A method for preparing high performance tantalum target blank
Through the process of upsetting, cutting, forging, annealing and cold rolling, the problems of grain orientation gradient and {111} striping in the thickness direction of the tantalum target are solved, and the uniformity of the sputtering coating and the improvement of the target life are achieved. promote.
Patent Information
- Application Number
- CN202210621832.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-06-02
AI Technical Summary
Existing tantalum targets have grain orientation gradients and {111} stripes in the thickness direction, resulting in uneven sputtering coatings and short target life.
By providing tantalum ingots for upsetting, cutting, forging and drawing, annealing, cold rolling and multiple annealing processes, we ensure that the texture of the target is evenly distributed in the thickness direction, eliminate {111} strips, and improve the life of the target. .
It achieves the thickness uniformity of sputtering coating and extends the target life, significantly reduces the enrichment of {111} oriented grains, and improves production efficiency and engineering operability.
Smart Images

Figure HDA0003677092400000011 
Figure HDA0003677092400000012 
Figure HDA0003677092400000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sputtering target material preparation, and in particular relates to a method for preparing a high-performance tantalum target blank. Background Art
[0002] Sputtering target is a key material for manufacturing semiconductor chips. The principle is that under the action of an external field, gaseous ions bombard the target at high speed, and the bombarded target atoms are deposited on the silicon wafer, eventually forming a complex wiring structure in the semiconductor chip. With the development of semiconductor chip technology, copper has replaced aluminum as a new generation of interconnection material. In order to prevent copper diffusion from causing damage to device performance, a diffusion barrier layer needs to be wrapped around the copper interconnection line. Tantalum target is the key material for preparing this barrier layer. Conventional tantalum target blanks or other BCC metal target blanks usually have a large grain orientation gradient in the thickness direction, and there is a {111} strip at the 1 / 2 thickness position. The existence of these phenomena will cause problems with the uniformity of the film during the target sputtering process. Summary of the invention
[0003] Furthermore, the present invention aims to solve two problems existing in the prior art: 1. The problem of uniformity of target sputtering coating: when there is a large orientation gradient in the thickness direction of the target blank, the sputtering rates of grains with different orientations are different, which will cause the problem of uneven film thickness on the wafer; 2. The problem of target material life: when sputtering to 1 / 2 of the thickness of the target blank, the appearance of {111} stripes will cause the target material to fail prematurely and fail to achieve the expected life.
[0004] In order to solve the above problems, the present invention proposes a method for preparing a tantalum target blank, including: step 1) providing a tantalum ingot, upsetting, and cutting to obtain a primary tantalum target blank; step 2) forging and stretching, annealing, to obtain an intermediate tantalum target blank; step 3) cold rolling 1, annealing, cold rolling 2, annealing, to obtain a final tantalum target blank. The tantalum target blank prepared by the method proposed by the present invention has a uniform texture distribution in the thickness direction, and the film has good thickness uniformity during sputtering coating. At the same time, the {111} strip on 1 / 2 thickness of the target blank is eliminated by the cutting method, thereby improving the target material life.
[0005] Compared with the process of multiple stretching, upsetting and then cutting (US 2020 / 0240006A1), this patent directly cuts and then stretches after upsetting. The advantages are: 1. Cutting after the initial upsetting can expose the {111} orientation on the surface, which can be removed in subsequent processing, and can also reduce the proportion of {111} orientation in the 1 / 2 thickness position of the target blank. 2. The process flow is simple and the production efficiency is high; 3. The target blank is light in weight after cutting and has high engineering operability. Compared with the conventional forging and rolling preparation methods, the present invention can significantly reduce the enrichment of {111} oriented grains in the 1 / 2 thickness direction of the Ta target blank, and the {100} / {110} / {111} texture distribution in the thickness direction is more uniform. The following is combined with the attached Figure 1 The preparation process is described in detail.
[0006] In step 1), S1 provides a high-purity tantalum ingot, the purity of the tantalum ingot is ≥99.995%. Generally, the purity requirements of high-purity tantalum targets for integrated circuits are relatively high, and the incoming material purity is 4N5 (99.995%) or above to ensure the purity of the prepared tantalum target blank. After providing the tantalum ingot, the tantalum ingot can also be cut by a sawing machine to form a tantalum ingot of suitable size for subsequent processing. S2 The deformation amount of upsetting is controlled at 40%-50%. During the upsetting process, if the deformation amount is less than 40%, it will lead to insufficient deformation, insufficient ingot deformation storage energy, and insufficient grain refinement during the subsequent annealing process; if the deformation amount is greater than 50%, the diameter of the tantalum ingot is large, it is not easy to cut by a sawing machine, and it will cause the shape of the subsequent forging ingot to be difficult to control. S3 cutting is to divide the ingot into two along a cross section perpendicular to the upsetting direction. It should be noted that the upsetting process is prone to produce a strong {111} texture at the 1 / 2 height position of the ingot. The ingot is divided into two at this position, and the strong {111} texture is placed on the surface, which is eliminated in subsequent processing, which can effectively avoid the generation of {111} stripes at the 1 / 2 thickness position of the target blank.
[0007] In step 2), the deformation of S4 forging and drawing is controlled at 50%-70%, which can further weaken the {111} texture. S5 annealing should ensure a vacuum environment and a temperature between 1000℃-1100℃. This heat treatment parameter can ensure that the ingot is fully recrystallized while effectively controlling the grain size.
[0008] In step 3), the total deformation of S6 cold rolling is controlled at 70%-80%, and the total deformation should be less than 80%. S7 annealing should ensure a vacuum environment, and the temperature should be 950℃-1100℃. The annealing temperature should be higher than 950℃ to ensure that the target blank is fully recrystallized and the rolled structure is eliminated. The total deformation of S8 cold rolling is controlled at 65%-75%, and the total deformation should be less than 75% to prevent the reformation of {111} strips on 1 / 2 thickness of the target blank, which loses the meaning of cutting. S9 annealing should ensure a vacuum environment, and the temperature should be 900℃-1100℃. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 The present invention provides a flow chart of the method for preparing the tantalum target blank.
[0010] Figure 2 This is the orientation distribution diagram of the longitudinal section of the tantalum target blank in Example 1 of the present invention.
[0011] Figure 3 It is the longitudinal cross-section orientation distribution diagram of the tantalum target blank in comparative example 1 of the present invention. DETAILED DESCRIPTION
[0012] Attached Figure 1 The flowchart of the preparation method of the tantalum target blank provided by the present invention, the double-direction arrow represents the central axis of the ingot, and the unidirectional arrow represents the force direction of the ingot. In order to make the features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the comparative examples and embodiments, the calculation of the deformation is based on the height of the ingot on the central axis.
[0013] Embodiment 1:
[0014] 1. Provide tantalum ingots with a purity of ≥99.995% and an ingot size of Φ150×200mm. Upset the tantalum ingots with a deformation of 40%. After upsetting, the target blank has a diameter of about 193mm and a thickness of about 120mm.
[0015] 2. The ingot is divided into two parts along the cross section perpendicular to the upsetting direction. The size of the target blank obtained is: about 193 mm in diameter and about 60 mm in thickness.
[0016] 3. The cut ingot is rotated 90° along the X-axis, forged and stretched to 90 mm, and the target blank diameter is about 158 mm.
[0017] 4. Vacuum recrystallization annealing, annealing temperature is 1050℃.
[0018] 5. The target blank is rotated 90° along the X axis and cold rolled 1, with a total deformation of 75%. After rolling, the target blank has a diameter of about 312 mm and a thickness of about 23 mm. The vacuum annealing temperature is 1000°C.
[0019] 6. Cold rolling 2 is performed, the total deformation is 65%, and the thickness after rolling is about 8 mm. The final vacuum annealing temperature is 1000°C.
[0020] Embodiment 2:
[0021] 1. Provide tantalum ingots with a purity of ≥99.995% and an ingot size of Φ150×200mm. Upset the tantalum ingots with a deformation of 40%. After upsetting, the target blank has a diameter of about 193mm and a thickness of about 120mm.
[0022] 2. The ingot is divided into two parts along the cross section perpendicular to the upsetting direction. The size of the target blank obtained is: about 193 mm in diameter and about 60 mm in thickness.
[0023] 3. The cut ingot is rotated 90° along the X axis, forged and stretched to 100 mm, and the target blank diameter is about 150 mm.
[0024] 4. Vacuum recrystallization annealing, annealing temperature is 1050℃.
[0025] 5. The target blank is rotated 90° along the X axis and cold rolled 1, with a total deformation of 73%. After rolling, the target blank has a diameter of about 289 mm and a thickness of about 27 mm. The vacuum annealing temperature is 1000°C.
[0026] 6. Cold rolling 2 is performed, the total deformation is 70%, and the target blank thickness after rolling is about 8 mm. The final vacuum annealing temperature is 980°C.
[0027] Embodiment 3:
[0028] 1. Provide tantalum ingots with a purity of ≥99.995% and an ingot size of Φ130×265mm. The tantalum ingots are upset with a deformation of 43%. After upset, the target blank has a diameter of about 172mm and a thickness of about 152mm.
[0029] 2. The ingot is divided into two parts along the cross section perpendicular to the upsetting direction. The size of the target blank obtained is: about 172 mm in diameter and about 76 mm in thickness.
[0030] 3. The cut ingot is rotated 90° along the X axis, forged and stretched to 114 mm, and the target blank has a diameter of about 140 mm.
[0031] 4. Vacuum recrystallization annealing, annealing temperature is 1050℃.
[0032] 5. The target blank is rotated 90° along the X axis and cold rolled 1, with a total deformation of 73%. After rolling, the target blank has a diameter of about 269 mm and a thickness of about 31 mm. The vacuum annealing temperature is 1000°C.
[0033] 6. Cold rolling 2 is performed, the total deformation is 74%, and the target blank thickness after rolling is about 8 mm. The final vacuum annealing temperature is 980°C.
[0034] Embodiment 4:
[0035] 1. Provide tantalum ingots with a purity of ≥99.995% and an ingot size of Φ130×265mm. The tantalum ingots are upset with a deformation of 43%. After upset, the target blank has a diameter of about 172mm and a thickness of about 152mm.
[0036] 2. The ingot is divided into two parts along the cross section perpendicular to the upsetting direction. The size of the target blank obtained is: about 172 mm in diameter and about 76 mm in thickness.
[0037] 3. The cut ingot is rotated 90° along the X-axis, forged and stretched to 118 mm, and the target blank diameter is about 138 mm.
[0038] 4. Vacuum recrystallization annealing, annealing temperature is 1050℃.
[0039] 5. The target blank is rotated 90° along the X axis and cold rolled 1, with a total deformation of 80%. After rolling, the target blank has a diameter of about 306 mm and a thickness of about 24 mm. The vacuum annealing temperature is 1000°C.
[0040] 6. Cold rolling 2 is performed, the total deformation is 67%, and the target blank thickness after rolling is about 8 mm. The final vacuum annealing temperature is 980°C.
[0041] Comparative Example 1:
[0042] 1. Provide tantalum ingots with purity ≥99.995% and ingot size Φ150×100mm.
[0043] 2. Directly upsetting to diameter 193mm and thickness 60mm.
[0044] 3. Forging and drawing to 90mm, the target blank diameter is about 158mm.
[0045] 4. Vacuum recrystallization annealing, annealing temperature is 1050℃.
[0046] 5. Cold rolling 1 is performed, the total deformation is 75%, and the target blank size after rolling is about 312 mm in diameter and about 23 mm in thickness. The vacuum annealing temperature is 1000°C.
[0047] 6. Cold rolling 2 is performed, the total deformation is 65%, and the thickness after rolling is about 8 mm. The final vacuum annealing temperature is 1000°C.
[0048] From the results of the comparison between Example 1 and Comparative Example 1, as shown in Table 1, the average grain size is less than 100 μm. The maximum {111} content of the sputtering surface of Example 1 is 32%, while the maximum {111} content of the sputtering surface of Comparative Example 1 is 89%. Figure 2 This is the longitudinal cross-sectional microstructure of Example 1. There is no {111} band at the 1 / 2 thickness position, and the {100} / {110} / {111} texture is evenly distributed in the thickness direction of the target blank. Figure 3The longitudinal section microstructure of comparative example 1 shows that a thicker (111) strip appears in comparative example 1, and the {100} / {110} / {111} texture distribution is uneven in the thickness direction of the target blank. Further, from the results of Examples 2-4, the average grain size is less than 90 μm, the maximum {111} content of the sputtering surface is about 40%, which is less than half of the comparative example, and the maximum {110} content of the sputtering surface is 10%, which is also less than half of the comparative example.
[0049] From the above, it can be seen that the Ta target material prepared by the method of the present invention has a more uniform orientation distribution and a corresponding better sputtering performance, which can meet the application requirements of high-end semiconductor integrated circuits.
[0050] Table 1 Comparison of target material preparation results between the embodiments of the present invention and the comparative examples
[0051] Grain size Maximum value of sputtering surface (111) Maximum value of sputtering surface (110) Example 1 88μm 32% 8% Example 2 79μm 40% 9% Example 3 85μm 42% 8% Example 4 87μm 39% 10% Comparative Example 1 96μm 89% 20%
Claims
1. A method for preparing a tantalum target blank, It is characterized in that The following steps are involved: 1) S1 provides high-purity tantalum ingots, S2 performs upsetting, and S3 performs cutting to obtain primary tantalum target blanks; 2) The primary tantalum target blank is subjected to S4 forging and drawing and S5 vacuum annealing to obtain an intermediate tantalum target blank; 3) performing S6 cold rolling 1, S7 vacuum annealing, S8 cold rolling 2, and S9 vacuum annealing on the intermediate tantalum target blank to obtain a final tantalum target blank; In the step 1), the deformation of the S2 upsetting is controlled at 40%-50%, In the step 1), the S3 cutting is to divide the ingot into two along a cross section perpendicular to the upsetting direction. In the step 2), the deformation of the S4 forging and drawing is controlled at 50%-70%; In the step 3), the total deformation of the S6 cold rolling is controlled at 70%-80%; In the step 3), the total deformation of the S8 cold rolling 2 is controlled at 65%-75%.
2. The method for preparing a tantalum target blank according to claim 1, It is characterized in that In the step 2), the S5 annealing is performed in a vacuum environment at a temperature of 1000°C-1100°C.
3. The method for preparing a tantalum target blank according to claim 1, It is characterized in that In the step 3), the S7 annealing is performed in a vacuum environment at a temperature of 950°C-1100°C.
4. The method for preparing a tantalum target blank according to claim 1, It is characterized in that In the step 3), the S9 annealing is performed in a vacuum environment at a temperature of 900°C-1100°C.