polyolefin B may be a single type or a combination of a plurality of types of (co)polymers.

[0084] A known metallocene catalyst can be used. For example, a catalyst obtained by combining the following components (1) and (2) and, if necessary, component (3) can be mentioned. Among them, the metallocene catalyst is preferably a catalyst obtained by combining the following components (1) and (2) and, if necessary, component (3).

[0085] Component (1): a transition metal compound of Groups 4 to 6 of the periodic table having at least one conjugated five-membered ring ligand, i.e., a metallocene complex;

[0086] Component (2): ion-exchange layered silicate;

[0087] Ingredient (3): an organoaluminum compound.

[0088] The structure of the polyolefin may be any of the isotactic structure, atactic structure, syndiotactic structure, etc., which are obtainable by common polymer compounds. Among these structures, in consideration of the adhesion to the polyolefin substrate, particularly the adhesion under low-temperature drying, the polyolefin having an isotactic structure which can be obtained when a metallocene catalyst is used is preferred.

[0089] As the component composition of the polyolefin, the propylene constituent unit content is preferably 30% by weight or more, more preferably 40% by weight or more, and further preferably 50% by weight or more. If the propylene component is 30% by weight or more, the adhesion (adhesion) to the polypropylene substrate can be better. It should be noted that the propylene constituent unit content of the polyolefin can be the usage ratio of the raw materials or the value calculated by NMR analysis.

[0090] Alternatively, an acid-modified product obtained by subjecting the above-mentioned polyolefin B to an acid modification treatment may be used instead of the polyolefin B. By adjusting the graft weight by acid modification treatment, the polarity of the chlorinated polyolefin resin can be adjusted. Therefore, the chlorinated polyolefin resin can be applied to various polar adherends.

[0091] In addition, the details of the acid modification treatment are as described above.

[0092] [1-3. Ratio]

[0093] The ratio (mass ratio) (A / B) of polyolefin A or its acid-modified product to polyolefin B or its acid-modified product in the raw material composition or the acid-modified raw material composition is not particularly limited, and is generally 10 / 90 to 90 / 10. If polyolefin A or its acid-modified product is less than 10 and polyolefin B or its acid-modified product exceeds 90, polyolefin B or its acid-modified product may not be completely dissolved in polyolefin A or its acid-modified product, and chlorination may become uneven. On the other hand, if polyolefin A or its acid-modified product exceeds 90 and polyolefin B or its acid-modified product is less than 10, the cohesive force of the obtained chlorinated polyolefin resin is insufficient, and sometimes adhesion to the polyolefin substrate cannot be obtained.

[0094] [1-4. Melt viscosity]

[0095] The melt viscosity of the chlorinated polyolefin resin at 80°C is preferably less than 100,000 mPa·s, and more preferably less than 70,000 mPa·s. The higher the chlorine content of the chlorinated polyolefin resin of the present invention, the higher the viscosity. As the chlorination proceeds, the viscosity increases in the reactor. If the melt viscosity at 80°C is 100,000 mPa·s or more, the resin becomes unable to flow in the final stage of the chlorination reaction, the shear force of the stirrer increases, and the dehydrochlorination reaction proceeds, causing the chlorinated polyolefin resin to be significantly colored. The lower limit of the melt viscosity is preferably more than 1,000 mPa·s, more preferably 1,500 mPa·s or more, and even more preferably 1,800 mPa·s or more. If the melt viscosity is 1,000 mPa·s or less, when the chlorinated polyolefin resin is prepared, the resin exhibits relatively low molecular weight / low melting point and other physical properties, which affects the direction in which the adhesion deteriorates, and is therefore not preferred.

[0096] The melt viscosity at 80° C. can be measured using a lamina viscometer (manufactured by Brookfield, model: CAP200H). Chlorinated polypropylene resins obtained using conventionally known chlorinated solvents cannot be sufficiently melted at 80° C. and do not exhibit melt viscosity.

[0097] [1-5. Optional ingredients]

[0098] The raw material composition may contain other optional components in addition to polyolefin A or its acid-modified product and polyolefin B or its acid-modified product. As an optional component, water may be mentioned, which may prevent the coloring of the resin during the chlorination reaction or reduce the melt viscosity.

[0099] [2-1. Resin composition]

[0100] The resin composition of the present invention contains the above-mentioned chlorinated polyolefin resin and an organic solvent. The resin composition of the present invention may contain a stabilizer to suppress the release of chlorine.

[0101] Examples of the organic solvent include aromatic solvents such as toluene and xylene; alicyclic hydrocarbon solvents such as cyclohexane and methylcyclohexane; hydrocarbon solvents such as hexane, heptane, and octane; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester solvents such as methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, and n-butyl acetate; and glycol solvents such as ethylene glycol, ethyl cellosolve, and butyl cellosolve. Among these, toluene, methylcyclohexane, ethyl acetate, propyl acetate, and butyl acetate are preferred.

[0102] The concentration of the resin composition (resin solid content concentration) can be appropriately selected according to the application. However, whether the concentration of the resin composition is too high or too low, coating workability is impaired, so it is preferably set to 15 to 70% by weight.

[0103] As the stabilizer, an epoxy compound is preferred. The epoxy compound is preferably an epoxy compound compatible with the chlorinated polyolefin resin.

[0104] Examples of the epoxy compound include epoxy compounds having an epoxy equivalent of about 100 to 500 and containing one or more epoxy groups in one molecule.

[0105] More specifically, the following compounds can be mentioned.

[0106] Epoxidized soybean oil or epoxidized linseed oil obtained by epoxidizing natural vegetable oils having unsaturated groups using peracids such as peracetic acid; epoxidized fatty acid esters obtained by epoxidizing unsaturated fatty acids such as oleic acid, tall oil fatty acid, and soybean oil fatty acid; epoxidized alicyclic compounds represented by epoxidized tetrahydrophthalic acid esters; bisphenol A glycidyl ether, ethylene glycol glycidyl ether, propylene glycol glycidyl ether, etc. obtained by condensing bisphenol A or polyols with epichlorohydrin (epichlorohydrin) Glycerol polyglycidyl ether, sorbitol polyglycidyl ether; monoepoxy compounds represented by butyl glycidyl ether, 2-ethylhexyl glycidyl ether, decyl glycidyl ether, stearyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, sec-butylphenyl glycidyl ether, tert-butylphenyl glycidyl ether, phenol polyethylene oxide glycidyl ether, etc.; metal soaps such as calcium stearate and lead stearate used as stabilizers for polyvinyl chloride resins; organic metal compounds such as dibutyltin dilaurate and dibutyl maleate; hydrotalcite compounds.

[0107] In addition, as a stabilizer, only one kind among these may be used, and you may use 2 or more types together.

[0108] [2-2. Aqueous dispersion]

[0109] The aqueous dispersion of the present invention contains the above-mentioned chlorinated polyolefin resin and water. In order to improve dispersion stability, the aqueous dispersion of the present invention may contain an emulsifier or an amphiphilic solvent such as butyl cellosolve.

[0110] The concentration of the aqueous dispersion (resin solid content concentration) can be appropriately selected according to the application. However, whether the concentration of the aqueous dispersion is too high or too low, coating workability is impaired, so the solid content concentration is preferably 15 to 50% by weight.

[0111] The pH of the aqueous dispersion is preferably 5 or more, more preferably 7 to 12. If the pH is 5 or more, neutralization is fully performed, which can prevent the modified polyolefin resin from not being dispersed in other components, or even if dispersed, it can prevent the storage stability from being deteriorated due to precipitation and separation over time. In addition, if the pH is 12 or less, compatibility with other components and safety in operation can be ensured.

[0112] The viscosity of the aqueous dispersion measured at 25° C. with a Brookfield viscometer is preferably 0.1 to 1000 mPa·s, more preferably 1 to 700 mPa·s, and still more preferably 2 to 400 mPa·s.

[0113] The viscosity can be measured using a Brookfield viscometer with a rotor #1 or #2 at a rotation speed of 60 rpm. The viscosity measurement is performed using an aqueous dispersion having a solid content concentration of 10 to 60% by mass.

[0114] [3. Method for producing chlorinated polyolefin resin]

[0115] The method for producing a chlorinated polyolefin resin of the present invention is a method comprising chlorinating a raw material composition containing at least polyolefin A or its acid-modified product and polyolefin B or its acid-modified product in the absence of an organic solvent. The polyolefin A, polyolefin B, raw material composition and chlorination step are as described above.

[0116] “In the absence of an organic solvent” means that the organic solvent that is inevitably mixed is removed. The organic solvent that is inevitably mixed refers to: a very small amount of organic solvent remaining after removing (e.g., distilling off) polyolefin A or polyolefin B, the solvent during acid treatment, etc. according to a conventional method; an organic solvent contained in an organic peroxide-based compound; and an organic solvent generated by the decomposition of an organic peroxide. Example

[0117] Hereinafter, the present invention will be described in detail by examples. The following examples are used to appropriately illustrate examples of the present invention and do not limit the present invention. It should be noted that, as long as there is no additional description, the measuring method of the physical property value etc. is the measuring method of the above-mentioned description. In addition, as long as there is no special description, "part" refers to mass parts.

[0118] (Production Example 1)

[0119] 2 parts of dicumyl peroxide were added to 100 parts of ethylene-propylene copolymer (weight average molecular weight of 60,000, melting point of about 60°C) with an ethylene content of about 12% by weight produced using a metallocene catalyst as a polymerization catalyst, and the mixture was supplied to a twin-screw extruder with a reaction zone temperature set at 300°C, thereby subjecting the mixture to thermal degradation to obtain polyolefin B with a weight average molecular weight of 20,000 and a melting point of about 60°C.

[0120] (Production Example 2)

[0121] 4 parts of maleic anhydride and 2 parts of dicumyl peroxide were added to 100 parts of ethylene-propylene copolymer (melting point of about 125° C.) having an ethylene content of about 3% by weight and produced using a metallocene catalyst as a polymerization catalyst, and the mixture was supplied to a twin-screw extruder with a reaction zone temperature set at 250° C., thereby obtaining a maleic anhydride-modified polyolefin, i.e., an acid-modified product of polyolefin B, having a weight average molecular weight of 50,000 and a melting point of about 125° C.

[0122] (Example 1)

[0123] 5 kg of ethylene-propylene copolymer (viscosity of 340 mPa·s at 40°C) which is liquid at room temperature as polyolefin A and 5 kg of polyolefin (weight average molecular weight of 20,000, melting point of about 60°C) obtained in Production Example 1 as polyolefin B were put into a glass-lined reactor, and stirring was started after the mixture was fully melted at a temperature of 95°C. 5 g of 2,2-azobisisobutyronitrile was added, and chlorine gas was blown into the reactor while the pressure inside the reactor was controlled to be above normal pressure and below 0.2 MPa, and then nitrogen gas was blown into the reactor to remove by-produced hydrogen chloride, thereby obtaining a chlorinated polyolefin resin. The melt viscosity of the obtained chlorinated polyolefin resin at 80°C was 2,000 mPa·s. After the pressure inside the reactor reached normal pressure, 400 g of epoxidized soybean oil and 24 kg of toluene were added, and the mixture was cooled to room temperature, thereby obtaining a chlorinated polyolefin resin composition having a chlorine content of 4%.

[0124] (Example 2)

[0125] 1 kg of ethylene-propylene copolymer (viscosity of 1,100 mPa·s at 40°C) which is liquid at room temperature as polyolefin A and 9 kg of ethylene-propylene copolymer (weight average molecular weight of 12,000, melting point of about 60°C) with an ethylene content of about 12% by weight produced by using a metallocene catalyst as a polymerization catalyst as polyolefin B were put into a glass-lined reactor, and stirring was started after the mixture was fully melted at a temperature of 95°C. 5 g of 2,2-azobisisobutyronitrile was added, and chlorine gas was blown into the reactor while the pressure in the reactor was controlled to be above normal pressure and below 0.2 MPa, and then nitrogen gas was blown into the reactor to remove by-produced hydrogen chloride, thereby obtaining a chlorinated polyolefin resin. The melt viscosity of the obtained chlorinated polyolefin resin at 80°C was 67,000 mPa·s. After the pressure in the reactor reached normal pressure, 400 g of epoxidized soybean oil and 24 kg of n-propyl acetate were added, and the mixture was cooled to room temperature, thereby obtaining a chlorinated polyolefin resin composition with a chlorine content of 28%.

[0126] (Example 3)

[0127] The same operation as in Example 2 was carried out except that 9 kg of an ethylene-propylene copolymer (viscosity of 150 mPa·s at 40°C) which was liquid at room temperature was used as polyolefin A and 1 kg of a maleic anhydride-modified polyolefin (weight average molecular weight of 50,000 and melting point of about 125°C) obtained in Production Example 2 as the acid-modified product of polyolefin B, thereby obtaining an acid-modified chlorinated polyolefin resin (melt viscosity of 93,000 mPa·s at 80°C) having a chlorine content of 43% and a composition thereof.

[0128] (Example 4)

[0129] The same operation as in Example 2 was carried out except that 7 kg of hydrogenated polybutadiene (viscosity at 40°C: 8,000 mPa·s) was used as polyolefin A and 3 kg of ethylene-propylene copolymer (weight average molecular weight: 60,000, melting point: about 60°C) having an ethylene content of about 12% by weight and produced using a metallocene catalyst as a polymerization catalyst was used as polyolefin B, thereby obtaining a chlorinated polyolefin resin (melt viscosity at 80°C: 40,000 mPa·s) having a chlorine content of 22% and a composition thereof.

[0130] (Example 5)

[0131] 8 kg of ethylene-propylene copolymer (viscosity at 40°C: 3,500 mPa·s) as polyolefin A and 2 kg of ethylene-propylene copolymer (weight average molecular weight: 12,000, melting point: about 60°C) with an ethylene content of about 12% by weight produced using a metallocene catalyst as a polymerization catalyst as polyolefin B were placed in a glass-lined reactor, and stirring was started after fully melting at a temperature of 130°C. After adding 100 g of maleic anhydride, 30 g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane was added, and the reaction was carried out for 4 hours. After that, the temperature was lowered and adjusted to 95°C, 5 g of 2,2-azobisisobutyronitrile was added, and chlorine gas was blown in while the pressure in the reactor was controlled to be above normal pressure and below 0.2 MPa, and then nitrogen gas was blown in to remove by-produced hydrogen chloride, thereby obtaining an acid-modified chlorinated polyolefin resin. The melt viscosity of the obtained chlorinated polyolefin resin at 80°C was 3,000 mPa·s. 400 g of epoxidized soybean oil and 24 kg of toluene were added, and the mixture was cooled to room temperature to obtain an acid-modified chlorinated polyolefin resin composition having a chlorine content of 22%.

[0132] (Comparative Example 1)

[0133] The same operation as in Example 2 was carried out except that 10 kg of an ethylene-propylene copolymer (viscosity of 150 mPa·s at 40°C) which is liquid at room temperature was used as polyolefin A and nothing was used as polyolefin B, thereby obtaining a chlorinated polyolefin resin (melt viscosity of 1,000 mPa·s at 80°C) having a chlorine content of 22% and a composition thereof.

[0134] (Comparative Example 2)

[0135] Using 1 kg of an ethylene-propylene copolymer (viscosity at 40°C: 1,100 mPa·s) which is liquid at room temperature as polyolefin A and 9 kg of an ethylene-propylene copolymer (weight average molecular weight: 12,000, melting point: about 60°C) having an ethylene content of about 12% by weight and produced using a metallocene catalyst as a polymerization catalyst as polyolefin B, the same operation as in Example 2 was carried out. Although significant coloration occurred in the final stage of the chlorination reaction, a chlorinated polyolefin resin (melt viscosity at 80°C: 124,000 mPa·s) having a chlorine content of 46% and a composition thereof were obtained.

[0136] (Comparative Example 3)

[0137] 5 kg of the polyolefin (weight average molecular weight of 20,000, melting point of about 60° C.) obtained in Production Example 1 as polyolefin B was put into a glass-lined reactor without using any substance as polyolefin A, and stirring was started after the mixture was fully melted at a temperature of 95° C. 5 g of 2,2-azobisisobutyronitrile was added, and chlorine gas was blown into the reactor while the pressure inside the reactor was controlled to be above normal pressure and below 0.2 MPa, but a significant decrease in the chlorine addition rate was observed due to the high viscosity, and the reaction could not be continued because the reaction became uneven.

[0138] (Comparative Example 4)

[0139] 9 kg of ethylene-propylene copolymer (viscosity of 150 mPa·s at 40°C) which is liquid at room temperature as polyolefin A and 1 kg of pyrolyzed polypropylene (weight average molecular weight of 5,000, melting point of about 160°C) which is a substitute for polyolefin B were placed in a glass-lined reactor and heated at 95°C. However, a sufficient melt state could not be obtained and a chlorination reaction could not be carried out.

[0140] (Example 6)

[0141] The same operation as in Example 2 was carried out except that 9 kg of an ethylene-propylene copolymer (viscosity at 40°C: 150 mPa·s) which was liquid at room temperature was used as polyolefin A and 1 kg of an ethylene-propylene copolymer (weight average molecular weight: 220,000, melting point: about 65°C) having an ethylene content of about 11% by weight and produced using a metallocene catalyst as a polymerization catalyst was used as polyolefin B, thereby obtaining a chlorinated polyolefin resin (melt viscosity at 80°C: 78,000 mPa·s) having a chlorine content of 32% and a composition thereof.

[0142] (Comparative Example 5)

[0143] 8 kg of ethylene-propylene copolymer (no fluidity at 40°C, viscosity at 40°C cannot be measured, viscosity at 100°C is 3,000 mPa·s) as a substitute for polyolefin A and 2 kg of ethylene-propylene copolymer (weight average molecular weight of 12,000, melting point of about 60°C) with an ethylene content of about 12% by weight produced using a metallocene catalyst as a polymerization catalyst as polyolefin B were put into a glass-lined reactor, and stirring was started after fully melting at a temperature of 95°C. 5 g of 2,2-azobisisobutyronitrile was added, and chlorine gas was blown in while the pressure in the reactor was controlled to be above normal pressure and below 0.2 MPa, but a significant decrease in the chlorine addition rate was observed due to the high viscosity, and the reaction could not be continued because the reaction became uneven.

[0144] (Comparative Example 6)

[0145] 2 kg of polyolefin B (weight average molecular weight of 20,000, melting point of about 60°C) obtained in Preparation Example 1 was placed in a glass-lined reactor, 40 L (liters, the same below) of chloroform was added, and after being fully dissolved at a pressure of 0.3 MPa and a temperature of 110°C, 1 g of azobisisobutyronitrile was added, and chlorine gas was blown into the reactor while the pressure in the reactor was controlled to 0.3 MPa to obtain a reaction liquid. Next, chloroform as a reaction solvent was removed by an evaporator, and then reduced pressure drying was performed in a vacuum dryer set at 62°C for 7 days to obtain a chlorinated polyolefin resin. The obtained chlorinated polyolefin resin did not fully melt at 80°C, and the melt viscosity could not be measured.

[0146] Epoxidized soybean oil was added to the obtained chlorinated polyolefin resin in an amount of 4% based on the weight of the chlorinated polyolefin resin, and toluene was added to dissolve the chlorinated polyolefin resin to obtain a chlorinated polyolefin resin composition having a solid content of 20% by weight and a chlorine content of 36%.

[0147] [Adhesion test]

[0148] 120g of commercially available gravure printing resin (manufactured by Sanyo Chemical, solid content is 30% by weight) and 160g of titanium dioxide (manufactured by Ishihara Industry, rutile type) were diluted with a mixed solution of 120g of ethyl acetate / isopropanol (weight ratio is 67 / 33), and then mixed with a sand mill for 1 hour to adjust (modulate) the ink. 20 parts of the (acid-modified) chlorinated polyolefin resin composition obtained in Examples 1 to 6 or Comparative Examples 1, 2, and 6 were added to 100 parts of the ink, and after sufficient oscillation and mixing, the ink was applied on the corona-treated surface of the OPP film (Futamura Chemical, 80μm) using a Meyer rod #5, and dried using a dryer. After standing at room temperature for 1 day, a transparent tape (manufactured by NICHIBAN, 24mm) was attached to the ink-coated surface to study the peeling state of the coated surface when it was peeled off in one breath (all at once). The peeling state was evaluated as follows.

[0149] The evaluation results are recorded in Table 1.

[0150] A: No peeling;

[0151] B: The peeling area is less than 50%;

[0152] C: The peeling area is more than 50%;

[0153] D: Almost the entire surface is peeled off.

[0154] [Flowability at 40°C]

[0155] The viscosity of polyolefin A was measured using a cone-type viscometer (manufactured by Brookfield, model: CAP200H) and evaluated according to the following evaluation criteria.

[0156] ○: It is liquid at 40℃ and the viscosity at 40℃ can be measured;

[0157] ×: Since the material does not melt at 40° C., the melt viscosity at 40° C. cannot be measured, or the melt viscosity at 40° C. exceeds 100,000 mPa·s.

[0158] <Gas chromatography analysis>

[0159] A gas chromatograph GC-2010 plus Tracera manufactured by Shimadzu Corporation (using a BID detector), carrier gas: helium (linear flow rate: 40 cm / sec), capillary column (Rtx-624 manufactured by Restek (inner diameter: 0.32 mm, film thickness: 1.8 μm, length: 30 m), sample introduction temperature (injection temperature): 160°C, column temperature: 60°C) was used. The chlorinated polyolefin resin was adjusted in p-xylene solvent to a concentration of 5 wt% and then introduced into the apparatus for analysis.

[0160] From the obtained analysis chart, it was determined whether or not there was a peak derived from a chlorine-based low molecular weight compound within a retention time of 4 to 7 minutes.

[0161] [Table 1]

[0162]

[0163] As can be seen from Table 1, chlorinated polyolefin resins (Examples 1 to 6) can be produced from the raw material composition containing polyolefin A and polyolefin B in the absence of an organic solvent.

[0164] The adhesion of the chlorinated polyolefin resin was poor when using only polyolefin A (Comparative Example 1). In addition, even when chlorination was performed from a raw material composition containing polyolefin A and polyolefin B in the absence of an organic solvent, the adhesion was poor when the chlorine content exceeded 45% by weight (Comparative Example 2).

[0165] When only polyolefin B was chlorinated, even with a raw material composition containing polyolefin A and polyolefin B, if the melting point of polyolefin B exceeded 150° or polyolefin A had no fluidity at 40°C, a chlorinated polyolefin resin could not be prepared (Comparative Examples 3 to 5).

[0166] In addition, as shown in Comparative Example 6, the chlorinated polyolefin resin obtained by using a chlorine-based solvent has excellent adhesion, but the presence of unremoved chlorine-based low-molecular compounds was confirmed.

[0167] Therefore, the chlorinated polyolefin resin of the present invention is suitable for primers, adhesives (for coatings and inks), adhesives, and laminates having an adhesive layer containing the chlorinated polyolefin resin because of its excellent adhesion. In particular, in the present invention, since it can be produced without using a halogen-based solvent, it is suitable for food packaging applications or precision industrial applications (for example, automotive applications, infrastructure applications, battery packaging materials, etc.) that require specifications that do not use chlorine-based solvents and do not produce by-products.

Claims

1. Application of chlorinated polyolefin resin in the manufacture of food packaging materials, characterized in that: The chlorinated polyolefin resin is a chlorinated polyolefin resin having a chlorine content of 1 to 45% by weight, which is obtained by chlorinating a raw material composition containing at least a polyolefin A having fluidity below 40° C. or its acid-modified product, and a polyolefin B having a melting point of more than 40° C. and less than 150° C. or its acid-modified product, in the absence of an organic solvent. When gas chromatography analysis was performed under the following conditions, no peaks derived from chlorine-based low molecular weight compounds were detected in the retention time range of 4 minutes to 7 minutes. The chlorinated polyolefin resin has a melt viscosity of less than 8,000 mPa·s at 80° C., The weight average molecular weight of polyolefin B is less than 250,000, The mass ratio of polyolefin A or its acid-modified product to polyolefin B or its acid-modified product is 10 / 90 to 90 / 10, <Gas chromatography analysis conditions> A gas chromatograph GC-2010plus Tracera manufactured by Shimadzu Corporation was used, wherein a BID detector was used, the carrier gas was helium with a linear flow rate of 40 cm / sec, the capillary column was Rtx-624 manufactured by Restek, and the capillary column had an inner diameter of 0.32 mm, a film thickness of 1.8 μm, and a length of 30 m. The sample input temperature, i.e., the injection temperature, was 160°C, and the column temperature was 60°C. The chlorinated polyolefin resin was adjusted in p-xylene solvent to a concentration of 5 wt% and then introduced into the apparatus for analysis.

2. The use according to claim 1, wherein: The raw material composition contains at least the polyolefin A and the acid-modified product of the polyolefin B, or contains at least the acid-modified product of the polyolefin A and the acid-modified product of the polyolefin B.

3. The use according to claim 1 or 2, wherein: The weight average molecular weight of the polyolefin B is 8000 or more and less than 250,000.

4. Food packaging material, characterized in that A chlorinated polyolefin resin comprising a chlorinated polyolefin resin having a chlorine content of 1 to 45% by weight, wherein the chlorinated polyolefin resin is obtained by chlorinating a raw material composition comprising at least a polyolefin A having fluidity at 40°C or less or an acid-modified product thereof and a polyolefin B having a melting point of more than 40°C and less than 150°C or an acid-modified product thereof in the absence of an organic solvent, When gas chromatography analysis was performed under the following conditions, no peaks derived from chlorine-based low molecular weight compounds were detected in the retention time range of 4 minutes to 7 minutes. The chlorinated polyolefin resin has a melt viscosity of less than 8,000 mPa·s at 80° C., The weight average molecular weight of polyolefin B is less than 250,000, The mass ratio of polyolefin A or its acid-modified product to polyolefin B or its acid-modified product is 10 / 90 to 90 / 10, <Gas chromatography analysis conditions> A gas chromatograph GC-2010plus Tracera manufactured by Shimadzu Corporation was used, wherein a BID detector was used, the carrier gas was helium with a linear flow rate of 40 cm / sec, the capillary column was Rtx-624 manufactured by Restek, and the capillary column had an inner diameter of 0.32 mm, a film thickness of 1.8 μm, and a length of 30 m. The sample input temperature, i.e., the injection temperature, was 160°C, and the column temperature was 60°C. The chlorinated polyolefin resin was adjusted in p-xylene solvent to a concentration of 5 wt% and then introduced into the apparatus for analysis.

Citation Information

Patent Citations

  • Chlorinated polyolefin resin composition

    JP2015209450A

  • Chlorinated polyolefin resin and method for producing same

    CN112437778A