A connected tubular nitrogen-doped carbon material, its preparation method and application

By using connected tubular nitrogen-doped carbon materials, the problems of limited energy density and potential window of supercapacitors are solved, and efficient capacitive performance and large-area applicable supercapacitor electrode materials are achieved.

CN114974908BActive Publication Date: 2024-10-29FOSHAN XIANHU LAB
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210463618.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-28
Publication Date
2024-10-29
Estimated Expiration
2042-04-28

AI Technical Summary

Technical Problem

Existing supercapacitors have limited energy density and potential windows, making it difficult to achieve high power density. Moreover, porous carbon materials have independent pore structures and poor capacitive performance, making them unable to work effectively under large currents.

Method used

A connected tubular nitrogen-doped carbon material with a three-dimensional network structure is used, using titanate nanorods as a template, combined with a polymer precursor for polymerization and calcination, to form a material with multiple tubular structures and interconnected tubular structures for preparation Electrode materials for supercapacitors.

Benefits of technology

It achieves high specific surface area and good capacitance performance, and can exhibit double-layer capacitance characteristics at a scan speed of 100mV·s-1. The discharge specific capacitance reaches 302.1F·g-1, and under the constant current condition of 1A·g-1 It has excellent charge and discharge performance and is suitable for large area and mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114974908B_ABST
    Figure CN114974908B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of carbon materials, and discloses a connected tubular nitrogen-doped carbon material and a preparation method and application thereof. The connected tubular nitrogen-doped carbon material provided by the present invention has a three-dimensional network structure, wherein a plurality of tubular structures are provided inside the material, the tubular structures are interconnected, the ends of the tubular structures have openings and are interconnected with the outside, and the specific surface area thereof is 1000-1300m 2 ·g ‑1 , at 1A·g ‑1 Under the conditions of constant current charge and discharge, ‑1~0V (vs.HgO / Hg), the discharge specific capacitance can reach 302.1F·g ‑1 , with good capacitance performance; the self-supporting flexible membrane electrode provided by the present invention has the advantages of large area, no need for metal current collector support, breaking strength of up to 2.77MPa, and breaking elongation of up to 3.89%; the ionic liquid double-layer supercapacitor assembled by the self-supporting flexible membrane electrode of the present invention has good operating voltage and energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon materials, and in particular relates to a connected tubular nitrogen-doped carbon material and a preparation method and application thereof. Background Art

[0002] Supercapacitors have the advantage of being able to perform multiple rapid charge and discharge cycles to provide high instantaneous energy, and are a very promising environmentally friendly energy storage device. Shorter charge and discharge times and longer lifespans allow supercapacitors to serve as excellent energy recycling systems, i.e., charges are physically stored on the electrode surface. Theoretically, there is no chemical reaction in the system, and the charge storage mechanism can be maintained for millions of cycles. In addition, supercapacitors are designed to achieve higher power density, but in practice this is difficult to achieve due to problems such as limited energy density and low potential window, and supercapacitors that can operate at low temperatures and have reasonable performance are essential for their outdoor applications.

[0003] Porous carbon materials are a representative type of traditional carbon-based electrode materials for supercapacitors. In order to improve the energy density of supercapacitor electrode materials and have reasonable performance at low temperatures, the most commonly used strategy is to use a hard template method to prepare porous carbon materials. A mixture of a carbon precursor and a hard template (usually SiO2 nanoparticles) is carbonized by high-temperature oxygen-free pyrolysis, and then the hard template is removed. However, the pores generated by direct preparation using the hard template method are mostly relatively independent, and their capacitance performance is poor, which is not suitable for working under large currents. This is obviously contrary to the advantages and working methods of supercapacitors to quickly obtain / release energy. In order to form a porous structure that is interconnected, the activity of substances such as KOH at high temperatures is usually used to etch the pore walls of porous carbon materials to increase the number of micropores inside the material. However, etching carbon materials with KOH usually requires a secondary calcination process, which often leads to a serious decrease in yield. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a connected tubular nitrogen-doped carbon material and a preparation method and application thereof. The connected tubular nitrogen-doped carbon material provided by the present invention has a plurality of tubular structures inside, and the tubular structures are interconnected, and has good capacitance performance.

[0005] The first aspect of the present invention provides a connected tubular nitrogen-doped carbon material, which has a three-dimensional network structure. The interior of the connected tubular nitrogen-doped carbon material has multiple tubular structures, which are interconnected, and the ends of the tubular structures have openings and are interconnected with the outside.

[0006] A second aspect of the present invention provides a method for preparing the interconnected tubular nitrogen-doped carbon material of the present invention, comprising the following steps:

[0007] Nanorods with a three-dimensional network structure are used as templates;

[0008] The titanate nanorods are mixed with a pore-forming agent, a polymer monomer, an initiator, a cross-linking agent and a solvent to carry out a polymerization reaction to obtain a polymer precursor (TiRDs / P-VIm / KNO3);

[0009] The polymer precursor is calcined to remove the template to obtain the interconnected tubular nitrogen-doped carbon material (NPHTC K ).

[0010] Preferably, the method for preparing the template comprises the following steps:

[0011] Titanium dioxide is mixed with alkali solution and subjected to hydrothermal reaction to obtain titanate nanorods; the alkali solution is potassium hydroxide or sodium hydroxide solution, and the concentration of the sodium hydroxide solution is 6 to 10 mol·L -1 In the solution after mixing titanium dioxide and alkali solution, the concentration of titanium dioxide is 0.02 to 0.1 g·mL -1 The temperature of the hydrothermal reaction is 150-180°C and the time is 24-48 hours.

[0012] Preferably, the pore-forming agent includes one of potassium nitrate, sodium nitrate or ammonium chloride, the polymer monomer includes one of 1-vinylimidazole, vinyl pyrrolidone or vinyl pyridine, the initiator includes one of 4,4′-azobiscyanovaleric acid, potassium persulfate or azobisisobutylamidine hydrochloride, the cross-linking agent includes one of N,N′-methylenebisacrylamide, divinylbenzene or diisocyanate, and the solvent includes one of water, N,N-dimethylformamide or dimethyl sulfoxide; the mass ratio of the template, the pore-forming agent and the polymer monomer is (0.5-1.25):(0.5-1.5):2.6.

[0013] Preferably, the polymerization reaction temperature is 70° C. to 80° C., and the polymerization time is 1 h to 1.5 h.

[0014] Preferably, the calcination temperature is 700° C. to 900° C., and the calcination time is 1 h to 3 h.

[0015] The third aspect of the present invention provides the use of the interconnected tubular nitrogen-doped carbon material of the present invention in a supercapacitor.

[0016] Based on the above application, the present invention provides a self-supporting flexible membrane electrode, comprising the interconnected tubular nitrogen-doped carbon material and an additive as described in the present invention.

[0017] Preferably, the auxiliary agent includes a conductive agent, a film-forming agent and a solvent; the conductive agent includes acetylene black or Ketjen black, the film-forming agent includes one of polyvinylidene fluoride, polymethyl methacrylate or polytetrafluoroethylene, and the solvent includes one of N,N-dimethylformamide, N-methylpyrrolidone or dimethyl sulfoxide.

[0018] Preferably, the sum of the masses of the interconnected tubular nitrogen-doped carbon material and the conductive agent accounts for 20% to 40% of the sum of the masses of the interconnected tubular nitrogen-doped carbon material, the conductive agent and the film-forming agent.

[0019] Preferably, the thickness of the self-supporting flexible membrane electrode is 70-80 μm.

[0020] The method for preparing the self-supporting flexible membrane electrode of the present invention comprises the following steps:

[0021] The interconnected tubular nitrogen-doped carbon material and the auxiliary agent are prepared into a slurry, which is then poured into a mold and dried to obtain the self-supporting flexible membrane electrode (SFME).

[0022] Preferably, the method for preparing the self-supporting flexible membrane electrode comprises the following steps:

[0023] The interconnected tubular nitrogen-doped carbon material and the acetylene black are mixed in a mass ratio of (4-2):1 to form a carbon-based material, and then the carbon-based material is mixed with the polyvinylidene fluoride and the N,N-dimethylformamide to form a slurry. The slurry is then spread flat on a polytetrafluoroethylene mold, and the solvent is dried to form a film to obtain a self-supporting flexible membrane electrode.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0025] The specific surface area of ​​the interconnected tubular nitrogen-doped carbon material provided by the present invention is 1000-1300m 2 ·g -1 , at 100mV·s -1 The cyclic voltammetry curve under the scanning rate showed a rectangular shape with double-layer capacitance characteristics. -1 Under the conditions of constant current charge and discharge, -1~0V (vs.HgO / Hg), the discharge specific capacitance can reach 302.1F·g -1 , with good capacitance performance.

[0026] The self-supporting flexible membrane electrode prepared based on the interconnected tubular nitrogen-doped carbon material of the present invention has the advantages of a large area (up to 10×10 cm), no need for metal current collector support, a fracture strength of up to 2.77 MPa, and a fracture elongation of up to 3.89%. The working voltage range at room temperature (about 25°C) is 0 to 3V; the ionic liquid double-layer supercapacitor assembled with the self-supporting flexible membrane electrode of the present invention has good working voltage and energy density, and the working voltage range at 1A·g -1 , 0~3V condition, the specific capacitance can reach 35F·g -1 , at a power density of 1500W·kg -1 The energy density can reach 43.8W·kg -1 .

[0027] The preparation method of the interconnected tubular nitrogen-doped carbon material and the self-supporting flexible membrane electrode of the present invention is simple, easy to operate, and easy to produce on a large scale and over a large area. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 These are SEM images of TiRDs and TiRDs / P-VIm / KNO3 of Example 1 of the present invention.

[0029] Figure 2 NPHTC of Example 1 of the present invention K SEM image of .

[0030] Figure 3 NPHTC of Examples 1-4 of the present invention K At 100mV·s -1 CV curves at 1A·g -1 The charge and discharge curves at .

[0031] Figure 4 NPHTC of Examples 1, 9 and 10 K At 1A·g -1 The charge and discharge curves at .

[0032] Figure 5 ] are SEM images of SFME of Example 11, wherein a and b are surface images, and c and d are cross-sectional images formed after quenching in liquid nitrogen.

[0033] Figure 6 The molding diagram of SFME of Examples 11-14.

[0034] Figure 7 Graph showing the tensile strength and elongation at break of the SFMEs of Examples 11-13.

[0035] Figure 8 The electrochemical performance test diagram of the capacitors assembled in Examples 11-13. DETAILED DESCRIPTION

[0036] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0037] Unless otherwise specified, the raw materials and reagents used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0038] Example 1

[0039] A method for preparing a connected tubular nitrogen-doped carbon material comprises the following steps:

[0040] (1) Add 1 g of titanium dioxide powder with a particle size of 25 nm to 50 mL of a 10 mol·L -1 After being stirred for 0.5 hours in a sodium hydroxide solution, the mixture was placed in a reactor and subjected to a hydrothermal reaction at 180°C for 24 hours. The reaction product was then washed with deionized water until neutral, and then placed in a freeze dryer for freeze drying and ground into a white powder to obtain titanate nanorods (TiRDs) for use as a template.

[0041] (2) 0.75 g of TiRDs, 1.25 g of potassium nitrate, 2.6 g of 1-vinylimidazole, 0.0375 g of 4,4′-azobiscyanovaleric acid and 0.0425 g of N,N′-methylenebisacrylamide were added to a flask containing 10 mL of deionized water, and ultrasonicated and stirred for 0.5 hours each. The mixed solution was then freeze-thawed and degassed three times with liquid nitrogen, and then placed in an oil bath at 80°C for polymerization reaction for 1.5 hours. The white solid obtained by polymerization was then freeze-dried to obtain a polymer precursor (TiRDs / P-VIm / KNO3);

[0042] (3) TiRDs / P-VIm / KNO3 was calcined at 800°C for 2 hours in an argon atmosphere, and the calcined product was poured into a hydrofluoric acid solution and soaked for 48 hours to remove the template, and then washed with deionized water until neutral, and dried to obtain a connected tubular nitrogen-doped carbon material (NPHTC K ).

[0043] Figure 1 a is a SEM image of the TiRDs prepared in Example 1. It can be clearly seen that all the TiRDs are of micrometer order in length, but have different diameters ranging from tens of nanometers to hundreds of nanometers. Figure 1b is the SEM image of TiRDs / P-VIm / KNO3 prepared in Example 1. Due to the large size of TiRDs, a stacked rod-like structure wrapped inside the polymer can be observed on the surface of TiRDs / PVIm-N / KNO3, indicating that the cross-linked polymer can effectively fix the template inside it while maintaining the three-dimensional stacking structure of the template.

[0044] Figure 2 a is NPHTC K The SEM image shows that after calcining and carbonizing TiRDs / PVIm-N / KNO3 and removing the TiRDs template, the three-dimensional structure and gaps of the material are still clearly visible, which is basically consistent with that before calcination, indicating that the material can effectively retain the stacking structure and template morphology during high-temperature calcination and subsequent treatment. It is worth noting that the ends of the tubular structure can be clearly observed to be open at the edge of the material, indicating that NPHTC K The tubular structure channels retained inside can effectively interact with the outside world. Figure 2 From the high-magnification SEM image in b, it can be seen that the tubular structures are interconnected and interconnected, rather than existing independently in the form of single carbon nanotubes.

[0045] Embodiment 2-4

[0046] The difference between Examples 2-4 and Example 1 is only that the amount of TiRDs used in step (2) is different, specifically: 0.5 g of TiRDs is used in Example 2, 1 g of TiRDs is used in Example 3, and 1.25 g of TiRDs is used in Example 4. The other components, usage amounts and preparation methods are the same as those in Example 1.

[0047] Effect of different TiRDs dosage on NPHTC K Performance Impact

[0048] Comparative Examples 1-4 (NPHTC prepared in Example 1 K NPHTC K -0.75, NPHTC prepared in Example 2 K NPHTC K -0.5, NPHTC prepared in Example 3 K NPHTC K -1, NPHTC prepared in Example 4 K NPHTC K -1.25), according to the cyclic voltammetry (CV) curve in the three-electrode system at room temperature (25°C) ( Figure 3 a) It can be seen that the NPHTC prepared by four different TiRDs dosages KSample at 100mV·s -1 The CV curves at the scanning rate all show a rectangular shape with double-layer capacitance characteristics. At the same time, the size and shape of the CV curves of different samples are different, indicating that different TiRDs dosages have different effects on NPHTC K In order to specifically evaluate the capacitance performance of each sample, a 1A·g -1 Constant current charge and discharge (GCD) test, such as Figure 3 As shown in Figure b, it can be seen that all samples show a relatively symmetrical triangular GCD curve that conforms to the characteristics of a double-layer capacitor at -1 to 0 V (vs. HgO / Hg). According to the formula, the discharge specific capacitances of NPHTCK-0.5 (Example 2), NPHTCK-0.75 (Example 1), NPHTCK-1 (Example 3) and NPHTCK-1.25 (Example 4) are 272, 302.1, 277.4 and 251.4 F·g, respectively. -1 , where the NPHTC prepared when the mass ratio of TiRDs to 1-vinyl imidazole is 0.75:2.6 K The NPHTC prepared in Example 1 has the best capacitance performance. K Best performance.

[0049] Embodiment 5-8

[0050] The difference between Examples 5-8 and Example 1 is only that the amount of potassium nitrate used in step (2) is different, specifically: the potassium nitrate used in Example 5 is 0.5 g, the potassium nitrate used in Example 6 is 0.75 g, the potassium nitrate used in Example 7 is 1 g, and the potassium nitrate used in Example 8 is 1.5 g. The other components, usage amounts and preparation methods are the same as those in Example 1.

[0051] Effect of different potassium nitrate dosage on NPHTC K Performance Impact

[0052] Comparative Examples 5-8, when the amount of potassium nitrate used was 0.5g, 0.75g, 1g and 1.5g, the discharge specific capacitances of the obtained samples were 248.5, 260, 283 and 269 F·g, respectively. -1 , indicating that with the increase of potassium nitrate dosage, NPHTC K The internal interconnected structure and micropores increase, and the capacitance performance is improved; however, excessive potassium nitrate will K Over-etching causes the merging and destruction of the pore structure, making NPHTC K The capacitance performance of NPHTC prepared when the mass ratio of potassium nitrate to 1-vinyl imidazole was 1.25:2.6 KThe NPHTC prepared in Example 1 has the best capacitance performance. K Best performance.

[0053] Examples 9-10

[0054] The difference between Examples 9-10 and Example 1 is only the calcination temperature in step (3), specifically: the calcination temperature of Example 9 is 700°C, and the calcination temperature of Example 10 is 900°C. The other components, usage amounts and preparation methods are the same as those of Example 1.

[0055] Effect of different calcination temperatures on NPHTC K Performance Impact

[0056] Figure 4 NPHTC prepared at different calcination temperatures in Examples 1, 9 and 10 K Materials at 1A·g -1 GCD curves at current densities of 2.3 %. The discharge specific capacitance at 700°C and 900°C is 266.3 F·g -1 and 280.6F·g -1 , are lower than 302.1F·g at 800℃ -1 This is because the addition of potassium nitrate can significantly increase the specific surface area and micropore content of the material, thereby effectively improving the capacitance performance of the material. As the calcination temperature increases, the etching effect of potassium nitrate is enhanced, the degree of graphitization of the material is improved, and the capacitance performance is improved; but too high a calcination temperature will cause potassium nitrate to over-etch the carbon material, destroying the skeleton and structure of the material, and the N doping amount in the material decreases, resulting in a decrease in capacitance performance. Therefore, the preparation of NPHTC K The most suitable calcination temperature of the material is 800°C, that is, the NPHTC prepared in Example 1 K Best performance.

[0057] Embodiment 11

[0058] A method for preparing a self-supporting flexible membrane electrode comprises the following steps:

[0059] 0.12 g of NPHTC K After mixing with 0.03 g of acetylene black (carbon-based material), it was mixed with 0.35 g of polyvinylidene fluoride, poured into 10 mL of N,N-dimethylformamide solution, stirred to form a slurry with a certain fluidity and viscosity, and poured into a polytetrafluoroethylene mold (10×10 cm), placed in an oven at 50°C and dried for 12 hours, and the film was taken out to obtain a self-supporting flexible membrane electrode (SFME-30wt%); wherein the mass of the carbon-based material accounts for 30% of the sum of the mass of the carbon-based material and polyvinylidene fluoride, that is, the mass of the carbon-based material accounts for 30%.

[0060] Examples 12-14

[0061] The difference between Examples 12-14 and Example 11 is only that the mass proportion of the carbon-based material is different, specifically: Example 12 (NPHTC K , acetylene black and polyvinylidene fluoride are 0.08g, 0.02g and 0.4g respectively, the mass of carbon-based materials accounts for 20%, and the obtained self-supporting flexible membrane electrode is recorded as SFME-20wt%), Example 13 (NPHTC K , acetylene black and polyvinylidene fluoride are 0.16g, 0.04g and 0.3g respectively, the mass of carbon-based materials accounts for 40%, and the obtained self-supporting flexible membrane electrode is recorded as SFME-40wt%), Example 14 (NPHTC K The masses of acetylene black and polyvinylidene fluoride are 0.2g, 0.05g and 0.25g respectively, the mass proportion of carbon-based materials is 50%, and the obtained self-supporting flexible membrane electrode is recorded as SFME-50wt%), and the other components, usage amounts and preparation methods are the same as Example 11.

[0062] Figure 5 is a SEM image of the self-supporting flexible membrane electrode prepared in Example 11, wherein Figure 5 a and Figure 5 b is its surface, Figure 5 c and Figure 5 d is the cross section formed after quenching in liquid nitrogen. Figure 5 It can be clearly seen in a that the self-supporting flexible membrane electrode (SFME-30wt%) prepared in Example 11 is a stacked film, in which pores are still retained due to the overflow of the gas dissolved in the slurry during the heating and drying process, which is consistent with the characteristics of the film prepared by the casting method. Figure 5 As shown in b, NPHTC can be clearly seen K The tubular structure is wrapped by polyvinylidene fluoride to form a thin film. Figure 5 The cross-sectional view in c shows that SFME-30wt% is a porous film with abundant pores and NPHTC K The tubular structure channels can also be magnified at higher magnifications. Figure 5 It can be clearly observed in d.

[0063] Effects of different mass proportions of carbon-based materials on the mechanical properties of self-supporting flexible membrane electrodes

[0064] Comparative Examples 11-14, pictures of slurries with different mass proportions of carbon-based materials poured into molds after drying but not demolding ( Figure 6) It can be judged that when the mass ratio of carbon material is less than 40wt%, a relatively flat and complete film can be formed in the mold by pouring and drying; when the mass ratio of carbon material is 40%, the formed film can only be partially removed, indicating that the mechanical properties of the film have decreased at this time; when the mass ratio of carbon material is 50wt%, the relative amount of polyvinylidene fluoride is low, which is insufficient to support the formation of a complete film, and it has been broken before demolding and cannot form a film.

[0065] Figure 7 The tensile strength and elongation at break of SFME-20wt%, SFME-30wt% and SFME-40wt% prepared from carbon-based materials with different mass percentages in Examples 11-13. During the test, the film was cut into a rectangle of 7×1cm, the gauge length was 30mm, and the tensile rate was 5mm·min -1 .from Figure 7 From the middle curve, we can see that SFME-40wt% has the worst mechanical strength, with a breaking strength of 0.59mPa and a breaking elongation of 0.88%; SFME-20wt% is second, with a breaking strength of 1.78mPa and a breaking elongation of 1.41%; and among the three, SFME-30wt% has the best mechanical properties, with a breaking strength of 2.77mPa and a breaking elongation of 3.89%. In summary, SFME-30wt% has the best mechanical properties.

[0066] Effects of different mass proportions of carbon-based materials on the electrical properties of self-supporting flexible membrane electrodes

[0067] SFME-20wt%, SFME-30wt% and SFME-40wt% prepared from carbon-based materials with different mass proportions in Examples 11-13 were cut into Φ14mm circular electrode sheets as electrodes, 2 mol·L -1 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) / acetonitrile (ACN) was used as the electrolyte, a glass fiber diaphragm (Φ16 mm) was used as the diaphragm, a gasket and a button cell shell (CR2016) were assembled into a button ionic liquid double-layer supercapacitor (SC-IL), and its capacitance performance was tested.

[0068] according to Figure 8 From the linear sweep voltammetry (LSV) curve at room temperature in a, it can be seen that without using a metal current collector to prepare the electrode, the starting potentials of the LSV curves of all devices at room temperature are very close, all around 3 V, indicating that the SC-IL assembled directly using SFME has good electrochemical stability and working voltage. Figure 8b records the Nyquist curve of the above device. It can be found that as the mass proportion of carbon material increases from 20wt% to 40wt%, the impedance of the assembled capacitor device decreases significantly, indicating that the increase in the mass proportion of carbon material in the membrane electrode can effectively reduce the impedance of the device. In addition, when using SFME-30wt% and SFME-40wt%, the low-frequency region of the Nyquist curve is almost perpendicular to the horizontal axis, indicating that the SC-IL assembled using these two membrane electrodes has a relatively excellent ion diffusion capacity. According to the starting potential of the LSV curve, CV and GCD tests were performed on the three devices in the voltage range of 0 to 3V. Figure 8 It can be clearly seen in c that at room temperature, the scan rate is 100 mV·s -1 When SFME-30wt% and SFME-40wt% are used as electrodes, the CV curves of the capacitors are relatively standard rectangular; when SFME-20wt% is used as an electrode, due to the insulating properties of polyvinylidene fluoride, the CV curves are non-rectangular, narrower, and sharper, further indicating that the performance of the SC-IL capacitors assembled with SFME-20wt% is not ideal. Figure 8 The GCD curve in d shows that at room temperature, when the current density is 1A·g -1 The specific capacitances of the SC-ILs assembled using the prepared SFME-20wt%, SFME-30wt%, and SFME-40wt% as electrodes were 22.7, 35, and 31 F·g, respectively. -1 After conversion, the three devices have a power density of 1500w·kg -1 The energy densities were 28.4, 43.8 and 38.8 Wh·kg -1 .

[0069] Combined with the mechanical properties of SFME, it can be seen that at room temperature, SFME-30wt% is a membrane electrode with good mechanical properties that can be formed on a large area, and when SFME-30wt% is used to assemble ionic liquid button double-layer supercapacitors, the device has a small impedance and excellent capacitance performance. Therefore, a mass proportion of 30% carbon-based materials is the best ratio for preparing slurry for preparing self-supporting flexible membrane electrodes.

[0070] The preferred embodiments of the present invention are described in detail above, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.

Claims

1. A self-supporting flexible membrane electrode, characterized in that: It is composed of interconnected tubular nitrogen-doped carbon materials and additives, and does not require metal current collector support; The auxiliary agent includes a conductive agent, a film-forming agent and a solvent; the conductive agent includes acetylene black or Ketjen black, the film-forming agent includes one of polyvinylidene fluoride, polymethyl methacrylate or polytetrafluoroethylene, and the solvent includes one of N,N-dimethylformamide, N-methylpyrrolidone or dimethyl sulfoxide; The sum of the masses of the interconnected tubular nitrogen-doped carbon material and the conductive agent accounts for 20% to 40% of the sum of the masses of the interconnected tubular nitrogen-doped carbon material, the conductive agent and the film-forming agent; The interconnected tubular nitrogen-doped carbon material has a three-dimensional network structure, the interior of the interconnected tubular nitrogen-doped carbon material has a plurality of tubular structures, the tubular structures are interconnected, and the ends of the tubular structures have openings and are interconnected with the outside; The interconnected tubular nitrogen-doped carbon material is prepared by a preparation method comprising the following steps: Titanate nanorods with a three-dimensional network structure are used as templates; The titanate nanorods are mixed with a pore-forming agent, a polymer monomer, an initiator, a cross-linking agent and a solvent to carry out a polymerization reaction to obtain a polymer precursor; calcining the polymer precursor and removing the template to obtain the interconnected tubular nitrogen-doped carbon material; The pore-forming agent includes one of potassium nitrate, sodium nitrate or ammonium chloride, the polymer monomer includes one of 1-vinylimidazole, vinyl pyrrolidone or vinyl pyridine, the initiator includes one of 4,4′-azobiscyanovaleric acid, potassium persulfate or azobisisobutylamidine hydrochloride, the cross-linking agent includes one of N,N′-methylenebisacrylamide, divinylbenzene or diisocyanate, and the solvent includes one of water, N,N-dimethylformamide or dimethyl sulfoxide; the mass ratio of the template, the pore-forming agent and the polymer monomer is 0.75:1.25:2.

6.

2. The self-supporting flexible membrane electrode according to claim 1, characterized in that: The method for preparing the template comprises the following steps: Titanium dioxide is mixed with alkali solution and subjected to hydrothermal reaction to obtain titanate nanorods; the alkali solution is potassium hydroxide or sodium hydroxide solution, and the concentration of the sodium hydroxide solution is 6 to 10 mol·L -1 In the solution after mixing titanium dioxide and alkali solution, the concentration of titanium dioxide is 0.02 to 0.1 g·mL -1 The temperature of the hydrothermal reaction is 150-180°C and the time is 24-48 hours.

3. The self-supporting flexible membrane electrode according to claim 1, characterized in that: The calcination temperature is 700° C. to 900° C., and the calcination time is 1 h to 3 h.

4. The method for preparing the self-supporting flexible membrane electrode according to claim 1, characterized in that: The following steps are involved: The interconnected tubular nitrogen-doped carbon material and the auxiliary agent are prepared into a slurry, which is then poured into a mold and dried to obtain the self-supporting flexible membrane electrode.

Citation Information

Patent Citations

  • Preparation method for MnO2 / C composite fibres

    CN105926083A

  • Method for preparing sulfur-oxygen co-doped porous carbon based on paper

    CN110902678A

  • Large-area continuous flexible self-supporting electrode and preparation method and application thereof

    CN111899990A

  • Negative electrode material of enhanced self-supporting lithium ion battery and preparation process thereof

    CN111916750A

  • Manufacturing method and application of sulfur-loaded wood-based carbon skeleton of self-supporting positive electrode