A composite film material and device for oil-water separation with wide applicability and preparation method
By performing hot pressing and femtosecond laser treatment on titanium foil and polyPTFE powder, composite films with superhydrophobic/superoleophilic and superhydrophilic/underwater superoleophobic surface properties were prepared, solving the difficulties in the existing technology. It is also applicable to the problem of oil-water separation of light oil and heavy oil, achieving high-efficiency, low-cost and large-volume oil-water separation.
Patent Information
- Application Number
- CN202210517948.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-05-12
AI Technical Summary
Existing oil-water separation technology is difficult to simultaneously separate mixtures of light oil and water and heavy oil and water, and traditional methods have problems such as low efficiency, high cost, and narrow scope of application.
Composite films are prepared using titanium foil and polyPTFE powder through a hot pressing process, and femtosecond laser is used for surface roughening and drilling to form superhydrophobic/superoleophilic and superhydrophilic/underwater superoleophobic surface properties, achieving Oil-water separation membranes have wide applicability and high separation efficiency.
It achieves efficient separation of different types of oil-water mixtures, improves separation efficiency and scope of application, reduces operating costs, and is suitable for large-scale oil-water separation.
Smart Images

Figure CN114953497B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional materials and laser micro-processing, and more specifically, relates to a method for preparing an oil-water separation film on a composite functional material by using laser. Background Art
[0002] As the source of human life, water pollution has always attracted widespread attention. At present, many industries and fields, such as the petroleum industry, catering industry, metallurgy industry, mining industry, textile and leather industry, and national defense industry, produce a large amount of oily wastewater every year. If it is directly discharged, it will cause serious pollution to the water body; at the same time, frequent crude oil spills will cause a large number of animals and plants in the ocean and rivers to die, causing serious damage to their ecological balance. Therefore, how to deal with oily wastewater will become a global problem and challenge in solving environmental pollution problems.
[0003] In order to separate oily wastewater, distillation, gravity, centrifugation, flotation, adsorption, coagulation, salting out and biological methods can be used according to the different physical, chemical and biological characteristics of water and oil phases. However, these methods still have the disadvantages of high energy consumption, low efficiency, narrow scope of application and possible secondary pollution, which greatly limits their scope of application. Therefore, it is particularly urgent to develop a low-cost, high-efficiency and widely applicable oil-water separation technology.
[0004] Due to the inconsistency of the surface tension of the oil phase and the water phase, the wetting properties on the surface of some functional materials are inconsistent. By utilizing this difference in wettability, under the action of the liquid's own gravity or external pressure, one component can be selectively allowed to penetrate through the film micropores, while the other component cannot penetrate through the film micropores, thereby achieving the separation of the oil-water mixture. Compared with traditional separation technology, membrane separation technology has the advantages of low operating cost, high separation efficiency, no secondary pollution and a wide range of applications.
[0005] As a typical hydrophobic polymer material (intrinsic water contact angle is about 114°), polytetrafluoroethylene (PTFE) has become an ideal material for preparing oil-water separation membranes because of its good resistance to high and low temperatures, chemical corrosion resistance, aging resistance, and good electrical insulation.
[0006] Titanium is a rare metal with good high and low temperature resistance, excellent ductility and plasticity. At the same time, its hardness is comparable to that of steel, but its mass is only half of that of steel of the same volume. At room temperature, titanium metal does not react with most strong acids, strong bases, or even aqua regia, and has good corrosion resistance, making it another ideal material for preparing oil-water separation membranes.
[0007] Compared with other construction methods, laser processing technology has the advantages of a wide range of processable materials, good regional selective processing, low pollution, and non-contact. In particular, it can perform precision processing with the help of computer software control, which makes it show great advantages in the preparation of oil-water separation membranes.
[0008] At present, there are many methods for constructing oil-water separation films on different functional materials using different methods. Jun Liu et al. reported in the journal (Surface & Coatings Technology, 2016, 307: 171-176) that a superhydrophilic and underwater superoleophobic film was obtained by spraying chitosan-silicon nanoparticles on a stainless steel mesh. Although the preparation method is simple and efficient, the long-term applicability of the oil-water separation film is poor due to the low adhesion between the coating and the stainless steel substrate material. At the same time, its inherent superhydrophilic / superoleophobic wetting properties make it mainly suitable for separating mixtures formed by light oil and water, while the mixture formed by heavy oil and water, due to the high density of heavy oil, is in the lower layer of the solution. During the separation process, the heavy oil will form a barrier layer, making the separation of such oil-water mixtures difficult to achieve, and its application is subject to certain limitations. Zhongli Qin et al. proposed in the journal (Material & Design, 2019, 184: 108200-108208) that a film that can be used for oil-water separation can be prepared by using picosecond infrared laser to roughen the surface of polytetrafluoroethylene film first and then laser etch and drill holes. Although this preparation method can obtain films with different separation properties, due to its unique super-hydrophobic / super-oleophilic properties, it is mainly suitable for separating mixtures formed by heavy oil and water. For mixtures formed by light oil and water, the light oil has a low density, and the denser water layer below will form a barrier layer, making the separation of such oil-water mixtures more difficult to achieve. Chunai Dai et al. published a paper in the journal (Soft Matter, 2014, 10 (40): 8116-8122) on the preparation of super-hydrophobic / super-oleophilic oil-water separation membranes using copper mesh as the substrate by combining chemical oxidation and impregnation. In order to overcome the difficulty in separating the mixture of light oil and water (the water phase is located at the bottom of the oil-water mixture due to its high density, thus forming a barrier layer), the separation device is tilted at a certain angle to allow the light oil to penetrate and flow out of the separation device smoothly. However, the device is only suitable for the separation of oil-water mixtures with a small volume, and is difficult to adapt to the separation of large quantities of oil-water mixtures. In summary, although oil-water separation membranes with different properties can be successfully constructed by different methods, they all face the difficulty of being suitable for separating mixtures formed by light oil and water and mixtures formed by heavy oil and water at the same time, which limits their application range to a certain extent. Therefore, it is particularly necessary to find a membrane or device with a wide range of applications, which can be applied to the separation of large quantities of oil-water mixtures, and can be simply and efficiently implemented in industrial production. Summary of the invention
[0009] In view of the above defects or improvement needs of the prior art, the present invention provides a method for preparing an oil-water separation device with a wide range of applicable performance, which uses titanium foil and poly-PTFE powder as raw materials, and prepares a composite film material with upper and lower layers of titanium foil and PTFE respectively through a hot pressing process, and then uses a femtosecond laser to roughen the upper and lower surfaces of the composite material, and then uses a femtosecond laser to punch holes on the surface of the composite film material after double-sided roughening, thereby obtaining a film material with adjustable oil-water separation rate (flow rate), high separation efficiency, and suitable for separating different types of oil-water mixtures. This solves the technical problem that the existing oil-water separation film cannot be used for large-scale separation of mixtures formed by light oil and water and mixtures formed by heavy oil and water at the same time.
[0010] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a composite film material for oil-water separation having a wide range of applicable properties is provided, characterized in that it comprises the following steps:
[0011] (S1) Preparation of composite thin film material: using polyvinylidene fluoride and polypropylene / TiO2 powder as raw materials, a composite thin film material having a polyvinylidene fluoride layer and a polypropylene / TiO2 layer as upper and lower layers is prepared by a hot pressing process;
[0012] (S2) Laser roughening the surface of the composite film material: using a femtosecond laser to perform laser scanning on the upper and lower surfaces of the composite material in step (S1), respectively, so that the surface of the polyvinylidene fluoride side of the composite material exhibits superhydrophobic / superoleophilic wetting properties, and the surface of the polypropylene / TiO2 side exhibits superhydrophilic / underwater superoleophobic wetting properties;
[0013] (S3) laser drilling: setting an appropriate laser drilling spacing and drilling diameter, and using a femtosecond laser to perform laser drilling on the surface of the composite film material in step (2), thereby obtaining an oil-water separation film with excellent adaptability;
[0014] (S4) Preparation of oil-water separation device: Take two oil-water separation composite films prepared in step (3), one of which has its polyvinylidene fluoride side facing the inside of the device, and the other has its polypropylene / TiO2 side facing the inside, and fix them on both sides of a "T-shaped" oil-water separation device, respectively, to obtain a device that can be used in large quantities to separate different types of oil-water mixtures.
[0015] Furthermore, in the above step (S1), the thickness of the polyvinylidene fluoride layer is 0.10 to 0.70 mm;
[0016] The total thickness of the composite film material prepared in step (S1) is 0.20 mm to 1.40 mm, wherein the upper and lower layers are respectively a polyvinylidene fluoride layer and a polypropylene / TiO2 layer.
[0017] Furthermore, in the composite film material preparation process in the above step (S1), the hot pressing temperature is 300-400°C, the hot pressing pressure is 1-8Mpa, and the hot pressing time is 0.5-2.0h.
[0018] Furthermore, in the above step (S2), the laser scanning method is grid scanning, and the laser scanning etching will construct a rough surface composed of micrometer size and nanometer size on the upper surface and the lower surface of the composite film material respectively;
[0019] The wavelength of the femtosecond laser in step (2) is in the infrared, visible or ultraviolet band, the laser power is preferably 0.5-12 W, the laser pulse frequency is preferably 100 KHz-20 MHz, the laser scanning line spacing is preferably 6-50 μm, and the laser scanning speed is preferably 100-2000 mm / s.
[0020] Furthermore, in the above step (S2), after the composite film material is roughened by laser, the water static contact angle of the polyvinylidene fluoride surface is greater than 150°, and the oil static contact angle is less than 10°; after the composite film material is roughened by laser, the oil static contact angle of the polypropylene / TiO2 layer surface under water is greater than 150°, and the water static contact angle is less than 10°.
[0021] Furthermore, the step (S3) above adopts femtosecond laser drilling, and the punched hole is a conical through hole, and the radius of the conical through hole ranges from 0.5 μm to 300 μm.
[0022] A composite film material for oil-water separation with wide applicability, characterized in that the composite film material is divided into an upper layer and a lower layer, wherein the upper layer and the lower layer are respectively a polyvinylidene fluoride layer and a polypropylene / TiO2 layer;
[0023] The surface of one side of the polyvinylidene fluoride layer exhibits super hydrophobic / super oleophilic wetting properties;
[0024] The surface of one side of the polypropylene / TiO2 layer exhibits superhydrophilic / underwater superoleophobic wetting properties;
[0025] The total thickness of the composite film material of the polyvinylidene fluoride layer and the polypropylene / TiO2 layer is 0.10 to 2.00 mm;
[0026] The surface of the composite film material is punched with conical through holes by laser, and the distance between the holes is 300 μm.
[0027] Furthermore, the diameter of the hole is 20 to 160 μm.
[0028] Furthermore, the composite film material is prepared by uniformly mixing polypropylene powder and TiO2 powder particles with a size of about 10 nm in a mass ratio of 20:1, and then weighing a certain mass of the mixed polypropylene / TiO2 powder and spreading it on a hot pressing molding machine, and then weighing the same mass of PVDF powder and spreading it on the polypropylene / TiO2 mixed powder, and then hot pressing is performed at a hot pressing temperature of 300°C, a pressure of 2.0 Mpa, and a hot pressing time of 1.0 h to prepare a composite film material with a total thickness of 0.40 mm.
[0029] An oil-water separation device, characterized in that any one of the above-mentioned composite film materials is installed on both ends of the oil-water separation device in both directions.
[0030] In general, the above technical solutions conceived by the present invention can achieve the following beneficial effects compared with the prior art:
[0031] (1) The present invention specifically selects polyvinylidene fluoride powder as the raw material for preparing the composite film. First, polyvinylidene fluoride is a typical hydrophobic material. After laser processing, the surface of polyvinylidene fluoride exhibits super hydrophobic and super oleophilic properties, making it an ideal material for preparing oil-water mixture separation films. Secondly, polyvinylidene fluoride has good resistance to high and low temperatures, chemical corrosion, and aging, so that the separation film prepared from polyvinylidene fluoride can be used for oil-water separation in any harsh environment, effectively improving the applicability of the prepared composite film material for separating oil-water mixtures.
[0032] (2) The present invention specifically selects polypropylene powder and nano-TiO2 as raw materials for preparing composite films. First, polypropylene is a hydrophilic polymer material. After laser processing, the surface of polypropylene will show super-hydrophilicity and underwater super-oleophobicity, which is an ideal material for preparing oil-water mixture separation films. Secondly, polypropylene has good mechanical properties, chemical stability, high and low temperature resistance and weather resistance, but its hardness, wear resistance and hardness are not very high. In order to modify its physical properties, TiO2 with good hydrophilicity is selected as a modifier, which can effectively improve the physical and chemical properties of the material, especially improve its super-hydrophilicity and underwater super-oleophobic wetting properties.
[0033] (3) After processing, the surface of the polypropylene / TiO2 layer of the composite film material of the present invention exhibits superhydrophilicity and underwater superoleophobicity, while the surface of the polyvinylidene fluoride layer exhibits superhydrophobicity and superoleophilicity, and the wetting properties of the two surfaces are exactly opposite. Utilizing the opposite wetting properties, in the design of an actual oil-water separation device, when the polypropylene / TiO2 layer of the composite film material faces the oil-water mixture, the water phase in the mixture can selectively permeate through the composite film material, while the oil phase cannot; and when the polyvinylidene fluoride side of the composite film material faces the oil-water mixture, the phase in the mixture can selectively permeate through the composite film material, while the water phase cannot. Therefore, in the design of the oil-water separation device, two processed composite film materials are set, and the two film materials are facing the oil-water mixture on different sides, which can ensure that the oil phase and the water phase can simultaneously permeate through the film facing the solution as the polyvinylidene fluoride side and the film facing the solution as the polypropylene / TiO2 layer side, respectively, thereby ensuring that the oil-water separation device can be simultaneously used for analyzing a mixture formed by heavy oil and water and a mixture formed by light oil and water.
[0034] (4) By utilizing the characteristics of laser processing, such as high precision, good controllability, and high efficiency, and the fact that the process parameters and processing graphics can be quickly changed and designed directly on a computer, it is possible to efficiently prepare oil-water separation membranes with different flow rates and sizes, thus making it have strong engineering application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Composite film preparation process flow chart,
[0036] The sequence is: mixing TiO2 nanoparticles with polypropylene powder → laying of polypropylene / TiO2 powder → laying of polyvinylidene fluoride powder → hot pressing → composite film;
[0037] Figure 2 Process flow chart for preparing composite membrane with oil-water separation function.
[0038] The sequence is: laser roughening of the surface of the polypropylene / TiO2 layer → laser roughening of the surface of the polyvinylidene fluoride → laser drilling;
[0039] Figure 3 Scanning electron microscope image of the surface morphology of the oil-water composite film obtained after laser roughening and drilling (observed from the polyvinylidene fluoride side);
[0040] Figure 4 For water and oil (petroleum ether) Figure 2 Schematic diagram of the static contact angle on one side of the surface of the prepared composite film polyvinylidene fluoride;
[0041] Figure 5 For water and oil (petroleum ether) Figure 2 Schematic diagram of the static contact angle on one side of the surface of the polypropylene / TiO2 layer of the prepared composite film;
[0042] Figure 6 Schematic diagram of the device design for using the prepared membrane to separate oil-water mixture. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0044] The present invention provides a method for preparing an oil-water separation film material and an application thereof in an oil-water separation device, characterized in that the method comprises the following steps:
[0045] (1) Preparation of composite film: Using polyvinylidene fluoride and polypropylene / TiO2 powder as raw materials, a hot pressing process is adopted to prepare a composite film material with a polyvinylidene fluoride layer and a polypropylene / TiO2 layer as the upper and lower layers. In step (1), although polypropylene has good mechanical properties, chemical stability, high and low temperature resistance and weather resistance, its hardness, wear resistance and hardness are not very high. In order to modify its physical properties, TiO2 with good hydrophilicity is specially selected as a modifier, which can effectively improve the physical and chemical properties of the material and enhance its super hydrophilicity and underwater super oleophobic wetting properties.
[0046] (2) Laser roughening of the composite surface: The upper and lower surfaces of the composite material obtained in step (1) are laser processed by femtosecond laser. By changing the laser processing parameters, the upper and lower surfaces of the composite material are roughened by the etching effect of the femtosecond laser to obtain a super-hydrophobic / super-oleophilic polyvinylidene fluoride surface and a super-hydrophilic / underwater super-oleophobic polypropylene / TiO2 surface. In step (2), the purpose of laser processing the upper and lower surfaces of the composite material is to increase the roughness of the upper and lower surfaces, so that the polyvinylidene fluoride surface exhibits super-hydrophobic / super-oleophilic wetting properties, while the polypropylene / TiO2 surface exhibits super-hydrophilic and underwater super-oleophobic wetting properties. In the process of roughening the upper and lower surfaces of the composite film material, due to the different etching thresholds of polyvinylidene fluoride and polypropylene / TiO2, the selected laser processing parameters are inconsistent. However, due to the limitation of the thin thickness of the prepared composite film, the laser processing parameters used for surface roughening are usually carried out at a lower laser power and a faster scanning rate. If the laser processing power is too high, the material on the upper or lower surface of the composite film will be completely etched away.
[0047] (3) Laser drilling: Set the appropriate laser drilling spacing and aperture size, and use a femtosecond laser to perform laser drilling on the roughened composite film material surface obtained in step (2); after cleaning and drying, obtain an oil-water separation film with a wide range of adaptability; in step (3), the laser processing method is to construct through holes of different aperture sizes in the composite film obtained in (2) according to the requirements of the engineering design. Since the composite film material needs to be punched through, the laser power required in the processing process is relatively large and the scanning speed is relatively small. However, in order to prevent the thermal effect during the processing from causing the constructed through hole to deform, thereby affecting the oil-water separation performance of the film, it is usually required that the laser scanning speed used in the drilling process should not be too low.
[0048] (4) Preparation of oil-water separation device: Take two sheets of the oil-water separation composite film prepared in step (3) and fix them on both sides of the "T-shaped" oil-water separation device, and place the two sheets of film material with different sides facing the oil-water mixture.
[0049] The simultaneous use of composite film materials is to ensure that when the prepared oil-water separation device separates any type of oil-water mixture, the presence of a certain liquid phase in the oil-water mixture will not become a barrier layer for another liquid phase in the separation process, thereby ensuring that the oil-water separation device has a wide range of applicability. In step (4), it is necessary to ensure that the two oil-water separation film materials used are oriented in different directions, that is, one side of the polypropylene / TiO2 layer of one of the oil-water separation films is oriented toward the oil-water mixture to be separated. Since the surface exhibits superhydrophilic and underwater superoleophobic wetting properties, the water phase in the oil-water mixture will penetrate and pass through the film, while the oil phase will be blocked and cannot pass through; at the same time, the polyvinylidene fluoride surface of the other oil-water separation film is oriented toward the oil-water mixture to be separated. Since the surface exhibits superhydrophobic / superoleophilic wetting properties, the oil phase in the oil-water mixture will penetrate and pass through the film, while the water phase will be blocked and cannot pass through. Therefore, by simply utilizing the different directions of the two oil-water separation composite films, the oil phase and the water phase in different types of oil-water mixtures can be easily separated from the two films respectively, effectively improving their wide performance and engineering application value.
[0050] In a preferred embodiment, the purpose of adding TiO2 to the polypropylene layer in step (1) of the present invention is to improve the hydrophilic wettability of the polypropylene layer and improve its physical and chemical properties. Since the melting point of polypropylene is only about 165°C, the heat resistance is not very high. As a typical inorganic oxide, TiO2 has a relatively high melting point (1850°C, rutile type) and boiling point (3200°C, rutile type). Adding it to polypropylene can significantly improve its heat resistance. At the same time, TiO2 has good hydrophilic properties and physical properties, and its addition is also helpful to improve the hydrophilic wettability and physical properties of the polypropylene layer.
[0051] In some embodiments, the size of the TiO2 nanoparticles added to the polypropylene layer in step (1) is preferably 5 nm to 100 nm.
[0052] In the preparation of the composite film of the present invention, the hot pressing process is preferably 300-400° C., the hot pressing pressure is preferably 1-8 MPa, and the hot pressing time is preferably 0.5-2.0 h.
[0053] In some embodiments, the total thickness of the prepared composite film material is 0.20-1.40 mm, wherein the thickness of the polyvinylidene fluoride sheet material is 0.10-0.70 mm.
[0054] In some embodiments, the laser scanning method used in step (2) to roughen the surfaces on both sides of the composite film is preferably grid scanning. The laser etching roughening can construct a conical micron-sized protrusion structure on the film surface. At the same time, the surface of the micron protrusion structure is also covered with a large number of nano protrusions and hole structures. The rough structure makes the wettability of the constructed surface is isotropic.
[0055] According to the Wenzel model in wetting theory, it can be seen that the presence of rough structures will amplify the wettability of the solid surface. Therefore, laser roughening treatment will make the surface of one side of the composite film PVDF more hydrophobic and oleophilic, making it a super-hydrophobic / super-oleophilic surface. At the same time, after roughening treatment, the surface of the polypropylene / TiO2 layer is more hydrophilic and oleophobic, making it a super-hydrophilic / underwater super-oleophobic surface. Therefore, laser roughening will amplify the wettability of the surfaces on both sides of the composite material at the same time, and the wettability on both sides is completely opposite.
[0056] The present invention utilizes the difference of wetting properties on both sides of composite film, and it can be applied to separate different types of oil-water mixtures. Wherein, after coarsening, one side of composite film PVDF presents super hydrophobic / super oleophilic wetting properties. If the surface is toward the oil-water mixture, only the oil phase therein can be passed, and the water phase cannot pass, and it is suitable for separating the mixture formed by heavy oil and water. And after coarsening, one side of composite film polypropylene / TiO2 layer presents super hydrophilic / underwater super oleophobicity. If the surface is toward the oil-water mixture, only the water phase therein can be passed, and the oil phase cannot pass, and it is suitable for separating the mixture formed by light oil and water. Therefore, by utilizing the difference of composite film towards after coarsening, different types of oil-water mixtures can be separated.
[0057] The present invention uses a high-power, low-scanning-speed laser to drill holes in a composite film, with the aim of constructing a large number of through holes in the composite film, so that under the action of the liquid's own gravity or external force, liquid close to the membrane material can penetrate and pass through, while liquid incompatible with the membrane material cannot spread on its surface and appears in a droplet shape. When the droplet radius is larger than the diameter of the through hole, even under the action of the liquid's own gravity or external force, it cannot penetrate and pass through the through hole, thereby achieving separation of the oil-water mixture.
[0058] The present invention utilizes computer software to accurately design the aperture of the processed through hole and the number of through holes per unit area. Combined with the characteristics of laser precision processing, oil-water separation films with different flow rates can be constructed according to the needs of engineering design, thereby meeting different engineering needs for oil-water separation.
[0059] In the present invention, the bond energy of the CF bond in the PVDF material is relatively large, and its laser etching threshold is relatively high. The polypropylene / TiO2 layer contains two materials, TiO2 and polypropylene, and its laser etching threshold is also inconsistent. Because, in order to obtain a better roughened surface and punched hole shape, a femtosecond laser is specially selected to roughen and punch the composite film, rather than a nanosecond laser and a picosecond laser. The main reason is that the pulse width of the femtosecond laser is in the femtosecond order, and the peak energy of the laser is relatively high. In the process of processing the composite film, it is mainly "cold" etching, and there is less thermal effect in the etching process, and it is easier to build a richer micro-nano structure on the surface of the composite film, which is extremely beneficial to improving the wetting properties of the material. However, due to the large pulse width and low peak energy of nanosecond lasers and picosecond lasers, the thermal effect in the processing process is relatively large, resulting in less nanostructure when the surface is roughened, and the roughening effect is not ideal. At the same time, when using nanosecond lasers and picosecond lasers for punching, the large thermal effect will also cause deformation problems in the punched through holes.
[0060] In a preferred embodiment, a "T-shaped" oil-water separation device is used in step (4) of the present invention. By utilizing the different orientations of the two oil-water separation composite membranes, the oil phase and the water phase in different types of oil-water mixtures can be separated from the two sides of the "T-shaped" oil-water separation device, respectively, thereby effectively improving its applicability. At the same time, the orientations of the two membranes can be changed at the same time, thereby increasing the service life of the oil-water separation membrane.
[0061] The following are examples:
[0062] Example 1
[0063] (1) Preparation of composite film material: The process flow for preparing the composite film material of the present invention is shown in Figure 1As shown, the sequence is: mixing TiO2 nanoparticles with polypropylene powder → laying of polypropylene / TiO2 powder → laying of polyvinylidene fluoride powder → hot pressing → composite film. The specific steps are: uniformly mixing polypropylene powder with TiO2 powder particles with a size of 5nm in a mass ratio of 20:1, then weighing a certain mass of the mixed polypropylene / TiO2 powder and laying it flat in a hot pressing machine, then weighing the same mass of PVDF powder and laying it flat on the polypropylene / TiO2 mixed powder, and then hot pressing, the hot pressing temperature is 300℃, the pressure is 2.0 Mpa, the hot pressing time is 1.0 h, and the thickness of the prepared composite film is 0.30mm.
[0064] Figure 2 The process flow chart for preparing a composite film with oil-water separation function is as follows: laser roughening of the surface of the polypropylene / TiO2 layer → laser roughening of the surface of the polyvinylidene fluoride → laser drilling.
[0065] (2) Laser roughening: The composite film prepared in step (1) is placed and fixed on a laser processing platform, and a femtosecond laser with a wavelength of 1030 nm and a focused spot diameter of 20 μm is used. The grid scanning method is used to first perform laser roughening on the surface of the polypropylene / TiO2 layer of the composite film. The laser processing parameters are: laser power of 3 W, pulse frequency of 400 KHz, scanning speed of 1200 mm / s, and scanning spacing of 30 μm. Then, the surface of the PVDF layer of the composite film is laser roughened. The laser processing parameters are: laser power of 4 W, pulse frequency of 400 KHz, scanning speed of 1000 mm / s, and scanning spacing of 30 μm.
[0066] (3) Laser drilling: According to the design requirements of the oil-water separation project, the designed hole diameter is 160 μm and the hole spacing is 300 μm. Then, a femtosecond laser with a wavelength of 800 nm and a focused spot diameter of 20 μm is used to drill holes in the composite film roughened in step (2) at a relatively high laser power. When drilling, ensure that the surface of the polypropylene / TiO2 layer of the composite film faces upward. The laser parameters for drilling are: laser power of 12 W, pulse frequency of 400 KHz, and scanning speed of 200 mm / s.
[0067] Figure 3 This is a scanning electron microscope image of the surface morphology of the composite film after laser roughening and drilling (observed from the polyvinylidene fluoride side). It can be seen that the surface of the polyvinylidene fluoride side of the composite film is covered with a large number of micron-sized cone protrusions. This rough structure can effectively improve its wetting properties. At the same time, the film surface is also covered with neatly arranged through-hole array structures, with a distance of 300μm between holes, which is achieved with the help of laser drilling.
[0068] Figure 4 (a) and (b) are the static contact angles of water and oil (petroleum ether) on one side of the composite film PVDF surface prepared in step (2). It can be seen that the laser roughening and drilling treatment makes the surface of one side of the composite film PVDF show super hydrophobic / super oleophilic wetting properties;
[0069] Figure 5 (a) and (b) are schematic diagrams of the static contact angles of water and oil (petroleum ether) on one side of the surface of the composite film polypropylene / TiO2 layer prepared in step (2). It can be seen that the laser roughening and drilling treatment makes the surface of one side of the composite film polypropylene / TiO2 layer show superhydrophilic / underwater superoleophobic wetting properties, which is also extremely beneficial to improving the efficiency of oil-water separation. The surface of the composite film material is laser-punched with conical through holes, and the hole diameter facing the laser is large, and the distance between the holes is 300μm.
[0070] (4) Preparation of oil-water separation device: Figure 6 Schematic diagram of the design of the prepared film for oil-water mixture separation device. The specific steps are: install the two composite films prepared in (3) at the two ends of the "T-shaped" oil-water separation device respectively, and during installation, ensure that the different sides of the two composite film materials face the oil-water mixture.
[0071] The oil-water separation performance of the prepared oil-water separation device was measured, and a mixture of petroleum ether and water (volume ratio 1:1) was used as the measuring medium. After 5 parallel experiments, the results showed that the time for 1000 ml of oil-water mixture to pass through the oil-water separation device with a membrane area of 30mm×30mm was 7.6s, and its total flow rate was 154.6 L / (m2·s). At the same time, after measurement, the corresponding oil-water separation efficiency reached 91.43%. Taking the separation efficiency lower than 90% as the basis for judging the service life of the oil-water separation membrane, the service life of the oil-water separation membrane can reach 8.65h.
[0072] Example 2
[0073] (1) Preparation of composite film materials: Polypropylene powder and TiO2 powder particles with a size of about 10 nm were uniformly mixed in a mass ratio of 20:1. Then, a certain mass of the mixed polypropylene / TiO2 powder was weighed and spread on a hot pressing machine. Then, the same mass of PVDF powder was weighed and spread on the polypropylene / TiO2 mixed powder. Then, hot pressing was performed at a temperature of 300 °C, a pressure of 2.0 MPa, and a time of 1.0 h to obtain a composite film with a total thickness of 0.40 mm.
[0074] (2) Laser roughening: The composite film prepared in step (1) is placed and fixed on a laser processing platform, and a femtosecond laser with a wavelength of 800 nm and a focused spot diameter of 20 μm is used to roughen the surface of the polypropylene / TiO2 layer of the composite film by a grid scanning method. The roughening parameters are: laser power of 4.0 W, pulse frequency of 400 KHz, scanning speed of 1500 mm / s, and scanning spacing of 30 μm. Then, the surface of the PVDF layer of the composite film is roughened. The laser processing parameters are: laser power of 4.0 W, pulse frequency of 200 KHz, scanning speed of 1300 mm / s, and scanning spacing of 30 μm.
[0075] (3) The drilling diameters were designed to be 20 μm, 40 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, and 160 μm, respectively. The distance between through holes was 300 μm. A femtosecond laser with a wavelength of 800 nm and a focused spot diameter of 20 μm was used for drilling. The drilling parameters were: laser power of 10 W, pulse frequency of 200 kHz, and scanning speed of 150 mm / s.
[0076] (4) Preparation of oil-water separation device: The two oil-water separation composite films prepared in (3) are installed at the two ends of the "T-shaped" oil-water separation device. During installation, ensure that different sides of the two film materials face the oil-water mixture.
[0077] The oil-water separation efficiency and flow rate were tested using a mixture of cyclohexane and water as the medium. The results are shown in Table 1.
[0078] Table 1 Separation efficiency and flow rate of oil-water separation devices with different through-hole diameters
[0079] .
[0080] It can be seen from Table 1 that as the through-hole diameter continues to increase, the flow rate of oil and water separated by the oil-water separation device continues to increase, while the corresponding oil-water separation efficiency continues to decrease.
[0081] (5) Comparative test of separation rate (flow rate) and service life
[0082] A single-layer polyvinylidene fluoride film and a single-layer film constructed of two materials, polypropylene powder and nano-TiO2, were selected, both of which were 0.40 mm thick. They were processed according to the same process conditions as those for preparing the composite film. Then, the two films were installed in a "T-type" oil-water separation. The separation rate and service life of the oil-water mixture were tested and compared with the composite film of the present invention. The results are shown in Table 2.
[0083] Table 2 Comparison of separation rate and service life of single-layer film and composite film materials
[0084] .
[0085] It can be seen from Table 2 that, under the condition of keeping the membrane separation efficiency almost the same, the oil-water separation rate of the composite membrane can be increased by about 40%, and the service life can be increased to 2.7 times the original service life.
Claims
1. A method for preparing a composite film material for oil-water separation with wide applicability, characterized in that: The steps include: (S1) Preparation of composite thin film material: using polyvinylidene fluoride and polypropylene / TiO2 powder as raw materials, a composite thin film material having a polyvinylidene fluoride layer and a polypropylene / TiO2 layer as upper and lower layers is prepared by a hot pressing process; (S2) Laser roughening the surface of the composite film material: using a femtosecond laser to perform laser scanning on the upper and lower surfaces of the composite material in step (S1), respectively, so that the surface of the polyvinylidene fluoride side of the composite material exhibits superhydrophobic / superoleophilic wetting properties, and the surface of the polypropylene / TiO2 side exhibits superhydrophilic / underwater superoleophobic wetting properties; (S3) laser drilling: setting an appropriate laser drilling spacing and drilling diameter, and using a femtosecond laser to perform laser drilling on the surface of the composite film material in step (2), thereby obtaining an oil-water separation film with excellent adaptability; (S4) Preparation of oil-water separation device: Take two oil-water separation composite films prepared in step (3), one of which has the polyvinylidene fluoride side facing the inside of the device, and the other has the polypropylene / TiO2 side facing the inside, and fix them respectively on both sides of the "T-shaped" oil-water separation device, so as to obtain a device that can separate different types of oil-water mixtures in large quantities.
2. The preparation method according to claim 1, characterized in that In the step (S1), the thickness of the polyvinylidene fluoride layer is 0.10 to 0.70 mm; The total thickness of the composite film material prepared in the step (S1) is 0.20 mm to 1.40 mm, wherein the upper and lower layers are respectively a polyvinylidene fluoride layer and a polypropylene / TiO2 layer.
3. The preparation method according to claim 1, characterized in that: In the composite film material preparation process of step (S1), the hot pressing temperature is 300-400°C, the hot pressing pressure is 1-8Mpa, and the hot pressing time is 0.5-2.0h.
4. The preparation method according to claim 1, characterized in that: In the step (S2), the laser scanning method is grid scanning, and the laser scanning etching will construct a rough surface composed of micrometer size and nanometer size on the upper surface and the lower surface of the composite film material respectively; The wavelength of the femtosecond laser in step (2) is in the infrared, visible or ultraviolet band, the laser power is 0.5-12W, the laser pulse frequency is 100KHz-20MHz, the laser scanning line spacing is 6-50μm, and the laser scanning speed is 100-2000mm / s.
5. The preparation method according to claim 1, characterized in that: In the step (S2), after the composite film material is roughened by laser, the water static contact angle of the polyvinylidene fluoride surface is greater than 150°, and the oil static contact angle is less than 10°; after the composite film material is roughened by laser, the oil static contact angle of the polypropylene / TiO2 layer surface under water is greater than 150°, and the water static contact angle is less than 10°.
6. The preparation method according to claim 1, characterized in that: The step (S3) uses femtosecond laser drilling, and the punched hole is a conical through hole, and the radius of the conical through hole ranges from 0.5 μm to 300 μm.