Preparation technology and equipment of reinforced magnesium-titanium composite materials

By annealing and surface coating treatment of magnesium and titanium plates, combined with rolling and leveling treatment, the problem of low interface strength of magnesium-titanium composites is solved, and the interface strength of magnesium-titanium composites is improved.

CN114953697BActive Publication Date: 2024-11-22BAOJI TITANIUM VALLEY LONG METAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210631467.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-06
Publication Date
2024-11-22
Estimated Expiration
2042-06-06

AI Technical Summary

Technical Problem

When magnesium-titanium composites are prepared by rolling composite, it is difficult for magnesium and titanium to form a stable metal interface, resulting in a lower interface strength.

Method used

By annealing the magnesium and titanium plates, adding metal coatings such as copper, aluminum or nickel to the surface, they are laminated, pressed and rolled, and then cut and annealed on the leveling machine to form a stable metal interface.

Benefits of technology

The interface strength of magnesium-titanium composite materials has been improved, and the problem that magnesium and titanium are difficult to form a stable interface is solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114953697B_ABST
    Figure CN114953697B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of material processing, and in particular to a process and equipment for preparing a reinforced magnesium-titanium composite material. First, the annealed magnesium plate and the titanium plate on which the coating is to be added are subjected to a decontamination and rust removal treatment, and then the coatings are respectively added to the cleaned magnesium plate and the titanium plate, wherein a copper coating is added to the magnesium plate, and an aluminum or nickel coating is added to the titanium plate. The coated sides of the magnesium plate and the titanium plate are respectively pressed together and rolled on a rolling mill, and then leveled on a leveling machine to cut off the uncompounded or cracked parts, and then the obtained composite plate is annealed to obtain the required magnesium-titanium plate. By adding the coating to the magnesium plate and the titanium plate, a stable metal interface can be formed between the magnesium plate and the titanium plate, thereby improving the interface strength of the magnesium-titanium plate formed by the composite of the magnesium plate and the titanium plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material processing, and in particular to a preparation process and equipment for a reinforced magnesium-titanium composite material. Background Art

[0002] Magnesium and magnesium alloys are the lightest metal structural materials in current engineering applications and are widely used in the automotive industry and aerospace fields. Existing technologies use explosive composite methods and rolling composite methods to prepare magnesium-titanium composite materials.

[0003] When the existing magnesium-titanium composite material is prepared by the explosion composite method, since the explosion will generate vibration, noise and smoke, which will have an impact on the environment, the magnesium-titanium composite material is prepared by the rolling composite method.

[0004] When magnesium-titanium composite materials are prepared by rolling composite method, as shown in the magnesium-titanium phase diagram ( Figure 5 ), it is difficult for magnesium and titanium to form a stable metal interface, resulting in a low interface strength of the formed composite material. Summary of the invention

[0005] The purpose of the present invention is to provide a process and equipment for preparing a reinforced magnesium-titanium composite material, which solves the technical problem that when the magnesium-titanium composite material is prepared by a rolling composite method, it is difficult for magnesium and titanium to form a stable metal interface, thereby resulting in low interface strength of the formed composite material.

[0006] To achieve the above object, the present invention provides a process for preparing a reinforced magnesium-titanium composite material, comprising the following steps:

[0007] Annealing of magnesium and titanium plates;

[0008] First, select the materials: AZ series and ZEK series for magnesium plates, and TA1, TA2 and TC4 for titanium plates;

[0009] Then the selected materials were annealed, specifically: the magnesium alloy plate was heated to 290°C, kept warm for 45 minutes, and air-cooled; the titanium plate was heated to 550°C, kept warm for 60 minutes, and air-cooled.

[0010] Plate surface treatment;

[0011] First: Use coarse sandpaper (60-80 mesh) to grind in one direction to remove the surface oxide layer;

[0012] Secondly: first use 3% to 5% NaOH solution, which is formed by mixing hot water (45 to 60° C.) and NaOH, then use 2% to 3% hydrochloric acid solution for cleaning, and finally use alcohol to clean and blow dry.

[0013] Adding coatings on the magnesium plate and the titanium plate respectively, wherein the thickness of the coatings is about 0.05 to 0.1 micrometers;

[0014] The magnesium plate to which the coating is added is pressed against the surface to be composited of the titanium plate, and then rolled on a rolling mill to obtain a magnesium-titanium plate;

[0015] The magnesium-titanium plate is leveled on a leveling machine, and the uncompounded or cracked parts on the four edges of the leveled magnesium-titanium plate are cut off to obtain the required reinforced magnesium-titanium plate.

[0016] Wherein, the coating is a metal coating of copper, aluminum or nickel, a copper coating is added to the magnesium plate, and an aluminum or nickel coating is added to the titanium plate.

[0017] The present invention also provides a reinforced magnesium-titanium composite material preparation device, including a processing table and an adjustment component; the adjustment component includes a support column, a mounting seat, a hydraulic cylinder, a transverse telescopic rod, a drive motor, a rotating rod and a steering plate, the support column is fixedly mounted on the upper surface of the processing table, the mounting seat is slidably connected to the support column and passes through the support column, the hydraulic cylinder is fixedly mounted on the lower surface of the mounting seat, the transverse telescopic rod is connected to the output end of the hydraulic cylinder and is located on the side of the hydraulic cylinder away from the mounting seat, the drive motor is fixedly mounted on one end of the transverse telescopic rod away from the hydraulic cylinder, the rotating rod is connected to the output end of the drive motor and is located on the side of the drive motor away from the transverse telescopic rod, and the steering plate is fixedly mounted on one end of the rotating rod away from the drive motor.

[0018] Wherein, the adjustment assembly further includes a first fixed block and a first movable block, wherein the first fixed block is fixedly mounted on the upper surface of the steering plate; the first movable block is slidably connected to the steering plate and is located on the upper surface of the steering plate.

[0019] Wherein, the reinforced magnesium-titanium composite material preparation equipment also includes a fixing component, and the fixing component is located above the processing table.

[0020] Wherein, the fixing assembly comprises a second fixing block and a second movable block, the second fixing block is fixedly mounted on the upper surface of the processing table; the second movable block is slidably connected to the processing table and is located on the upper surface of the processing table.

[0021] Among them, the fixing assembly also includes a second electric cylinder and a second telescopic rod, the second electric cylinder is fixedly installed on the upper surface of the processing table; the two ends of the second telescopic rod are respectively connected to the output end of the second electric cylinder and the second movable block, and the second telescopic rod is located between the second electric cylinder and the second movable block.

[0022] The present invention provides a process and equipment for preparing a reinforced magnesium-titanium composite material. First, the annealed magnesium plate and the side of the titanium plate to which the coating is to be added are subjected to a decontamination and rust removal treatment. Then, the coating is added to the cleaned magnesium plate and the titanium plate, respectively, wherein a copper coating is added to the magnesium plate, and an aluminum or nickel coating is added to the titanium plate. The magnesium plate and the titanium plate are respectively pressed together on the sides to which the coating is added, and rolled on the rolling mill. After leveling on the leveling machine, the uncompounded or cracked parts are cut off, and the resulting composite plate is annealed to obtain the required magnesium-titanium plate. By adding the coating to the magnesium plate and the titanium plate, a stable metal interface can be formed between the magnesium plate and the titanium plate, thereby improving the interface strength of the magnesium-titanium plate formed by the composite of the magnesium plate and the titanium plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 It is a flowchart of the first embodiment of the present invention.

[0025] Figure 2 It is a schematic diagram of the overall structure of the first embodiment of the present invention.

[0026] Figure 3 It is a schematic diagram of the connection between the cylinder and the vertical telescopic rod according to the second embodiment of the present invention.

[0027] Figure 4 It is a schematic diagram of the overall structure of the third embodiment of the present invention.

[0028] Figure 5 It is the magnesium-titanium phase diagram in the background technology of the present invention.

[0029] In the figure: 101-processing table, 102-adjusting component, 103-support column, 104-mounting seat, 105-hydraulic cylinder, 106-lateral telescopic rod, 107-driving motor, 108-rotating rod, 109-steering plate, 110-first fixed block, 111-first movable block, 112-first electric cylinder, 113-first telescopic rod, 114-connecting plate, 115-cylinder, 116-vertical telescopic rod, 201-fixed component, 202-second fixed block, 203-second movable block, 204-second electric cylinder, 205-second telescopic rod. DETAILED DESCRIPTION

[0030] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0031] In the description of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, in the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined.

[0032] First embodiment:

[0033] See also Figure 1 , Figure 1 The present invention provides a process for preparing a reinforced magnesium-titanium composite material, which includes the following steps:

[0034] S101, magnesium plate and titanium plate annealing;

[0035] First, select the material.

[0036] First, select the materials: AZ series and ZEK series for magnesium plates, and TA1, TA2 and TC4 for titanium plates;

[0037] Then the selected materials were annealed, specifically: the magnesium alloy plate was heated to 290°C, kept warm for 45 minutes, and air-cooled; the titanium plate was heated to 550°C, kept warm for 60 minutes, and air-cooled.

[0038] S102, sheet surface treatment;

[0039] First: Use coarse sandpaper (60-80 mesh) to grind in one direction to remove the surface oxide layer;

[0040] Secondly: first use 3% to 5% NaOH solution, which is formed by mixing hot water (45 to 60° C.) and NaOH, then use 2% to 3% hydrochloric acid solution for cleaning, and finally use alcohol to clean and blow dry.

[0041] S103, adding a coating to the magnesium plate and the titanium plate respectively, wherein the coating has a thickness of about 0.05 to 0.1 micrometers;

[0042] S104, laminating and pressing the magnesium plate to which the coating is added and the surface to be composited of the titanium plate, and rolling them on a rolling mill to obtain a magnesium-titanium plate;

[0043] S105, leveling the magnesium-titanium plate on a leveling machine, and cutting off the uncompounded or cracked parts on the four edges of the leveled magnesium-titanium plate to obtain the required reinforced magnesium-titanium plate.

[0044] Wherein, the coating is a metal coating of copper, aluminum or nickel, a copper coating is added to the magnesium plate, and an aluminum or nickel coating is added to the titanium plate.

[0045] When using a process for preparing a reinforced magnesium-titanium composite material according to the present embodiment, the annealed magnesium plate and the titanium plate on the side to which the coating is to be added are firstly subjected to a decontamination and rust removal treatment, and then the coating is added to the cleaned magnesium plate and the titanium plate respectively, wherein a copper coating is added to the magnesium plate and an aluminum or nickel coating is added to the titanium plate, and the magnesium plate and the titanium plate on the sides to which the coating is added are respectively bonded and pressed, and then rolled on a rolling mill.

[0046] Before rolling, the magnesium plate and the titanium plate after adding the coating are preheated in a heating furnace at a preheating temperature of 380°C for 20 minutes. Then hot rolling is carried out at a hot rolling temperature of 400° to 450°C, an initial reduction of 25%, a rolling rate of 0.1 m / s, a total reduction of 35% to 40%, and three rolling passes.

[0047] During the rolling process, the heated magnesium plate and the titanium plate are placed on a rolling mill, and the magnesium plate and the titanium plate are compressed between two rotating rollers by utilizing the plasticity of the metal to produce plastic deformation, thereby obtaining the desired magnesium-titanium plate, and then the rolled magnesium-titanium plate is leveled on a leveling machine, and the uncompounded or cracked parts are cut off, and then the obtained composite plate is annealed at a temperature of 220°C, an annealing time of 90 minutes, and air cooling. Thus, the desired magnesium-titanium plate is obtained, and by adding a coating to the magnesium plate and the titanium plate, a stable metal interface can be formed between the magnesium plate and the titanium plate, thereby improving the interface strength of the magnesium-titanium plate formed by the composite of the magnesium plate and the titanium plate.

[0048] Second embodiment:

[0049] Based on the first embodiment, please refer to Figure 2 and Figure 3 , Figure 2 is a schematic structural diagram of a reinforced magnesium-titanium composite material preparation device according to a second embodiment, Figure 3It is a schematic diagram of the connection between the cylinder 115 and the vertical telescopic rod 116. The present invention provides a reinforced magnesium-titanium composite material preparation device including a processing table 101 and an adjustment component 102. The adjustment component 102 includes a support column 103, a mounting seat 104, a hydraulic cylinder 105, a lateral telescopic rod 106, a drive motor 107, a rotating rod 108, a steering plate 109, a first fixed block 110, a first movable block 111, a first electric cylinder 112, a first telescopic rod 113, a connecting plate 114, a cylinder 115 and a vertical telescopic rod 116.

[0050] In this embodiment, the adjustment component 102 is located on the processing table 101, so that the magnesium plate after coating is turned over and placed on the titanium plate for fitting and pressing.

[0051] The support column 103 is fixedly mounted on the upper surface of the processing table 101, the mounting seat 104 is slidably connected to the support column 103 and penetrates the support column 103, the hydraulic cylinder 105 is fixedly mounted on the lower surface of the mounting seat 104, the transverse telescopic rod 106 is connected to the output end of the hydraulic cylinder 105 and is located on the side of the hydraulic cylinder 105 away from the mounting seat 104, the drive motor 107 is fixedly mounted on the end of the transverse telescopic rod 106 away from the hydraulic cylinder 105, the rotating rod 108 is connected to the output end of the drive motor 107 and is located on the side of the drive motor 107 away from the transverse telescopic rod 106 The steering plate 109 is fixedly mounted on one end of the rotating rod 108 away from the driving motor 107. The mounting seat 104 has a through hole, and the support column 103 passes through the through hole of the mounting seat 104, so that the mounting seat 104 can slide vertically on the support column 103. The output end of the hydraulic cylinder 105 is connected to the transverse telescopic rod 106, and drives the transverse telescopic rod 106 to extend and retract, so that the driving motor 107 moves laterally. The output end of the driving motor 107 is connected to the rotating rod 108, and drives the rotating rod 108 to rotate, so that the steering plate 109 rotates following the rotating rod 108.

[0052] Secondly, the first fixed block 110 is fixedly installed on the upper surface of the steering plate 109; the first movable block 111 is slidably connected to the steering plate 109 and is located on the upper surface of the steering plate 109. The first fixed block 110 and the first movable block 111 are both L-shaped. The first movable block 111 slides vertically on the steering plate 109, so that the magnesium plate can be fixed between the first fixed block 110 and the first movable block 111.

[0053] At the same time, the first electric cylinder 112 is fixedly installed on the upper surface of the steering plate 109; the two ends of the first telescopic rod 113 are respectively connected to the output end of the first electric cylinder 112 and the first movable block 111, the first telescopic rod 113 is located between the first electric cylinder 112 and the first movable block 111, the output end of the first electric cylinder 112 is connected to the first telescopic rod 113, and drives the first telescopic rod 113 to extend and retract, so that the first movable block 111 can slide vertically on the steering plate 109.

[0054] In addition, the connecting plate 114 is fixedly mounted on the upper surface of the support column 103; the cylinder 115 is fixedly mounted on the lower surface of the connecting plate 114; the two ends of the vertical telescopic rod 116 are respectively connected to the output end of the cylinder 115 and the mounting seat 104, and the vertical telescopic rod 116 is located between the cylinder 115 and the mounting seat 104. The cylinder 115 is supported by the connecting plate 114, so that the power output from the output end of the cylinder 115 drives the vertical telescopic rod 116 to extend and retract, thereby causing the mounting seat 104 to move vertically on the support column 103.

[0055] When using a reinforced magnesium-titanium composite material preparation device of this embodiment, the magnesium plate is placed on the steering plate 109, and the first electric cylinder 112 is started, so that the power output from the output end of the first electric cylinder 112 drives the first telescopic rod 113 to extend and retract, so that the first movable block 111 slides vertically on the steering plate 109, and then the magnesium plate is fixed between the first fixed block 110 and the first movable block 111. After adding a coating to the magnesium plate, the cylinder 115 is started, so that the power output from the output end of the cylinder 115 drives the vertical telescopic rod 116 to extend and retract, so that the mounting seat 104 moves vertically, and then the steering plate 109 moves upward, and the driving cylinder 115 is started. The motor 107 is driven, so that the power output from the output end of the driving motor 107 drives the rotating rod 108 to rotate, so that the steering plate 109 can be flipped 180 degrees, and then the hydraulic cylinder 105 is started, so that the power output from the output end of the hydraulic cylinder 105 drives the transverse telescopic rod 106 to be telescoped, so that the driving motor 107 moves laterally, and then the flipped steering plate 109 can be moved to just above the titanium plate, and then the steering plate 109 is moved downward until the magnesium plate on the steering plate 109 contacts the titanium plate, and at this time the first movable block 111 is moved vertically, so that the fixed state of the magnesium plate is released, so that the magnesium plate and the titanium plate can be pressed together for rolling processing.

[0056] Third embodiment:

[0057] Based on the second embodiment, please refer to Figure 4 , Figure 4 It is a structural schematic diagram of the fixing component 201 of the reinforced magnesium-titanium composite material preparation equipment of the third embodiment. The present invention also provides a reinforced magnesium-titanium composite material preparation equipment, which also includes a fixing component 201, and the fixing component 201 includes a second fixed block 202, a second movable block 203, a second electric cylinder 204 and a second telescopic rod 205.

[0058] In this embodiment, the fixing assembly 201 is located above the processing table 101 to facilitate fixing the titanium plate.

[0059] Among them, the second fixed block 202 is fixedly installed on the upper surface of the processing table 101; the second movable block 203 is slidably connected to the processing table 101 and is located on the upper surface of the processing table 101, and the second fixed block 202 and the second movable block 203 are both L-shaped. The second movable block 203 is vertically slid on the processing table 101, so that the titanium plate can be fixed between the second fixed block 202 and the second movable block 203.

[0060] Secondly, the second electric cylinder 204 is fixedly installed on the upper surface of the processing table 101; the two ends of the second telescopic rod 205 are respectively connected to the output end of the second electric cylinder 204 and the second movable block 203, the second telescopic rod 205 is located between the second electric cylinder 204 and the second movable block 203, the output end of the second electric cylinder 204 is connected to the second telescopic rod 205, and drives the second telescopic rod 205 to extend and retract, so that the second movable block 203 can slide vertically on the processing table 101.

[0061] When using a reinforced magnesium-titanium composite material preparation device of this embodiment, the second electric cylinder 204 is started, so that the power output from the output end of the second electric cylinder 204 drives the second telescopic rod 205 to extend and retract, thereby making the second movable block 203 slide vertically on the processing table 101, and further making the titanium plate fixed between the second fixed block 202 and the second movable block 203.

[0062] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A process for preparing a reinforced magnesium-titanium composite material, comprising the following steps: Annealing of magnesium and titanium plates; First, select the materials: AZ series and ZEK series for magnesium plates, and TA1, TA2 and TC4 for titanium plates; Then, the selected materials were annealed, specifically: the magnesium alloy plate was heated to 290°C, kept at this temperature for 45 minutes, and air-cooled; the titanium plate was heated to 550°C, kept at this temperature for 60 minutes, and air-cooled; Plate surface treatment; First: Use 60-80 mesh coarse sandpaper to grind in one direction to remove the surface oxide layer; Secondly: first use 3%~5% NaOH solution, which is formed by mixing 45~60°C hot water and NaOH, then use 2%~3% hydrochloric acid solution for cleaning, and finally use alcohol to clean and blow dry; Adding coatings on the magnesium plate and the titanium plate respectively, wherein the coating thickness is 0.05-0.1 micrometers; The magnesium plate to which the coating is added is pressed against the surface to be composited of the titanium plate, and then rolled on a rolling mill to obtain a magnesium-titanium plate; The magnesium-titanium plate is leveled on a leveling machine, and the uncompounded or cracked parts on the four sides of the leveled magnesium-titanium plate are cut off to obtain the required reinforced magnesium-titanium plate; The coating is a metal coating of copper, aluminum or nickel, a copper coating is added to the magnesium plate, and an aluminum or nickel coating is added to the titanium plate; Before rolling, the magnesium plate and the titanium plate after adding the coating are preheated in a heating furnace, the preheating temperature is 380°C, the holding time is 20 minutes, and then hot rolling is performed, the hot rolling temperature is 400°C~450°C, the first reduction is 25%, the rolling rate is 0.1m / s, the total reduction is 35%~40%, the rolling pass is 3 times, and then the obtained composite plate is annealed, the annealing temperature is 220°C, the annealing time is 90 minutes, and air cooling is performed to obtain the required magnesium-titanium plate; The preparation equipment used in the preparation process of the reinforced magnesium-titanium composite material includes a processing table, Also included are adjustment components; The adjusting assembly comprises a support column, a mounting seat, a hydraulic cylinder, a transverse telescopic rod, a driving motor, a rotating rod and a steering plate, wherein the support column is fixedly mounted on the upper surface of the processing table, the mounting seat is slidably connected to the support column and penetrates the support column, the hydraulic cylinder is fixedly mounted on the lower surface of the mounting seat, the transverse telescopic rod is connected to the output end of the hydraulic cylinder and is located on a side of the hydraulic cylinder away from the mounting seat, the driving motor is fixedly mounted on an end of the transverse telescopic rod away from the hydraulic cylinder, the rotating rod is connected to the output end of the driving motor and is located on a side of the driving motor away from the transverse telescopic rod, and the steering plate is fixedly mounted on an end of the rotating rod away from the driving motor; The adjustment assembly further includes a first fixed block and a first movable block, wherein the first fixed block is fixedly mounted on the upper surface of the steering plate; the first movable block is slidably connected to the steering plate and is located on the upper surface of the steering plate; The preparation equipment also includes a fixing component, which is located above the processing table.

2. The process for preparing the reinforced magnesium-titanium composite material according to claim 1, characterized in that: The fixing assembly includes a second fixing block and a second movable block, wherein the second fixing block is fixedly mounted on the upper surface of the processing table; and the second movable block is slidably connected to the processing table and is located on the upper surface of the processing table.

3. The process for preparing the reinforced magnesium-titanium composite material according to claim 2, characterized in that: The fixing assembly also includes a second electric cylinder and a second telescopic rod, wherein the second electric cylinder is fixedly mounted on the upper surface of the processing table; the two ends of the second telescopic rod are respectively connected to the output end of the second electric cylinder and the second movable block, and the second telescopic rod is located between the second electric cylinder and the second movable block.